Positive electrode active material and secondary battery

By using Li2+xNi1-yA1yO2-zA2z cathode active material in lithium-ion batteries, the problem of low electrochemical activity of Li2NiO2 is solved by replacing nickel and oxygen atoms to form a microcrystalline structure and LiF surface coverage, achieving high capacity and capacity maintenance of secondary batteries.

CN112424976BActive Publication Date: 2024-10-29PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201980042648.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-02-21
Publication Date
2024-10-29
Estimated Expiration
2039-02-21

AI Technical Summary

Technical Problem

The low electrochemical activity of Li2NiO2 in lithium-ion batteries results in reduced charging capacity and becomes an obstacle to the realization of high-capacity lithium-ion batteries.

Method used

Li2+xNi1-yA1yO2-zA2z is used as the positive active material, where A1 contains Ga, Bi, Ba, Y, Sn, Ca, W and Ta, and A2 contains halogen and S. By replacing the nickel and oxygen atoms in Li2NiO2, it forms The microcrystalline structure increases the diffusion distance and reactive points of Li, combined with LiF surface coverage to protect the cathode material.

Benefits of technology

A high-capacity secondary battery has been realized, with an increased initial charge capacity, good capacity maintenance during repeated charge and discharge cycles, and reduced capacity reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112424976B_ABST
    Figure CN112424976B_ABST
Patent Text Reader

Abstract

Provided is a positive electrode active material comprising Li 2+x Ni 1‑ y A 1 y O 2‑z A 2 z A first lithium oxide that satisfies 0.5≤x≤0.3, 0≤y≤0.1, and 0≤z≤0.3, wherein at least one of y and z is not 0. 1 Contains at least one selected from the group consisting of Ga, Bi, Ba, Y, Sn, Ca, W and Ta. 2 At least one selected from the group consisting of halogen and S is contained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material for a secondary battery and a secondary battery. Background Art

[0002] As a positive electrode active material for lithium ion batteries having a large theoretical capacity, Li 2 NiO 2 (For example, refer to Patent Document 1). 2 NiO 2 1 mol of Ni contains 2 mol of Li. 2 NiO 2 When used as a positive electrode active material, its theoretical capacity is very large, about 550mA / g.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 3403568 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] However, for the use of Li 2 NiO 2 Lithium-ion batteries, due to Li 2 NiO 2 The low electrochemical activity leads to a decrease in charge capacity, thus becoming an obstacle to the realization of high-capacity lithium-ion batteries.

[0008] Solutions for solving problems

[0009] One aspect of the present invention relates to a positive electrode active material for a secondary battery, comprising a composition formula (1): Li 2+ x Ni 1-y A 1 y O 2-z A 2 z A first lithium oxide that satisfies -0.5≤x≤0.3, 0≤y≤0.1, and 0≤z≤0.3, at least one of y and z is not 0, A 1 Contains at least one selected from the group consisting of Ga, Bi, Ba, Y, Sn, Ca, W and Ta, A 2 At least one selected from the group consisting of halogen and S is contained.

[0010] Another aspect of the present invention relates to a secondary battery comprising: a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode includes the positive electrode active material according to the above aspect.

[0011] Effects of the Invention

[0012] By using the positive electrode active material of the present invention, a high-capacity secondary battery can be realized.

[0013] Although the novel features of the present invention are described in the appended claims, the present invention relates to both structural and content aspects, which will be better understood through the following detailed description taken in conjunction with other objects and features of the present invention and with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a partially cutaway perspective view of a secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION

[0015] The positive electrode active material according to the embodiment of the present invention is a positive electrode active material for a secondary battery, and includes Li 2+ x Ni 1-y A 1 y O 2-z A 2 z A represents a first lithium oxide that satisfies -0.5≤x≤0.3, 0≤y≤0.1, and 0≤z≤0.3. At least one of y and z is not 0. 1 Contains at least one selected from the group consisting of Ga, Bi, Ba, Y, Sn, Ca, W and Ta. 2 It contains at least one selected from the group consisting of halogen and S. As the halogen, F and Cl are preferred.

[0016] Li 2 NiO 2 It has a crystal structure belonging to the space group Immm. 2 NiO 2 In the graph, four oxygen atoms are coordinated in a plane around Ni to form a planar 4-coordinated NiO 4 Cluster. Adjacent NiO 4 The clusters are connected to each other on the same plane by sharing two O atoms, forming a NiO 2 The above NiO 2 The straight chains are stacked in parallel to each other to form a layered structure. Li exists in the NiO 2 More specifically, Li in NiO 2The side ends of the one-dimensional linear chain are coordinated with two oxygen atoms and are connected to the NiO atoms located above and below them. 2 Each oxygen atom of the one-dimensional straight chain is coordinated to form a tetrahedral coordination with the O atom.

