A kind of acoustic wave resonator and its preparation method

By forming a high defect density damage layer in the piezoelectric material layer and removing the damage layer, forming a suspended piezoelectric film, the problem that existing acoustic resonators cannot meet the needs of 5G communications is solved, and the effect of increasing the device frequency and bandwidth is achieved. Mass production.

CN112688657BActive Publication Date: 2024-11-19SHANGHAI INST OF MICROSYSTEM & INFORMATION TECH CHINESE ACAD OF SCI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202011560361.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-11-19
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

Existing acoustic resonators cannot meet the high frequency and broad bandwidth requirements of 5G communications, especially in the Sub-6 GHz band, it is difficult to achieve the requirement of the center frequency of the RF front-end filter to reach 3.5~5.0GHz and the relative bandwidth maximum of about 8.8%. .

Method used

By ion implantation and post-annealing in the piezoelectric material layer, high defect density damage layer is formed, and high defect density damage layer is removed through the corrosion window to form a suspended piezoelectric film, using the extreme mismatch between the air gap and the piezoelectric film. Impedance limits the energy of higher-order acoustic modes, thereby increasing the frequency, electromechanical coupling coefficient and bandwidth of the device.

Benefits of technology

It has achieved simplified process flow, reduced production complexity, and improved the bandwidth and frequency band coverage of the acoustic resonator, suitable for large-scale production, and meets the high-frequency and broadband needs of 5G communication.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112688657B_ABST
    Figure CN112688657B_ABST
Patent Text Reader

Abstract

The present invention provides an acoustic wave resonator and a preparation method thereof, the preparation method comprising: providing a piezoelectric material layer; performing ion implantation and post-annealing treatment on at least part of the upper surface of the piezoelectric material layer to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer; forming at least one corrosion window exposing the high defect density damage layer on the upper surface of the piezoelectric material layer; removing at least part of the high defect density damage layer based on the corrosion window to form an air gap in the piezoelectric material layer; wherein the air gap divides the piezoelectric material layer into a piezoelectric substrate and a piezoelectric film, the piezoelectric film is located above the air gap, and the piezoelectric film and the piezoelectric substrate are in contact at the edge of the air gap; and forming a patterned electrode on the upper surface of the piezoelectric film. The acoustic wave resonator and the preparation method thereof provided by the present invention solve the problem that the existing acoustic wave resonator cannot meet the 5G communication requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to an acoustic wave resonator and a preparation method thereof. Background Art

[0002] Compared with 4G and 4G-LTE communications, 5G communications require the use of higher frequency spectrum, which places higher requirements on the center frequency, bandwidth, quality factor, etc. of RF filters. Taking the domestic Sub-6 GHz frequency band as an example, it requires the center frequency of the RF front-end filter to reach 3.5-5.0 GHz, and the maximum relative bandwidth is about 8.8%; however, currently commercial RF acoustic filters are difficult to meet the above requirements.

[0003] In view of this, it is necessary to design a new acoustic wave resonator and its preparation method to meet the needs of 5G communications. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide an acoustic wave resonator and a preparation method thereof, so as to solve the problem that the existing acoustic wave resonator cannot meet the 5G communication requirements.

[0005] In order to achieve the above-mentioned object and other related objects, the present invention provides a method for preparing an acoustic wave resonator, the preparation method comprising:

[0006] a) providing a piezoelectric material layer;

[0007] b) performing ion implantation and post-annealing treatment on at least a portion of the upper surface of the piezoelectric material layer to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer;

[0008] c) forming at least one corrosion window on the upper surface of the piezoelectric material layer to expose the high defect density damaged layer;

[0009] d) removing at least a portion of the high defect density damaged layer based on the etching window to form an air gap in the piezoelectric material layer; wherein the air gap divides the piezoelectric material layer into a piezoelectric substrate and a piezoelectric film, the piezoelectric film is located above the air gap, and the piezoelectric film and the piezoelectric substrate are in contact at the edge of the air gap;

[0010] e) forming a patterned electrode on the upper surface of the piezoelectric film.

[0011] Optionally, the order of executing the steps in the preparation method is a), b), c), d), e), a), e), b), c), d), a), b), e), c), d), or a), b), c), e), d); wherein, when the order of executing the steps in the preparation method is a), e), b), c), d), a), b), e), c), d), or a), b), c), e), d), e) is to form a patterned electrode on the upper surface of the piezoelectric material layer.

[0012] Optionally, before forming the corrosion window, the preparation method also includes: a step of forming a first protective layer on the surface of the piezoelectric material layer or the surface of the piezoelectric material layer and the surface of the patterned electrode; after forming the corrosion window, the preparation method also includes: a step of removing the first protective layer; wherein the material of the first protective layer includes any one of silicon dioxide, silicon nitride, chromium, and gold.

[0013] Optionally, before forming the air gap, the preparation method also includes: a step of forming a second protective layer on the surface of the piezoelectric material layer or the surface of the piezoelectric material layer and the surface of the patterned electrode; after forming the air gap, the preparation method also includes: a step of removing the second protective layer; wherein the material of the second protective layer includes any one of silicon dioxide, silicon nitride, chromium, and gold.

[0014] Optionally, the preparation method further comprises: a step of forming a heat dissipation accelerating layer at least on the upper surface of the piezoelectric film and the surface of the patterned electrode.

[0015] Optionally, b) is to perform ion implantation on the entire upper surface of the piezoelectric material layer and then perform annealing to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer; at this time, d) is to remove part of the high defect density damage layer based on the corrosion window to form an air gap in the piezoelectric material layer.

[0016] Optionally, the method for forming the corrosion window in c) includes:

[0017] The position of the air gap is defined in the piezoelectric material layer, and a patterned window mask is formed on the upper surface of the piezoelectric material layer, wherein an opening pattern defining the shape and position of the etching window is formed in the patterned window mask, and the opening pattern is located in the defined area where the air gap is located;

[0018] Etching the piezoelectric material layer based on the patterned window mask to form at least one corrosion window exposing the high defect density damaged layer;

[0019] The patterned window mask is removed.

[0020] Optionally, b) is to perform ion implantation on a portion of the upper surface of the piezoelectric material layer and then perform annealing to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer; in this case, d) is to remove all of the high defect density damage layer based on the corrosion window to form an air gap in the piezoelectric material layer.

[0021] Optionally, the method of forming the high defect density damaged layer in b) comprises:

[0022] Forming a patterned implantation mask on the upper surface of the piezoelectric material layer, wherein an opening pattern defining the shape and position of the high defect density damaged layer is formed in the patterned implantation mask;

[0023] Performing ion implantation and post-annealing treatment on the piezoelectric material layer based on the patterned implantation mask to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer;

[0024] removing the patterned implant mask;

[0025] At this time, the method for forming the corrosion window in c) includes:

[0026] Forming a patterned window mask on the upper surface of the piezoelectric material layer, wherein an opening pattern defining the shape and position of the etching window is formed in the patterned window mask;

[0027] Etching the piezoelectric material layer based on the patterned window mask to form at least one corrosion window exposing the high defect density damaged layer;

[0028] The patterned window mask is removed.

[0029] Optionally, the ion implantation is performed in multiple times; wherein the dosages of the multiple ion implantations are the same but the energies are different, and the energy values ​​of the multiple ion implantations decrease in sequence.

[0030] Optionally, the contact between the piezoelectric film and the piezoelectric substrate at the edge of the air gap is defined based on the shape and position of the corrosion window; wherein the piezoelectric film and the piezoelectric substrate have at least one contact point at the edge of the air gap, and / or the piezoelectric film and the piezoelectric substrate have at least one contact surface at the edge of the air gap.

[0031] Optionally, the patterned electrode includes: one or more combinations of interdigitated electrodes, fan-shaped strip electrodes, circular ring-shaped strip electrodes or hexagonal plate electrodes.

[0032] Optionally, when the patterned electrodes are interdigital electrodes and the number of pairs of interdigital electrodes is plural, the plural pairs of interdigital electrodes form an interdigital transducer.

[0033] Optionally, the preparation method further comprises: a step of forming a reflective gate electrode on the upper surface of the piezoelectric film or the upper surface of the piezoelectric substrate on both sides of the interdigital transducer.

