Compression set

By using a specific combination of compounds in the reaction of polyols and isocyanates, the porosity and stability of molded thermosetting flexible PU foam were improved, the problem of shape recovery after compression was solved, and the effects of low emissions and efficient shape recovery were achieved.

CN112778751BActive Publication Date: 2024-10-22EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011222515.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-07
Filing Date
2020-11-05
Publication Date
2024-10-22
Estimated Expiration
2040-11-05

AI Technical Summary

Technical Problem

Existing molded thermosetting flexible PU foam products are prone to material fatigue during compression and transportation, making it difficult to restore their original shape, especially after prolonged compression.

Method used

By using compounds of formula (1a) and formula (1b) in specific proportions as foam stabilizers in the reaction of polyol components with isocyanate components, the porosity and stability of foam are improved, thereby restoring the original shape after compression.

Benefits of technology

It enables molded thermosetting flexible PU foam products to effectively recover their original shape after being compressed for at least 20 hours, reduces the emission of low molecular weight siloxanes, and meets low emission standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_33
    Figure SMS_33
Patent Text Reader

Abstract

The invention relates to compression set. The invention describes a shaped thermosetting flexible PU foam article, preferably a mattress and / or a cushion, wherein the thermosetting flexible polyurethane foam is obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b) and at least one blowing agent and at least one catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of polyurethane (PU) foams. In particular, the present invention relates to providing shaped heat-cured soft PU foam products, such as mattresses and / or cushions. Background Art

[0002] Molded thermosetting soft PU foam articles, such as mattresses and / or cushions containing thermosetting soft PU foam, have long been known from the prior art and are used worldwide. There has been no lack of attempts to achieve greater improvements. The need for optimization has not yet been fully met.

[0003] One problem with molded heat-cured flexible PU foam products is their transportation and storage. Molded heat-cured flexible PU foam products (such as mattresses) are very bulky and therefore, for space considerations, are often compressed, especially compressed and vacuum packed, for storage and transportation. Large distributors are increasingly shipping certain mattresses in compressed and rolled form.

[0004] This type of packaging is widely used in particular for mattresses. In vacuum packaging, a mattress is placed in a bag, for example made of plastic film. The mattress thus prepackaged is then placed in a press and compressed, with one end of the bag open. The air is exhausted. The open end of the bag is then welded closed in an airtight manner. The vacuum packaging thus obtained is then rolled up and placed in an outer bag. Since the outer bag holds the mattress in rolled-up form, the mattress cannot expand again.

[0005] Depending on the mattress, flattening the mattress to the extent achieved by the machine during rolling, for example, requires a force of between 40,000 and 250,000 N. This corresponds to a weight exerted by a mass of 4 to 25 tonnes.

[0006] Obviously, such forces associated with compression of shaped heat-cured flexible PU foam articles may lead to material fatigue.It is a very significant problem to provide shaped heat-cured flexible PU foam articles that are able to recover their original dimensions even after long-term compression.

[0007] In this context, an object of the present invention is in particular to provide shaped heat-cured flexible PU foam articles, such as in particular mattresses and / or cushions containing heat-cured flexible PU foam, having a good ability to recover their original shape after being compressed for a period of at least 20 hours.

[0008] In the context of the present invention, it has now been found that, surprisingly, this object can be achieved by the subject matter of the present invention. Summary of the invention

[0009] The present invention provides a shaped thermosetting soft PU foam product, preferably a mattress and / or a cushion, wherein the thermosetting soft PU foam is obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b) and at least one blowing agent and at least one catalyst,

[0010] in

[0011] Formula (1a): [R 1 Me 2 SiO 1 / 2 ] a [Me 2 SiO 2 / 2 ] b [R 2 MeSiO 2 / 2 ] c [MeSiO 3 / 2 ] d [SiO 4 / 2]e

[0012] in

[0013] a=2 to 10, preferably 2 to 8, more preferably 2 to 5

[0014] b=25 to 200, preferably 40 to 150, more preferably 45 to 120

[0015] c=2 to 40, preferably 2 to 30, more preferably 3 to 20

[0016] d=0 to 10, preferably 0 to 8, more preferably 0 to 5

[0017] e=0 to 5, preferably 0 to 3, more preferably 0 to 2

[0018] in:

