Long-life laser chamber electrode and laser having the same

By using CoCu (5-15wt%) or Cu60Ag40wt%) alloy materials as electrodes, the problem of electrode corrosion was solved, the electrode life was extended, the energy density and gas flow clearance of the laser chamber were improved, and the voltage difference and energy loss were reduced.

CN112739837BActive Publication Date: 2024-10-01SIMMER GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980061865.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-20
Filing Date
2019-08-28
Publication Date
2024-10-01
Estimated Expiration
2039-08-28

AI Technical Summary

Technical Problem

The chemical reaction between the electrode material and fluorine gas leads to the continuous formation and growth of the reef-like layer, resulting in uneven electrode corrosion and shortening the service life of the laser cavity electrodes.

Method used

An alloy material is used as the electrode, such as CoCu (5-15wt%) or Cu60Ag40wt%) alloy, where the free energy of the formation of the first metal with fluorine is greater than or equal to that of the formation of copper with fluorine, and the free energy of the formation of the second metal with fluorine is less than that of the formation of the first metal with fluorine. This alloy forms a dense and continuous protective layer to slow down corrosion.

Benefits of technology

It extends the lifespan of the electrodes, reduces the electrode erosion rate, improves the energy density and airflow clearance rate of the laser chamber, and reduces voltage difference and energy loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112739837B_ABST
    Figure CN112739837B_ABST
Patent Text Reader

Abstract

An electrode for a laser chamber is disclosed. The electrode includes an alloy of a first metal and a second metal. A first free energy of formation of the first metal with fluorine is greater than or equal to a free energy of formation of copper with fluorine. A second free energy of formation of the second metal with fluorine is less than the first free energy.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Application No. 62 / 733,708, filed on September 20, 2018, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The presently disclosed subject matter relates to light sources such as those produced by lasers used in integrated circuit lithography manufacturing processes. Background Art

[0004] In laser discharge chambers, such as ArF power ring amplifier excimer discharge chambers ("PRA") or KrF excimer discharge chambers, electrode erosion imposes a significant limitation on the service life of chamber modules. One measure to extend the service life of KrF excimer discharge chamber modules is to make the anodes from wear-resistant materials. For example, information on materials suitable for use as anode materials can be found in U.S. Pat. No. 7,301,980, issued on November 27, 2007, and U.S. Pat. No. 6,690,706, issued on February 10, 2004, both of which are assigned to the applicant of the present application and are incorporated herein by reference in their entirety.

[0005] Fluorine-containing plasmas are highly corrosive to metals and thus cause electromechanical corrosion and erosion during operation of the chamber. For example, nucleation and growth of localized areas of corrosion product accumulation may occur on the surface of the anode. This results in uneven discharge between the electrodes and downstream arcing. The accumulation of these corrosion islands may be referred to as a "reef" formation or "reefing". The electrode extends further into the plasma at the point where the reef occurs than the rest of the electrode's surface. In this way, the reef can cause arcing in the plasma. Arcing in the plasma is undesirable because it robs the laser chamber of energy because the energy goes into the arc discharge rather than into the laser chamber. Therefore, when a large amount of arcing occurs in the plasma, the electrode must be replaced to keep the laser chamber running efficiently. In this way, the reef shortens the life of the electrode that can be effectively used in the laser chamber.

[0006] Erosion results in an increase in the width of the discharge gap and a widening of the discharge. Both of these phenomena result in a lower energy density in the discharge which in turn drives the need to increase the voltage difference across the electrodes necessary to maintain energy output. Additionally, the widening of the discharge reduces the clearing rate of the gas flow, resulting in increased downstream arcing, leading to energy losses and resulting dose errors. Once the dose error rate increases above a predetermined threshold, the chamber is considered to have reached the end of its useful life and must be replaced.

