Polymer composition and method for producing the same, film-forming agent and cosmetic composition

By controlling the proportion and type of polymer monomers, a polymer composition with excellent oil resistance was developed, which solved the problem of diffusion and powder loss of cosmetics or medicines during use, and reduced the content of harmful substances and improved the stability of the product Sex and safety.

CN112708007BActive Publication Date: 2024-11-01LG HOUSEHOLD & HEALTH CARE LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011144061.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-25
Filing Date
2020-10-23
Publication Date
2024-11-01
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Functional polymers in existing cosmetics or medicines are prone to spread or become powder and fall into powder during use due to sebum, tears and sweat, and may contain harmful substances, affecting the effectiveness and safety of use.

Method used

Develop a polymer composition to prepare a polymer composition with excellent oil resistance by controlling the proportion and type of specific monomers, and to make film-forming agents or cosmetics to ensure that there is no diffusion or powder loss during use. And minimize the content of methanol and formaldehyde.

Benefits of technology

The oil resistance and powder removal resistance of polymer compositions are achieved, the stability and safety of cosmetics or medicines are ensured during use, and the presence of harmful substances is reduced, and the use effect and safety of the product are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112708007B_ABST
    Figure CN112708007B_ABST
Patent Text Reader

Abstract

The present application relates to a polymer composition, a film-forming agent, a cosmetic composition and a method for producing the polymer composition. The polymer composition comprises a polymer, wherein the polymer comprises: a homopolymer having a solubility parameter of 11.0 (cal / cm 3 ) 1 / 2 The first monomer polymerization unit above; and the solubility parameter of the homopolymer is less than 11.0 (cal / cm 3 ) 1 / 2 The second monomer polymerization unit is contained in the polymer, the proportion of the first monomer polymerization unit in the polymer is in the range of 1 to 40 weight %, and the polymer contains 150 to 4000 parts by weight of the second monomer polymerization unit relative to 100 parts by weight of the first monomer polymerization unit. The purpose of the present application is to provide a polymer composition and a film-forming agent or cosmetics made using the polymer composition, wherein the polymer composition has excellent oil resistance and can form cosmetics that do not spread or fall off during use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority based on Korean Patent Application Nos. 10-2019-0133543 and 10-2019-0133542 filed on October 25, 2019, and incorporates the contents disclosed in the Korean patent application documents as part of this specification.

[0002] The present application relates to a polymer composition, a film-forming agent, a cosmetic composition and a method for producing the polymer composition. Background Art

[0003] Functional polymers are sometimes required in the production of cosmetics, pharmaceuticals, etc. For example, functional polymers are required in the production of cosmetics or pharmaceuticals that are directly applied to the skin, such as smoky makeup (mascara).

[0004] Such functional polymers are required to have resistance to oily components such as sebum, that is, oil resistance, and may also be required to have appropriate spreadability or film-forming ability.

[0005] In addition, the functional polymer may be required to prevent the cosmetics or medicines from spreading due to sebum, tears, sweat, etc. during use, and prevent them from turning into powder and falling off.

[0006] In addition, since cosmetics and medicines are often used in direct contact with the human body, they should not contain harmful substances. Summary of the invention

[0007] The present application provides a polymer composition, a film-forming agent, a cosmetic composition, and a method for producing the polymer composition. The purpose of the present application is to provide a polymer composition and a film-forming agent or cosmetics etc. produced using the polymer composition, wherein the polymer composition has excellent oil resistance and can form cosmetics etc. that do not spread or fall off during use.

[0008] The polymer composition of the present application may include only the polymer described below, or may include the polymer described below and other components.

[0009] For example, in the polymer composition, based on weight, the ratio of the polymer described later can be about more than 5 weight %, more than 10 weight %, more than 15 weight %, more than 20 weight %, more than 25 weight %, more than 30 weight %, more than 35 weight %, more than 40 weight %, more than 45 weight %, more than 50 weight %, more than 55 weight %, more than 60 weight %, more than 65 weight %, more than 70 weight %, more than 75 weight %, more than 80 weight %, more than 85 weight %, more than 90 weight % or more than 95 weight %. The polymer composition can only be composed of the polymer, so the ratio of the polymer can be about less than 100 weight %, less than 99 weight % or less than 98 weight %. When the composition is dispersed or dissolved in the solvent by manufacturing the polymer composition, the ratio of the polymer is the ratio calculated without counting the weight of the solvent.

[0010] The polymer contained in the polymer composition contains polymer units of specific types of monomers, and the ratio of the polymer units can be adjusted. By controlling the types and ratios of these monomers, a polymer composition that can form a film-forming agent, cosmetic or pharmaceutical product with desired physical properties such as oil resistance and prevention of diffusion or powdering during use can be obtained.

[0011] The ratio of a certain monomer mentioned in this specification (for example, weight % or weight part, etc.) may refer to the ratio of the monomer used when manufacturing a polymer, or the ratio of polymerization units of the monomer contained in the polymer.

[0012] The polymer may include: a solubility parameter of 11 (cal / cm 3 ) 1 / 2 The polymerized unit of the first monomer above; and a solubility parameter less than 11 (cal / cm 3 ) 1 / 2 The polymerized units of the second monomer.

[0013] In the present specification, a polymerized unit of a certain monomer or compound means a form in which the monomer or compound is contained in a polymer as a monomer unit after a polymerization reaction.

[0014] The term solubility parameter refers to the solubility parameter of a homopolymer produced by polymerizing the monomer, by which the degree of hydrophilicity and hydrophobicity of the monomer can be determined. The method for obtaining the solubility parameter is not particularly limited and can be obtained by methods known in the art. For example, the solubility parameter can be calculated or obtained by the so-called group contribution method known in the art, the Method of Hoftyzer and Van Krevelen.

[0015] Compared to the second monomer, the first monomer is a relatively hydrophilic monomer, which can help ensure the desired oil resistance. In other examples, the solubility parameter of the first monomer can also be about 11.5 (cal / cm 3 ) 1 / 2 Above, 12(cal / cm 3 ) 1 / 2 Above, 12.5 (cal / cm 3 ) 1 / 2 Above, 13(cal / cm 3 ) 1 / 2 Above, 13.5 (cal / cm 3 ) 1 / 2 Above or 14 (cal / cm 3 ) 1 / 2 Above, or about 20 (cal / cm 3 ) 1 / 2 Below, 19(cal / cm 3 ) 1 / 2 Below, 18(cal / cm 3 ) 1 / 2 Below, 17(cal / cm 3 ) 1 / 2 Below, 16 (cal / cm 3 ) 1 / 2 Below, 15(cal / cm 3 ) 1 / 2 Below, 14(cal / cm 3 ) 1 / 2 Below, 13(cal / cm 3 ) 1 / 2 Below or 12.5 (cal / cm 3 ) 1 / 2 the following.

[0016] As the first monomer, a monomer appropriately selected from monomers known to have the above solubility parameter may be used.

[0017] For example, as the first monomer, the glass transition temperature (hereinafter, Tg) may be in the range of -40° C. to 400° C. The Tg of a monomer mentioned in the present specification is a well-known Tg for a homopolymer produced from the monomer.

[0018] In other examples, the Tg of the first monomer can be about -35°C or more, -30°C or more, -25°C or more, -20°C or more, -15°C or more, -10°C or more, -5°C or more, 0°C or more, 10°C or more, 20°C or more, 30°C or more, 40°C or more, 50°C or more, 60°C or more, 70°C or more, 80°C or more, 90°C or more, 100°C or more, 110°C or more, 120°C or more, 130°C or more, 140°C or more, 150°C or more, 160°C or more, 170°C or more, 180°C or more, 190°C or more, 200°C or more, or 210°C or more, or about 390°C or less, 380°C or less, 370°C or less, 360°C or less, 350°C or less, 340°C or less, 330°C or less, 320°C or less, 310°C or less, 300°C or less, 290°C or less, 280°C or less, 270°C or less, 260°C or less, 250°C or less, 240°C or less, 230°C or less, 220°C or less, 210°C or less, 200°C or less, 190°C or less, 180°C or less, 170°C or less, 160°C or less, 150°C or less, 140°C or less, 130°C or less, 120°C or less, 110°C or less, 100°C or less, 90°C or less, 80°C or less, 70°C or less, 60°C or less, 50°C or less, 40°C or less, 30°C or less, 20°C or less, 10°C or less, 5°C or less, 0°C or less, -5°C or less, or -10°C or less.