[0019] a+b+c+d+e>48

[0020] R 1 =Me or R 2

[0021] R 2 = the same or different polyethers obtainable from the polymerization of ethylene oxide, propylene oxide and / or other alkylene oxides such as butylene oxide or styrene oxide, preferably polyethers of the general formula (c),

[0022]

[0023] in

[0024] f=0-6, preferably 0-4, more preferably 0 or 3

[0025] g=0 to 150, preferably 3 to 100, more preferably 3 to 70

[0026] h=0 to 150, preferably 0 to 100, more preferably 0 to 80

[0027] in

[0028] g+h>0

[0029] R 3 =OH, alkyl or acetyl, preferably OH, C 1 To C 6 - alkyl or acetyl, more preferably OH, methyl, acetyl or butyl

[0030] And among them

[0031] Formula (1b): [R 4 Me 2 SiO 1 / 2 ] i [Me 2 SiO 2 / 2 ] j [R 5 MeSiO 2 / 2 ] k [MeSiO 3 / 2 ] l [SiO 4 / 2 ] m

[0032] in

[0033] i=2 to 10, preferably 2 to 8, more preferably 2 to 5

[0034] j=0 to 20, preferably 0 to 18, more preferably 0 to 15

[0035] k=0 to 20, preferably 0 to 15, more preferably 0 to 10

[0036] l=0 to 10, preferably 0 to 8, more preferably 0 to 5

[0037] m=0 to 5, preferably 0 to 3, more preferably 0 to 2

[0038] in:

[0039] i+j+k+l+m<20

[0040] R 4 =Me or R 5

[0041] R 5= the same or different polyethers obtainable from the polymerization of ethylene oxide, propylene oxide and / or other alkylene oxides such as butylene oxide or styrene oxide, preferably polyethers of the general formula (d), or alkyl C 3 To C 15 ,

[0042]

[0043] in

[0044] n=0-6, preferably 0-4, more preferably 0 or 3

[0045] o=0 to 100, preferably 0 to 50, more preferably 0 to 25

[0046] p=0 to 100, preferably 0 to 50, more preferably 0 to 25

[0047] in

[0048] o+p>0

[0049] R 6 =OH, alkyl or acetyl, preferably OH, C 1 To C 6 -alkyl or acetyl, more preferably OH, methyl, acetyl or butyl.

[0050] Formulas (1a) and (1b) should be regarded as average empirical formulas. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figures 1 to 3 The results of the roll-up deformation test are shown as a function of the change in air permeability. The roll-up deformation test is explained in further detail below. It allows the dimensional recovery of a shaped PU foam after compression to be assessed. The air permeability is a measure of the porosity of the PU foam in question. The results of the roll-up deformation test are plotted on the ordinate in each case. The air permeability is plotted on the abscissa in each case. Figures 1 to 3 It is shown that the inventive use of at least one compound of the formula (1a) and at least one compound of the formula (1b) in the production of heat-cured flexible PU foams enables an improvement in the dimensional recovery of shaped PU foam articles having comparable porosity after compression.

[0052] Optionally, other conventional additives, active substances and auxiliaries can also be used advantageously in addition. In the context of the present invention, mattresses are particularly preferred. This also applies advantageously to all the following preferred embodiments.

[0053] Advantageously, the shaped heat-cured flexible PU foam articles thus provided using the compounds of formula (1a) and (1b) therefore have a good ability to recover their original shape even after prolonged compression over a period of at least 20 hours.

[0054] A further advantage is that the shaped heat-cured flexible PU foam articles in question have particularly low emissions with regard to the emissions of low molecular weight linear and cyclic siloxanes.

[0055] More specifically, in the context of the present invention, "low emission" with respect to low molecular weight siloxanes means that the siloxane emission of the heat-cured flexible PU foam produced according to the present invention is ≥ 0 μg / m 3 To ≤500 μg / m 3 , preferably ≤200μg / m 3 , more preferably ≤100 μg / m 3 , which is suitably determined 24 hours after the laboratory is loaded by a laboratory method based on DIN standard DIN EN ISO 16000-9:2008-04. This method is precisely described in EP 3205680 A1, in particular in paragraph

[0070] , which document is incorporated herein by reference.