[0034] The present invention also provides an acoustic wave resonator, comprising:

[0035] a piezoelectric material layer;

[0036] An air gap with a preset thickness is formed at a preset depth of the piezoelectric material layer based on an etching window; the air gap divides the piezoelectric material layer into a piezoelectric substrate and a piezoelectric film, the piezoelectric film is located above the air gap, and the piezoelectric film and the piezoelectric substrate are in contact at the edge of the air gap;

[0037] The patterned electrode is formed on the upper surface of the piezoelectric film.

[0038] Optionally, the target elastic wave excited by the piezoelectric film includes one or more of: Rayleigh wave, horizontal shear wave, symmetric Lamb wave, antisymmetric Lamb wave, body wave or quasi-body wave.

[0039] Optionally, the piezoelectric film and the piezoelectric substrate have at least one contact point at an edge of the air gap, and / or the piezoelectric film and the piezoelectric substrate have at least one contact surface at an edge of the air gap.

[0040] Optionally, the patterned electrode includes: one or more combinations of interdigitated electrodes, fan-shaped strip electrodes, circular ring-shaped strip electrodes or hexagonal plate electrodes.

[0041] Optionally, when the patterned electrodes are interdigital electrodes and the number of pairs of interdigital electrodes is plural, the plural pairs of interdigital electrodes form an interdigital transducer.

[0042] Optionally, the acoustic wave resonator further includes: at least one pair of reflective gate electrodes formed on an upper surface of the piezoelectric film or an upper surface of the piezoelectric substrate on both sides of the interdigital transducer.

[0043] Optionally, the thickness of the patterned electrode is smaller than the thickness of the piezoelectric film, and the ratio of the thickness of the piezoelectric film to the wavelength of the target elastic wave excited by the piezoelectric film is smaller than 0.5.

[0044] Optionally, the acoustic wave resonator further includes: an accelerating heat dissipation layer formed at least on the upper surface of the piezoelectric film and the surface of the patterned electrode.

[0045] Optionally, the material of the piezoelectric material layer includes: any one of quartz, aluminum nitride, zinc oxide, lithium tantalate, lithium niobate, lithium tetraborate, bismuth germanate, bismuth silicate, lanthanum gallium silicate, and zirconium titanium lead acid.

[0046] As described above, an acoustic wave resonator and a preparation method thereof of the present invention have the following beneficial effects: the preparation method of the present invention uses ion implantation and post-annealing to form a high defect density damage layer inside the piezoelectric material layer, and then removes the high defect density damage layer through an etching window to obtain a suspended piezoelectric film, without the need for complex process steps such as bonding, transfer, peeling, and polishing, thereby reducing the complexity of preparation. The preparation method of the present invention has a simple process, high material utilization rate, and low manufacturing cost, which is beneficial to improving the bandwidth and coverage frequency band of the resonator and filter, and is suitable for large-scale production and use. The present invention utilizes the extreme mismatch between the acoustic impedance of the suspended piezoelectric film and the air gap, and effectively limits the energy of the high-order acoustic wave mode with a higher sound velocity to the piezoelectric film, thereby improving the frequency, electromechanical coupling coefficient, bandwidth and quality factor of the device to meet the needs of 5G communications. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 Shown is a flow chart of the method for preparing the acoustic wave resonator of the present invention.

[0048] Figure 2a-2e It is a schematic diagram showing the structure of each step in a method for preparing the acoustic wave resonator of the present invention; wherein, Figure 2a is a schematic diagram of the structure of the piezoelectric material layer. Figure 2b Schematic diagram of the structure of the high defect density damage layer. Figure 2c A schematic diagram of the structure for forming a patterned electrode. Figure 2d The schematic diagram of the structure for forming the corrosion window is shown in Figure 1. Figure 2e Schematic diagram of the structure for forming an air gap.

[0049] Figure 3a-3e It is a schematic diagram showing the structure of each step in another method for preparing the acoustic wave resonator of the present invention; wherein, Figure 3a is a schematic diagram of the structure of the piezoelectric material layer. Figure 3b Schematic diagram of the structure of the high defect density damage layer. Figure 3c A schematic diagram of the structure for forming a patterned electrode. Figure 3d The schematic diagram of the structure for forming the corrosion window is shown in Figure 1. Figure 3e Schematic diagram of the structure for forming an air gap.

[0050] Figure 4-11 The contact form between the piezoelectric film and the piezoelectric substrate defined based on different positions and shapes of the etching window in the acoustic wave resonator of the present invention is shown; wherein, Figure 4-5 There is point contact between the piezoelectric film and the piezoelectric substrate. Figure 6-7The piezoelectric film and the piezoelectric substrate are in surface contact. Figure 8-11 There are point contact and surface contact between the piezoelectric film and the piezoelectric substrate.

[0051] Fig.12 Shown is a schematic diagram of the structure of the suspended thin film type acoustic wave resonator described in Examples 1-5.

[0052] Fig.13 Shown is a schematic structural diagram of the solid-state assembled acoustic wave resonator described in Comparative Examples 1-5.

[0053] Fig.14a The electromechanical coupling coefficient K of the acoustic wave resonator in Example 1 and Comparative Example 1 under the zero-order horizontal shear wave SH0 mode is shown as follows: 2 Curves showing the change of in-plane propagation angle (0°-180°), Fig.14b The electromechanical coupling coefficient K of the acoustic wave resonator in Example 1 and Comparative Example 1 in the SH0 mode changes as the acoustic wave wavelength λ changes from 0.5 to 0.04. 2 The change curve of Fig.14c The vibration energy diagram of the acoustic wave resonator in Example 1 in the SH0 mode is shown. Fig.14d Shown is the vibration energy diagram of the acoustic wave resonator described in Comparative Example 1 in the SH0 mode.

[0054] Fig.15a The following is the admittance curve of the acoustic wave resonator described in Example 2 in the zero-order symmetric Lamb wave S0 mode. Fig.15b Shown is the admittance curve of the acoustic wave resonator in Comparative Example 2 in S0 mode, Fig.15c The vibration energy diagram of the acoustic wave resonator in Example 2 in the S0 mode is shown. Fig.15d The vibration energy diagram of the acoustic wave resonator in the S0 mode of the comparative example 2 is shown. Fig.15e The electromechanical coupling coefficient K of the acoustic wave resonator in Example 2 in the S0 mode is shown as h / λ changes from 0.5 to 0.04. 2 The change curve.

[0055] Fig.16a The electromechanical coupling coefficient K of the acoustic wave resonator in Example 3 and Comparative Example 3 under the zero-order horizontal shear wave SH0 mode is shown as follows: 2 Curves showing the change of in-plane propagation angle (0°-180°), Fig.16b The electromechanical coupling coefficient K of the acoustic wave resonator in Example 3 and Comparative Example 3 in the SH0 mode changes as the acoustic wave wavelength λ changes from 0.5 to 0.04. 2 The change curve of Fig.16c The vibration energy diagram of the acoustic wave resonator in the SH0 mode described in Example 3 is shown. Fig.16dShown is the vibration energy diagram of the acoustic wave resonator described in Comparative Example 3 in the SH0 mode.

[0056] Fig.17a The electromechanical coupling coefficient K of the acoustic wave resonator in Example 4 in the first-order antisymmetric Lamb wave A1 mode is shown as h / λ changes from 0.5 to 0.04. 2 The change curve of Fig.17b The following is the admittance curve of the acoustic wave resonator in Example 4 in the A1 mode. Fig.17c Shown is the admittance curve of the acoustic wave resonator in Comparative Example 4 in the A1 mode, Fig.17d The vibration energy diagram of the acoustic wave resonator in the A1 mode described in Example 4 is shown. Fig.17e Shown is the vibration energy diagram of the acoustic wave resonator described in Comparative Example 4 in the A1 mode.

[0057] Fig.18a The electromechanical coupling coefficient K is shown as follows: the acoustic wavelength λ of the acoustic wave resonator in the first-order antisymmetric Lamb wave A1 mode changes as h / λ changes from 0.5 to 0.04. 2 The change curve of Fig.18b The following is the admittance curve of the acoustic wave resonator in Example 5 in the A1 mode. Fig.18c Shown is the admittance curve of the acoustic wave resonator in comparative example 5 in the A1 mode, Fig.18d The vibration energy diagram of the acoustic wave resonator in the A1 mode described in Example 5 is shown. Fig.18e The vibration energy diagram of the acoustic wave resonator in the comparative example 5 in the A1 mode is shown. Fig.18f Shown is a vibration energy diagram of the acoustic wave resonator described in Example 5 in the quasi-bulk wave A3 mode.