[0017] The first lithium oxide is Li 2 NiO 2 As the base material, and with element A 1 Replacement of Li 2 NiO 2 A portion of the nickel atoms in the 2 Replacement of Li 2 NiO 2 Therefore, when the first lithium oxide is used as the positive electrode active material, the initial charge capacity increases.

[0018] By using element A 1 Replacement of Li 2 NiO 2 Ni site or element A 2 The O site is replaced, and strain is generated starting from the replacement element. This strain hinders crystal growth, so the crystallite becomes smaller. As the crystallite shrinks, the diffusion distance of Li becomes shorter, the active points of the reaction increase, and the charge capacity increases.

[0019] LiF may also be included in the positive electrode material. LiF can cover the surface of the first lithium oxide as the positive electrode active material. Thus, the first lithium oxide can be protected from reaction with the electrolyte component and the side reaction of the first lithium oxide with the electrolyte component can be suppressed. In this case, it is preferred that LiF is biased on the surface of the first lithium oxide.

[0020] The first lithium oxide can be prepared by mixing, for example, lithium oxide (Li 2 O), nickel(II) oxide (NiO), and nickel(II) oxide containing element A 1 and / or element A 2 The first lithium oxide contains fluorine as the element A. 2 In the case of calcination, LiF may be added and calcined. In this case, depending on the calcination conditions and the amount of LiF added, LiF may not be dissolved in the LiF. 2 NiO 2 The fluorine in the first lithium oxide will precipitate in the form of LiF. In this case, LiF can be formed in a manner that covers the crystal surface of the first lithium oxide. Preferably, the LiF is contained in a ratio of 10% or less, and more preferably, the LiF is contained in a ratio of 6% or less. The ratio of LiF refers to the ratio of the first lithium oxide Li 2+x Ni 1-y A 1y O 2-z A 2 z Ni and element A contained in 1 When the total number of atoms of LiF is Nx and the number of F atoms contained in LiF is Ny, R=Ny / (Nx+Ny).

[0021] The first lithium oxide can be used in a mixture with other positive electrode active materials that can release lithium ions. Examples of other positive electrode active materials include Li a M 1 O 2 A second lithium oxide that represents and satisfies 0.95≤a≤1.2. 1 At least one selected from the group consisting of Ni, Mn and Co is contained.

[0022] The second lithium oxide has a small irreversible capacity and is excellent in initial efficiency. By using the first and second lithium oxides in combination, a positive electrode material can be obtained that has a high initial capacity and can maintain a high capacity even after repeated charge and discharge cycles.

[0023] The second lithium oxide is preferably made of Li a Ni b Co c M 2 1-b-c O 2 M represents a substance that satisfies 0.95≤a≤1.2, 0.3≤b≤0.95, 0<c≤0.5 and b+c<1. 2 The second lithium oxide contains at least one selected from the group consisting of Mn and Al. The second lithium oxide has an operating voltage close to that of the first lithium oxide, and is therefore suitable for being mixed with the first lithium oxide to form a positive electrode active material. The second lithium oxide is not limited to one type, and the active material may contain multiple types.

[0024] When the positive electrode active material includes the second lithium oxide, the ratio of the first lithium oxide to the total positive electrode active material can be 1 to 20 mass %. By mixing the first lithium oxide and the second lithium oxide within this range, the initial capacity of the total positive electrode active material is improved, and the capacity reduction caused by repeated charge and discharge cycles is suppressed.

[0025] The negative electrode active material may use materials used in conventional lithium-ion secondary batteries. In particular, the negative electrode active material preferably includes an alloy material containing at least one element selected from the group consisting of Si, Sn, Ga, or In. Examples of alloy materials containing Si include silicon alone, silicon alloys, and silicon compounds. Examples of alloy materials containing Sn include tin alone, tin alloys, and tin compounds. Examples of alloy materials containing Ga or In include Ga alloys and In alloys. Examples of silicon compounds and tin compounds include oxides and / or nitrides, respectively. Among the alloy materials containing Si, SiO x (0.5≤x<2.0), lithium silicate composite particles. Among them, SiO x Is SiO 2 The lithium silicate composite particles are composed of a lithium silicate phase (Li 2x SiO 2+x (0<x<2)) Composite particles with tiny silicon dispersed therein.

