Fuel cell electrode catalyst layer and solid polymer fuel cell using the same

By using conductive inorganic oxide carriers and conductive hydrophilic materials in the catalyst layer of the fuel cell to construct appropriate water drainage channels, the problem of overflow phenomenon at high current density is solved and the stability of the fuel cell voltage is achieved. .

CN112424978BActive Publication Date: 2024-10-15MITSUI MINING & SMELTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980046914.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-08-09
Filing Date
2019-06-04
Publication Date
2024-10-15
Estimated Expiration
2039-06-04

AI Technical Summary

Technical Problem

Under high current densities, the catalyst layer of polymer electrolyte fuel cells is prone to overflow, resulting in a reduction in battery voltage. It is difficult for existing hydrophobic materials to effectively ensure water drainage channels.

Method used

Conductive inorganic oxides are used as carriers to support catalysts, and conductive hydrophilic materials are added to the catalyst layer to control their content and particle size to build appropriate water drainage channels and prevent overflow.

Benefits of technology

It effectively prevents the reduction of battery voltage and ensures stable operation of the fuel cell under high current density conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002895220770000101
    Figure BDA0002895220770000101
Patent Text Reader

Abstract

The subject of the present invention is to provide an electrode catalyst layer for a fuel cell that can effectively prevent the cell voltage from decreasing in a high current density region. The electrode catalyst layer for a fuel cell of the present invention comprises: a catalyst-loaded carrier in which a catalyst is loaded on a carrier formed of a conductive inorganic oxide; and a hydrophilic material. The hydrophilic material is an aggregate of hydrophilic particles having conductivity. The content of the hydrophilic material in the catalyst layer is 2% by mass or more and less than 20% by mass relative to the total of the carrier and the hydrophilic material. The ratio of the particle size d1 of the hydrophilic particles to the particle size D of the catalyst-loaded carrier is 0.5 or more and 3.0 or less. The ratio of the particle size d2 of the hydrophilic material to the thickness T of the catalyst layer is 0.1 or more and 1.2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrode catalyst layer for a fuel cell and a solid polymer fuel cell using the same. Background Art

[0002] The solid polymer fuel cell has the following structure: a catalyst layer is arranged on each surface of the solid polymer electrolyte membrane, and a gas diffusion layer is arranged outside the catalyst layer. The catalyst layer is generally a porous layer composed of a catalyst-loaded carrier formed by loading a precious metal catalyst on the surface of the carrier particles. In the porous layer, fuel gas such as hydrogen and methanol, or oxidants such as oxygen and air flow, and an electrode reaction occurs at the three-phase interface. As a result of the reaction, water is generated in the catalyst layer.

[0003] The generated water escapes from the catalyst layer. However, water sometimes accumulates in the catalyst layer. If this accumulates, the catalyst layer can no longer fully accommodate the water, and the so-called overflow phenomenon occurs. In particular, when a conductive metal oxide is used as a catalyst carrier, the overflow phenomenon is prone to occur because its surface is relatively hydrophilic. It is believed that the overflow phenomenon is one of the causes of the reduction in battery voltage.

[0004] Patent Document 1 proposes a catalyst-supported powder obtained by adsorbing a hydrophobic surface protection substance on the surface of a catalyst support formed of an inorganic material such as a metal oxide, and then supporting a catalyst substance, in order to prevent water wetting of a catalyst support powder. In addition, Patent Document 2 proposes the use of a catalyst layer, the catalyst layer comprising: a catalyst-supported support in which a catalyst is supported on a support formed of an inorganic oxide; and a highly hydrophobic substance having a higher hydrophobicity than the inorganic oxide.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-099486

[0008] Patent Document 2: US2017 / 141407A1 Summary of the invention

[0009] Even when a hydrophobic material is used as in Patent Documents 1 and 2, especially when the fuel cell is operated at a high current density, since a large amount of water is generated, it is sometimes difficult to fully ensure a channel for discharging the generated water (hereinafter also referred to as a "discharge passage") within the catalyst layer, and there is a problem of overflow.

[0010] Therefore, an object of the present invention is to provide an electrode catalyst layer for a fuel cell which can effectively prevent a decrease in cell voltage by preventing the occurrence of a flooding phenomenon.