[0058] Component number description

[0059] 101, 201 piezoelectric material layer

[0060] 102, 202 High defect density damaged layer

[0061] 103, 203, 303 patterned electrodes

[0062] 104, 204 Reflective grid electrode

[0063] 105, 205 Corrosion Window

[0064] 106, 206 air gap

[0065] 107, 207, 301 piezoelectric substrate

[0066] 108, 208, 302 Piezoelectric film DETAILED DESCRIPTION

[0067] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0068] See also Figure 1 to Figure 18e It should be noted that the illustrations provided in this embodiment are only schematic illustrations of the basic concept of the present invention. Although the illustrations only show components related to the present invention and are not drawn according to the number, shape and size of components in actual implementation, the form, quantity and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complicated.

[0069] like Figure 1 As shown, this embodiment provides a method for preparing an acoustic wave resonator, the preparation method comprising:

[0070] a) providing a piezoelectric material layer 101 / 201;

[0071] b) performing ion implantation and post-annealing treatment on at least a portion of the upper surface of the piezoelectric material layer 101 / 201 to form a high defect density damaged layer 102 / 202 with a preset thickness at a preset depth in the piezoelectric material layer 101 / 201;

[0072] c) forming at least one corrosion window 105 / 205 on the upper surface of the piezoelectric material layer 101 / 201 to expose the high defect density damaged layer 102 / 202;

[0073] d) removing at least a portion of the high defect density damaged layer 102 / 202 based on the etching window 105 / 205 to form an air gap 106 / 206 in the piezoelectric material layer 101 / 201; wherein the air gap 106 / 206 divides the piezoelectric material layer 101 / 201 into a piezoelectric substrate 107 / 207 and a piezoelectric film 108 / 208, the piezoelectric film 108 / 208 is located above the air gap 106 / 206, and the piezoelectric film 108 / 208 is in contact with the piezoelectric substrate 107 / 207 at the edge of the air gap 106 / 206;

[0074] e) forming a patterned electrode 103 / 203 on the upper surface of the piezoelectric film 108 / 208 .

[0075] Optionally, the execution order of the steps in the preparation method is a), b), c), d), e), a), e), b), c), d), a), b), e), c), d), or a), b), c), e), d); wherein, when the execution order of the steps in the preparation method is a), e), b), c), d), a), b), e), c), d), or a), b), c), e), d), e) is to form a patterned electrode 103 / 203 on the upper surface of the piezoelectric material layer 101 / 201.

[0076] The following describes in detail the method for preparing the acoustic wave resonator described in this embodiment by taking the execution order of steps a), b), e), c), and d) as an example.

[0077] Step 1) Provide a piezoelectric material layer 101 / 201 (such as Figure 2a / 3a).

[0078] As an example, the piezoelectric material layer 101 / 201 is a single crystal piezoelectric material, and its material includes: any one of quartz, aluminum nitride, zinc oxide, lithium tantalate, lithium niobate, lithium tetraborate, bismuth germanate, bismuth silicate, lanthanum gallium silicate, and zirconium titanium lead acid; of course, other piezoelectric materials that can be used to make acoustic wave resonators are also applicable to this example.

[0079] Step 2) performing ion implantation and post-annealing treatment on at least a portion of the upper surface of the piezoelectric material layer 101 / 201 to form a high defect density damaged layer 102 / 202 (e.g., Figure 2b / 3b).

[0080] In one example, step 2) is to perform ion implantation and post-annealing on the entire upper surface of the piezoelectric material layer 101 to form a high defect density damaged layer 102 (e.g., Figure 2b shown).

[0081] In another example, step 2) is to perform ion implantation and post-annealing treatment on a portion of the upper surface of the piezoelectric material layer 201 to form a high defect density damaged layer 202 (such as Figure 3bAs shown). Specifically, the method for forming the high defect density damage layer 202 includes: first forming a patterned injection mask on the upper surface of the piezoelectric material layer 201, wherein an opening pattern defining the shape and position of the high defect density damage layer 202 is formed in the patterned injection mask; then, based on the patterned injection mask, ion implantation is performed on the piezoelectric material layer 201 and then annealing is performed to form a high defect density damage layer 202 with a preset thickness H at a preset depth D in the piezoelectric material layer 201; and finally, the patterned injection mask is removed. In this example, the high defect density damage layer 202 is formed by patterned ion implantation, which has the advantages of being easy to set the etching cutoff boundary, ensuring that the edge of the active area of ​​the device is a solid contact type, that is, an air gap is formed only directly below the suspended piezoelectric film, which not only fully utilizes the advantage of limiting the energy of the acoustic wave achieved by the impedance mismatch between the piezoelectric film and the air, but also maximizes the contact area between the device and the piezoelectric substrate, effectively improving the heat dissipation and structural stability of the device.

[0082] As an example, when ion implantation is performed on the piezoelectric material layer 101 / 201, the ion implantation can be performed in multiple times to control the thickness of the ion implantation layer, that is, to control the thickness H of the high defect density damage layer 102 / 202; wherein the dosages of the multiple ion implantations are the same but the energies are different, and the energy values ​​of the multiple ion implantations decrease successively, so as to avoid the influence of the ion implantation with a large energy value on the ion implantation with a small energy value, thereby improving the longitudinal uniformity of the ion implantation. For example, the piezoelectric material layer 101 / 201 is subjected to two ion implantations, with the same dosage and different energies. The energy of the ion implantation depends on the formation depth of the high defect density damaged layer 102 / 202. A large amount of energy is first injected to form a first ion implantation layer of a certain thickness at a deeper position, and then a small amount of energy is injected to form a second ion implantation layer of a certain thickness at a shallower position. By reasonably designing the energy of the two ion implantations, the upper surface of the first ion implantation layer can be made to coincide with the lower surface of the second ion implantation layer, thereby obtaining an ion implantation layer with a larger thickness. In specific applications, the injected ions can be Gaussian distributed in the piezoelectric material layer 101 / 201, and the energy of each ion implantation can be obtained by simulation using the simulation software SRIM. This is well known to those skilled in the art and will not be described in detail. It should be noted that by controlling the energy of ion implantation, the thickness of the high defect density damaged layer 102 / 202 can be made equal to the difference between the thickness of the piezoelectric material layer 101 / 201 and the preset depth D; however, for the purpose of device processing and preservation, the thickness of the high defect density damaged layer 102 / 202 is usually made smaller than the difference between the thickness of the piezoelectric material layer 101 / 201 and the preset depth D. Specifically, the ion implantation can be achieved by hydrogen ions, helium ions, or hydrogen and helium co-injection.

[0083] As an example, since the preset depth D is the thickness of the subsequently formed piezoelectric film 108 / 208, when ion implantation is performed on the piezoelectric material layer 102 / 202, the ratio of the preset depth D to the wavelength of the target elastic wave excited by the piezoelectric film 108 / 208 can be designed to be less than 0.5, so that the ratio of the thickness of the subsequently formed piezoelectric film 108 / 208 to the wavelength of the target elastic wave excited by it is less than 0.5, thereby obtaining a larger electromechanical coupling coefficient; further, the ratio can be less than 0.25 to obtain a larger electromechanical coupling coefficient.

[0084] As an example, the post-annealing process temperature is not higher than 550°C, and the process time is not more than 4 hours, so as to restore the defects introduced into the piezoelectric material layer 101 / 201 by ion implantation and aggregate the defects, but not to the extent of causing the formed high defect density damaged layer 102 / 202 to bubble and crack. It should be noted that for piezoelectric material layers of different materials, the corresponding post-annealing process temperature and process time are different, and for different cuts of the same piezoelectric material layer, the corresponding post-annealing process temperature and process time are also different; therefore, in actual applications, the appropriate post-annealing temperature and time can be selected according to the specific selected piezoelectric material.

[0085] Step 3) forming a patterned electrode 103 / 203 (such as Figure 2c / 3c).