[0019] As the first monomer, for example, a hydroxyl-containing monomer such as 2-hydroxyalkyl (meth)acrylate; a polymerizable heterocyclic monomer such as vinyl pyrrolidone; a (meth)acrylamide-based monomer such as (meth)acrylamide, N-alkyl (meth)acrylamide or N,N-dialkyl (meth)acrylamide; an acidic monomer such as (meth)acrylic acid, maleic acid or itaconic acid; glyceryl (meth)acrylate; or a monomer containing an alkylene oxide unit, etc. Among the monomers, an acidic monomer can be suitable as the first monomer.

[0020] In the present specification, the term (meth)acrylic acid means acrylic acid or methacrylic acid.

[0021] In this specification, unless otherwise specified, the term alkyl or alkane group refers to a linear, branched or cyclic alkyl or alkane group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms or 1 to 4 carbon atoms. The alkyl or alkane group may be an alkyl or alkane group arbitrarily substituted with one or more substituents, or an unsubstituted alkyl or alkane group.

[0022] As mentioned above, as the monomer including an alkylene oxide unit, for example, a monomer represented by the following Chemical Formula 1 or 2 can be exemplified.

[0023] [Chemical formula 1]

[0024]

[0025] In Chemical Formula 1, Q is hydrogen or an alkyl group, U is an alkylene group, Z is hydrogen or an alkyl group, and m is an arbitrary number.

[0026] [Chemical formula 2]

[0027]

[0028] In Chemical Formula 2, Q is hydrogen or an alkyl group, A and U are each independently an alkylene group, X is hydrogen, an alkyl group, a hydroxyl group or a cyano group, and n is an arbitrary number.

[0029] In Chemical Formulae 1 and 2, the alkylene group may be an alkylene group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The alkylene group may be linear, branched, or cyclic. The alkylene group may be arbitrarily substituted with one or more substituents.

[0030] In Chemical Formulae 1 and 2, the alkyl groups present in Q and Z include alkyl groups having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The alkyl group may be linear, branched, or cyclic. In addition, the alkyl group may be arbitrarily substituted with one or more substituents.

[0031] In Chemical Formulae 1 and 2, m and n are arbitrary numbers, for example, and may be independently values ​​within the range of 1 to 100, 1 to 90, 1 to 80, 1 to 70, 1 to 60, 1 to 50, 1 to 40, 1 to 30, 1 to 20, 1 to 16, or 1 to 12, respectively.

[0032] In one example, as the first monomer, a compound in which Q in Chemical Formula 1 is hydrogen or an alkyl group having 1 to 4 carbon atoms, U is an alkylene group having 1 to 4 carbon atoms, Z is hydrogen or an alkyl group having 1 to 4 carbon atoms, and m is approximately 1 to 30 can be used, but is not limited thereto.

[0033] In the polymer, the ratio of the polymerization unit of the first monomer as described above can be controlled by taking target physical properties such as oil resistance into consideration.

[0034] For example, the proportion of the polymerized units of the first monomer in the total polymerized units included in the polymer may be about 1 to 40 wt%. In other examples, the proportion may be about 1.5 wt% or more, 2 wt% or more, 2.5 wt% or more, 3 wt% or more, 3.5 wt% or more, 4.5 wt% or more, 5 wt% or more, 5.5 wt% or more, 6 wt% or more, 6.5 wt% or more, 7 wt% or more, 7.5 wt% or more, 8 wt% or more, 8.5 wt% or more, 9 wt% or more, 9.5 wt% or more, 10 wt% or more, 11 wt% or more, 12 wt% or more, 13 wt% or more, 14 wt% or more, or 14.5 wt% or more, or about 39 wt% or less, 38 wt% or less, 37 wt% or less, 36 wt% or less, 35 wt% or less. %, 34 wt %, 33 wt %, 32 wt %, 31 wt %, 30 wt %, 29 wt %, 28 wt %, 27 wt %, 26 wt %, 25 wt %, 24 wt %, 23 wt %, 22 wt %, 21 wt %, 20 wt %, 19 wt %, 18 wt %, 17 wt %, 16 wt %, 15 wt %, 14 wt %, 13 wt %, 12 wt %, 11 wt %, 10 wt %, 9 wt %, 8 wt %, 7 wt %, 6 wt % or 5.5 wt %. Under this ratio, a polymer composition with a desired physical property can be provided. For example, the higher the ratio of the polymerized unit of the first monomer, the more favorable the oil resistance can be. However, since the first monomer is a relatively hydrophilic monomer, it exhibits a thickening effect, for example, in an emulsion polymerization process in an aqueous solvent, and thus it is not easy to include the first monomer in the polymer at an appropriate level. However, when the so-called seed emulsion polymerization method is used, a polymer composition containing a relatively high proportion of the first monomer as described above can also be effectively manufactured.

[0035] Therefore, in one example, the polymer may be a seed emulsion polymer. The seed emulsion polymer refers to a polymer formed by seed emulsion polymerization. Such seed emulsion polymerization may also be performed in the manner described in the present specification as described later.

[0036] Compared to the first monomer, the second monomer is a relatively hydrophobic monomer. In other examples, the solubility parameter of the second monomer can also be about 10.5 (cal / cm 3 ) 1 / 2 Below, 10(cal / cm 3 ) 1 / 2 Below, 9.5 (cal / cm 3) 1 / 2 Below or 9 (cal / cm 3 ) 1 / 2 Below, or can be about 4 (cal / cm 3 ) 1 / 2 Above, 5(cal / cm 3 ) 1 / 2 Above, 6 (cal / cm 3 ) 1 / 2 Above, 7(cal / cm 3 ) 1 / 2 Above, 8(cal / cm 3 ) 1 / 2 Above, 8.5 (cal / cm 3 ) 1 / 2 Above, 9(cal / cm 3 ) 1 / 2 Above, 9.5 (cal / cm 3 ) 1 / 2 Above or 10(cal / cm 3 ) 1 / 2 above.

[0037] As the second monomer, a monomer appropriately selected from monomers known to have the above solubility parameter may be used. Such a second monomer is included in the polymer together with the first monomer, thereby helping to form a film-forming agent, cosmetic or medicine that ensures oil resistance and does not powder or spread.

[0038] As the monomer that can be used as the second monomer, there can be exemplified an alkyl (meth) acrylate or an aromatic (meth) acrylate. In the present application, the term (meth) acrylate may refer to either an acrylate or a methacrylate.

[0039] As the alkyl group contained in the alkyl (meth)acrylate, there can be mentioned a linear, branched or cyclic alkyl group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms or 2 to 8 carbon atoms, and the alkyl group may be arbitrarily substituted with one or more substituents. As such a monomer, there can be mentioned ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, amyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, n-octyl (meth)acrylate, isobornyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate or lauryl (meth)acrylate, but are not limited thereto.

[0040] As the aromatic (meth)acrylate, aryl (meth)acrylate or aryl alkyl (meth)acrylate can be exemplified. The aryl group or aryl alkyl group may be, for example, an aryl group having 6 to 24 carbon atoms, 6 to 18 carbon atoms, or 6 to 12 carbon atoms. In addition, the alkyl group of the arylalkyl group may be, for example, an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The alkyl group may be linear, branched, or cyclic, and the alkyl or aryl group may be arbitrarily substituted with one or more substituents.

[0041] Examples of the aryl group or arylalkyl group include, but are not limited to, phenyl, phenethyl, phenylpropyl, and naphthyl.

[0042] As the second monomer, for example, a monomer represented by the following Chemical Formula 3 may be used.

[0043] [Chemical formula 3]

[0044]

[0045] In Chemical Formula 3, Q is hydrogen or an alkyl group, and B may be a linear or branched alkyl group having 2 or more carbon atoms, an alicyclic hydrocarbon group, or an aromatic substituent such as the aryl group or arylalkyl group.

[0046] In Chemical Formula 3, the alkyl group present in Q may be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The alkyl group may be linear, branched, or cyclic. The alkyl group may be arbitrarily substituted with one or more substituents.

[0047] In Chemical Formula 3, B may be a linear or branched alkyl group having 2 or more carbon atoms, 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, or 2 to 10 carbon atoms.

[0048] In other examples, B in Chemical Formula 3 may be an alicyclic hydrocarbon group, for example, an alicyclic hydrocarbon group having 3 to 20 carbon atoms, 3 to 16 carbon atoms, or 6 to 12 carbon atoms, and examples of such hydrocarbon groups include alicyclic alkyl groups having 3 to 20 carbon atoms, 3 to 16 carbon atoms, or 6 to 12 carbon atoms, such as cyclohexyl or isobornyl. Compounds having an alicyclic hydrocarbon group as described above are also known to be relatively hydrophobic compounds.