[0011] The present invention provides an electrode catalyst layer for a fuel cell, which comprises: a catalyst-loaded carrier in which a catalyst is loaded on a carrier formed of a conductive inorganic oxide; and a hydrophilic material, wherein the hydrophilic material is an aggregate of hydrophilic particles having conductivity, the content of the hydrophilic material in the catalyst layer is greater than 2% by mass and less than 20% by mass relative to the total of the carrier and the hydrophilic material, the ratio of the particle size d1 of the hydrophilic particles to the particle size D of the catalyst-loaded carrier is greater than 0.5 and less than 3.0, and the ratio of the particle size d2 of the hydrophilic material to the thickness T of the catalyst layer is greater than 0.1 and less than 1.2. DETAILED DESCRIPTION

[0012] The fuel cell electrode catalyst layer of the present invention comprises a catalyst-loaded carrier in which a catalyst is loaded on a carrier. The carrier is formed by inorganic oxide particles. As the inorganic oxide, for example, metal oxides, non-metallic oxides or semi-metallic oxides can be used. From the viewpoint of improving the conductivity of the catalyst layer, it is advantageous for the inorganic oxide to have conductivity. The inorganic oxide preferably has a volume resistivity of, for example, 100 kΩcm or less. The volume resistivity is measured using, for example, a pressed powder resistance measurement system (Mitsubishi Chemical Analysis Company PD-51) and a resistivity meter (Mitsubishi Chemical Analysis Company MCP-T610). Specifically, 1 g of the sample is put into the probe cylinder, and the probe unit is set in PD-51. A cylindrical pellet with a diameter of 20 mm is made by applying a load of 57.3 MPa using a hydraulic jack. The resistance value of the obtained pellet is measured by using MCP-T610.

[0013] As examples of inorganic oxides, one or more selected from indium oxides, tin oxides, titanium oxides, zirconium oxides, selenium oxides, tungsten oxides, zinc oxides, vanadium oxides, tantalum oxides, niobium oxides and rhenium oxides can be cited. As more preferred inorganic oxides, for example, products obtained by containing one or more elements of indium, niobium, tantalum, antimony and tungsten in tin oxide can be cited. In addition, products obtained by containing fluorine in tin oxide can be cited. Specifically, tin oxides containing (doped) metals or non-metals such as tin oxides containing indium, tin oxides containing antimony, tin oxides containing fluorine, tin oxides containing fluorine tungsten, tin oxides containing tantalum, tin oxides containing tantalum antimony, tin oxides containing tungsten and tin oxides containing niobium can be cited.

[0014] From the aspect of increasing the specific surface area of ​​the carrier, the particle size of the inorganic oxide is preferably 10 nm or more and 100 nm or less, particularly preferably 10 nm or more and 50 nm or less, and particularly preferably 20 nm or more and 50 nm or less. The particle size D of the catalyst-supported carrier formed by the catalyst being supported on the inorganic oxide is also preferably within this range. The particle size of the inorganic oxide and the catalyst-supported carrier is obtained by the following method: an electron microscope image is observed on the cross section of the catalyst layer, and the maximum cross-sectional length is measured with more than 500 particles as the object, and the average value is calculated to obtain. The observation magnification is set to 100,000 times, and the object confirmed as the smallest unit of the particle is determined as the object from the geometric morphology on the appearance at this magnification, and measured.

[0015] As a catalyst supported on a carrier formed by an inorganic compound, the same catalyst as that used so far in the technical field can be used. For example, platinum, alloys of platinum and precious metals other than platinum, alloys of platinum and base metals, etc. can be listed. As precious metals other than platinum, palladium, ruthenium, rhodium and iridium can be listed. As base metals, vanadium, chromium, cobalt, nickel, iron and titanium can be listed. From the aspect of the efficient manifestation of catalytic ability, it is preferred that the average particle size of these catalysts at the surface of the carrier is more than 1nm and less than 10nm. The particle size of the catalyst can be measured in the same manner as the determination method of the particle size of the above-mentioned inorganic oxide and catalyst-supported carrier. The observation magnification is set to 500,000 times.