[0086] As an example, the patterned electrode 103 / 203 is formed on the upper surface of the piezoelectric material layer 101 / 201 by a sputtering process or an electron beam evaporation process; wherein the material of the patterned electrode 103 / 203 includes at least one of aluminum, gold, chromium, tungsten, titanium, copper, and silver. Of course, the material of the patterned electrode 103 / 203 can also be an alloy composed of two or more of the above metals. Specifically, the patterned electrode 103 / 203 can be a single-layer structure or a multi-layer structure.

[0087] As an example, the patterned electrode 103 / 203 includes: one or more combinations of interdigitated electrodes, fan-shaped strip electrodes, circular strip electrodes or hexagonal plate electrodes. Specifically, when the patterned electrode 103 / 203 is an interdigitated electrode, the interdigitated fingers in the interdigitated electrode are arranged parallel to each other, and the arrangement direction of each interdigitated finger is parallel to the direction of the bus bar. At the same time, each interdigitated finger may have an inclination angle of less than ±5° in the direction perpendicular to the bus bar. Specifically, when the patterned electrode 103 / 203 is an interdigitated electrode and the number of pairs of interdigitated electrodes is multiple pairs, the multiple pairs of interdigitated electrodes form an interdigitated transducer to generate an electric field. Optionally, the preparation method also includes: a step of forming at least one pair of uniformly distributed reflective gate electrodes 104 / 204 on the upper surface of the piezoelectric material layer 101 / 201 on both sides of the interdigital transducer to limit the energy of the sound wave by utilizing its reflection; wherein the reflective gate electrodes 104 / 204 can be formed on the upper surface of a suspended piezoelectric material layer (i.e., a piezoelectric film) or on the upper surface of a non-suspended piezoelectric material layer (i.e., a piezoelectric substrate), which has no effect on its function.

[0088] As an example, the thickness of the patterned electrode 103 / 203 is less than a preset depth D, so that the thickness of the patterned electrode 103 / 203 is less than the thickness of the piezoelectric film 108 / 208 formed subsequently.

[0089] Step 4) forming at least one corrosion window 105 / 205 (such as Figure 2d / 3d).

[0090] In one example, when step 2) is to perform ion implantation on the entire upper surface of the piezoelectric material layer 101, the method for forming the etching window 105 at this time includes: first defining the position of the air gap 106 in the piezoelectric material layer 101 (such as Figure 2d The piezoelectric material layer 101 is formed with a patterned window mask on the upper surface of the piezoelectric material layer 101; wherein the patterned window mask is formed with an opening pattern defining the shape and position of the etching window, and the opening pattern is located in the defined area where the air gap 106 is located; then, the piezoelectric material layer 101 is etched based on the patterned window mask to form at least one etching window 105 exposing the high defect density damaged layer 102; finally, the patterned window mask (such as Figure 2d shown).

[0091] In another example, when step 2) is to perform ion implantation on a portion of the upper surface of the piezoelectric material layer 201, the method for forming the etching window 205 at this time includes: first forming a patterned window mask on the upper surface of the piezoelectric material layer 201, wherein an opening pattern defining the shape and position of the etching window 205 is formed in the patterned window mask; then etching the piezoelectric material layer 201 based on the patterned window mask to form at least one etching window 205 exposing the high defect density damaged layer 202; and finally removing the patterned window mask (such as Figure 3d Specifically, the etching window 205 may be formed above the high defect density damaged layer 202 , or may be formed outside the high defect density damaged layer 202 .

[0092] As an example, the piezoelectric material layer 101 / 201 may be etched by a dry etching process or a wet etching process to form the corrosion window 105 / 205 .

[0093] As an example, before forming the etching window 105 / 205, the preparation method further includes: a step of forming a first protective layer (not shown in the figure) on the surface of the piezoelectric material layer 101 / 201 and the surface of the patterned electrode 103 / 203, so as to protect the piezoelectric material layer 101 / 201 and the patterned electrode 103 / 203 when the etching window 105 / 205 is subsequently formed; accordingly, after forming the etching window 105 / 205, the preparation method further includes: a step of removing the first protective layer; wherein the material of the first protective layer includes any one of silicon dioxide, silicon nitride, chromium, and gold. Optionally, when the preparation method further includes the step of forming a reflective gate electrode 104 / 204, the first protective layer is also formed on the surface of the reflective gate electrode 104 / 204, so as to protect the reflective gate electrode 104 / 204 when the etching window 105 / 205 is subsequently formed. Specifically, the first protective layer may be formed by a chemical vapor deposition process, a physical vapor deposition process, a molecular beam epitaxy process, an atomic layer deposition process, a pulsed laser deposition process, a sputtering process or an electron beam evaporation process.

[0094] Step 5) Based on the etching window 105 / 205, at least a portion of the high defect density damaged layer 102 / 202 is removed to form an air gap 106 / 206 in the piezoelectric material layer 101 / 201; wherein the air gap 106 / 206 divides the piezoelectric material layer 101 / 201 into a piezoelectric substrate 107 / 207 and a piezoelectric film 108 / 208, the piezoelectric film 108 / 208 is located above the air gap 106 / 206, and the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 are in contact at the edge of the air gap 106 / 206 (such as Figure 2e / 3e).

[0095] In one example, when step 2) is to perform ion implantation on the entire upper surface of the piezoelectric material layer 101, step 5) is based on the etching window 105 to remove a portion of the high defect density damaged layer 102 to form an air gap 106 in the piezoelectric material layer 101 (specifically, Figure 2e Specifically, a dry etching process or a wet etching process may be used to etch a portion of the high defect density damaged layer 102 to form the air gap 106. In practical applications, the etching size of the high defect density damaged layer 102 by the etching gas or the etching liquid may be controlled by controlling the lateral etching time, so as to avoid the high defect density damaged layer 102 being completely etched away while forming the air gap 106.

[0096] In another example, when step 2) is to perform ion implantation on a portion of the upper surface of the piezoelectric material layer 201, step 5) is to remove all of the high defect density damaged layer 202 based on the etching window 205 to form an air gap 206 in the piezoelectric material layer 201 (specifically, Figure 3e Specifically, a dry etching process or a wet etching process may be used to etch a portion of the high defect density damaged layer 102 to form the air gap 106 .

[0097] As an example, the contact between the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 at the edge of the air gap 106 / 206 is defined based on the shape and position of the etching window 105 / 205, so that the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 have at least one contact point at the edge of the air gap 106 / 206 (e.g., Figure 4-5As shown, the contact point is hollowed out below), at this time, except for the contact point connection, the piezoelectric film 108 / 208 is completely suspended on the piezoelectric substrate 107 / 207; the advantage of this structure is that the four end faces of the piezoelectric film 108 / 208 in two directions are directly in contact with the air, forming an extreme impedance mismatch, which can better limit the energy of the sound wave, improve the electromechanical coupling coefficient, and reduce the appearance of the stray mode. Of course, the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 can also have at least one contact surface at the edge of the air gap 106 / 206 (such as Figure 6-7 As shown, the contact surface is not hollowed out below), the advantage of this structure is that at least one of the four end faces of the piezoelectric film 108 / 208 in two directions is connected to the piezoelectric substrate 107 / 207 to ensure that the device and the piezoelectric substrate 107 / 207 have "solid-state" contact, thereby enhancing the heat dissipation and structural stability of the device; of course, the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 can also have at least one contact point and at least one contact surface at the edge of the air gap 106 / 206 (such as Figure 8-11 As shown, Figure 8-9 The middle contact point is hollowed out, but the contact surface is not hollowed out. Figure 10-11 The contact points and the area below the contact surface are not hollowed out). The advantage of this structure is that at least one of the four end faces of the piezoelectric film 108 / 208 in two directions is connected to the piezoelectric substrate 107 / 207 to ensure that there is "solid-state" contact between the device and the piezoelectric substrate 107 / 207, thereby enhancing the heat dissipation and structural stability of the device.

[0098] As an example, before forming the air gap 106 / 206, the preparation method further includes: a step of forming a second protective layer (not shown in the figure) on the surface of the piezoelectric material layer 101 / 201 and the surface of the patterned electrode 103 / 203, so as to protect the piezoelectric material layer 101 / 201 and the patterned electrode 103 / 203 when the air gap 106 / 206 is subsequently formed; accordingly, after forming the air gap 106 / 206, the preparation method further includes: a step of removing the second protective layer; wherein the material of the second protective layer includes any one of silicon dioxide, silicon nitride, chromium, and gold. Optionally, when the preparation method further includes the step of forming a reflective gate electrode 104 / 204, the second protective layer is also formed on the surface of the reflective gate electrode 104 / 204, so as to protect the reflective gate electrode 104 / 204 when the air gap 106 / 206 is subsequently formed. Specifically, the second protective layer may be formed by a chemical vapor deposition process, a physical vapor deposition process, a molecular beam epitaxy process, an atomic layer deposition process, a pulsed laser deposition process, a sputtering process or an electron beam evaporation process.