[0026] These alloy materials have low initial efficiency, are irreversibly captured in the initial charge, and have a large number of lithium ions that do not contribute to capacity in the subsequent charge and discharge. However, in the case where the positive electrode active material includes the first lithium oxide, the irreversible capacity of the negative electrode can be offset by the irreversible capacity of the positive electrode. That is, the lithium ions irreversibly consumed in the negative electrode can be provided by the lithium ions irreversibly released by the first lithium oxide. Thus, a secondary battery in which the capacity reduction is suppressed in the charge and discharge cycle after the initial charge and discharge can be obtained.

[0027] A portion of the positive electrode material may also have a Li 1+x Ni 1-y A 1 y O 2-z A 2 z The amorphous material is mainly composed of Li ions. During the initial charge, lithium ions are extracted from the first lithium oxide, and the amorphous material derived from the first lithium oxide can be introduced into the positive electrode material. The amorphous material can be Li 1+x Ni 1-y A 1 y O 2-z A 2 z In addition, the amorphous material has low reactivity, and the amorphous surface can inhibit the decomposition of the electrolyte and the generation of gas.

[0028] By Li 1+x Ni 1-y A 1 y O 2-zA 2 z The amorphous phase as the main component means that, for example, the half-peak width w of the diffraction line corresponding to the (101) plane of the first lithium oxide measured by X-ray diffraction is w>0.5°. From the viewpoint of enhancing the inhibitory effect of electrolyte decomposition caused by the amorphous phase, w>1.5° is preferred.

[0029] Moreover, in the positive electrode active material mixed with the first and second lithium oxides, when the half-peak width of the diffraction line corresponding to the (101) plane of the first lithium oxide obtained by X-ray diffraction measurement is 7 times or more of the half-peak width of the strongest diffraction line of the second lithium oxide, it can be said that a part of the positive electrode material has Li 1+x Ni 1-y A 1 y O 2-z A 2 z From the viewpoint of enhancing the inhibitory effect of electrolyte decomposition and the like due to the amorphous phase, the half-peak width of the first lithium oxide is preferably 10 times or more the half-peak width of the strongest diffraction line of the second lithium oxide.

[0030] In the present invention, the X-ray diffraction measurement method and the analysis conditions of the obtained data are as follows, for example.

[0031] Measurement device: MiniFlex, a tabletop X-ray diffraction device manufactured by Rigaku Corporation

[0032] Analysis software: Rigaku Corporation, comprehensive powder X-ray analysis software PDXL

[0033] Measurement conditions: 10°~80°

[0034] For cathode: Cu-Kα

[0035] Tube voltage: 40kV

[0036] Tube current: 10mA

[0037] Counting time: 0.5 seconds

[0038] Divergence slit: 1.25°

[0039] Scattering slit: 8.0mm

[0040] Light receiving slit: 13.0mm

[0041] The diffraction line of the (101) plane of the first lithium oxide (2θ=25 to 26°) and the strongest diffraction line of the second lithium oxide were used.

[0042] Figure 1 It is a perspective view schematically showing a secondary battery according to one embodiment of the present invention. Figure 1 In FIG. 1 , a part of the main part of the secondary battery 1 is cut away to show the structure of the main part.

[0043] The secondary battery 1 includes a positive electrode, a negative electrode including a negative electrode material, and an electrolyte. The positive electrode includes the positive electrode material including the first lithium oxide.

[0044] Figure 1 In the example of , the positive electrode and the negative electrode are wound with a separator sandwiched therebetween to form a flat wound electrode group 10. The electrode group 10 is housed in a square battery case 11 together with an electrolyte (not shown), thereby realizing a square wound battery. However, in the present invention, there is no particular limitation on the type, shape, etc. of the secondary battery.

[0045] One end of a positive lead 14 is connected to the positive current collector of the positive electrode included in the electrode group 10. The other end of the positive lead 14 is connected to a sealing plate 12 that functions as a positive terminal. One end of a negative lead 15 is connected to the negative current collector, and the other end of the negative lead 15 is connected to a negative terminal 13 disposed approximately in the center of the sealing plate 12. A gasket 16 is disposed between the sealing plate 12 and the negative terminal 13 to insulate the two. A frame 18 formed of an insulating material is disposed between the sealing plate 12 and the electrode group 10 to insulate the negative lead 15 from the sealing plate 12. The sealing plate 12 is joined to the open end of the square battery case 11 to seal the square battery case 11. An injection hole 17a is formed on the sealing plate 12, and the electrolyte is injected into the square battery case 11 from the injection hole 17a. Then, the injection hole 17a is sealed by a sealing plug 17.

[0046] (positive electrode)

[0047] The positive electrode comprises a positive electrode collector and a positive electrode material layer disposed on the surface of the positive electrode collector. The positive electrode collector may be a sheet-shaped positive electrode collector. The positive electrode material layer contains a positive electrode active material. The positive electrode material layer may be formed on one surface of the sheet-shaped positive electrode collector or on both surfaces.