[0007] Therefore, a key issue is the chemical reaction between the electrode material and the fluorine gas, which leads to the continuous formation and growth of a reef-like layer, resulting in the reef preventing efficient plasma formation at the electrode due to uneven electrode corrosion. Summary of the invention

[0008] A simplified overview of one or more embodiments is presented below in order to provide a basic understanding of the present invention. This overview is not an exhaustive overview of all contemplated embodiments, and is not intended to identify key or important elements of all embodiments, nor is it intended to delineate the scope of any or all embodiments. Its sole purpose is to present some concepts of one or more embodiments in a simplified form as a prelude to a more detailed description that will be presented later.

[0009] According to one aspect of the embodiment, an electrode for a laser chamber is disclosed, the electrode comprising an alloy of a first metal and a second metal, wherein a first free energy of formation of the first metal with fluorine is greater than or equal to a free energy of formation of copper with fluorine, and a second free energy of formation of the second metal with fluorine is less than the first free energy. The first metal may be cobalt because it has a greater formation energy in a CO-Cu alloy. The second metal may be copper because it has a lower formation energy in a CO-Cu alloy. The alloy may be CoCu (5-15wt%). The alloy may be Co90Cu10wt%. The second metal may be silver. The alloy may be Cu(x)Ag(100-x)wt%, wherein x is in the range of about 95 to about 60. The alloy may be Cu60Ag40wt%.

[0010] According to another aspect of the embodiment, a laser is disclosed, the laser having a discharge chamber and a first electrode at least partially located in the discharge chamber, the first electrode comprising an alloy of a first metal and a second metal, the first free energy of formation of the first metal with fluorine being greater than or equal to the free energy of formation of copper with fluorine, and the second free energy of formation of the second metal with fluorine being less than the first free energy. The electrode may be an anode. The first metal may be cobalt. The second metal may be copper. The alloy may be CoCu (5-15wt%). The alloy may be Co90Cu10wt%. The second metal may be silver. The alloy may be Cu(x)Ag(100-x)wt%, wherein x is in the range of about 95 to about 60. The alloy may be Cu60Ag40wt%.

[0011] Further embodiments, features, and advantages of the present invention, as well as the structure and operation of various embodiments are described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The accompanying drawings, which are incorporated herein and form a part of the specification, illustrate the methods and systems of embodiments of the present invention by way of example and not limitation. Together with the detailed description, the accompanying drawings are also used to explain the principles of the methods and systems proposed herein and enable those skilled in the relevant art to make and use the methods and systems proposed herein. In the accompanying drawings, the same reference numerals represent the same or functionally similar elements.

[0013] Figure 1 A schematic view (not drawn to scale) showing an overall broad concept of a lithography system according to aspects of the disclosed subject matter is shown.

[0014] Figure 2 A schematic view (not drawn to scale) showing an overall broad concept of an illumination system according to aspects of the disclosed subject matter is shown.

[0015] Figure 3 A diagrammatic (not to scale) cross-sectional view of a discharge chamber for an excimer laser is shown in accordance with various aspects of the disclosed subject matter.

[0016] Figure 4A and Figure 4B is a diagram comparing protective layers on two electrodes of different materials.

[0017] Figure 5A and Figure 5B are diagrams illustrating some theoretical principles according to various aspects of the disclosed subject matter.

[0018] The further features and advantages of the present invention and the structure and operation of various embodiments of the present invention are described in detail below with reference to the accompanying drawings. Note that the present invention is not limited to the specific embodiments described herein. Such embodiments proposed herein are for illustrative purposes only. Based on the teachings contained herein, additional embodiments will be apparent to those skilled in the relevant art. DETAILED DESCRIPTION

[0019] Various embodiments are now described with reference to the accompanying drawings, wherein throughout the text, similar reference numerals are used to refer to similar elements. In the following description, many specific details are set forth for the purpose of explanation, so as to facilitate a thorough understanding of one or more embodiments. However, it may be apparent in some cases or all cases that any embodiment described below can be practiced without adopting the specific design details described below. In other examples, known structures and equipment are shown in block diagram form, so as to facilitate the description of one or more embodiments. A simplified overview of one or more embodiments is presented below, so as to provide a basic understanding of the embodiments. This overview is not an exhaustive overview of all intended embodiments, and is not intended to identify the key or important elements of all embodiments, nor is it intended to describe the scope of any embodiment or all embodiments.