[0049] In order to ensure desired physical properties, at least two or more monomers may be mixed and used as the second monomer.

[0050] For example, as the second monomer, a monomer (A) having a relatively high glass transition temperature (hereinafter, Tg) and a monomer (B) having a relatively low Tg can be used. Therefore, for example, the polymer may include a monomer (A) polymerization unit having a Tg of 20°C or more and a monomer (B) polymerization unit having a Tg of less than 20°C as the second monomer polymerization unit.

[0051] The Tg of a monomer referred to in this specification is a well-known Tg of a homopolymer produced from the monomer.

[0052] In other examples, the Tg of the monomer (A) may also be about 25°C or more, 30°C or more, 35°C or more, 40°C or more, 45°C or more, 50°C or more, 55°C or more, 60°C or more, 65°C or more, 70°C or more, 75°C or more, 80°C or more, 85°C or more, 90°C or more, 95°C or more, or about 150°C or less, 145°C or less, 140°C or less, 135°C or less, 130°C or less, 125°C or less, 120°C or less, 115°C or less, 110°C or less, 105°C or less, 100°C or less, 95°C or less, 90°C or less, 85°C or less, 80°C or less, 75°C or less, or 70°C or less. In addition, in other examples, the Tg of monomer (B) may be 15°C or less, 10°C or less, 5°C or less, 0°C or less, -5°C or less, -10°C or less, -15°C or less, -20°C or less, -25°C or less, -30°C or less, -35°C or less, -40°C or less, or may be -150°C or more, -145°C or more, -140°C or more, -135°C or more, -130°C or more, -125°C or more, -120°C or more, -115°C or more, -110°C or more, -105°C or more, -100°C or more, -95°C or more, -90°C or more, -85°C or more, -80°C or more, -75°C or more, -70°C or more, -65°C or more, -60°C or more, or -55°C or more.

[0053] When the two monomers described above are mixed and used as the second monomer, the Tg of the entire polymer can be maintained at an appropriate level, and it is advantageous to form a polymer having both oil resistance and other desired physical properties (for example, prevention of diffusion or powdering).

[0054] As the monomer (A) and the monomer (B), appropriate kinds can be selected from the monomers mentioned as the second monomer by considering Tg that the monomer has.

[0055] For example, as the monomer (A), a compound in which Q in the chemical formula 3 is an alkyl group, such as an alkyl group or methyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, and B is a linear or branched alkyl group having 2 or more carbon atoms can be used. In this case, the alkyl group of B can be a linear or branched alkyl group having 2 to 4 carbon atoms.

[0056] For example, as the monomer (B), a compound in which Q in the chemical formula 3 is hydrogen and B is a linear or branched alkyl group having 2 or more carbon atoms, 4 or more carbon atoms, or 6 or more carbon atoms can be used. In this case, the upper limit of the number of carbon atoms of the alkyl group of B is not particularly limited, and for example, can be approximately 20, 18, 16, 14, 12, or 10.

[0057] In the polymer, the ratio of the second monomer polymerization unit relative to 100 parts by weight of the first monomer polymerization unit can be in the range of 150 to 4000 parts by weight. In other examples, the ratio can also be about 200 parts by weight or more, 250 parts by weight or more, 300 parts by weight or more, 350 parts by weight or more, 400 parts by weight or more, 450 parts by weight or more, 500 parts by weight or more, 550 parts by weight or more, 600 parts by weight or more, 650 parts by weight or more, 700 parts by weight or more, 750 parts by weight or more, 800 parts by weight or more, 850 parts by weight or more, 900 parts by weight or more, 950 parts by weight or more, 1000 parts by weight or more, 1100 parts by weight or more, 1200 parts by weight or more, 1300 parts by weight or more, 1400 parts by weight or more, 1500 parts by weight or more, 1600 parts by weight or more, 1700 parts by weight or more, 1800 parts by weight or more, Parts by weight or more or 1850 parts by weight or more, or can be about 2350 parts by weight or less, 2300 parts by weight or less, 2250 parts by weight or less, 2200 parts by weight or less, 2150 parts by weight or less, 2100 parts by weight or less, 2050 parts by weight or less, 2000 parts by weight or less, 1950 parts by weight or less, 1900 parts by weight or less, 1800 parts by weight or less, 1700 parts by weight or less, 1600 parts by weight or less, 1500 parts by weight or less, 1400 parts by weight or less, 1300 parts by weight or less, 1200 parts by weight or less, 1100 parts by weight or less, 1000 parts by weight or less, 900 parts by weight or less, 800 parts by weight or less, 700 parts by weight or less, or 600 parts by weight or less.

[0058] When the monomer (A) and the monomer (B) are used as polymerization units of the second monomer, the weight ratio (A / B) of the polymerization units of the monomer (A) to the polymerization units of the monomer (B) may be in the range of 0.25 to 5. In other examples, the weight ratio (A / B) may also be about 0.3 or more, 0.35 or more, 0.4 or more, 0.45 or more, 0.5 or more, 0.55 or more, 0.6 or more, 0.65 or more, 0.7 or more, 0.75 or more, 0.8 or more, 0.85 or more, 0.9 or more, 0.95 or more, 1.0 or more, 1.5 or more, or 2 or more, or about 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.95 or less, 0.9 or less, 0.85 or less, 0.8 or less, 0.75 or less, or 0.7 or less.

[0059] In addition to the first monomer and the second monomer, the polymer may appropriately contain other known monomers within a range that does not impair desired physical properties.

[0060] For example, the Tg of the polymer of the present application as described above may be in the range of about -30°C to 30°C. In other examples, the Tg of the polymer may also be about above -25°C, above -20°C, above -15°C or above -10°C, or may be about below 25°C, below 20°C, below 15°C, below 10°C, below 5°C, below 0°C or below -5°C. The Tg is a theoretical value obtained from the monomer composition of the polymer by the so-called Fox equation. For example, the Tg as described above may be useful when the polymer is used as a film-forming agent for cosmetics or pharmaceuticals, etc. By using the polymer within the range of the Tg, a film with excellent oil resistance can be effectively formed without stickiness, diffusion or breakage.

[0061] In the present application, the weight average molecular weight (Mw) of the polymer may be in the range of 100,000 to 2,000,000. For example, the weight average molecular weight in the present application may be a converted value of standard polystyrene measured using GPC (Gel Permeation Chromatograph), and unless otherwise specifically specified, the term molecular weight may be referred to as the weight average molecular weight. For example, the molecular weight (Mw) as described above may be useful when the polymer is used as a film-forming agent. By using the polymer within the range of the molecular weight (Mw), a film having excellent oil resistance can be effectively formed without causing stickiness, diffusion or breakage, etc.

[0062] In other examples, the molecular weight (Mw) can also be approximately 150,000 or more, 200,000 or more, 250,000 or more, 300,000 or more, 350,000 or more, 400,000 or more, 450,000 or more, or can be approximately 1.9 million or less, 1.8 million or less, 1.7 million or less, 1.6 million or less, 1.5 million or less, 1.4 million or less, 1.3 million or less, 1.2 million or less, 1.1 million or less, 1 million or less, 900,000 or less, 800,000 or less, or 700,000 or less.

[0063] The polymer composition of the present application containing the polymer as described above may not contain methanol, or may contain minimum methanol. For example, the methanol content of the polymer composition may also be about 30ppm or less, 25ppm or less, 20ppm or less, 15ppm or less, 10ppm or less, 5ppm or less, 4ppm or less, 3ppm or less, 2ppm or less, 1ppm or less or 0.5ppm or less. That is, in the polymer known to be used for manufacturing film-forming agents, the type or proportion of the monomer is controlled in order to adjust Tg, etc., and methanol is generated by hydrolysis, etc. in the monomers known as these monomers. For example, methyl (meth)acrylate is used very frequently to adjust Tg when manufacturing polymers for forming film-forming agents, but the methyl (meth)acrylate generates methanol by hydrolysis, etc. The generated methanol generates formaldehyde as a typical harmful substance in polymer compositions, film-forming agents, cosmetics or medicines. However, in the case of the present application, in the monomers forming the macromolecule, the monomers generating methanol are not used or the ratio of the monomers generating methanol is minimized, so that a macromolecular composition, a film former, a cosmetic or a medicine that does not contain methanol or contains minimal methanol can be provided. However, since the monomer generating methanol is a monomer that is known to be very effective in regulating the physical properties such as Tg of the macromolecule, it is not easy to achieve the target physical property without using this monomer. However, in the present application, by using the first monomer and the second monomer, monomer (A) and monomer (B) of the aforementioned kind, a macromolecular composition having a desired physical property can be provided even if methanol is not included or less included. Since it is most appropriate not to include methanol in the macromolecular composition, the lower limit of the methanol ratio can be about 0ppm.