[0099] As an example, the preparation method further includes: forming an accelerating heat dissipation layer (not shown in the figure) at least on the upper surface of the piezoelectric film 108 / 208 and the surface of the patterned electrode 103 / 203 to accelerate the heat dissipation of the device; of course, the accelerating heat dissipation layer can also be formed on the upper surface of the entire device structure. Specifically, the accelerating heat dissipation layer is made of a high thermal conductivity material such as silicon, silicon carbide, aluminum nitride, etc. Optionally, when the preparation method further includes the step of forming a reflective gate electrode 104 / 204, the accelerating heat dissipation layer is also formed on the surface of the reflective gate electrode 104 / 204.

[0100] Correspondingly, if Figure 2e , 3e As shown in 4-11, this embodiment also provides an acoustic wave resonator, and the acoustic wave resonator includes:

[0101] Piezoelectric material layer 101 / 201;

[0102] An air gap 106 / 206 with a preset thickness is formed at a preset depth of the piezoelectric material layer 101 / 201 based on the etching window 105 / 205; the air gap 106 / 206 divides the piezoelectric material layer 101 / 201 into a piezoelectric substrate 107 / 207 and a piezoelectric film 108 / 208, the piezoelectric film 108 / 208 is located above the air gap 106 / 206, and the piezoelectric film 108 / 208 is in contact with the piezoelectric substrate 107 / 207 at the edge of the air gap 106 / 206;

[0103] The patterned electrode 103 / 203 is formed on the upper surface of the piezoelectric film 108 / 208 .

[0104] As an example, the piezoelectric material layer 101 / 201 is a single crystal piezoelectric material, and its material includes: any one of quartz, aluminum nitride, zinc oxide, lithium tantalate, lithium niobate, lithium tetraborate, bismuth germanate, bismuth silicate, lanthanum gallium silicate, and zirconium titanium lead acid; of course, other piezoelectric materials that can be used to make acoustic wave resonators are also applicable to this example.

[0105] As an example, the etching window 105 / 205 may be formed above the air gap 106 / 206, or may be formed outside the air gap 106 / 206. Specifically, the contact between the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 at the edge of the air gap 106 / 206 is defined based on the shape and position of the etching window 105 / 205, so that the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 have at least one contact point at the edge of the air gap 106 / 206 (e.g., Figure 4-5 As shown, the contact point is hollowed out below), at this time, except for the contact point connection, the piezoelectric film 108 / 208 is completely suspended on the piezoelectric substrate 107 / 207; the advantage of this structure is that the four end faces of the piezoelectric film 108 / 208 in two directions are directly in contact with the air, forming an extreme impedance mismatch, which can better limit the energy of the sound wave, improve the electromechanical coupling coefficient, and reduce the appearance of the stray mode. Of course, the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 can also have at least one contact surface at the edge of the air gap 106 / 206 (such as Figure 6-7 As shown, the contact surface is not hollowed out below), the advantage of this structure is that at least one of the four end faces of the piezoelectric film 108 / 208 in two directions is connected to the piezoelectric substrate 107 / 207 to ensure that the device and the piezoelectric substrate 107 / 207 have "solid-state" contact, thereby enhancing the heat dissipation and structural stability of the device; of course, the piezoelectric film 108 / 208 and the piezoelectric substrate 107 / 207 can also have at least one contact point and at least one contact surface at the edge of the air gap 106 / 206 (such as Figure 8-11 As shown, Figure 8-9 The middle contact point is hollowed out, but the contact surface is not hollowed out. Figure 10-11 The contact points and the area below the contact surface are not hollowed out). The advantage of this structure is that at least one of the four end faces of the piezoelectric film 108 / 208 in two directions is connected to the piezoelectric substrate 107 / 207 to ensure that there is "solid-state" contact between the device and the piezoelectric substrate 107 / 207, thereby enhancing the heat dissipation and structural stability of the device.

[0106] As an example, the ratio of the thickness of the piezoelectric film 108 / 208 to the wavelength of the target elastic wave it excites is less than 0.5, thereby obtaining a larger electromechanical coupling coefficient; further, the ratio may be less than 0.25, thereby obtaining an even larger electromechanical coupling coefficient.

[0107] As an example, the patterned electrode 103 / 203 includes: one or more combinations of forked electrodes, fan-shaped strip electrodes, circular ring-shaped strip electrodes or hexagonal plate electrodes; wherein the material of the patterned electrode 103 / 203 includes at least one of aluminum, gold, chromium, tungsten, titanium, copper and silver. Of course, the material of the patterned electrode 103 / 203 can also be an alloy composed of two or more of the above metals. Specifically, the patterned electrode 103 / 203 can be a single-layer structure or a multi-layer structure. Specifically, when the patterned electrode 103 / 203 is a forked electrode, the forked fingers in the forked electrode are arranged parallel to each other, and the arrangement direction of each forked finger is parallel to the direction of the bus bar. At the same time, each forked finger can have an inclination angle of less than ±5° in the direction perpendicular to the bus bar. Specifically, when the patterned electrode 103 / 203 is a forked electrode and the number of pairs of forked electrodes is multiple pairs, multiple pairs of the forked electrodes form a forked transducer to generate an electric field. Optionally, the acoustic wave resonator also includes: at least one pair of reflection gate electrodes 104 / 204, formed on both sides of the interdigital transducer, for limiting the acoustic wave energy by utilizing its reflection; wherein the reflection gate electrode 104 / 204 can be formed on the upper surface of the piezoelectric film 108 / 208, or on the upper surface of the piezoelectric substrate 107 / 207, which has no effect on its function.

[0108] As an example, the thickness of the patterned electrode 103 / 203 is smaller than the thickness of the piezoelectric film 108 / 208 .

[0109] As an example, the acoustic wave resonator further includes: an accelerating heat dissipation layer (not shown in the figure), which is formed at least on the upper surface of the piezoelectric film 108 / 208 and the surface of the patterned electrode 103 / 203 to accelerate the heat dissipation of the device; of course, the accelerating heat dissipation layer can also be formed on the upper surface of the entire device structure. Specifically, the accelerating heat dissipation layer is made of a high thermal conductivity material such as silicon, silicon carbide, aluminum nitride, etc. Optionally, when the acoustic wave resonator further includes a reflective gate electrode 104 / 204, the accelerating heat dissipation layer is also formed on the surface of the reflective gate electrode 104 / 204.

[0110] As an example, the target elastic waves excited by the piezoelectric film 108 / 208 include: one or more (i.e., two or more) of Rayleigh waves, horizontal shear waves, symmetric Lamb waves, antisymmetric Lamb waves, body waves, or quasi-body waves. In practical applications, when the patterned electrode is a forked electrode, the arrangement direction of the forked fingers of the forked electrode can be adjusted so that the piezoelectric film can excite one or more different types of acoustic wave modes. For example, by adjusting the arrangement direction of the forked fingers of the forked electrode, the piezoelectric film can excite one of Rayleigh waves, horizontal shear waves, symmetric Lamb waves, antisymmetric Lamb waves, body waves, and quasi-body waves, or the piezoelectric film can excite two or more of Rayleigh waves, horizontal shear waves, symmetric Lamb waves, antisymmetric Lamb waves, body waves, and quasi-body waves, and the piezoelectric film can even excite all of the above acoustic wave modes simultaneously. When the target elastic wave excited by the piezoelectric film 108 / 208 is an acoustic wave mode with a relatively low wave velocity (such as Rayleigh wave and horizontal shear wave), the acoustic wave resonator described in this embodiment uses the suspended piezoelectric film to improve device performance, such as making the device have a higher electromechanical coupling coefficient and quality factor; when the target elastic wave excited by the piezoelectric film 108 / 208 is an acoustic wave mode with a relatively high wave velocity (such as symmetric Lamb wave and antisymmetric Lamb wave), the acoustic wave resonator described in this embodiment uses the suspended piezoelectric film to confine the energy of high-order acoustic wave modes within the suspended piezoelectric film, thereby increasing the frequency and bandwidth of the device by exciting high-order acoustic wave modes, and at the same time making the device have a larger electromechanical coupling coefficient.