[0020] refer to Figure 1 , the lithography system 100 includes an illumination system 105. As described more fully below, the illumination system 105 includes a light source that generates a pulsed light beam 110 and directs it to a lithography exposure device or scanner 115, which patterns microelectronic features on a wafer 120. The wafer 120 is placed on a wafer stage 125, which is constructed to hold the wafer 120 and is connected to a positioner that is configured to accurately position the wafer 120 according to certain parameters.

[0021] The photolithography system 100 uses a light beam 110 having a wavelength in the deep ultraviolet (DUV) range (e.g., having a wavelength of 248 nanometers (nm) or 193 nm). The minimum size of a microelectronic feature that can be patterned on a wafer 120 depends on the wavelength of the light beam 10, with shorter wavelengths resulting in smaller minimum feature sizes. For example, when the wavelength of the light beam 110 is 248 nm or 193 nm, the minimum size of a microelectronic feature can be 50 nm or less. The bandwidth of the light beam 110 can be the actual instantaneous bandwidth of its spectrum (or emission spectrum), which contains information about how the light energy of the light beam 110 is distributed over different wavelengths. The scanner 115 includes an optical configuration having, for example, one or more condenser lenses, a mask, and an objective lens arrangement. The mask can be moved along one or more directions (such as, along the optical axis of the light beam 110 or in a plane perpendicular to the optical axis). The objective lens arrangement includes a projection lens and enables an image to be transferred from the mask to the photoresist on the wafer 120. The illumination system 105 adjusts the range of angles for which the light beam 110 is incident on the mask. The illumination system 105 also uniformizes (homogenizes) the intensity distribution of the light beam 110 on the mask.

[0022] Among other features, the scanner 115 may include a lithography controller 130, air conditioning, and power supplies for various electrical components. The lithography controller 130 controls how layers are printed on the wafer 120. The lithography controller 130 includes a memory that stores information such as a process recipe. For example, the process program or recipe determines the length of the exposure on the wafer 120 based on the mask used and other factors that affect the exposure. During lithography, multiple pulses of the light beam 110 illuminate the same area of ​​the wafer 120 to constitute an exposure dose.

[0023] The lithography system 100 also preferably includes a control system 135. Typically, the control system 135 includes one or more of digital electronic circuitry, computer hardware, firmware, and software. The control system 135 also includes a memory, which may be a read-only memory and / or a random access memory. Storage devices suitable for tangibly embodying computer program instructions and data include all forms of non-volatile memory, including, for example: semiconductor memory devices, such as EPROM, EEPROM, and flash memory devices; magnetic disks, such as internal hard disks and removable disks; magneto-optical disks; and CD-ROM disks;

[0024] The control system 135 may also include one or more input devices (such as a keyboard, a touch screen, a microphone, a mouse, a handheld input device, etc.) and one or more output devices (such as a speaker or a monitor). The control system 135 also includes one or more programmable processors and one or more computer program products, which are tangibly embodied in a computer-readable storage device for execution by the one or more programmable processors. One or more programmable processors can be a program of instructions to perform the desired function by operating on input data and generating appropriate outputs. Typically, the processor receives instructions and data from a memory. Any of the foregoing contents can be supplemented or incorporated by a specially designed ASIC (application-specific integrated circuit). The control system 135 can be centralized, or can be distributed partially or completely throughout the lithography system 100.