[0064] The polymer composition of the present application does not contain methanol or contains minimal methanol, and therefore does not contain or contains minimal formaldehyde generated thereby as a harmful substance. For example, the formaldehyde content of the polymer composition can be about 30ppm or less, 25ppm or less, 20ppm or less, 15ppm or less, 10ppm or less, 5ppm or less, 4ppm or less, 3ppm or less, 2ppm or less, 1ppm or less or 0.5ppm or less. Since it is most appropriate not to contain formaldehyde in the polymer composition, the lower limit of the formaldehyde ratio can be about 0ppm.

[0065] The above-mentioned methanol ratio and formaldehyde ratio are measured in the manner described in the Examples described below.

[0066] In order to form a polymer composition having the above-mentioned methanol ratio and formaldehyde ratio, the polymer may not contain a polymerization unit of a monomer that generates methanol. As a monomer that generates methanol by hydrolysis, methyl methacrylate or metal acrylate are widely used in the manufacture of film-forming agents.

[0067] As a relatively hydrophobic monomer (e.g., the second monomer of the present application) or a relatively high Tg monomer (e.g., the monomer (A) of the present application), a monomer having a methyl group such as methyl methacrylate is often used to form a polymer such as a film-forming agent. However, in the present application, the monomers of the type mentioned as the second monomer do not generate methanol, or even if generated, only a very small amount of methanol is generated. Therefore, in the present application, it is suitable to use only the monomers of the type mentioned above as the second monomer, especially as the monomer (A) in at least the second monomer.

[0068] Therefore, in one example, the polymer may include only the polymerization unit of the monomer represented by the following Chemical Formula 3 as the polymerization unit of the second monomer or monomer (A).

[0069] For example, in the polymer, only the polymerization unit of a compound in which Q in the chemical formula 3 is an alkyl group, for example, an alkyl group or methyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms; and B is a linear or branched alkyl group having 2 or more carbon atoms can be used as at least the polymerization unit of the monomer (A), in which case the alkyl group of B can be a linear or branched alkyl group having 2 to 4 carbon atoms.

[0070] The polymer composition of the present application may contain only the polymer, or may further contain other essential components in the polymer.

[0071] As such an essential component, for example, a formaldehyde remover can be cited. As usable formaldehyde removers, ammonia, urea, sodium bisulfite and / or sodium metabisulfite can be cited, but are not limited thereto. In the polymer composition, the proportion of the formaldehyde remover can be an appropriate level, for example, relative to 100 parts by weight of the polymer, it can be about 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, or 3 parts by weight or less. Relative to 100 parts by weight of the polymer, the formaldehyde remover can also be about 0 parts by weight or more, greater than 0 parts by weight, 0.5 parts by weight or more, 1 part by weight or more, 1.5 parts by weight or more, or 2.5 parts by weight or more.

[0072] The polymer composition may further appropriately contain necessary additives in addition to the polymer and / or formaldehyde remover.

[0073] Examples of such additives include, but are not limited to, oils, surfactants, purified water, polyols (e.g., glycerin, propylene glycol, butylene glycol, etc.), organic powders, inorganic powders, ultraviolet absorbers, preservatives, defoaming agents, antibacterial agents, antioxidants, cosmetic ingredients, fragrances, thickeners, gelling agents, metal soaps, water-soluble polymers, fat-soluble polymers, fibers (nylon, rayon, etc.), pigments and / or pearlescent agents.

[0074] The polymer composition can be produced by various known methods. However, considering the formation efficiency and application efficiency of the polymer, it is effective to use emulsion polymerization. For example, emulsion polymerization using an aqueous solvent such as water as a continuous phase can be used.

[0075] In particular, when the first monomer is included as a polymer and a polymer having a high ratio of polymerized units of the first monomer is to be further formed, it is particularly effective to apply a seed emulsion polymerization method in the emulsion polymerization method. Seed emulsion polymerization is a polymerization method in which a relatively small particle of pre-polymerized emulsion polymer is used as a seed and monomers of the same or different species are polymerized in the seed to grow the particles. If this method is applied, the polymer desired in the present application can be produced more effectively.

[0076] For example, the seeded emulsion polymerization method may include a seed polymerization step and a seed growth step.

[0077] In one example, the polymerization method may include: a first step of performing seed emulsion polymerization on a reaction solution containing a monomer mixture, an aqueous solvent, and a surfactant; and a second step of performing emulsion polymerization while adding the reaction solution containing the monomer mixture to the seed emulsion polymer of the first step, thereby growing the seeds generated in the first step.

[0078] The monomer mixture used in the first step and the second step may include the first monomer and the second monomer, and as the second monomer, may include the monomer (A) and the monomer (B) mentioned above. In this case, the ratio of the various monomers in the monomer mixture may be adjusted so that the polymerized units of the ratio may be formed, and, in one example, may be substantially similar to the ratio of the polymerized units mentioned above.

[0079] For example, in the monomer mixture, the first monomer may be about 1 to 40 wt %. In other examples, the ratio may be about 1.5 wt %, 2 wt %, 2.5 wt %, 3 wt %, 3.5 wt %, 4.5 wt %, 5 wt %, 5.5 wt %, 6 wt %, 6.5 wt %, 7 wt %, 7.5 wt %, 8 wt %, 8.5 wt %, 9 wt %, 9.5 wt %, 10 wt %, 11 wt %, 12 wt %, 13 wt %, 14 wt %, or 14.5 wt %, or may be about 39 wt %, 38 wt %, 37 wt %, 36 wt %, 35 wt %, or about 39 wt %, 38 wt %, 37 wt %, 36 wt %, 37 wt %, 38 ... 5 wt % or less, 15 wt % or less, 16 wt % or less, 17 wt % or less, 18 wt % or less, 19 wt % or less, 19 wt % or less, 18 ...

[0080] In addition, the monomer mixture may include 150 to 4000 parts by weight of the second monomer relative to 100 parts by weight of the first monomer. In other examples, the ratio may also be about 200 parts by weight or more, 250 parts by weight or more, 300 parts by weight or more, 350 parts by weight or more, 400 parts by weight or more, 450 parts by weight or more, 500 parts by weight or more, 550 parts by weight or more, 600 parts by weight or more, 650 parts by weight or more, 700 parts by weight or more, 750 parts by weight or more, 800 parts by weight or more, 850 parts by weight or more, 900 parts by weight or more, 950 parts by weight or more, 1000 parts by weight or more, 1100 parts by weight or more, 1200 parts by weight or more, 1300 parts by weight or more, 1400 parts by weight or more, 1500 parts by weight or more, 1600 parts by weight or more, 1700 parts by weight or more, 1800 parts by weight or more, Parts by weight or more or 1850 parts by weight or more, or can also be about 2350 parts by weight or less, 2300 parts by weight or less, 2250 parts by weight or less, 2200 parts by weight or less, 2150 parts by weight or less, 2100 parts by weight or less, 2050 parts by weight or less, 2000 parts by weight or less, 1950 parts by weight or less, 1900 parts by weight or less, 1800 parts by weight or less, 1700 parts by weight or less, 1600 parts by weight or less, 1500 parts by weight or less, 1400 parts by weight or less, 1300 parts by weight or less, 1200 parts by weight or less, 1100 parts by weight or less, 1000 parts by weight or less, 900 parts by weight or less, 800 parts by weight or less, 700 parts by weight or less, or 600 parts by weight or less.

[0081] In addition, when the monomer (A) and the monomer (B) are used as the second monomer in the monomer mixture, the weight ratio (A / B) of the monomer (A) and the monomer (B) may be in the range of 0.25 to 5. In other examples, the weight ratio (A / B) may also be about 0.3 or more, 0.35 or more, 0.4 or more, 0.45 or more, 0.5 or more, 0.55 or more, 0.6 or more, 0.65 or more, 0.7 or more, 0.75 or more, 0.8 or more, 0.85 or more, 0.9 or more, 0.95 or more, 1.0 or more, 1.5 or more, or 2 or more, or about 4.5 or less, 4 or less, 3.5 or less, 3 or less, 2.5 or less, 2 or less, 1.5 or less, 1 or less, 0.95 or less, 0.9 or less, 0.85 or less, 0.8 or less, 0.75 or less, or 0.7 or less.