[0111] Embodiment 1

[0112] The suspended film type acoustic wave resonator (corresponding to the structure as shown in the figure) as described in the present invention is made of X-cut LN (lithium niobate) piezoelectric single crystal material. Fig.12 As shown in Example 1, a solid-state assembled acoustic wave resonator is fabricated using silicon as a substrate and X-cut LN piezoelectric single crystal material as a piezoelectric film (the corresponding structure is as shown in Fig.13 As shown in the figure, Example 1 is used as Comparative Example 1 to illustrate the performance of the suspended thin film acoustic wave resonator of the present invention under the zero-order horizontal shear wave SH0 mode; wherein, Example 1 differs from Comparative Example 1 only in the device structure, and the others are the same, such as the thickness of the piezoelectric film is 500nm, and the wavelength λ of the excited acoustic wave is 2μm.

[0113] Fig.14a is the electromechanical coupling coefficient K of the acoustic wave resonator described in Example 1 and Comparative Example 1 in the SH0 mode 2 The curves of the change of the in-plane propagation angle (0°-180°) show that the K of the two structures 2 The variation trend with the in-plane propagation angle is consistent, and the K of Example 1 2 Obviously greater than the K of comparative example 1 2 .

[0114] Fig.14b The electromechanical coupling coefficient K of the acoustic wave resonator in Example 1 and Comparative Example 1 in the SH0 mode is as follows: 2 The change curve of K of the two structures can be seen from the figure: 2 The variation trend with h / λ is quite different. 2 With the change of h / λ, it presents a maximum value, that is, at h / λ=0.25, K max 2 =19.8%; K of Example 1 2 As h / λ decreases, it increases rapidly. When h / λ<0.4, K of Example 1 2 The K of comparative example 1 is obviously larger than that of comparative example 1. 2 , when h / λ=0.04, K of Example 1 2 Up to 40%; it can be seen that the suspended film type acoustic wave resonator described in Example 1 can play a role in improving the electromechanical coupling coefficient in the SH0 mode, and this dispersion characteristic can be used to adjust and select the appropriate piezoelectric film thickness and interdigital electrode period.

[0115] Fig.14c This is the vibration energy diagram of the acoustic wave resonator described in Example 1 in the SH0 mode (its in-plane propagation angle is 10°). It can be seen from the figure that the SH0 elastic wave in the piezoelectric film is effectively confined inside the piezoelectric film.

[0116] Fig.14d This is a vibration energy diagram of the acoustic wave resonator in comparative example 1 in the SH0 mode (its in-plane propagation angle is 10°). It can be seen from the diagram that the SH0 elastic wave in the piezoelectric film still has a little energy leaking to the bottom substrate.

[0117] It can be seen that compared with the solid-state assembled acoustic wave resonator with Si as the substrate, the suspended thin film acoustic wave resonator of the present invention has a larger electromechanical coupling coefficient in the SH0 mode.

[0118] Embodiment 2

[0119] The suspended film type acoustic wave resonator (corresponding to the structure as shown in the figure) as described in the present invention is made of X-cut LN (lithium niobate) piezoelectric single crystal material. Fig.12 As shown in Example 2, a solid-state assembled acoustic wave resonator is fabricated using silicon as a substrate and X-cut LN piezoelectric single crystal material as a piezoelectric film (the corresponding structure is as shown in Fig.13 As shown in the figure, Example 2 is used as Comparative Example 2 to illustrate the performance of the suspended thin film acoustic wave resonator of the present invention under the zero-order symmetric Lamb wave S0 mode; wherein, Example 2 differs from Comparative Example 2 only in the device structure, and the others are the same, such as the thickness of the piezoelectric film is 500nm, and the wavelength λ of the excited acoustic wave is 2μm.

[0120] Fig.15a This is the admittance curve of the acoustic wave resonator described in Example 2 in the S0 mode. It can be seen from the figure that the S0 elastic wave in the piezoelectric film can resonate effectively.

[0121] Fig.15b This is the admittance curve of the acoustic wave resonator in Comparative Example 2 in the S0 mode. It can be seen from the figure that the S0 elastic wave in the piezoelectric film cannot form an effective resonance peak, that is, no resonance can be formed.

[0122] Fig.15c This is the vibration energy diagram of the acoustic wave resonator described in Example 2 in the S0 mode (its in-plane propagation angle is 30°). It can be seen from the figure that the S0 elastic wave in the piezoelectric film is effectively confined inside the piezoelectric film.

[0123] Fig.15d This is the vibration energy diagram of the acoustic wave resonator in comparative example 2 in the S0 mode (its in-plane propagation angle is 30°). It can be seen from the figure that the S0 elastic wave energy in the piezoelectric film is severely leaked to the Si substrate, that is, the Si substrate cannot limit the higher S0 mode of the acoustic wave.

[0124] Fig.15e The electromechanical coupling coefficient K of the acoustic wave resonator in Example 2 in the S0 mode is as h / λ changes from 0.5 to 0.04. 2 The change curve of K 2 It can reach 31%. From the variation trend, it can be seen that when the thickness of the piezoelectric film is determined, h / λ can be adjusted by changing the value of λ. When h / λ decreases, K 2 Continue to increase; obviously, this reflects the advantage of the suspended thin film acoustic wave resonator described in Example 2 in limiting the energy of high-speed acoustic waves. It can more effectively constrain the acoustic wave energy, prevent the acoustic wave energy from leaking to the lower layer, and thereby improve the electromechanical coupling coefficient of the S0 mode and the electromechanical conversion efficiency, thereby improving the bandwidth and quality factor of the acoustic wave resonator.

[0125] It can be seen that compared with the solid-state assembled acoustic wave resonator with Si as the substrate, the suspended thin film acoustic wave resonator of the present invention can excite the S0 mode with a higher sound velocity and keep the energy from leaking, and at the same time has a larger electromechanical coupling coefficient.

[0126] Embodiment 3

[0127] The suspended film type acoustic wave resonator (corresponding to the structure as shown in the figure) as described in the present invention is made of Y42°LT (lithium tantalate) piezoelectric single crystal material. Fig.12 As shown in Example 3, a solid-state assembled acoustic wave resonator is fabricated using silicon as a substrate and Y42°LT piezoelectric single crystal material as a piezoelectric film (the corresponding structure is as shown in Fig.13As shown) is used as comparative example 3, to illustrate the performance of the suspended thin film acoustic wave resonator of the present invention under the zero-order horizontal shear wave SH0 mode; wherein, Example 3 and comparative example 3 differ only in the device structure, and the others are the same, such as the thickness of the piezoelectric film is 500nm, and the wavelength λ of the excited acoustic wave is 2μm.

[0128] Fig.16a is the electromechanical coupling coefficient K of the acoustic wave resonator described in Example 3 and Comparative Example 3 in the SH0 mode 2 The curves of the change of the in-plane propagation angle (0°-180°) show that the K of the two structures 2 The variation trend with the in-plane propagation angle is consistent, and the K of Example 3 2 Obviously greater than the K of comparative example 3 2 .

[0129] Fig.16b The electromechanical coupling coefficient K of the acoustic wave resonator in Example 3 and Comparative Example 3 in the SH0 mode is as follows: 2 The change curve of K of the two structures can be seen from the figure: 2 The variation trend with h / λ is quite different. The acoustic wave resonator described in Comparative Example 3 does not have obvious dispersion in the SH0 mode, that is, K 2 It does not change with h / λ and remains at about 8.6%. However, the acoustic wave resonator described in Example 3 has a K value of 0. 2 As h / λ decreases, it increases rapidly. When h / λ<0.15, K 2 >15%, which shows that the acoustic wave resonator described in Example 3 can play a role in improving the electromechanical coupling coefficient, and this dispersion characteristic can be used to adjust and select the appropriate piezoelectric film thickness and interdigital electrode period.

[0130] Fig.16c This is the vibration energy diagram of the acoustic wave resonator described in Example 3 in the SH0 mode (its in-plane propagation angle is 0°). It can be seen from the figure that the SH0 elastic wave in the piezoelectric film is effectively confined inside the piezoelectric film.