[0016] There is no particular restriction on the method for loading the catalyst on the surface of the carrier, and the same method as the method known so far in the technical field can be used. For example, when platinum is used as a catalyst, chloroplatinic acid hexahydrate (HPtCl6·6H2O), dinitrodiammine platinum (Pt(NH3)2(NO2)2) and the like are used as platinum sources, and they are reduced by known techniques such as liquid phase chemical reduction, gas phase chemical reduction, impregnation-reduction thermal decomposition, colloid method, surface modified colloid thermal decomposition reduction, so that platinum can be loaded on the carrier. The loading amount of the catalyst is preferably set to 1% by mass or more and 70% by mass or less relative to the mass of the carrier, and is particularly preferably set to 5% by mass or more and 20% by mass or less. On the other hand, when an alloy of platinum and a base metal is used as a catalyst, for example, a dispersion liquid containing a platinum compound such as a platinum complex, a platinum salt, a base metal complex, a base metal salt and a reducing agent is heated. Thus, platinum and a base metal are reduced to generate a platinum alloy, and the platinum alloy can be loaded on the carrier.

[0017] The fuel cell electrode catalyst layer of the present invention further comprises a hydrophilic material. The hydrophilic material may be hydrophilic as long as at least its surface is hydrophilic. As such a hydrophilic material, an aggregate of hydrophilic particles and the like may be cited. By using an aggregate of hydrophilic particles, the effective specific surface area of ​​the hydrophilic material becomes larger, making it easier to ensure a water discharge path in the catalyst layer. In addition, since no generated water is produced inside the aggregate of the hydrophilic particles, the discharge of water can be made more efficient.

[0018] The shape of the hydrophilic particles is not particularly limited as long as the specific surface area can be increased, and various shapes such as spherical, polyhedral, plate-like, spindle-like, or a mixture thereof can be adopted.

[0019] As a measure of hydrophilicity, "hydrophobicity" can be used. Hydrophobicity can be measured as follows using a powder wettability tester (WET101P manufactured by Rhesca Co., Ltd.). 50 mg of the object to be measured is added to 60 ml of water (temperature is 25°C) and stirred with a stirring blade. In this state, methanol is dripped into the water. At the same time, a laser with a wavelength of 780 nm is irradiated to the methanol aqueous solution to measure its transmittance. When the object to be measured is wetted and precipitated or suspended, the volume concentration of methanol when the transmittance becomes 80% is set as the hydrophobicity. The smaller the value, the higher the degree of hydrophilicity is judged to be. In the present invention, the hydrophobicity is preferably less than 2 volume%. It should be noted that the hydrophobicity of inorganic oxide particles that have not been hydrophobized, such as described in Patent Document 2, is substantially 0 volume%. The so-called hydrophobicity of 0 volume% means that if the object to be measured is added to water, it will immediately settle and the hydrophobicity cannot be measured.

[0020] Examples of the hydrophilic particles constituting the hydrophilic material include particles of inorganic oxides. From the viewpoint of improving the conductivity of the catalyst layer, it is advantageous for the hydrophilic particles to have conductivity, and for example, hydrophilic particles having a volume resistivity of 100 kΩcm or less are preferably used.

[0021] As examples of inorganic oxides constituting hydrophilic particles, similar to the inorganic oxides used in the above-mentioned carriers, one or more selected from indium oxides, tin oxides, titanium oxides, zirconium oxides, selenium oxides, tungsten oxides, zinc oxides, vanadium oxides, tantalum oxides, niobium oxides and rhenium oxides can be cited. As more preferred inorganic oxides, for example, products obtained by containing one or more elements of indium, niobium, tantalum, antimony and tungsten in tin oxide can be cited. In addition, products obtained by containing fluorine in tin oxide can be cited. Specifically, tin oxides containing indium, tin oxides containing antimony, tin oxides containing fluorine, tin oxides containing fluorine tungsten, tin oxides containing tantalum, tin oxides containing tantalum antimony, tin oxides containing tungsten and tin oxides containing niobium, etc., containing (doped) metals or non-metals can be cited. The inorganic compound constituting the hydrophilic particles may be the same as or different from the inorganic compound constituting the carrier.

[0022] The content of the hydrophilic material in the catalyst layer is preferably 2% by mass or more and less than 20% by mass relative to the total of the carrier and the hydrophilic material, more preferably 2.5% by mass or more and 18% by mass or less, and particularly preferably 2.5% by mass or more and 15% by mass or less. By making the content of the hydrophilic material within the above range, it is possible to properly discharge the generated water, and by preventing the occurrence of overflow, it is possible to prevent the reduction of the cell voltage in the high current density region.