[0082] The ratio of the first monomer, the second monomer, the monomer (A) and the monomer (B) in the above-mentioned monomer mixture can be a ratio determined based on the sum of all monomer mixtures used in the first step and the second step. That is, as described below, in the polymerization method of the present application, first, the components such as monomers and surfactants are dispersed in a solvent (an aqueous solvent such as water) to produce a reaction solution, and then a part of them is separated to first perform seed emulsion polymerization in the first step, and then the remaining part can be added to the reaction solution in the second step. Therefore, the ratio of the monomers can be a ratio determined based on the sum of the monomer mixtures used in the first monomer and the second monomer.

[0083] In order to carry out the emulsion polymerization, a surfactant is applied together with the monomer mixture. As a surfactant, a known surfactant used in emulsion polymerization can be used. As this surfactant, an anionic or nonionic surfactant can be exemplified, specifically, an anionic surfactant such as sodium lauryl sulfate (sodium lauryl sulfate, SLS), sodium dodecyl benzene sulfonate (sodium dodecyl benzene sulfate, SDBS), ammonium lauryl sulfate (ammonium laurylsulfate, ALS), sodium cetyl stearyl sulfate or sodium lauryl ether sulfate (sodium lauryl ether sulfate, SLES) can be exemplified, or a nonionic surfactant known by the name of Triton (Triton) or Tween (Tween) can be exemplified, and one or more of the above-mentioned mixtures can be applied.

[0084] The proportion of the surfactant can be appropriately adjusted according to the purpose. For example, about 0.5 to 20 parts by weight of the surfactant can be included in the reaction solution relative to 100 parts by weight of the monomer mixture. In other examples, the proportion can also be about 1 part by weight or more, 1.5 parts by weight or more, 2 parts by weight or more, 2.5 parts by weight or more, 3 parts by weight or more, 3.5 parts by weight or more, or about 18 parts by weight or less, 16 parts by weight or less, 14 parts by weight or less, 12 parts by weight or less, 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, or 6 parts by weight or less.

[0085] The ratio of the surfactant may be the ratio in the reaction liquid of the first step, or, if a surfactant is also present in the second step, it may be the ratio based on the total of the reaction liquids in the first step and the second step, as in the case of the monomer mixture.

[0086] The reaction solution can be manufactured by dispersing the monomer mixture and / or surfactant into a solvent (e.g., an aqueous solvent such as water). Therefore, the reaction solution can further include the solvent. There is no particular restriction on the proportion of the solvent. In one example, the concentration of the monomer mixture in the solvent can be roughly controlled within the range of 5 to 90 weight %.

[0087] There is no particular limitation on the manner in which the first step is performed by starting polymerization of the reaction solution as described above. For example, the first step can be performed by adding a known polymerization initiator to the reaction solution and controlling the conditions so that a polymerization reaction initiated by the initiator proceeds.

[0088] As such an initiator, a known initiator can be used, for example, a known water-soluble initiator, and examples thereof include potassium persulfate (KPS), ammonium persulfate (APS), sodium persulfate and / or hydrogen peroxide, but are not limited thereto.

[0089] There is no particular limitation on the ratio of the initiator, and an appropriate ratio can be used according to the purpose. There is no particular limitation on the method of starting the polymerization initiated by the initiator, for example, if the initiator is a thermal initiator, a method of applying appropriate heat can be used, and if it is a photoinitiator, a method of irradiating appropriate light can be used.

[0090] As described above, in the method, the reaction solution can be manufactured by dispersing the monomer mixture and the surfactant etc. in a solvent, a portion of which is subjected to the seed polymerization reaction of the first step, and then the remaining portion is added to the seed polymer of the first step and the second step is carried out. In this case, the method can include the following steps before the first step: after dispersing the monomer mixture and the surfactant etc. in a solvent to manufacture the total reaction solution, a portion of which is separated as the reaction solution of the first step. The ratio of the reaction solution separated and applied to the first step is not particularly limited, for example, about 1 to 10 weight % of the total reaction solution can be used as the reaction solution of the first step.

[0091] In the method of the present application, the reaction solution added in the second step may not only contain the monomer mixture, but may further contain an aqueous solvent and a surfactant. For example, in the case where the total reaction solution mentioned above is separated to perform the first step and the remaining reaction solution is applied to the second step, the reaction solution of the second step also contains a surfactant, etc., similar to the case of the reaction solution of the first step, and even in the case where other reaction solutions are added in the second step without applying the method, the surfactant, etc. may be contained in the reaction solution of the second step.

[0092] The rate of adding the reaction solution in the second step can be controlled. By controlling the rate of adding the reaction solution, a polymer having a desired monomer composition and physical properties can be formed more efficiently.

[0093] For example, in the second step, the speed of adding the reaction liquid may be adjusted to be slower than the reaction speed of the monomers.

[0094] The method of adding the reaction solution and starting polymerization to carry out the second step as described above is not particularly limited. For example, the second step can be carried out by adding a known polymerization initiator together with the reaction solution and controlling the conditions to carry out a polymerization reaction initiated by the initiator, as in the case of the first step. In this case, the type of initiator or its ratio that can be applied, and the method of starting the polymerization initiated by the initiator are the same as in the case of the first step.

[0095] The method for producing the polymer composition of the present application may further include a step of mixing the formed polymer with other necessary components such as the formaldehyde remover after the first step and the second step.

[0096] The present application also relates to a film-forming agent, a cosmetic composition or a cosmetic comprising the polymer. When the polymer is used, a uniform film (film) can be formed by applying, etc., and even when applied to the skin, it can show high stability, and can provide a film-forming agent that is excellent in oil resistance, diffusion resistance, and powder loss resistance and minimizes the proportion of harmful components.

[0097] Thus, the polymer can be used in the manufacture of film-forming agents or cosmetic compositions that can be used to manufacture various cosmetics, including beauty masks, smoky makeup applied to the corners of the mouth and eyes, nail polish, lipstick, eye shadow, hairspray or eyeliner that can be applied to fingernails or toenails, etc. In addition, due to the above-mentioned characteristics, the polymer or film-forming agent can also be used for medical purposes, and as medical uses, there can be exemplified bandages or percutaneous absorption preparations.

[0098] The ratio of the polymer in the film-forming agent, the cosmetic composition or the cosmetic is not particularly limited and may be selected in consideration of the application, etc. For example, when the polymer is applied to the cosmetic composition, the concentration of the polymer in the composition may be in the range of 1 wt % to 20 wt %, but is not limited thereto.