[0048] (Positive electrode collector)

[0049] Examples of the positive electrode current collector include metal foil and metal sheet. Materials for the positive electrode current collector include stainless steel, aluminum, aluminum alloy, titanium, etc. The thickness of the positive electrode current collector can be selected from a range of 3 to 50 μm, for example.

[0050] (Positive electrode material layer)

[0051] The case where the positive electrode material layer is a mixture (composite material) containing positive electrode active material particles is described. The positive electrode material layer may contain a positive electrode active material and a binder as essential components, and a conductive agent as an optional component. The amount of binder contained in the positive electrode material layer is preferably 0.1 to 20 parts by mass, more preferably 1 to 5 parts by mass relative to 100 parts by mass of the positive electrode active material. The thickness of the positive electrode material layer is, for example, 10 to 100 μm.

[0052] The positive electrode active material comprises the above-mentioned first lithium oxide. Other known positive electrode active materials having the function of absorbing and releasing lithium ions may also be used in combination with the first lithium oxide. As examples of such positive electrode active materials, although not limited, lithium-containing transition metal oxides are preferred. As transition metal elements, Sc, Y, Mn, Fe, Co, Ni, Cu, Cr, Zr, W, etc. may be cited. Among these, Ni, Co, Mn, Fe, Cu, Cr are preferred, and Mn, Co, Ni are more preferred. For lithium-containing transition metal oxides, lithium nickel composite oxides containing Li, Ni and other metals are preferred in terms of obtaining high capacity.

[0053] The lithium-containing transition metal oxide may contain one or more typical metal elements as required. Typical metal elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, Bi, etc. Typical metal elements may also be Al, etc.

[0054] There is no particular restriction on the crystal structure of the lithium-containing transition metal oxide, and a crystal structure belonging to the space group R-3m can be used. Since the lattice expansion and contraction of this positive electrode active material accompanying charging and discharging is small, it is not easy to deteriorate even when a non-aqueous electrolyte is used, and excellent cycle characteristics are easily obtained. The positive electrode active material belonging to the space group R-3m can be, for example, the above-mentioned second lithium oxide, that is, a positive electrode active material containing Ni, Co, and Mn and / or Al. In this positive electrode active material, the ratio of Ni to the sum of the number of atoms of Ni, Co, Mn and Al can be 50 atomic % or more. For example, in the case where the positive electrode active material contains Ni, Co and Al, the ratio of Ni can be 50 atomic % or more, or it can be 80 atomic % or more. In the case where the positive electrode active material contains Ni, Co and Mn, the ratio of Ni can also be 50 atomic % or more.

[0055] For the lithium-containing transition metal oxide (second lithium oxide) used in combination with the first lithium oxide, it is more preferable that Ni is present in the M 1 The ratio b of M satisfies 0.85≤b≤1. In addition, from the viewpoint of the stability of the crystal structure, it is preferable to contain Ni, Co and Al as M 1 Li a Nib Co c Al d O 2 (0.95≤a≤1.2, 0.85≤b<1, 0<c<0.15, 0<d≤0.1, b+c+d=1).

[0056] Specific examples of lithium-containing transition metal oxides (second lithium oxides) include lithium-nickel-cobalt-manganese composite oxides (LiNi 0.5 Co 0.2 Mn 0.3 O 2 、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 、LiNi 0.4 Co 0.2 Mn 0.4 O 2 etc.), lithium-nickel-cobalt composite oxide (LiNi 0.8 Co 0.2 O 2 etc.), lithium-nickel-cobalt-aluminum composite oxide (LiNi 0.8 Co 0.15 Al 0.05 O 2 、LiNi 0.8 Co 0.18 Al 0.02 O 2 、LiNi 0.88 Co 0.09 Al 0.03 O 2 )wait.

[0057] When the positive electrode active material includes the first lithium oxide and the second lithium oxide, the content ratio of the first lithium oxide with respect to the entire positive electrode active material is, for example, 1 to 20% by mass.

[0058] From the viewpoint of improving the filling property of the positive electrode active material in the positive electrode material layer, it is desired that the average particle size (D50) of the positive electrode active material particles is sufficiently small relative to the thickness of the positive electrode material layer. The average particle size (D50) of the positive electrode active material particles is, for example, preferably 5 to 30 μm, more preferably 10 to 25 μm. It should be noted that the average particle size (D50) refers to the median particle size when the cumulative volume in the volume-based particle size distribution is 50%. The average particle size is measured, for example, using a laser diffraction / scattering particle size distribution measuring device.