[0025] refer to Figure 2 , an exemplary illumination system 105 is a pulsed laser source that generates a pulsed laser beam as the light beam 110 . Figure 2 A gas discharge laser system according to an embodiment of certain aspects of the disclosed subject matter is schematically illustrated in block diagram form. For example, the gas discharge laser system can include a solid state or gas discharge seed laser system 140, an amplification stage (e.g., a power ring amplifier ("PRA") stage 145), relay optics 150, and a laser system output subsystem 160. For example, the seed system 140 can include a master oscillator ("MO") chamber 165.

[0026] The seed laser system 140 may also include a master oscillator output coupler ("MO OC") 175, which may include: a partially reflecting mirror formed with a reflective grating (not shown) in a line narrowing module ("LNM") 170; an oscillator chamber in which the seed laser 140 forms a seed laser output pulse, i.e., forms a master oscillator ("MO"). The system may also include a line core analysis module ("LAM") 180. The LAM 180 may include an etalon spectrometer for fine wavelength measurement and a grating spectrometer for coarser resolution. The MO wavefront engineering box ("WEB") 185 may be used to redirect the output of the MO seed laser system 140 toward the amplifier stage 145, and may include, for example, beam expansion using a multi-prism beam expander (not shown) and coherent blanking, for example, in the form of an optical delay path (not shown).

[0027] The amplifier stage 145 may include, for example, a PRA lasing chamber 200, which may also be an oscillator formed, for example, by seed beam injection, and output coupling optics (not shown) which may be incorporated into the PRA WEB 210 and may be redirected back through the gain medium in the chamber 200 by the beam reverser 220. The PRA WEB 210 may incorporate a partially reflecting input / output coupler (not shown) and a maximum reflector for a nominal operating wavelength (e.g., at about 193 nm for ArF systems) and one or more prisms.

[0028] A bandwidth analysis module ("BAM") 230 at the output of the amplifier stage 145 can receive the pulsed output laser beam from the amplifier stage and pick off a portion of the beam for measurement purposes (e.g., to measure the output bandwidth and pulse energy). The pulsed laser output beam then passes through an optical pulse stretcher ("OPuS") 240 and an output combined automatic mask measurement module ("CASMM") 250, which can also be the location of a pulse energy meter. For example, one purpose of the OPoS 240 can be to convert a single output laser pulse into a pulse train. The secondary pulses generated by the original single output pulse can be delayed relative to each other. By distributing the original laser pulse energy into a series of secondary pulses, the effective pulse length of the laser can be extended while reducing the peak pulse intensity. Thus, the OPoS 240 can receive the laser beam from the PRA WEB 210 via the BAM 230 and direct the output of the OPoS 240 to the CASMM 250.

[0029] As is known in the art, the PRA lasing chamber 200 and MO 165 are configured as a chamber where a discharge between electrodes can cause a lasing gas discharge in a lasing gas to create an inverted group of high energy molecules (e.g., Ar, Kr, and / or Xe) to produce a relatively broad band radiation that can be a line narrowed to a relatively very narrow bandwidth and a center wavelength selected in a line narrowing module ("LNM") 170. Figure 3 A configuration for such a chamber 300 is shown in , which is a highly stylized cross-sectional view of a discharge chamber. Chamber 300 includes an upper electrode 310 that functions as a cathode and a lower electrode 320 that functions as an anode. One or both of lower electrode 320 and upper electrode 310 may be fully contained within the pressure envelope of chamber 300 defined by chamber walls 305, or one of the electrodes may not be contained. A lasing gas discharge occurs between the two electrodes in a gap having a width A. In Figure 3 Also shown in FIG. 3 are an upper insulator 315 and a lower insulator 325. The lower electrode 320 is electrically connected to the wall 305 of the chamber 300. For safety reasons, it is desirable to keep the chamber wall 300, and therefore the lower electrode 320, at ground potential. Figure 3 In the illustrated embodiment, the upper electrode 310 is driven by the power supply 340 at a negative voltage relative to the lower electrode 320 .