[0099] According to the purpose, the film-forming agent, the cosmetic composition or the cosmetic may further contain other active ingredients. As additional active ingredients, not only cosmetic ingredients such as whitening or UV protection can be exemplified, but also pharmaceutical ingredients, physiologically active ingredients or pharmacologically active ingredients can be exemplified. As these active ingredients, local anesthetic ingredients (lidocaine, dibucaine hydrochloride, dibucaine, ethyl aminobenzoate, etc.), analgesic ingredients (salicylic acid derivatives such as methyl salicylate, indomethacin, piroxicam, ketoprofen, felbinac, etc.), anti-inflammatory ingredients (glycyrrhizic acid, glycyrrhizic acid dipotassium and other glycyrrhizic acid salts; glycyrrhetinic acid, stearyl glycyrrhetinic acid ester, butylbenzyl hydroxy acid, benzyl nicotinate, hydrocortisone, hydrocortisone butyrate, hydrocortisone acetate, prednisolone acetate valerate, prednisone acetate, prednisone, dexamethasone, dexamethasone acetate, dimethyl isopropyl glycolate can be exemplified. Ibuprofen, arnica extract, scutellaria extract, toad grass extract, chamomile extract, calamine, licorice extract, guaiac, gardenia extract, gentian extract, black tea extract, tocopherol, tocopherol acetate, purple root extract, perilla extract, peony extract, sage extract, Japanese swertia extract, mulberry bark extract, pyridoxine hydrochloride, peach leaf extract, cornflower extract, saxifrage extract, mugwort extract, Roman chamomile extract, etc.), antihistamine ingredients (chlorpheniramine maleate, diphenhydramine, diphenhydramine hydrochloride, salicylic acid diphenhydramine, etc.), local irritants (ammonia, l-menthol, dl-camphor, peppermint oil, benzyl nicotinate, nonanoic acid vanillamide, etc.), antipruritic ingredients (crotamiton, etc.), preservatives or bactericidal ingredients (acrinol, chlorhexidine gluconate, chlorhexidine hydrochloride, benzalkonium chloride, benzethonium chloride, povidone iodine, iodoform, iodine, potassium iodide, merbromin, oxides, cresol, triclosan, phenol, isopropyl methylphenol, thymol, sodium salicylate, undecylenic acid, photosensitizer, hinokitiol, phenoxyethanol, chlorobutanol, quaternary ammonium salt-73 , zinc pyrithione, parabens, eucalyptus extract, resorcinol rosemary extract, etc.), antifungal ingredients (imidazole antifungals such as clotrimazole, clotrimazole acetate, miconazole acetate, econazole acetate, bifonazole, oxiconazole acetate, sulconazole acetate, neconazole hydrochloride, bifonazole, tioconazole, omeprazole acetate, etc.; allylamine antifungals such as terbinafine, terbinafine hydrochloride, and naftifine; benzylamine antifungals such as butenafine; allylamine antifungals such as apomorphine hydrochloride; thiocarbamic acid antifungals such as tolnaftate and tolcylcerate;Pyrrolidine, isabiprofen, ciclopirox olamine, etc.), tissue repair ingredients (allantoin, heparin-like substances, vitamin A palmitate, vitamin D2, retinol acetate, retinol, vitamin A oil, panthenol, etc.), astringent ingredients (zinc oxide, Acanthopanax senticosus extract, aluminum chloride, Phellodendron amurense extract, its salt, citric acid, birch extract, tea extract, hops extract, horse chestnut extract, etc.), keratin softening ingredients (urea, glycerin, concentrated glycerin, potassium hydroxide, salicylic acid, sulfur, colloidal sulfur, resorcinol, gluconic acid, lactic acid, sodium sulfate, etc.), moisturizing ingredients (butylene glycol, sodium pyrrolidone carboxylate, propylene glycol , sodium ribonucleic acid, angelica leaf extract, aspartic acid, alanine, arginine, sodium alginate, marshmallow extract, aloe extract, oyster extract, hydrolyzed keratin, hydrolyzed collagen, hydrolyzed conchiolin, hydrolyzed eggshell membrane, hydrolyzed egg white, hydrolyzed silk, brown algae extract, papaya extract, raspberry extract, xylitol, chitosan, cucumber extract, quince seed extract, glycine, glycerin, glucose, good hope aloe extract, cystin, cysteine, mallow extract, serine, sorbitol, trehalose, sodium lactate, sodium hyaluronate, placenta extract, loofah extract , multifunctional materials, mannitol, lily extract, lactoferrin, lysine, apple extract, royal jelly extract, etc.), moisturizing ingredients (almond oil, avocado oil, olive oil, oleic acid, Atlantic snapper oil, cocoa butter, carrot extract, squalene, ceramide, evening primrose oil, grape seed oil, jojoba oil, macadamia oil, mineral oil, mink oil, eucalyptus oil, rosehip oil, vaseline, etc.), whitening ingredients (ascorbic acid, ascorbic acid derivatives, arbutin, retinol, ellagic acid, glutathione, kojic acid, rosehip extract, kiwi extract, etc.), UV protection ingredients (para-aminobenzoic acid, ethyl aminobenzoate, p-aminobenzoic acid glyceride, p-dimethylaminobenzoic acid amyl alcohol ester, p-dimethylaminobenzoic acid 2-ethylhexyl ester, tert-butyl methoxydibenzoylmethane, oxybenzones, octyl triazone, octyl salicylate, ethyl diisopropyl cinnamate, methyl diisopropyl cinnamate, cinnamic ether ester, dimethoxycinnamic acid caprylic glyceride, dimethoxybenzylidene dioxoimidazolidine propionate octyl ester, tea extract, drometrizole, isopropyl p-methoxycinnamate, homosalate, methoxycinnamic acid octyl ester, etc.), herbal extract ingredients, vitamins, amino acids or minerals, but not limited to these. ;

[0100] The film-forming agent, the cosmetic composition or the cosmetic may contain other solvents, additives or the like according to the application.

[0101] As the solvent or solvent component mentioned above, for example, alcohols (for example, polyethylene glycol, etc.), ethers (except diethyl ether, etc., glycol ethers (cellosolve types such as methyl cellosolve; dialkylene glycol alkyl ethers such as diethylene glycol monoethyl ether, etc.), nitriles (acetonitrile, etc.), ketones (acetone, etc.) or esters (carboxylic acid alkyl esters such as ethyl acetate, etc.) can be cited according to the purpose of the composition, the form of use, etc.

[0102] In addition, as additives, not only plasticizers, wetting agents, defoaming agents, colorants, preservatives, aromatics, flavoring agents, pigments or thickeners, but also conventional ingredients used in quasi-drugs, medicines or cosmetics, such as powdered bases or carriers (binders, disintegrants, excipients or lubricants, etc.), oily bases or carriers (animal and vegetable oils, waxes, vaseline, paraffin oil, silicone oil, higher fatty acid esters or higher fatty acids, etc.), aqueous bases or carriers (gel bases such as xanthan gum, etc.), preservatives, chelating agents, antioxidants, cooling agents, stabilizers, fluidizers, emulsifiers, thickeners, buffers, dispersants, adsorbents, humectants, wetting agents, anti-humidifying agents, antistatic agents or other resins (polyamide resins, olefin resins such as hydrogenated polybutene, etc.), etc., but are not limited to these.

[0103] The method for producing the film-forming agent, the cosmetic composition, the cosmetic, etc. using the above-mentioned components or, if necessary, other known components is not particularly limited, and a known method can be applied.

[0104] The object of the present application is to provide a polymer composition and a film-forming agent or cosmetics produced using the polymer composition, wherein the polymer composition has excellent oil resistance and can form cosmetics that do not spread or fall off during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0105] Figure 1 and Figure 2 These are photographs of the polymers produced in Examples 3 and 4, respectively.

[0106] Figure 3 and Figure 4 These are photographs of the polymers produced in Reference Examples 4 and 5, respectively. DETAILED DESCRIPTION

[0107] Hereinafter, the polymers and the like of the present application will be described in detail by way of Examples and Comparative Examples, but the scope of the polymers and the like is not limited to the following Examples. In the following Examples and Comparative Examples, various physical properties were evaluated in the following manner.

[0108] 1. Determination of methanol ratio and formaldehyde ratio

[0109] The proportion of methanol was confirmed by GC-FID (Gas Chromatography Flame Ionization Detector). A 7890B GC System from Agilent Technologies was used as the measuring instrument, and the sample was diluted in ACN (Acetonitrile) to confirm the proportion of methanol. The measuring conditions for confirming the proportion of methanol were as follows.

[0110] <Measurement Conditions>

[0111] Analyzer: 7890B GC System (Agilent Technologies)

[0112] Chromatographic column: HP-FFAP (19091F-115) (50m*320μm*0.5μm)

[0113] Injector temperature: 220℃

[0114] Oven temperature: 60℃ / 10min-25℃ / min-220℃ / 13min

[0115] Flow rate: 1.5mL / min

[0116] Injection volume: Inject 1.5 μL

[0117] The proportion of formaldehyde was confirmed by LC-UV (Liquid Chromatography-UV). As the measuring instrument, the 1260 Infinity II LC product of Agilent Technologies was used. The sample was calibrated with water and extracted by ultrasonic extraction for 1 hour, and then the formaldehyde proportion was confirmed. The measuring conditions for confirming the formaldehyde proportion were as follows.

[0118] <Measurement Conditions>

[0119] Chromatographic column: C18 (5μm, 4.6*250mm)

[0120] Mobile phase: ACN: water = 60:40

[0121] Oven temperature: 30°C

[0122] Injection volume: 10 μL

[0123] Detection wavelength: 360nm

[0124] 2. Molecular weight determination

[0125] The weight average molecular weight (Mw) and molecular weight distribution (PDI) were measured using GPC under the following conditions, and the measurement results were converted using standard polystyrene of the Agilent system for the preparation of a calibration curve.

[0126] <Measurement Conditions>

[0127] Analyzer: Agilent GPC (Agilent 1200 series, US)

[0128] Chromatographic columns: connect two PL Mixed B

[0129] Column temperature: 40°C

[0130] Eluent: THF (Tetrahydrofuran)

[0131] Flow rate: 1.0mL / min

[0132] Concentration: ~1mg / mL (inject 100μL)

[0133] 3. Calculation of glass transition temperature

[0134] The glass transition temperature (Tg) was calculated from the monomer composition by the following mathematical formula.