[0056] Another advantage is that the shaped thermosetting flexible PU foam article in question can also comply with emission regulations such as CertiPur. Here, low emissions according to CertiPur refer to total emissions of volatile organic compounds (TVOC) less than 500 μg / m 3 Additional technical details of the requirements of the CertiPUR standard (version 1, July 2017) can be found at: https: / / www.europur.org / images / CertiPUR_Technical_Paper_-_Full_Version_-_2017.pdf. This latter document (version 1, July 2017) can also be ordered directly at EUROPUR, B-1000, Avenue de Cortenbergh 71, Brussels, Belgium.

[0057] PU foams (polyurethane foams) and their production are well known to the person skilled in the art and do not require any further explanation per se. Molded articles in the context of the present invention are shaped bodies of different shapes. Preferred shapes in the context of the present invention are, for example, geometric shapes such as spheres, cubes, cylinders and the like. Molded PU foam articles in the context of the present invention are therefore shaped bodies made of polyurethane foam. Particularly preferred shaped thermosetting flexible PU foam articles in the context of the present invention are mattresses and / or cushions, and generally also foam blocks.

[0058] Mattresses themselves and their production are known. They usually consist of a mattress core (e.g., comprising foam, latex, natural products and / or spring cores) and a cover surrounding the mattress. The corresponding situation applies to cushions. In the context of the present application, the term mattress and / or cushion is understood to mean that there is at least one part made of soft heat-cured PU foam in the mattress and / or cushion. This preferably means that at least a part of the mattress and / or cushion consists of soft heat-cured PU foam. Based on the total weight of the mattress and / or cushion, this part can account for at least 1% by weight or 5% by weight or 25% by weight, preferably at least 50% by weight, and in particular at least 75% by weight. It is also possible to make the mattress and / or cushion completely consist of soft heat-cured PU foam except for the cover.

[0059] The production of polyurethane foams is generally known per se. They are formed by reacting at least one polyol component with at least one isocyanate component in a polyaddition reaction in the presence of at least one blowing agent, such as water. It is essential for the present invention that the foam is a flexible, heat-curing PU foam and that the reaction is carried out in the presence of at least one compound of the formula (1a) and at least one compound of the formula (1b) as defined above.

[0060] The polyurethane foam according to the invention is a thermosetting flexible polyurethane foam, or a combination of these flexible PU foams is used, for example two of these flexible PU foams. The term "flexible thermosetting PU foam" is known per se to those skilled in the art; this is a fixed technical term established accordingly in the professional field, but is briefly explained here.

[0061] Soft PU foams are elastic and deformable and usually have open cells. Therefore, when compressed, air can easily escape. In addition, there are also hard PU foams, which are inelastic and usually have closed cells, which are used for insulation purposes and are not in the focus of the present invention. There are many soft PU foams. For example, the person skilled in the art knows, among others, ester foams (made of polyester polyols), soft heat-curing PU foams and cold-curing PU foams. Viscoelastic soft PU foams are a relatively new type, which are considered heat-curing soft PU foams. Therefore, in the context of the present invention, viscoelastic flexible PU foams are also included in the term "flexible heat-cured PU foam". The key difference between heat-cured flexible PU foams and cold-cured PU foams lies in the different mechanical properties. Soft heat-cured PU foams can be distinguished from soft cold-cured PU foams by, in particular, the resilience, also known as ball rebound (BR) or rebound resilience. For example, a method for determining the rebound resilience is described in DIN EN ISO 8307:2008-03. Here, a steel ball with a fixed mass is dropped from a certain height onto a test specimen and the rebound height is then measured as a percentage of the drop height. The values ​​discussed for cold-cured flexible PU foams are preferably in the region of >50%. Therefore, cold-cured flexible PU foams are also often referred to as HR foams (HR: high resilience). In contrast, the rebound values ​​of heat-cured flexible PU foams are preferably from 1% to not more than 50%. In the context of a preferred embodiment of the present invention, the rebound values ​​of the heat-cured flexible PU foams according to the invention are therefore preferably from 1% to not more than 50%, which can be determined according to DIN EN ISO 8307:2008-03. Another mechanical criterion is the relaxation or comfort factor. In this case, the foam samples are compressed according to DIN EN ISO 2439 and the ratio of the compression stress at 65% to 25% compression is measured. Here, the relaxation or comfort factor of cold-curing flexible PU foams is preferably >2.5. The value for heat-curing flexible PU foams is preferably <2.5. In a preferred embodiment of the present invention, the relaxation or comfort factor of the heat-curing flexible PU foams of the present invention is therefore preferably <2.5, which can be determined as described in detail above.