[0030] When the lower electrode 320 is Figure 3 When used as an anode as shown, it is advantageously made of a material that does not show wear but actually grows a corrosion resistant coating 330. For illustrative purposes, Figure 3 The size of the coating 330 is exaggerated in FIG.

[0031] As mentioned above, in Figure 3 Also shown is a voltage source 340 that establishes a voltage gradient across the cathode 310 and anode 320. Although a sign (-) is shown for the polarity of the output of the voltage source 340, it should be understood that this is a relative, rather than an absolute, polarity, i.e., relative to the polarity of the lower electrode 320, which is generally in electrical contact with the body of the chamber 300 and must be maintained at ground (0) potential. The upper electrode (cathode 310) is charged to a large (e.g., approximately 20 kV) negative voltage.

[0032] In MO, reefing and high corrosion rates are a problem. This is the result of the reaction of fluorine with the electrode material. According to one aspect of the embodiment, the electrode is made of an alloy, the alloy comprising a first metal and a second metal, the energy formed by the first metal and F2 is equal to or greater than the energy formed by copper and F2, and the energy formed by the second metal and F2 is less than the energy formed by the first metal and F2. The alloy comprises a metal (such as copper) that has good thermal and electrical conductivity and good resistance to fluorination. Other such metals would include nickel, cobalt and silver. Non-alloyed pure elements are generally relatively soft compared to ordinary structural metals and have very high thermal expansion that will result in high erosion rates. Therefore, it is advantageous to alloy them with another metal (such as copper) to increase hardness and potentially reduce erosion rates.

[0033] The free energy of formation, also called the standard Gibbs free energy of formation of a compound, is the change in Gibbs free energy with the formation of one mole of a substance from its constituent elements in their standard state (the most stable form of the element at 1 bar pressure and a specified temperature, usually 298.15 K or 25 °C).

[0034] The protective layer formed on top of the electrode surface due to the reaction of the second metal with fluorine also plays an important role in reducing the reaction of fluorine with the bulk material of the electrode. The denser and more uniform the protective layer, the more it can be expected that the erosion rate will be reduced. Co90Cu10wt% shows dense and continuous film layer formation under operating conditions. This is within the range of relative weight percentage CoCu (5-15wt%), in which it can also be expected to show dense and continuous film layer formation under operating conditions.

[0035] As mentioned above, silver also exhibits a low standard free energy of formation with F2. Cu60Ag40wt% also shows dense and continuous thin film layer formation under operating conditions. This is within the range of relative weight percentages 5-40wt% Ag-Cu, which relative weight percentages can also be expected to show dense and continuous thin film layer formation under operating conditions.

[0036] exist Figure 4A and Figure 4B The opposite effect of using these alloys to conventional materials is shown in . Figure 4A The effect of the reaction of fluorine with the overall material 400 of the electrode made of brass is shown. It can be seen that a protective layer 410 is formed on the overall material 400, but the layer 410 is not uniform and exhibits cracks. On the other hand, Figure 4BThe effect of fluorine reacting with the bulk material 420 of an electrode made of Co90Cu10wt% is shown. It can be seen that a protective layer 430 is formed on the bulk material 420, but the layer 430 is more uniform and exhibits fewer cracks than the layer 410. These layers are formed on CO-Cu and Ag-Cu samples placed in a TGA (thermogravimetric analysis) furnace (similar to the chamber conditions) at 450°C and 1% F2. The passivation layer was detected in SEM-EDX.

[0037] Return to reference Figure 3 , when the lower electrode 320 is used as an anode, it can be advantageously made of the alloy described above so that the corrosion-resistant coating (passivation layer) 330 formed in use is denser and more continuous and has good adhesion to the body of the electrode.