[0023] By making the particle size d1 of the hydrophilic particles constituting the hydrophilic material be greater than 10 nm and less than 100 nm, particularly greater than 20 nm and less than 50 nm, the specific surface area becomes larger, which is preferred from the perspective of increasing the allowable amount of generated water. The particle size of the hydrophilic particles is obtained by observing the cross section of the catalyst layer with an electron microscope, measuring the maximum cross-sectional length with more than 500 particles as the object, and calculating the average value. The observation magnification is set to 100,000 times, and the object that is confirmed as the smallest unit of the particle from the geometric morphology of the appearance at this magnification is taken as the object for measurement.

[0024] The particle size d1 of the hydrophilic particles is preferably not significantly different from the particle size of the catalyst carrier. Specifically, the ratio of the particle size d1 of the hydrophilic particles to the particle size D of the catalyst carrier, i.e., the value of d1 / D, is preferably 0.5 or more and 3.0 or less, more preferably 0.7 or more and 2.0 or less, and particularly preferably 0.8 or more and 1.5 or less. By making the particle size d1 of the hydrophilic particles not significantly different from the particle size of the catalyst carrier D, it is easy to construct an appropriate discharge passage. In the case where the material of the hydrophilic particles is the same as that of the catalyst carrier, when the particle size d1 of the hydrophilic particles is measured by microscopic observation, it is measured in the same way as the above-mentioned method for measuring the particle size of the hydrophilic particles, and can be measured in the following manner: by using an energy dispersive X-ray spectrometer attached to an electron microscope to extract the area where the catalyst is distributed, thereby distinguishing the hydrophilic particles from the catalyst carrier for measurement.

[0025] From the viewpoint of facilitating the appropriate construction of a water discharge passage, it is preferred that the particle size d2 of the hydrophilic material formed by the aggregate of the hydrophilic particles is set in the form of a ratio relative to the thickness T of the catalyst layer. From this viewpoint, the ratio of the particle size d2 of the hydrophilic material to the thickness T of the catalyst layer, i.e., the value of d2 / T, is preferably 0.1 to 1.2, more preferably 0.2 to 1.0, and particularly preferably 0.3 to 0.7.

[0026] The thickness T of the catalyst layer is obtained by observing the cross section of the catalyst layer under an electron microscope, measuring the thickness of the thickest part and the thickness of the thinnest part in the observation field, and calculating the average value. In the present invention, from the viewpoint of preventing the resistance from becoming unstable when manufacturing a fuel cell and from the viewpoint of ensuring a volume that is good enough to obtain the catalyst activity, the thickness T of the catalyst layer is preferably 1 μm or more, more preferably 1.5 μm or more, and further preferably 2 μm or more. On the other hand, from the viewpoint of preventing the resistance from excessively increasing when manufacturing a fuel cell and preventing the diffusion resistance of gas and water from increasing, it is preferably set to 10 μm or less.

[0027] The particle size d2 of the hydrophilic material can be measured by the following method. That is, the catalyst layer containing the hydrophilic material is cut, and the cut surface is observed using an electron microscope image. Next, an energy dispersive X-ray spectrometer attached to the electron microscope is used to identify the hydrophilic material. The maximum cross-sectional length is measured by arbitrarily extracting more than 50 of the hydrophilic materials, and the average value is calculated to obtain the particle size. The observation magnification is set to 10,000 times, and the object that is confirmed as the smallest unit of the particle based on the geometric morphology of the appearance at this magnification is taken as the object for measurement.

[0028] As a method for producing a hydrophilic material, various granulation methods such as spray drying, tumbling granulation, fluidized bed granulation, stirring granulation, compression granulation, extrusion granulation, and crushing granulation can be cited. Among these granulation methods, by using the spray drying method, a hydrophilic material with a pore diameter of about 5 to 100 nm can be easily obtained, which is preferred from the viewpoint of being able to appropriately construct a water discharge path. Granulation is preferably carried out in the following manner: the particle size d2 of the hydrophilic material becomes 0.2 μm or more and 10 μm or less, particularly 0.5 μm or more and 5 μm or less.