[0131] Fig.16d This is a vibration energy diagram of the acoustic wave resonator described in comparative example 3 in the SH0 mode (its in-plane propagation angle is 0°). It can be seen from the diagram that the SH0 elastic wave in the piezoelectric film still has a little energy leaking to the substrate.

[0132] It can be seen that compared with the solid-state assembled acoustic wave resonator with Si as the substrate, the suspended thin film acoustic wave resonator of the present invention has a larger electromechanical coupling coefficient in the SH0 mode.

[0133] Embodiment 4

[0134] The suspended film type acoustic wave resonator (corresponding to the structure as shown in the figure) as described in the present invention is made of Y128°LN (lithium niobate) piezoelectric single crystal material. Fig.12 As shown in Example 4, a solid-state assembled acoustic wave resonator is fabricated using silicon as a substrate and Y128°LN piezoelectric single crystal material as a piezoelectric film (the corresponding structure is as shown in Fig.13 As shown in the figure, Example 4 is used as a comparative example 4 to illustrate the performance of the suspended thin film acoustic wave resonator of the present invention under the first-order antisymmetric Lamb wave A1 mode; wherein, Example 4 differs from Comparative Example 4 only in the device structure, and the others are the same, such as the thickness of the piezoelectric film is 500nm, and the wavelength λ of the excited acoustic wave is 2μm.

[0135] Fig.17a The electromechanical coupling coefficient K of the acoustic wave resonator in the A1 mode is as follows: the acoustic wave wavelength λ of the acoustic wave resonator in Example 4 changes from 0.5 to 0.04 2 The change curve of K shows that the A1 mode shows obvious dispersion. 2 It continues to increase as h / λ decreases. When h / λ<0.2, K 2 >20%, the operating frequency covers 3.5~5.3GHz; when h / λ<0.0625, K 2 It can reach more than 50%, and the operating frequency is also in the high frequency range of 3.5 to 4.5 GHz; moreover, at h / λ = 0.12, K 2 There is a trend of accelerating increase, which is very suitable for the demand for high-frequency and large-bandwidth filters in 5G communications.

[0136] Fig.17b This is the admittance curve of the acoustic wave resonator described in Example 4 in the A1 mode. It can be seen from the figure that the A1 elastic wave in the piezoelectric film can resonate effectively.

[0137] Fig.17c This is the admittance curve of the acoustic wave resonator in Comparative Example 4 in the A1 mode. It can be seen from the figure that the A1 elastic wave in the piezoelectric film cannot form an effective resonance peak, that is, no resonance can be formed.

[0138] Fig.17d This is the vibration energy diagram of the acoustic wave resonator described in Example 4 in the A1 mode (its in-plane propagation angle is 0°). It can be seen from the figure that the A1 elastic wave in the piezoelectric film can be effectively confined inside the piezoelectric film.

[0139] Fig.17e This is the vibration energy diagram of the acoustic wave resonator in comparative example 4 in the A1 mode (its in-plane propagation angle is 0°). It can be seen from the figure that the A1 elastic wave energy in the piezoelectric film is severely leaked to the substrate, that is, the Si substrate cannot limit the higher A1 mode of the acoustic wave.

[0140] It can be seen that compared with the solid-state assembled acoustic wave resonator with Si as the substrate, the suspended thin film acoustic wave resonator of the present invention can excite the A1 mode with a higher sound velocity and keep the energy from leaking, and at the same time has a larger electromechanical coupling coefficient.

[0141] Embodiment 5

[0142] The suspended film type acoustic wave resonator as described in the present invention is made of Z-cut LN (lithium niobate) piezoelectric single crystal material (corresponding structure as shown in FIG. Fig.12 As shown in Example 5, a solid-state assembled acoustic wave resonator is fabricated using silicon as a substrate and a Z-cut LN piezoelectric single crystal material as a piezoelectric film (the corresponding structure is as shown in Fig.13 As shown in the figure, Example 5 is used as Comparative Example 5 to illustrate the performance of the suspended thin film acoustic wave resonator of the present invention under the first-order antisymmetric Lamb wave A1 mode; wherein, Example 5 differs from Comparative Example 5 only in the device structure, and the others are the same, such as the thickness of the piezoelectric film is 500nm, and the wavelength λ of the excited acoustic wave is 2μm.

[0143] Fig.18a The electromechanical coupling coefficient K of the acoustic wave resonator in the A1 mode in Example 5 is as follows: the acoustic wave wavelength λ changes from 0.5 to 0.04 2 The change curve of K shows that the A1 mode shows obvious dispersion. 2 It continues to increase as h / λ decreases. When h / λ<0.15, K 2 >20%, the operating frequency covers 3.6~4.7GHz; when h / λ=0.04, K 2 It can reach 40%, and the operating frequency is also in the high frequency range of 3.5 to 4.3 GHz, which is also very suitable for the needs of 5G communications for high-frequency and large-bandwidth filters.

[0144] Fig.18b This is the admittance curve of the acoustic wave resonator described in Example 5 in the A1 mode. It can be seen from the figure that the A1 elastic wave in the piezoelectric film can resonate effectively.

[0145] Fig.18c This is the admittance curve of the acoustic wave resonator in Comparative Example 5 in the A1 mode. It can be seen from the figure that the A1 elastic wave in the piezoelectric film cannot form an effective resonance peak, that is, no resonance can be formed.

[0146] Fig.18d This is the vibration energy diagram of the acoustic wave resonator described in Example 5 in the A1 mode (its in-plane propagation angle is 30°). It can be seen from the figure that the A1 elastic wave in the piezoelectric film can be effectively confined inside the piezoelectric film.

[0147] Fig.18eThis is the vibration energy diagram of the acoustic wave resonator in comparative example 5 in the A1 mode (its in-plane propagation angle is 30°). It can be seen from the figure that the A1 elastic wave energy in the piezoelectric film is severely leaked to the bottom substrate, that is, the Si substrate cannot limit the higher A1 mode of the acoustic wave.

[0148] It can be seen that compared with the solid-state assembly type acoustic wave resonator with Si as the substrate, the suspended film type acoustic wave resonator of the present invention can excite the A1 mode with a higher sound velocity and keep the energy from leaking, and at the same time has a larger electromechanical coupling coefficient. Fig.18b It can be seen that the suspended film type acoustic wave resonator described in this example can not only excite and confine the high-order first-order antisymmetric Lamb wave mode, but also excite and confine the higher-order quasi-bulk wave A3 mode. Fig.18f It can also be seen from the vibration energy diagram (with an in-plane propagation angle of 30°) that the A3 elastic wave in the piezoelectric film can be effectively confined inside the piezoelectric film; among them, the resonant frequency of the first-order antisymmetric Lamb wave mode is 5.9 GHz, and the electromechanical coupling coefficient K 2 is 16.78%; the resonant frequency of the quasi-bulk wave mode is 13.8 GHz, and the electromechanical coupling coefficient K 2 This means that it is possible to expand resonators and filters to higher frequency bands and no longer be limited to the crowded 3 GHz band.

[0149] In summary, an acoustic wave resonator and a preparation method thereof of the present invention have the following beneficial effects: the preparation method of the present invention utilizes ion implantation and post-annealing to form a high defect density damage layer inside the piezoelectric material layer, and then removes the high defect density damage layer through an etching window to obtain a suspended piezoelectric film, without the need for complex processes such as bonding, transfer, peeling, and polishing, thereby reducing the complexity of preparation. The preparation method of the present invention has a simple process, high material utilization rate, and low manufacturing cost, which is beneficial to improving the bandwidth and coverage frequency band of the resonator and filter, and is suitable for large-scale production and use. The present invention utilizes the extreme mismatch between the suspended piezoelectric film and the air gap acoustic impedance, and effectively limits the energy of the high-order acoustic wave mode with a higher sound velocity to the piezoelectric film, thereby improving the frequency, electromechanical coupling coefficient, bandwidth and quality factor of the device to meet the needs of 5G communications. Therefore, the present invention effectively overcomes the various shortcomings in the prior art and has a high industrial utilization value.