[0062] A precise definition of the properties can also be taken from, for example, the data sheet “PUR-Kaltschaum” [Cold-Cure PU Foam] from Fachverband Schaumkunststoffe und Polyurethane eV [Specialist Association Foamed Plastics and Polyurethanes], reference KAL20160323, last updated on March 23, 2016. (https: / / www.fsk-vsv.de / wp-content / uploads / 2017 / 03 / Produktbeschreibung-PUR-Kaltschaum.pdf). The data sheet can also be ordered directly from Fachverband Schaumkunststoffe und Polyurethane eV (FSK), mailing address: Stammheimerstr. 35, D-70435 Stuttgart.

[0063] The historical development of PU technology explains the two names of hot-cure soft PU foam and cold-cure soft PU foam, which do not necessarily mean different temperatures occurring during the foaming process.

[0064] The different mechanical properties of heat-curing PU foams and cold-curing PU foams are caused by the differences in the formulations used to produce the foams. In the case of cold-curing flexible PU foams, polyols with significantly higher reactivity, which have primary OH groups and an average molar mass>4000 g / mol, are generally used. Optionally, low molecular weight crosslinkers are also used, and the role of the crosslinker can also be assumed by isocyanates with higher functionality. In the case of heat-curing flexible PU foams, polyols with secondary OH groups and an average molar mass of <4000 g / mol and relatively significantly unreactive are generally used. In the case of cold-curing flexible PU foams, the reaction of isocyanate groups with hydroxyl groups therefore occurs as early as the expansion stage (CO 2 By –NCO and H 2O formation) will occur. Due to the increase in viscosity, this fast polyurethane reaction usually leads to a relatively high intrinsic stability of the foam during the foaming process. Therefore, other foam stabilizers with different siloxane structures are required compared to heat-cured soft PU foams, which is why the present invention does not extend to cold-cured soft PU foams. Cold-cured soft PU foams are usually high-elastic foams. Due to the high intrinsic stability, the holes are usually not fully opened at the end of the foaming operation, and the hole structure must be opened by mechanical crushing. In contrast, in the case of heat-cured soft PU foams, this is usually not necessary. The significantly greater stability achieved by the high molecular weight polyether siloxane structure is important here. The corresponding highly active stabilizer is defined by formula (1a). In the case of the heat-cured soft PU foam according to the present invention and the stabilizer of formula (1a), a silicone compound of formula (1b) is additionally used in production.

[0065] The open-cell, heat-cured, flexible PU foam preferably has a gas permeability (also referred to as "porosity") in the range of 1 to 6.5 scfm. This is measured by applying a pressure difference according to ASTM D 3574 (2011-00) and measuring the volume of air flowing through. This method is described in detail in the examples (see porosity determined by the flow method therein). Scfm (standard cubic feet per minute) is measured under standard conditions (23°C, 100 kPa).

[0066] Depending on the application, the heat-cured soft PU foam preferably has a weight of 8-80 kg / m 3 In particular, when such heat-cured flexible PU foams are used as mattresses, mattress components and / or cushions, the foams are differentiated according to regional requirements and consumer needs, requirements and preferences. Preferred heat-cured flexible PU foams for mattress applications have a foam density of preferably 25-30 kg / m3.

[0067] A specific class of thermosetting flexible PU foams is a class of viscoelastic PU foams. These are also known as "memory foams" and exhibit low resilience (preferably <10%) and slow, gradual recovery after compression (recovery time is preferably 2-10s). Such materials are well known in the art and are highly valued, inter alia, for their energy and sound absorption properties. Typical viscoelastic flexible foams generally have a lower porosity and a high density (or high foam density (FD)) compared to other thermosetting flexible PU foams. The cushion has preferably 30-50 kg / m 3 The foam density is therefore at the lower end of the density range peculiar to viscoelastic foams, whereas viscoelastic PU foams for mattresses preferably have a density of 50-130 kg / m 3 Density within the range.