[0038] Figure 5A and Figure 5B Principles believed to underlie the observed effects are depicted. Figure 5A An electrode overall material 500 is shown consisting of atoms of a first metal 510 and atoms of a second metal 520 in an environment where the overall material 500 is exposed to fluorine molecules 530. As described above, the free energy of formation of the first metal with fluorine is equal to or greater than the free energy of formation of copper with fluorine. For example, the first metal can be cobalt or silver. The free energy of formation of the second metal with fluorine is less than the energy of formation of the first metal with fluorine. For example, the second metal can be copper. Figure 5B As shown, atoms of the second metal 520 migrate to the interface with the fluorine-containing environment where they combine with the fluorine to form the passivation layer 540. Of course, other or additional principles may also contribute to the observed effects, and embodiments are not limited to arrangements to which these principles apply.

[0039] The above description includes examples of multiple embodiments. Of course, for the purpose of describing the above-mentioned embodiments, it is impossible to describe every possible combination of parts or methods, but those of ordinary skill in the art will recognize that many other combinations and permutations of various embodiments are possible. Therefore, the described embodiments are intended to cover all such changes, modifications and variations that fall within the spirit and scope of the appended claims. In addition, to the extent that the term "comprise" is used in the detailed description or claims, the term is intended to be included in a manner similar to the term "comprises", because when a transition term is adopted in a claim, "comprises" is interpreted as "comprising". In addition, although the elements of the described aspects and / or embodiments may be described or claimed in the singular, the plural form may be conceived unless the limitation to the singular form is explicitly stated. Additionally, unless otherwise stated, all or part of any aspect and / or embodiment may be used together with all or part of any other aspect and / or embodiment.

[0040] Other aspects of the invention are set out in the following numbered clauses.

[0041] 1. An electrode for a laser chamber, the electrode comprising an alloy of a first metal and a second metal, a first free energy of formation of the first metal with fluorine being greater than or equal to a free energy of formation of copper with fluorine, and a second free energy of formation of the second metal with fluorine being less than the first free energy.

[0042] 2. An electrode for a laser chamber as described in clause 1, wherein the first metal is cobalt.

[0043] 3. An electrode for a laser chamber as described in clause 1, wherein the second metal is copper.

[0044] 4. An electrode for a laser chamber as described in clause 1, wherein the first metal is cobalt and the second metal is copper.

[0045] 5. An electrode for a laser chamber as described in clause 4, wherein the alloy is CoCu (5-15 wt%).

[0046] 6. An electrode for a laser chamber as described in clause 5, wherein the alloy is Co90Cu10wt%.

[0047] 7. An electrode for a laser chamber as described in clause 1, wherein the second metal is silver.

[0048] 8. An electrode for a laser chamber as described in clause 1, wherein the first metal is copper and the second metal is silver.

[0049] 9. An electrode for a laser chamber as described in clause 8, wherein the alloy is Cu(x)Ag(100-x) wt%, wherein x is in the range of about 95 to about 60.

[0050] 10. An electrode for a laser chamber as described in clause 9, wherein the alloy is Cu60Ag40wt%.

[0051] 11. An electrode for a laser chamber, the electrode comprising an alloy of cobalt and copper.

[0052] 12. An electrode for a laser chamber as described in clause 11, wherein the alloy is CoCu (5-15 wt%).

[0053] 13. An electrode for a laser chamber as described in clause 11, wherein the alloy is Co90Cu10wt%.

[0054] 14. An electrode for a laser chamber, the electrode comprising an alloy of copper and silver.

[0055] 15. An electrode for a laser chamber as described in clause 14, wherein the alloy is Cu(x)Ag(100-x) wt%, wherein x is in the range of about 95 to about 60.

[0056] 16. An electrode for a laser chamber as described in clause 14, wherein the alloy is Cu60Ag40wt%.

[0057] 17. A laser comprising:

[0058] a discharge chamber; and

[0059] The first electrode is at least partially located in the discharge chamber, the first electrode includes an alloy of a first metal and a second metal, a first free energy of formation of the first metal with fluorine is greater than or equal to a free energy of formation of copper with fluorine, and a second free energy of formation of the second metal with fluorine is less than the first free energy.