[0135] <Mathematical formula>

[0136] 1 / Tg=ΣWn / Tn

[0137] In the above mathematical formula, Wn is the weight fraction of various monomers of the polymer, Tn is the glass transition temperature exhibited when the monomers form a homopolymer, and the right side of the mathematical formula is the result of adding up all the calculated values ​​after dividing the weight fraction of the monomer used for each monomer by the glass transition temperature exhibited when the monomer forms a homopolymer (Wn / Tn).

[0138] 4. Diffusion evaluation

[0139] The diffusion evaluation was performed as follows. First, a sample (smoky makeup preparation) was applied to a glass plate at a thickness of about 100 μm and then dried at 25°C for 24 hours. Then, 0.1 g of artificial sebum was dropped on a surface about 4 cm from the dried sample. 2 On the area, after wetting for 10 minutes, paper was placed thereon, a 500 g weight was used to perform 20 horizontal reciprocating movements, and an image analysis was performed on the extent of artificial sebum sticking to the paper.

[0140] As artificial sebum, artificial sebum containing 40 wt% of triglycerides, 2.2 wt% of diglycerides, 16.4 wt% of free fatty acids, 12 wt% of squalene, 25 wt% of wax esters, 1.4 wt% of cholesterol, and 2 wt% of cholesterol ester was used.

[0141] Image analysis confirmed that the value obtained by dividing the colorimetric value of the paper in the above case where the sample was applied and dried and then artificial sebum was dropped on the paper by the colorimetric value obtained by dropping artificial sebum on the paper without applying the preparation, and that a larger value indicates a better anti-diffusion property.

[0142] 5. Loss of fans evaluation

[0143] The powder fall evaluation was performed in the following manner. First, the smoky makeup preparation was applied to a human hair tress 10 times, dried, and then the dried human hair sample was immersed in 25°C distilled water for 5 seconds and taken out. After the human hair was dried for 3 minutes, the powder that fell off was analyzed by image analysis with a nylon brush with an amplitude of less than 2 cm and compared. The powder fall value is the value obtained by applying the preparation to a human hair tress, drying it, immersing it in water, taking it out, and applying friction to measure the amount of powder that fell off.

[0144] 6. Special panel evaluation

[0145] A smoky makeup use test was conducted by a panel of 20 experts (aged 25 to 50). The panel applied smoky makeup and then, after 6 hours, the spread (degree of sebum adhesion) and powder fall were evaluated on a 5-point scale according to the following criteria, and the average value was used for judgment.

[0146] <Evaluation criteria for spreading and powder loss>

[0147] A: Average score of 4.5 or above

[0148] B: Average score is 3.5 or above and less than 4.5

[0149] C: Average score is 2.5 or above and less than 3.5

[0150] D: Average less than 2.5 points

[0151] <Score Evaluation Criteria>

[0152] <Diffusion Evaluation>

[0153] 5 points: No spread

[0154] 4 points: Slightly diffuse

[0155] 3 points: General

[0156] 2 points: Severe spread

[0157] 1 point: The spread is very serious

[0158] <Loss of fans evaluation>

[0159] 5 points: No powder loss

[0160] 4 points: A small amount of powder loss

[0161] 3 points: General

[0162] 2 points: A large number of fans have been lost

[0163] 1 point: Very large amount of fans lost

[0164] Example 1.

[0165] 200 g of purified water and 5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0166] In the reactor 2 equipped with another stirrer, 100 g of purified water and 10 g of acrylic acid (solubility parameter: 13.6 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 110 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 80 g of ethyl methacrylate (solubility parameter: 9.7 (cal / cm 3 ) 1 / 2 , Tg: 65°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5% by weight of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. Through the above process, a polymer solution with excellent phase stability can be obtained without increasing the viscosity. The molecular weight (Mw) of the manufactured polymer solution is about 500,000 to 650,000, and the Tg is about -8.6°C. Next, 5g of an ammonia solution (28% by weight) as a formaldehyde remover was mixed in the polymer solution to produce a polymer composition. Next, the polymer composition was mixed with other components shown in the following Table 1 to obtain a smoky makeup preparation. The numerical values ​​in the following Table 1 are weight ratios.

[0167] Example 2.

[0168] 200 g of purified water and 5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0169] In the reactor 2 equipped with another stirrer, 100 g of purified water and 10 g of methacrylic acid (solubility parameter: 12.3 (cal / cm 3 ) 1 / 2 , Tg: 225°C), 115 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 75 g of ethyl methacrylate (solubility parameter: 9.7 (cal / cm 3 ) 1 / 2 , Tg: 65°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5% by weight of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. Through the above process, a polymer solution with excellent phase stability can be obtained without increasing the viscosity. The molecular weight (Mw) of the manufactured polymer solution is about 500,000 to 650,000, and the Tg is about -9.0°C. Next, 5g of an ammonia solution (28% by weight) as a formaldehyde remover was mixed in the polymer solution to produce a polymer composition. Next, the polymer composition was mixed with other components shown in Table 1 below to obtain a smoky makeup preparation.

[0170] Example 3.

[0171] 200 g of purified water and 2.5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0172] In the reactor 2 equipped with another stirrer, 100 g of purified water and 30 g of 2-hydroxyethyl acrylate (solubility parameter: 14.1 (cal / cm 3 ) 1 / 2 , Tg: -15°C), 90 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 )1 / 2 , Tg: -50°C), 80 g of ethyl methacrylate (solubility parameter: 9.7 (cal / cm 3 ) 1 / 2 , Tg: 65°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5 wt% of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. Figure 1 This is a photograph of a polymer solution obtained by the above process. By the above process, a polymer solution with excellent phase stability can be obtained without increasing the viscosity. The molecular weight (Mw) of the produced polymer solution is about 500,000 to 650,000, and the Tg is about -9°C. Then, 4 g of an aqueous ammonia solution (28 wt%) as a formaldehyde remover is mixed into the polymer solution to produce a polymer composition. Then, the smoky makeup preparation is obtained by mixing the polymer composition with other ingredients shown in Table 1 below.

[0173] Example 4.

[0174] 200 g of purified water and 2.5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0175] In the reactor 2 equipped with another stirrer, 100 g of purified water and 30 g of 2-hydroxyethyl acrylate (solubility parameter: 14.1 (cal / cm 3 ) 1 / 2 , Tg: -15°C), 55 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 115 g of methyl methacrylate (solubility parameter: 10.1 (cal / cm 3 ) 1 / 2, Tg: 105°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5 wt% of the emulsion was separated from the emulsion in reactor 2, added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. Figure 2 This is a photograph of a polymer solution obtained through the above process. Through the above process, a polymer solution with excellent phase stability can be obtained without increasing the viscosity. The molecular weight (Mw) of the produced polymer solution (polymer composition) is about 500,000 to 650,000, and the Tg is about 26.5°C. Next, the smoky makeup preparation is obtained by mixing the polymer composition with other ingredients shown in Table 1 below.

[0176] Comparative Example 1.

[0177] 200 g of purified water and 5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0178] In the reactor 2 equipped with another stirrer, 100 g of purified water and 120 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 80 g of methyl methacrylate (solubility parameter: 10.1 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5 wt% of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. The molecular weight (Mw) of the manufactured polymer solution (polymer composition) is about 500,000 to 650,000, and the Tg is about -6.2°C. Next, the smoky makeup preparation is obtained by mixing the polymer composition with other ingredients shown in Table 1 below.

[0179] [Table 1]

[0180]

[0181] The evaluation results of the physical properties of the above-mentioned respective Examples and Comparative Examples are summarized and recorded in the following Table 2 (the methanol ratio and formaldehyde ratio in Table 2 are ratios with respect to the polymer composition, and the unit is ppm).

[0182] [Table 2]

[0183]

[0184] Reference Example 1

[0185] 200 g of purified water and 5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0186] In the reactor 2 equipped with another stirrer, 100 g of purified water and 10 g of acrylic acid (solubility parameter: 13.6 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 110 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 80 g of ethyl methacrylate (solubility parameter: 9.7 (cal / cm 3 ) 1 / 2 , Tg: 65°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5 wt% of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. The Tg of the manufactured polymer solution (polymer composition) was about -8.6°C. As a result of confirming the polymer composition in the same manner as in the examples and comparative examples, no methanol was detected, and the proportion of formaldehyde was about 20.8ppm.