[0059] Examples of binders include fluororesins such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), and tetrafluoroethylene-hexafluoropropylene copolymer (HFP); acrylic resins such as polymethyl acrylate and ethylene-methyl methacrylate copolymer; rubber-like materials such as styrene-butadiene rubber (SBR) and acrylic rubber; and water-soluble polymers such as carboxymethyl cellulose (CMC) and polyvinyl pyrrolidone.

[0060] As the conductive agent, carbon black such as acetylene black and Ketjen black is preferred.

[0061] The positive electrode material layer can be formed by mixing positive electrode active material particles, a binder, etc. with a dispersion medium to prepare a positive electrode slurry, applying the positive electrode slurry to the surface of the positive electrode collector, and rolling after drying. As a dispersion medium, water; alcohols such as ethanol; ethers such as tetrahydrofuran; N-methyl-2-pyrrolidone (NMP) and the like are used. When water is used as a dispersion medium, it is preferred to use a rubber-like material and a water-soluble polymer as a binder.

[0062] (negative electrode)

[0063] The negative electrode comprises a negative electrode current collector and a negative electrode material layer disposed on the surface of the negative electrode current collector. The negative electrode current collector may be a sheet-shaped current collector. The negative electrode material layer contains a negative electrode active material. The negative electrode material layer may be formed on one surface of the sheet-shaped negative electrode current collector or on both surfaces.

[0064] (Negative electrode current collector)

[0065] Examples of the negative electrode current collector include metal foil, metal sheet, mesh, punched sheet, expanded metal, etc. The negative electrode current collector may be made of stainless steel, nickel, copper, copper alloy, etc. The thickness of the negative electrode current collector may be selected from the range of 3 to 50 μm, for example.

[0066] (Negative electrode material layer)

[0067] The negative electrode material layer can be formed using a negative electrode slurry containing a negative electrode active material, a binder (binding agent) and a dispersion medium according to the method for manufacturing the positive electrode material layer. The negative electrode material layer may also contain optional components such as a conductive agent as needed. The amount of binder contained in the negative electrode material layer is preferably 0.1 to 20 parts by mass, more preferably 1 to 5 parts by mass relative to 100 parts by mass of the negative electrode material layer. The thickness of the negative electrode material layer is, for example, 10 to 100 μm.

[0068] The negative electrode active material may be a non-carbon material, a carbon material, or a combination thereof. The carbon material used as the negative electrode active material is not particularly limited, but is preferably at least one selected from the group consisting of graphite and hard carbon. Among them, graphite has a high capacity and a small irreversible capacity, and is more preferred.

[0069] Graphite is a general term for carbon materials with a graphite structure, including natural graphite, artificial graphite, expanded graphite, graphitized mesophase carbon particles, etc. Examples of natural graphite include flaky graphite and earthy graphite. Generally, the interplanar spacing d of the 002 plane of the graphite structure calculated from the X-ray diffraction spectrum is 002 Carbon materials with a 0.02-0.10 angstrom spacing d are classified as graphite. On the other hand, hard carbon is a carbon material in which minute graphite crystals are arranged in random directions and graphitization is almost non-existent. 002 Greater than 3.44 angstroms.

[0070] As the non-carbon material used as the negative electrode active material, an alloy material is preferred. The alloy material preferably includes any one selected from silicon, tin, Ga, and In, and silicon alone and silicon compounds are preferred. Silicon compounds include silicon oxides and silicon alloys.

[0071] As the negative electrode active material, metallic lithium or a lithium alloy may be used.

[0072] (Separator)

[0073] As the separator, a microporous film, nonwoven fabric, woven fabric, etc. made of resin can be used. As the resin, polyolefins such as polyethylene (PE) and polypropylene (PP), polyamide, polyamide-imide, etc. can be used.

[0074] (Electrolytes)

[0075] The electrolyte includes a solvent and a solute dissolved in the solvent. Various lithium salts can be used as the solute. The concentration of the lithium salt in the electrolyte is, for example, 0.5 to 2 mol / L. The electrolyte may also contain a known additive.

[0076] Examples of the solvent include non-aqueous solvents such as cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, and water.

[0077] As cyclic carbonate, ethylene carbonate (EC), fluoroethylene carbonate (FEC), propylene carbonate (PC), butylene carbonate, vinylene carbonate, vinyl ethylene carbonate and their derivatives etc. can be used.They can be used alone, and more than 2 kinds can be used in combination.From the viewpoint of the ionic conductivity of electrolyte, preferably use at least one selected from the group consisting of ethylene carbonate, fluoroethylene carbonate, propylene carbonate.