[0060] 18. The laser of clause 17, wherein the electrode is an anode.

[0061] 19. The laser of clause 17, wherein the first metal is cobalt.

[0062] 20. The laser of clause 17, wherein the second metal is copper.

[0063] 21. The laser of clause 17, wherein the first metal is cobalt and the second metal is copper.

[0064] 22. The laser of clause 21, wherein the alloy is CoCu (5-15 wt%).

[0065] 23. The laser of clause 22, wherein the alloy is Co90Cu10wt%.

[0066] 24. The laser of clause 17, wherein the second metal is silver.

[0067] 25. The laser of clause 17, wherein the first metal is copper and the second metal is silver.

[0068] 26. The laser of clause 25, wherein the alloy is Cu(x)Ag(100-x) wt%, wherein x is in the range of about 95 to about 60.

[0069] 27. The laser of clause 26, wherein the alloy is Cu60Ag40wt%.

[0070] 28. A laser comprising:

[0071] a discharge chamber; and

[0072] The first electrode is at least partially located in the discharge chamber, and the first electrode includes an alloy of cobalt and copper.

[0073] 29. The laser of clause 28, wherein the alloy is CoCu (5-15 wt%).

[0074] 30. The laser of clause 28, wherein the alloy is Co90Cu10wt%.

[0075] 31. A laser comprising:

[0076] a discharge chamber; and

[0077] The first electrode is at least partially located in the discharge chamber, and the first electrode includes an alloy of copper and silver.

[0078] 32. The laser of clause 31, wherein the alloy is Cu(x)Ag(100-x) wt%, wherein x is in the range of about 95 to about 60.

[0079] 33. The laser of clause 31, wherein the alloy is Cu60Ag40wt%.

[0080] 34. An electrode for a laser chamber, the electrode comprising an alloy of a first metal and a second metal, the first metal having a first free energy of formation with fluorine greater than or equal to a free energy of formation with copper and fluorine, and the second metal having a second free energy of formation with fluorine less than the first free energy.

Claims

1. An electrode for a laser chamber, the electrode comprising an alloy of a first metal and a second metal, the first metal having a first free energy of formation with fluorine, the first free energy being greater than the free energy of formation of copper with fluorine, and the second metal having a second free energy of formation with fluorine, the second free energy being less than the first free energy, wherein the first metal is cobalt, the second metal is copper, the alloy is a CoCu alloy, and Cu accounts for 5wt% to 15wt% of the CoCu alloy.

2. The electrode for a laser chamber according to claim 1, wherein the alloy is Co90Cu10wt%.

3. An electrode for a laser chamber, the electrode comprising an alloy of cobalt and copper, wherein the alloy is a CoCu alloy, and Cu accounts for 5 wt % to 15 wt % of the CoCu alloy.

4. The electrode for a laser chamber according to claim 3, wherein the alloy is Co90Cu10wt%.

5. A laser comprising: a discharge chamber; as well as A first electrode is at least partially located within the discharge chamber, the first electrode comprising an alloy of a first metal and a second metal, the first metal having a first free energy of formation with fluorine, the first free energy being greater than a free energy of formation with copper with fluorine, and the second metal having a second free energy of formation with fluorine, the second free energy being less than the first free energy, wherein the first metal is cobalt, wherein the second metal is copper, wherein the alloy is a CoCu alloy, and Cu accounts for 5 wt % to 15 wt % of the CoCu alloy.

6. The laser of claim 5, wherein the electrode is an anode.

7. The laser of claim 5, wherein the alloy is Co90Cu10wt%.

8. A laser comprising: a discharge chamber; as well as A first electrode is at least partially located in the discharge chamber, wherein the first electrode comprises an alloy of cobalt and copper, wherein the alloy is a CoCu alloy, and Cu accounts for 5 wt % to 15 wt % of the CoCu alloy.

9. The laser of claim 8, wherein the alloy is Co90Cu10wt%.