[0068] In heat-cured flexible PU foams, hard (high glass transition temperature) and soft (low glass transition temperature) segments adapt relative to each other during the reaction and then spontaneously separate from each other to form morphologically different phases within the "bulk polymer". Such materials are also referred to as "phase-separated" materials. The glass transition temperature in the case of viscoelastic foams is preferably between -20°C and +15°C. In contrast, the glass transition temperatures of other heat-cured flexible PU foams and cold-cured flexible PU foams are typically below -35°C. Such "structural viscoelasticity" (which is essentially based on the glass transition temperature of the polymer) in the case of open-cell viscoelastic heat-cured flexible PU foams should be distinguished from aerodynamic effects. In the latter case, the pore structure is relatively closed (low porosity). Due to the low air permeability, the air only flows back gradually after compression, which slows down the recovery.

[0069] With regard to the foam stabilizers used, in the context of the present invention, compounds of the formula (1a) are used for viscoelastic PU foams. The addition of compounds of the formula (1b) leads in particular to an improvement according to the invention in the roll-up compression properties. If flexible, heat-curing PU foams are described below, this also includes viscoelastic, flexible PU foams—even if they are not mentioned separately.

[0070] The various heat-cured flexible PU foams are classified not only according to the foam density but also often according to their compressive strength (also called load-bearing capacity) for specific applications. For example, for heat-cured flexible PU foams, the compressive strength of 40% according to DIN EN ISO 3386-1:2015-10 CLD (compressive load deflection) is preferably in the range of 2.0-8.0 kPa; viscoelastic polyurethane foams preferably have values ​​of 0.1-5.0 kPa, in particular values ​​of 0.5-2.5 kPa.

[0071] In a preferred embodiment of the present invention, the heat-cured flexible PU foam to be used according to the invention has the following preferred properties with regard to resilience, foam density and / or porosity: a resilience of 1% to 50% measured according to DIN EN ISO 8307:2008-03, and / or a porosity of 5-150 kg / m 3 The foam density of the present invention is 1-6 scfm, in particular 1.5-4.5 scfm, more preferably 1.75-4.25 scfm. It is particularly preferred that all three criteria regarding resilience, foam density and / or porosity as described above are met. Specifically, the heat-cured flexible PU foam used according to the present invention has a compressive strength of 0.1-8.0 kPa at a CLD of 40% according to DIN EN ISO 3386-1:2015-10.

[0072] Heat-cured flexible PU foams and their production are known per se. For the purposes of the present invention, in a preferred embodiment, the heat-cured flexible PU foam is particularly characterized in that it has a compressive strength of 2.0-8.0 kPa at a CLD of 40% according to DIN EN ISO 3386-1:2015-10, and / or a rebound resilience of 1-50% measured according to DIN EN ISO 8307:2008-03, and / or a strength of 8-80 kg / m 3 The foam density of the present invention is preferably 1-6 scfm, and / or a porosity of 1.5-4.5 scfm, more preferably 1.75-4.25 scfm. Possible production methods are described, for example, in EP 2 481 770 A2 or EP 2 182 020 A1. For the purposes of the present invention, in a preferred embodiment, the viscoelastic flexible PU foam is particularly characterized in that it has a glass transition temperature between -20°C and +15°C, and / or a compressive strength of 0.1-5.0 kPa, in particular 0.5-2.5 kPa, according to DIN EN ISO 3386-1:2015-10 CLD 40%, and / or a rebound resilience of <10% measured according to DIN EN ISO 8307:2008-03, and / or a strength of 30-130 kg / m 3 The foam density of 1-6 scfm, in particular 1.5-4.5 scfm, more preferably 1.75-4.25 scfm (after crushing the foam). Possible production methods are described, for example, in WO 2013 / 131710A2. The glass transition temperature can be measured using dynamic mechanical analysis (DMA) (DIN 53513: 1990-03) or using differential scanning calorimetry (DSC) (ISO 11357-2: 2013). Strictly speaking, it is the glass transition range that extends over the temperature range. Therefore, the reported values ​​are average values.

[0073] In a preferred embodiment of the present invention, the shaped heat-cured soft PU foam article according to the present invention, in particular the mattress according to the present invention, has a height of at least 1 cm to no more than 50 cm and a width of at least 20 cm to no more than 300 cm, and a length of at least 20 cm to no more than 300 cm. Preferred dimensions are, for example, a height in the range of 5 cm to 40 cm, a width in the range of 70 cm to 200 cm, and a length in the range of 150 cm to 220 cm. In a preferred embodiment of the present invention, the shaped PU foam article according to the present invention, in particular the cushion according to the present invention, may also have a height of at least 1 cm to no more than 40 cm and a width of at least 15 cm to no more than 200 cm, and a length of at least 15 cm to no more than 200 cm, examples of preferred dimensions being a height in the range of 2 cm to 30 cm, a width in the range of 15 cm to 50 cm, and a length in the range of 15 cm to 50 cm.