[0029] The fuel cell electrode catalyst layer of the present invention may contain, in addition to the substances described above, a binder for bonding particles together, an ionomer, and other materials similar to those known in the art as needed. In particular, it is preferred that the catalyst layer does not contain a nonionic polymer.

[0030] The electrode catalyst layer for the fuel cell of the present invention can be formed by a known method. For example, by preparing an ink for coating by making a catalyst-supported carrier and a hydrophilic material into an ink, the ink is coated on a solid polymer electrolyte membrane, so that a catalyst layer can be formed on at least one side of the electrolyte membrane. In order to make the catalyst-supported carrier and the hydrophilic material into an ink, for example, the catalyst-supported carrier and the hydrophilic material are mixed with a liquid medium. It is simple to use water as a liquid medium. As required, a water-soluble organic solvent can also be used in combination with water. As a water-soluble organic solvent, for example, monohydric lower alcohols such as ethanol and 2-propanol can be used. These water-soluble organic solvents can be used alone or in combination of two or more. It is preferred to add a proton conductive polymer compound to the ink. As the polymer compound, a polymer compound obtained by introducing sulfonic acid into the side chain of a fluorinated polyolefin resin can be cited. The above components are mixed to obtain the target ink. For mixing, a planetary ball mill can be used, for example.

[0031] The obtained ink is used to form a catalyst layer on a solid polymer electrolyte membrane. The catalyst layer can be formed by any of the following methods: a method of directly applying ink on a solid polymer electrolyte membrane; a method of applying ink to a transfer sheet to form a catalyst layer and then transferring the catalyst layer to a solid polymer electrolyte membrane. For the transfer sheet, for example, polytetrafluoroethylene can be used. For the application of the ink, for example, a spraying method, a spin coating method, a scraper method, a screen printing method, and a rod coating method can be used. For the drying of the coating, for example, hot air drying and hot pressing can be used. In this way, a catalyst layer-coated electrolyte membrane (CCM) is obtained.

[0032] As the solid polymer electrolyte membrane, a solid polymer electrolyte membrane that is chemically stable in the environment of the fuel cell and has high proton conductivity can be used. In addition, the solid polymer electrolyte membrane is also preferably a solid polymer electrolyte membrane that is non-conductive and thus less likely to cause gas interlacing. As such a material, for example, a polymer electrolyte membrane obtained by combining a sulfonic acid group with a perfluoro polyethylene main chain can be cited as a preferred material. In addition, polysulfones, polyethersulfones, polyetherethersulfones, polyetheretherketones, and materials obtained by sulfonating hydrocarbon polymers can also be used.

[0033] By further stacking a gas diffusion layer on the catalyst layer side of the above-mentioned CCM, a membrane electrode assembly (MEA) for a fuel cell is obtained. The cathode and the anode are formed by a catalyst layer (cathode catalyst layer and anode catalyst layer) and a gas diffusion layer. As a gas diffusion layer, it is preferred to use a material having conductivity and a structure that allows a fuel gas or an oxidant to diffuse into the catalyst layer. As such a material, a porous body mainly formed of a carbonaceous material can be used. Specifically, porous carbon formed of carbon fibers such as carbon paper, carbon cloth, and carbon nonwoven fabrics is used. In addition, products obtained by surface treatment such as hydrophobic treatment or hydrophilic treatment of these materials can also be used. In this way, a solid polymer fuel cell is obtained.

[0034] Example

[0035] The present invention is described in more detail below by way of examples. However, the scope of the present invention is not limited to these examples. Unless otherwise specified, "%" means "mass %".

[0036] [Example 1]

[0037] (1) Formation of cathode electrode catalyst layer

[0038] (A) Preparation of hydrophilic materials

[0039] Particles of tantalum-antimony-containing tin oxide (hereinafter referred to as "Ta, Sb-SnO2") obtained by making SnO2 contain Ta and Sb were used as hydrophilic particles. Ta, Sb-SnO2 particles are manufactured by the method described in WO2017 / 022499, and the particle size d1 is 31.5nm. The particles are coarsely crushed with an agate mortar, and then crushed with a ball mill using yttrium-stabilized zirconia spheres. In the crushing using a ball mill, 40g of hydrophilic particles are mixed with 700mL of pure water and 40g of ethanol to form a slurry, and the slurry is used for crushing. After crushing, the slurry and the spheres are separated, and the separated slurry is used to granulate by spray drying to obtain a hydrophilic material with a particle size d2 of 2.0μm. Granulation conditions were set to inlet temperature: 220°C, outlet temperature: 60°C, spray pressure: 0.15-0.2MPa, liquid feeding rate: 8.3mL / min, slurry concentration: 10g / 250mL. Then, the mixture was calcined at 700°C for 5 hours in the atmosphere. When the hydrophobicity of the obtained hydrophilic material was measured by the above method, the hydrophilic material precipitated in water before methanol was added, so the hydrophobicity was 0% by volume.