[0078] Examples of the chain carbonate include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).

[0079] Examples of the cyclic carboxylic acid ester include γ-butyrolactone (GBL) and γ-valerolactone (GVL).

[0080] As the chain carboxylic acid ester, methyl acetate (MA), ethyl acetate (EA), propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and the like can be used.

[0081] These solvents may be used alone or in combination of two or more.

[0082] As lithium salt, LiPF 6 , LiBF 4 、LiClO 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(SO 2 F) 2 、LiN(SO 2 CF 3 ) 2 The lithium salt may be used alone or in combination of two or more.

[0083] [Example]

[0084] Hereinafter, the positive electrode material and the secondary battery of the present invention will be specifically described based on Examples and Comparative Examples, but the positive electrode material and the secondary battery of the present invention are not limited to the following Examples.

[0085] 《Example 1》

[0086] A secondary battery for positive electrode evaluation using metal Li as a counter electrode was produced according to the following procedure.

[0087] (1) Synthesis of the first lithium oxide

[0088] Lithium oxide (Li 2 O), nickel(II) oxide (NiO), and gallium trioxide (Ga 2 O 3 ) were mixed in a predetermined molar ratio and pulverized by a ball mill in an Ar atmosphere. The pulverized product was calcined in an Ar atmosphere at 650° C. to obtain a first lithium oxide (Li 2 Ni 0.97 Ga 0.03 O 2 ).

[0089] (2) Preparation of positive electrode

[0090] The first lithium oxide, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder are mixed at a mass ratio of the first lithium oxide: AB: PVdF = 100: 1: 0.9, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) is added and stirred to prepare a positive electrode slurry. Then, the obtained positive electrode slurry is applied to one side of an aluminum foil (positive electrode collector) and dried, and the coating film of the positive electrode material layer is rolled using a roller.

[0091] The obtained laminate of the positive electrode current collector and the positive electrode material layer is cut into an electrode size to produce a positive electrode including the positive electrode material layer on one surface of the positive electrode current collector.

[0092] (3) Preparation of electrolyte

[0093] 1 part by mass of vinylene carbonate was added to 100 parts by mass of a mixed solution containing EC and EMC at a mass ratio of 1:3 to obtain a non-aqueous solvent. 6 The non-aqueous electrolyte was prepared by dissolving it in a non-aqueous solvent at a concentration of 1.0 mol / L.

[0094] (4) Battery production

[0095] Lead wires were installed on the positive electrode and the Li metal counter electrode obtained above. The positive electrode and the Li metal counter electrode were made to face each other with a separator of 0.015 mm thick made of PP and PE sandwiched between them. The electrode body was sealed in an outer body made of aluminum laminate film together with a non-aqueous electrolyte to make a secondary battery A1.

[0096] (5) Evaluation

[0097] Charge at a constant current of 0.05C until the closed-circuit voltage of the battery reaches 4.3V (based on the Li counter electrode), then charge at a constant voltage of 4.3V until the current value is lower than 0.02C. Calculate the initial charge capacity C of the battery. 1 .

[0098] After that, discharge at a constant current of 0.05C until the closed circuit voltage of the battery reaches 2.5V (based on the Li counter electrode), and calculate the discharge capacity C 2 . 2 / C 1 The initial efficiency was evaluated. Note that the charge and discharge were performed in an environment of 25°C.

[0099] 《Example 2》

[0100] Lithium oxide (Li 2O), nickel (II) oxide (NiO) and lithium fluoride (LiF) were mixed in a predetermined molar ratio such that the number of F atoms contained in lithium fluoride was 0.1 equivalent when the number of Li atoms contained in lithium oxide was 2 equivalents, and the mixture was pulverized by a ball mill in an Ar atmosphere. The pulverized mixture was calcined in an Ar atmosphere at 650° C. to obtain a first lithium oxide (LiF) containing F. 2 NiO 1.9 F 0.1 ).

[0101] The surface composition of the obtained first lithium oxide was investigated by X-ray photoelectron spectroscopy (XPS), and as a result, the F / Ni ratio was 0.67.

[0102] A secondary battery A2 was produced in the same manner as in Example 1 except for the above.

[0103] 《Example 3》

[0104] In Example 2, the blending amount of lithium fluoride was doubled that of Example 2, and a first lithium oxide containing F was synthesized.

[0105] A secondary battery A3 was produced in the same manner as in Example 1 except for the above.

[0106] 《Example 4》

[0107] In Example 2, the blending amount of lithium fluoride was 3 times that of Example 2, and the first lithium oxide containing F was synthesized.