[0150] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing an acoustic wave resonator, characterized in that: The preparation method comprises: a) providing a piezoelectric material layer; b) performing ion implantation and post-annealing treatment on at least part of the upper surface of the piezoelectric material layer to form a high defect density damaged layer with a preset thickness at a preset depth in the piezoelectric material layer; wherein the ion implantation is performed in multiple times, the doses of the multiple ion implantations are the same, the energies are different, and the energy values ​​of the multiple ion implantations decrease in sequence, and the process temperature of the post-annealing is not higher than 550° C. and the process time is not more than 4 hours, so as to restore the defects introduced into the piezoelectric material layer by the ion implantation and aggregate the defects, but not to cause the formed high defect density damaged layer to bubble and crack; c) forming at least one corrosion window on the upper surface of the piezoelectric material layer to expose the high defect density damaged layer; d) removing at least a portion of the high defect density damaged layer based on the etching window to form an air gap in the piezoelectric material layer; wherein the air gap divides the piezoelectric material layer into a piezoelectric substrate and a piezoelectric film, the piezoelectric film is located above the air gap, and the piezoelectric film and the piezoelectric substrate are in contact at the edge of the air gap; e) forming a patterned electrode on the upper surface of the piezoelectric film; The order of executing the steps in the preparation method is a), b), c), d), e), a), e), b), c), d), a), b), e), c), d), or a), b), c), e), d); when the order of executing the steps in the preparation method is a), e), b), c), d), a), b), e), c), d), or a), b), c), e), d), e) is to form a patterned electrode on the upper surface of the piezoelectric material layer.

2. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: Before forming the corrosion window, the preparation method also includes: a step of forming a first protective layer on the surface of the piezoelectric material layer or the surface of the piezoelectric material layer and the surface of the patterned electrode; after forming the corrosion window, the preparation method also includes: a step of removing the first protective layer; wherein the material of the first protective layer includes any one of silicon dioxide, silicon nitride, chromium, and gold.

3. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: Before forming the air gap, the preparation method also includes: a step of forming a second protective layer on the surface of the piezoelectric material layer or the surface of the piezoelectric material layer and the surface of the patterned electrode; after forming the air gap, the preparation method also includes: a step of removing the second protective layer; wherein the material of the second protective layer includes any one of silicon dioxide, silicon nitride, chromium, and gold.

4. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: The preparation method further comprises: forming a heat dissipation accelerating layer at least on the upper surface of the piezoelectric film and the surface of the patterned electrode.

5. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: b) performing ion implantation and post-annealing treatment on the entire upper surface of the piezoelectric material layer to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer; At this time, d) is to remove a portion of the high defect density damaged layer based on the etching window to form an air gap in the piezoelectric material layer.

6. The method for preparing an acoustic wave resonator according to claim 5, characterized in that: c) The method for forming the corrosion window comprises: The position of the air gap is defined in the piezoelectric material layer, and a patterned window mask is formed on the upper surface of the piezoelectric material layer, wherein an opening pattern defining the shape and position of the etching window is formed in the patterned window mask, and the opening pattern is located in the defined area where the air gap is located; Etching the piezoelectric material layer based on the patterned window mask to form at least one corrosion window exposing the high defect density damaged layer; The patterned window mask is removed.

7. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: b) performing ion implantation and post-annealing treatment on a portion of the upper surface of the piezoelectric material layer to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer; At this time, d) is to remove all of the high defect density damaged layer based on the etching window to form air gaps in the piezoelectric material layer.

8. The method for preparing an acoustic wave resonator according to claim 7, characterized in that: b) The method for forming the high defect density damaged layer comprises: Forming a patterned implantation mask on the upper surface of the piezoelectric material layer, wherein an opening pattern defining the shape and position of the high defect density damaged layer is formed in the patterned implantation mask; Performing ion implantation and post-annealing treatment on the piezoelectric material layer based on the patterned implantation mask to form a high defect density damage layer with a preset thickness at a preset depth in the piezoelectric material layer; removing the patterned implant mask; At this time, the method of forming the corrosion window in c) includes: Forming a patterned window mask on the upper surface of the piezoelectric material layer, wherein an opening pattern defining the shape and position of the etching window is formed in the patterned window mask; Etching the piezoelectric material layer based on the patterned window mask to form at least one corrosion window exposing the high defect density damaged layer; The patterned window mask is removed.

9. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: The contact between the piezoelectric film and the piezoelectric substrate at the edge of the air gap is defined based on the shape and position of the corrosion window; wherein the piezoelectric film and the piezoelectric substrate have at least one contact point at the edge of the air gap, and / or the piezoelectric film and the piezoelectric substrate have at least one contact surface at the edge of the air gap.

10. The method for preparing an acoustic wave resonator according to claim 1, characterized in that: The patterned electrodes include: one or more combinations of interdigitated electrodes, fan-shaped strip electrodes, annular strip electrodes or hexagonal plate electrodes.

11. The method for preparing an acoustic wave resonator according to claim 10, characterized in that: When the patterned electrodes are interdigital electrodes and there are multiple pairs of interdigital electrodes, the multiple pairs of interdigital electrodes form an interdigital transducer.

12. The method for preparing an acoustic wave resonator according to claim 11, characterized in that: The manufacturing method further comprises the step of forming a reflective gate electrode on the upper surface of the piezoelectric film or the upper surface of the piezoelectric substrate at both sides of the interdigital transducer.

13. An acoustic wave resonator prepared by the preparation method according to any one of claims 1 to 12, characterized in that: The acoustic wave resonator comprises: a piezoelectric material layer; An air gap with a preset thickness is formed at a preset depth of the piezoelectric material layer based on an etching window; the air gap divides the piezoelectric material layer into a piezoelectric substrate and a piezoelectric film, the piezoelectric film is located above the air gap, and the piezoelectric film and the piezoelectric substrate are in contact at the edge of the air gap; The patterned electrode is formed on the upper surface of the piezoelectric film.

14. The acoustic wave resonator according to claim 13, characterized in that The target elastic waves excited by the piezoelectric film include: one or more of: Rayleigh waves, horizontal shear waves, symmetric Lamb waves, antisymmetric Lamb waves, body waves or quasi-body waves.

15. The acoustic wave resonator according to claim 13, characterized in that The piezoelectric film and the piezoelectric substrate have at least one contact point at an edge of the air gap, and / or the piezoelectric film and the piezoelectric substrate have at least one contact surface at an edge of the air gap.

16. The acoustic wave resonator according to claim 13, characterized in that The patterned electrodes include: one or more combinations of interdigitated electrodes, fan-shaped strip electrodes, annular strip electrodes or hexagonal plate electrodes.

17. The acoustic wave resonator according to claim 16, characterized in that When the patterned electrodes are interdigital electrodes and there are multiple pairs of interdigital electrodes, the multiple pairs of interdigital electrodes form an interdigital transducer.

18. The acoustic wave resonator according to claim 17, characterized in that The acoustic wave resonator further includes: at least one pair of reflective gate electrodes formed on the upper surface of the piezoelectric film or the upper surface of the piezoelectric substrate at both sides of the interdigital transducer.

19. The acoustic wave resonator according to claim 13, characterized in that The thickness of the patterned electrode is smaller than the thickness of the piezoelectric film, and the ratio of the thickness of the piezoelectric film to the wavelength of the target elastic wave excited by the piezoelectric film is smaller than 0.

5.

20. The acoustic wave resonator according to claim 13, characterized in that The acoustic wave resonator further includes: an accelerating heat dissipation layer formed at least on the upper surface of the piezoelectric film and the surface of the patterned electrode.

21. The acoustic wave resonator according to claim 13, characterized in that The material of the piezoelectric material layer includes: any one of quartz, aluminum nitride, zinc oxide, lithium tantalate, lithium niobate, lithium tetraborate, bismuth germanate, bismuth silicate, lanthanum gallium silicate, and zirconium titanium lead acid.

Citation Information

Patent Citations

  • Film bulk acoustic resonator structure and manufacture method thereof

    CN103296992A

  • Piezoelectric device and method for manufacturing the same

    CN104079251A

  • Semiconductor device and manufacturing method thereof

    CN105609419A

  • Single-crystal piezoelectric thin film-based sound wave resonator and fabrication method thereof

    CN108493326A

  • Cavity type bulk acoustic wave resonator without preparing sacrificial layer and preparation method of cavity type bulk acoustic wave resonator

    CN109981070A