[0040] (B) Formation of Electrode Catalyst Layer

[0041] Particles of tin oxide containing fluorine tungsten (hereinafter referred to as "F, W-SnO2") obtained by adding F and W to SnO2 were used as carriers. F, W-SnO2 particles were manufactured by the method described in WO2016 / 098399. A product in which 20% of an alloy of platinum and nickel was loaded on the carrier by a colloid method was used as a catalyst-loaded carrier (the carrier accounted for 80% and the alloy of platinum and nickel accounted for 20% in the catalyst-loaded carrier). The particle size D of the catalyst-loaded carrier was 30.0 nm.

[0042] 1.46 g of catalyst-loaded carrier and 0.03 g of hydrophilic material were placed in a container, and then pure water, ethanol and 2-propanol were added in a mass ratio of 35:45:20 (3.06 g as a mixed solution). The ink obtained in this way was dispersed by ultrasound for 3 minutes. Next, yttrium-stabilized zirconia balls with a diameter of 10 mm were placed in the container and stirred at 800 rpm for 20 minutes using a planetary ball mill (THINKY ARE310). Furthermore, 5% Nafion (registered trademark) (274704-100ML, manufactured by Sigma-Aldrich) was added to the ink, and the same stirring as above was carried out using ultrasonic dispersion and a planetary ball mill. The amount of Nafion added was set to an amount that the mass ratio of Nafion / (carrier+hydrophilic material) was 0.074.

[0043] The ink thus obtained was applied to a polytetrafluoroethylene sheet using a bar coater, and the coating was dried at 60° C. The thickness T of the obtained catalyst layer was 5.4 μm. In addition, the ratio of the particle size d1 of the hydrophilic particles to the particle size D of the catalyst support was 1.05, and the ratio of the particle size d2 of the hydrophilic material to the thickness T of the catalyst layer was 0.37.

[0044] (2) Formation of electrode catalyst layer for anode

[0045] 1.00 g of platinum-loaded carbon black (TEC10E50E) manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. was placed in a container, and pure water, ethanol and 2-propanol were added in a mass ratio of 45:35:20 (12.8 g as a mixed solution) in sequence. The ink obtained in this way was dispersed by ultrasound for 3 minutes. Next, yttrium-stabilized zirconia balls with a diameter of 10 mm were placed in the container and stirred at 800 rpm for 20 minutes using a planetary ball mill (THINKY ARE310). 5% Nafion (registered trademark) (274704-100ML, manufactured by Sigma-Aldrich) was further added to the ink, and the same stirring as above was continued using ultrasonic dispersion and a planetary ball mill. The amount of Nafion added was set to an amount that the mass ratio of Nafion / carbon black was 0.70. The ink obtained in this way was applied to a polytetrafluoroethylene sheet using a rod coater, and the coating was dried at 60°C.

[0046] (3) Manufacturing of CCM

[0047] The obtained polytetrafluoroethylene sheet with cathode and anode electrode catalyst layers was cut into a 54 mm square shape, and superposed on a Nafion (registered trademark) (NRE-212, manufactured by DuPont) electrolyte membrane, and heated at 140°C and 25 kgf / cm 2 The transfer was performed by heat pressing in the atmosphere for 2 minutes under the condition of . In this way, cathode and anode catalyst layers were formed on each surface of the solid polymer electrolyte membrane formed of Nafion.

[0048] (4) Fuel cell assembly

[0049] A fuel cell was assembled using the CCM obtained in (3) above. As the gas diffusion layer, SIGRACET (registered trademark) 29BC (manufactured by SGL Corporation) was used.