[0108] A secondary battery A4 was produced in the same manner as in Example 1 except for the above.

[0109] 《Example 5》

[0110] In Example 1, Bi 2 O 3 Instead of gallium trioxide, the first lithium oxide containing Bi (Li 2 Ni 0.97 Bi 0.03 O 2 ).

[0111] A secondary battery A5 was produced in the same manner as in Example 1 except for the above.

[0112] Example 6

[0113] In Example 1, Y 2 O 3 Instead of gallium trioxide, the first lithium oxide containing Y (Li 2 Ni 0.97 Y 0.03 O 2 ).

[0114] A secondary battery A6 was produced in the same manner as in Example 1 except for the above.

[0115] Example 7

[0116] In Example 1, CaO was used instead of gallium trioxide to synthesize the first lithium oxide containing Ca (Li 2 Ni 0.97 Ca 0.03 O 2 ).

[0117] A secondary battery A7 was produced in the same manner as in Example 1 except for the above.

[0118] 《Example 8》

[0119] The first lithium oxide (Li 2 NiO 1.9 F 0.1 ) and LiNi as the second lithium oxide 0.82 Co 0.15 Al 0.03 O 2 The mixture was prepared by mixing so that the ratio of the first lithium oxide to the total of the first and second lithium oxides was 20 mass %.

[0120] The mixture was mixed with acetylene black (AB) as a conductive material and polyvinylidene fluoride (PVdF) as a binder to prepare a positive electrode slurry, and a positive electrode was manufactured in the same manner as in Example 1.

[0121] A secondary battery A8 was produced in the same manner as in Example 1 except for the above.

[0122] Comparative Example 1

[0123] Lithium oxide (Li 2 O) and nickel (II) oxide (NiO) were mixed at a predetermined molar ratio and pulverized using a ball mill in an Ar atmosphere. The pulverized product was calcined in an Ar atmosphere at 650°C to synthesize Li 2 NiO 2 .

[0124] A secondary battery B1 was produced in the same manner as in Example 1 except for the above.

[0125] Comparative Example 2

[0126] As the second lithium oxide LiNi 0.82 Co 0.15 Al 0.03 O 2, acetylene black (AB) as a conductive material and polyvinylidene fluoride (PVdF) as a binder are mixed in a mass ratio of the second lithium oxide:AB:PVdF=100:1:0.9, and further an appropriate amount of N-methyl-2-pyrrolidone (NMP) is added and stirred to prepare a positive electrode slurry, and a positive electrode is made using the same method as in Example 1.

[0127] A secondary battery B2 was produced in the same manner as in Example 1 except for the above.

[0128] 《Comparative Example 3》

[0129] The Li obtained in Comparative Example 1 2 NiO 2 and LiNi as the second lithium oxide 0.82 Co 0.15 Al 0.03 O 2 The mixture was prepared by mixing so that the ratio of the first lithium oxide to the total of the first and second lithium oxides was 20 mass %.

[0130] A secondary battery B3 was produced in the same manner as in Example 8 except for the above.

[0131] For Examples 1, 2 and Comparative Example 1, the initial charge capacity C 1 , discharge capacity C 2 The evaluation results of the initial efficiency are shown in Table 1.

[0132] [Table 1]

[0133]

[0134] With the use of Li 2 NiO 2 Compared with the secondary battery B1, which uses Li as the positive electrode material 2 Ni 0.97 Ga 0.03 O 2 Secondary battery A1 and Li 2 NiO 1.9 F 0.1 The initial charge capacity of the secondary battery A2 as the positive electrode material was greatly improved. The initial discharge capacity and initial efficiency of the secondary batteries A1 and A2 were improved compared with the secondary battery B1.

[0135] In addition, the first lithium oxide used in Examples 2 to 4 was measured by X-ray diffraction, and diffraction lines of LiF were observed. The results of analyzing the diffraction intensity showed that the LiF ratio R was less than 1% in Examples 2 and 3, and 5% in Example 4.

[0136] The first lithium oxide used in Examples 1, 2, and 5 to 7 and the Li used in Comparative Example 1 2 NiO 2 X-ray diffraction measurement was performed, and the crystallite size calculated based on the diffraction line of the (101) plane corresponding to the space group Immm is shown in Table 2. As shown in Table 2, it can be seen that by using element A 1 Replacement of Li 2 NiO 2 Ni sites, and / or with element A 2 Replacement of Li 2 NiO 2 O sites, which can make the crystallite size smaller than Li 2 NiO 2 .