[0187] Reference Example 2

[0188] 200 g of purified water and 5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0189] In the reactor 2 equipped with another stirrer, 100 g of purified water and 10 g of acrylic acid (solubility parameter: 13.6 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 60 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 130 g of ethyl methacrylate (solubility parameter: 9.7 (cal / cm 3 ) 1 / 2 , Tg: 65°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5 wt% of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. The Tg of the manufactured polymer solution (polymer composition) was about 21.1°C. The results of measuring the methanol ratio and formaldehyde ratio of the polymer composition in the same manner as in the examples and comparative examples showed that no methanol was detected and the formaldehyde ratio was 21.6ppm. In addition, the results of the diffusion test, powder loss test, diffusion test (panel evaluation) and powder loss test (panel evaluation) of the smoky makeup preparation that was the same as Example 1 except that the polymer composition was used were 93.4, 10, B and D, respectively.

[0190] Reference Example 3

[0191] 200 g of purified water and 5 g of sodium bicarbonate (as a neutralizing agent and saturated) were added to the reactor 1 equipped with a cooler, a nitrogen injector, a thermometer and a stirrer, and the mixture was uniformly mixed, and the temperature was raised to 70°C.

[0192] In the reactor 2 equipped with another stirrer, 100 g of purified water and 10 g of acrylic acid (solubility parameter: 13.6 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 85 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2, Tg: -50°C), 105 g of methyl methacrylate (solubility parameter: 10.1 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 4g of sodium lauryl sulfate and 4g of Triton X-405 and emulsified. 5 wt% of the emulsion in reactor 2 was separated and added to reactor 1, and 0.5g of initiator (ammonium persulfate) was added to carry out seed polymerization for 30 minutes. After the seed polymerization, the remaining emulsion in reactor 2 was introduced into reactor 1. When the remaining emulsion in reactor 2 was introduced, 0.5g of initiator (ammonium persulfate) dissolved in purified water was added together, and polymerization was carried out for 24 hours. During this process, the introduction rate of the emulsion was controlled at about 85mL / min. The Tg of the manufactured polymer solution (polymer composition) was about 18.8°C. The results of measuring the methanol ratio and formaldehyde ratio of the polymer composition in the same manner as in the examples and comparative examples were that the methanol ratio and the formaldehyde ratio were 19ppm and 38.1ppm, respectively. In addition, the results of the diffusion test, powder loss test, diffusion test (panel evaluation) and powder loss test (panel evaluation) of the smoky makeup preparation that was the same as Example 1 except that the polymer composition was used were 95.5, 14, A and D, respectively.

[0193] Reference Example 4

[0194] In a reactor equipped with a cooler, a nitrogen injector, a thermometer, and a stirrer, 300 g of purified water, 30 g of 2-hydroxyethyl acrylate (solubility parameter: 14.1 (cal / cm 3 ) 1 / 2 , Tg: -15°C), 90 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 80 g of ethyl methacrylate (solubility parameter: 9.7 (cal / cm 3 ) 1 / 2 , Tg: 65°C), 4g of sodium lauryl sulfate, 4g of Triton X-405 and 2.5g of saturated sodium bicarbonate as a neutralizer were emulsified and the temperature was raised to 70°C. Then, 1g of initiator (ammonium persulfate) was added and polymerization was carried out for 24 hours. The Tg of the produced polymerization solution was about -9°C. Figure 3 This is a photograph of the polymer solution obtained through the process described above.

[0195] Reference Example 5

[0196] 300 g of purified water and 30 g of 2-hydroxyethyl acrylate (solubility parameter: 14.1 (cal / cm 3 ) 1 / 2 , Tg: -15°C), 55 g of 2-ethylhexyl acrylate (solubility parameter: 8.8 (cal / cm 3 ) 1 / 2 , Tg: -50°C), 115 g of methyl methacrylate (solubility parameter: 10.1 (cal / cm 3 ) 1 / 2 , Tg: 105°C), 4g of sodium lauryl sulfate, 4g of Triton X-405 and 2.5g of saturated sodium bicarbonate as a neutralizer were emulsified and the temperature was raised to 70°C. Then, 1g of initiator (ammonium persulfate) was added and polymerization was carried out for 24 hours. The Tg of the produced polymerization solution was about 26.5°C. Figure 4 This is a photograph of the polymer solution obtained through the process described above.

Claims

1. A cosmetic composition, wherein: The polymer comprises: a homopolymer having a solubility parameter of 11.0 (cal / cm 3 ) 1 / 2 The first monomer polymerization unit above; and the solubility parameter of the homopolymer is less than 11.0 (cal / cm 3 ) 1 / 2 The second monomer polymerization unit, In the polymer, the proportion of the first monomer polymerization unit is in the range of 1 to 40% by weight, The polymer comprises 150 to 4000 parts by weight of the second monomer polymerization unit relative to 100 parts by weight of the first monomer polymerization unit, The second monomer polymerization unit comprises: a monomer A polymerization unit having a glass transition temperature of 20° C. or more; and a monomer B polymerization unit having a glass transition temperature of less than 20° C., The weight ratio A / B of the polymerization units of the monomer A and the polymerization units of the monomer B is in the range of 0.25 to 1.5, The second monomer is represented by the following chemical formula 3: Chemical formula 3 In the chemical formula 3, Q is hydrogen or an alkyl group, B is a straight chain or branched chain alkyl group or an alicyclic hydrocarbon group having 2 or more carbon atoms, The polymer is a seed emulsion polymer.

2. The cosmetic composition according to claim 1, wherein The methanol ratio was 30 ppm or less.

3. The cosmetic composition according to claim 1, wherein The formaldehyde content is below 30 ppm.

4. The cosmetic composition according to claim 1, wherein The polymer does not contain polymerized units of methanol-generating monomers.

5. The cosmetic composition according to claim 4, wherein The methanol generating monomer is methyl (meth)acrylate.

6. The cosmetic composition according to claim 1, wherein The glass transition temperature of the first monomer is in the range of -40°C to 400°C.

7. The cosmetic composition according to claim 1, wherein The first monomer is a hydroxyl-containing monomer, a (meth)acrylamide-based monomer, an acidic monomer, glycerol (meth)acrylate, or a monomer containing an alkylene oxide unit.

8. The cosmetic composition according to claim 1, wherein The first monomer is a polymerizable heterocyclic monomer.

9. The cosmetic composition according to claim 1, wherein The glass transition temperature of the polymer is in the range of -30°C to 30°C.

10. The cosmetic composition according to claim 1, wherein The weight average molecular weight of the polymer is in the range of 100,000 to 2,000,000.

11. The cosmetic composition according to claim 1, wherein Also includes wetting agents, waxes and pigments.

12. The cosmetic composition according to claim 1, wherein Further comprising a formaldehyde remover.

13. A method for producing a cosmetic composition, wherein: include: The first step is to perform seed emulsion polymerization on a reaction solution containing a monomer mixture, an aqueous solvent and a surfactant; as well as In the second step, a reaction solution containing a monomer mixture is added to the seed emulsion polymer of the first step while performing emulsion polymerization to grow the seed generated in the first step, The monomer mixtures in the first step and the second step respectively include: a solubility parameter of the homopolymer of 11.0 (cal / cm 3 ) 1 / 2 The first monomer of the above; and the solubility parameter of the homopolymer is less than 11.0 (cal / cm 3 ) 1 / 2 The second monomer, In the first step and the second step, the ratio of the first monomer in the monomer mixture is in the range of 1 to 40 wt %, The monomer mixture includes 150 to 4000 parts by weight of the second monomer relative to 100 parts by weight of the first monomer, The second monomer polymerization unit includes: a monomer A polymerization unit having a glass transition temperature of 20° C. or more; and a polymerized unit of monomer B having a glass transition temperature of less than 20°C, The weight ratio A / B of the polymerization units of the monomer A and the polymerization units of the monomer B is in the range of 0.25 to 1.5, The second monomer is represented by the following chemical formula 3: Chemical formula 3 In the chemical formula 3, Q is hydrogen or an alkyl group, B is a straight chain or branched chain alkyl group or an alicyclic hydrocarbon group having 2 or more carbon atoms, The polymer is a seed emulsion polymer.

14. The method for producing a cosmetic composition according to claim 13, wherein: Prior to the first step, the method includes separating a portion of the total reaction solution prepared by mixing the monomer mixture, the aqueous solvent, and the surfactant and using the portion as the reaction solution for the first step.

15. The method for producing a cosmetic composition according to claim 13, wherein: The method further comprises the following step: mixing the polymer obtained through the second step with a formaldehyde remover.