[0050] [Example 2]

[0051] A fuel cell was obtained in the same manner as in Example 1 except that 1.43 g of the catalyst-supporting carrier and 0.06 g of the hydrophilic material were used.

[0052] [Example 3]

[0053] A fuel cell was obtained in the same manner as in Example 1 except that 1.35 g of the catalyst-supporting carrier and 0.12 g of the hydrophilic material were used.

[0054] [Comparative Example 1]

[0055] A fuel cell was obtained in the same manner as in Example 1 except that the hydrophilic material of Example 1 was not used and 1.20 g of the catalyst-supporting carrier was used.

[0056] [Comparative Example 2]

[0057] A fuel cell was obtained in the same manner as in Example 3 except that Ta, Sb-SnO2 particles (hydrophobicity: 0 volume %) with a primary particle size of 31.5 nm and not granulated were used as the hydrophilic material instead of the hydrophilic material of Example 3.

[0058] [Comparative Example 3]

[0059] A fuel cell was obtained in the same manner as in Example 3 except that TiO2 particles (hydrophobicity: 0 volume %) having a primary particle size of 400 nm and not granulated were used as the hydrophilic material instead of the hydrophilic material of Example 3.

[0060] [Comparative Example 4]

[0061] A fuel cell was obtained in the same manner as in Example 1 except that 1.20 g of the catalyst-supporting carrier and 0.24 g of the hydrophilic material were used.

[0062] [evaluate]

[0063] The power generation characteristics of the fuel cells obtained in Examples 1 to 3 and Comparative Examples 1 to 4 were evaluated. After the anode and cathode of the fuel cell were stabilized by flowing nitrogen heated to 80°C and humidified to 100% RH, humidified hydrogen was supplied to the anode, and humidified air was supplied to the cathode. The degree of humidification was set to 100% RH. The power generation characteristics (current-voltage characteristics) were measured under this condition. The current density was calculated from the measurement results to be 1.5 A / cm 2 The results are shown in Table 1.

[0064] Table 1

[0065]

[0066] 1) Not granulated.

[0067] 2) Not granulated.

[0068] 3) The ratio of the hydrophilic material to the total of the carrier and the hydrophilic material is shown.

[0069] As can be seen from the results shown in Table 1, the fuel cells of the examples effectively prevented a decrease in the cell voltage in a region where the current density was high, compared to the fuel cells of the comparative examples.

[0070] Industrial Applicability

[0071] According to the present invention, since a channel for discharging generated water is constructed in the catalyst layer, the generated water can be appropriately discharged to the outside of the catalyst layer, and overflow can be prevented. As a result, even when the fuel cell is operated at a high current density, a decrease in the cell voltage can be effectively prevented.

Claims

1. A fuel cell electrode catalyst layer, comprising: a catalyst-supported carrier in which a catalyst is supported on a carrier formed of a conductive inorganic oxide; and a hydrophilic material, wherein: The hydrophilic material is an aggregate of hydrophilic particles having conductivity. The content of the hydrophilic material in the catalyst layer is greater than 2 mass % and less than 20 mass % relative to the total of the carrier and the hydrophilic material. The ratio of the particle size d1 of the hydrophilic particles to the particle size D of the catalyst-loaded carrier is greater than 0.5 and less than 3.

0. The ratio of the particle size d2 of the hydrophilic material to the thickness T of the catalyst layer is greater than 0.1 and less than 1.

2. The particle size d1 is greater than 10 nm and less than 100 nm, and the particle size d2 is greater than 0.2 μm and less than 10 μm.

2. The fuel cell electrode catalyst layer according to claim 1, wherein The catalyst is formed of platinum, or an alloy of platinum and a noble metal or a base metal other than platinum.

3. The fuel cell electrode catalyst layer according to claim 1 or 2, wherein: The hydrophilic particles include particles of one or more selected from indium oxides, tin oxides, titanium oxides, zirconium oxides, selenium oxides, tungsten oxides, zinc oxides, vanadium oxides, tantalum oxides, niobium oxides, and rhenium oxides. 4 . A fuel cell membrane electrode assembly, comprising a fuel cell electrode catalyst layer according to claim 1 formed on at least one surface of a solid polymer electrolyte membrane.

5. A polymer electrolyte fuel cell comprising the membrane electrode assembly according to claim 4, wherein the electrode catalyst layer is used as a cathode catalyst layer.