[0137] [Table 2]

[0138]

[0139] Regarding Example 8 and Comparative Examples 2 and 3, the initial charge capacity C 1 The evaluation results of the capacity retention rate of the second cycle are shown in Table 3. The capacity retention rate of the second cycle is the discharge capacity of the second cycle relative to the initial discharge capacity C 1 It should be noted that the charge and discharge conditions of the second cycle are the same as those for calculating the initial charge capacity C 1 and discharge capacity C 2 The charging and discharging conditions are the same.

[0140] [Table 3]

[0141]

[0142] Compared with the secondary battery B2, the secondary batteries A8 and B3 can confirm the increase of the charging capacity. On the other hand, the capacity retention rate of the second cycle is compared. The secondary battery B3 is reduced compared with B2, but A8 maintains the same value as B2. The initial charging capacity of the secondary battery A8 is improved compared with the secondary battery B2, and the second cycle capacity retention rate is improved compared with the secondary battery B3.

[0143] For Example 8, the results of X-ray diffraction measurement of the positive electrode active material obtained by disassembling the secondary battery A8 after charging and discharging obtained diffraction lines corresponding to a mixture of the first lithium oxide and the second lithium oxide, and the half-peak width of the diffraction line corresponding to the (101) plane of the first lithium oxide was 12.3 times the half-peak width of the strongest diffraction line of the second lithium oxide.

[0144] The present invention has been described with respect to the preferred embodiments at this stage, but these disclosures are not to be construed as limiting. Various modifications and changes should be apparent to those skilled in the art of the present invention upon reading the above disclosures. Therefore, it should be construed that the scope of the appended claims includes all modifications and changes without departing from the true spirit and scope of the present invention.

[0145] Industrial Applicability

[0146] The positive electrode of the present invention is useful as a positive electrode of a secondary battery used in a driving power source for personal computers, mobile phones, mobile devices, portable information terminals (PDAs), portable game consoles, cameras, etc., a main power source or auxiliary power source for driving a motor in a hybrid vehicle, plug-in HEV, etc., a driving power source for electric tools, vacuum cleaners, robots, etc.

[0147] Description of Reference Numerals

[0148] 1: secondary battery, 10: wound electrode group, 11: square battery case, 12: sealing plate, 13: negative terminal, 14: positive electrode lead, 15: negative electrode lead, 16: gasket, 17: sealing plug, 17a: injection hole, 18: frame

Claims

1. A positive electrode active material, which is a positive electrode active material for a secondary battery, comprising a composition formula (1): Li 2+ x Ni 1-y A 1 y O 2-z A 2 z A first lithium oxide is represented and satisfies -0.5≤x≤0.3, 0≤y≤0.1 and 0≤z≤0.3, At least one of y and z is not 0, A 1 contains at least one selected from the group consisting of Bi, Ba, Y, Sn, Ca, W and Ta, A 2 At least one selected from the group consisting of halogen and S is contained.

2. The positive electrode active material according to claim 1, wherein The A 2 At least F. The positive electrode active material according to claim 2 , further comprising LiF.

4. The positive electrode active material according to claim 3, wherein The LiF covers the surface of the first lithium oxide.

5. The positive electrode active material according to claim 1 or 2, wherein The first lithium oxide has a composition formula (2): Li a M 1 O2 represents a second lithium oxide mixture satisfying 0.95≤a≤1.2, M 1 At least one selected from the group consisting of Ni, Mn and Co is contained.

6. The positive electrode active material according to claim 5, wherein The second lithium oxide has a composition formula (2a): Li a Ni b Co c M 2 1-b-c O2 represents and satisfies 0.95≤a≤1.2, 0.3≤b≤0.95, 0<c≤0.5 and b+c<1, M 2 At least one selected from the group consisting of Mn and Al is contained.

7. The positive electrode active material according to claim 6, wherein The ratio of the first lithium oxide to the entire positive electrode active material is 1 to 20% by mass.

8. A secondary battery comprising: a positive electrode, a negative electrode and an electrolyte, The positive electrode includes the positive electrode active material according to any one of claims 1 to 7.

9. The secondary battery according to claim 8, wherein The negative electrode comprises a negative electrode active material, The negative electrode active material includes an alloy material containing at least one element selected from the group consisting of Si, Sn, Ga, and In.

10. The secondary battery according to claim 8 or 9, wherein The positive electrode comprises Li 1+x Ni 1-y A 1 y O 2-z A 2 z The main component is amorphous.

Citation Information

Patent Citations

  • Lithium ion secondary battery, positive electrode active material, positive electrode, and electrical tool

    CN102569878A

  • Positive electrode active material and battery

    CN107431201A

  • Manufacturing method of positive active material for lithium rechargeable batteries and positive active material made by the same

    KR1020150079362A