[0074] In another preferred embodiment of the present invention, the shaped thermosetting soft PU foam product takes the form of a mattress and preferably takes the form of a multi-zone mattress. The different zones differ, in particular, in the respective hardness. Such multi-zone mattresses and their production are known per se. They are widely sold commercially. In particular, the mattress has up to seven zones of different hardness, which extend in the longitudinal direction of the mattress and are given an appropriate width. When the mattress has zones of various hardness distributed over its area and these zones are formed, in particular, by cutouts and / or hollow spaces in the mattress, this constitutes another preferred embodiment of the present invention.

[0075] In another preferred embodiment of the present invention, the molded heat-cured soft PU foam product can also be a cold-cured PU foam mattress, a viscoelastic soft PU foam mattress, a heat-cured soft PU foam mattress, a PU gel foam mattress, a latex mattress or a frame spring mattress, each of which contains at least a portion made of the heat-cured soft PU foam according to the present invention. These types of mattresses are known per se to those skilled in the art and are also sold worldwide under these names. Mattresses made solely of heat-cured soft PU foam are often referred to on the market as foam mattresses. The term mattress for the purposes of the present invention also encompasses corresponding mattress covers and linings.

[0076] In a preferred embodiment of the present invention, the shaped heat-cured soft PU foam product (preferably a mattress) is characterized in that, based on its initial volume, the shaped heat-cured soft PU foam product is compressed by at least 20%, preferably at least 30%, and in particular at least 40%, and is maintained in a compressed form for at least 20 hours by an auxiliary device, in particular a packaging device.

[0077] Suitable auxiliary devices, in particular packaging devices, are bags and / or films such as are known, for example, from the field of roll-up mattresses. The bag and / or film can be sealed by any desired means, such as by clips or by tape or by welding. The function of the auxiliary device is to maintain the compressed shape until the end user of the shaped thermosetting flexible PU foam product wants to use the shaped product in a normal way again. After the removal of the auxiliary device, in particular the packaging device, the compressed shaped product expands again and in the best case recovers its original shape and size. The invention makes it possible to allow an improved dimensional recovery after a period of compression of at least 20 hours.

[0078] In another preferred embodiment, the shaped heat-cured flexible PU foam article is in a compressed and vacuum-packed state, and is particularly a rolled-up mattress in a vacuum-packed and compressed state.

[0079] The provision of various heat-curing flexible PU foams which can be used in the context of the present invention is known per se and all proven processes can be utilized, provided that the heat-curing flexible PU foam is produced in the presence of at least one compound of the formula (1a) and at least one compound of the formula (1b).

[0080] The production of the corresponding heat-cured flexible PU foam does not require further explanation in principle, but some preferred details of the production of PU foam for the purposes of the present invention will be given below. The subject matter of the present invention will be illustrated below by way of example, without intending to limit the present invention to these exemplary embodiments. When the range, general formula or category of the compound is described in detail below, these are intended to cover not only the corresponding compound range or group clearly mentioned, but also all compound sub-ranges and sub-groups that can be obtained by removing the individual values ​​(ranges) of the compound. When a document is cited in the context of the present invention, its entire content, especially the subject matter forming the context of the cited document, is intended to form part of the disclosure of the present invention. Unless otherwise stated, percentages are weight percentages. When an average value is reported below, the value discussed is a weight average, unless otherwise stated. When the parameters determined by measurement are reported below, the measurement is carried out at a temperature of 23°C and a pressure of 100kPa, unless otherwise stated. Unless otherwise stated, the compression of the foam in the context of the present invention refers to the initial volume of the foam, and the foam is preferably compressed by at least 20% in a period of at least 20 hours.

[0081] For the purposes of the present invention, polyurethane is all reaction products derived from isocyanate, especially polyisocyanate and appropriately isocyanate reactive molecules. These include polyisocyanurate, polyurea and isocyanate or polyisocyanate reaction products containing allophanate, biuret, uretdione, uretonimine or carbodiimide. Obviously, those skilled in the art who attempt to produce different flexible polyurethane foam types (such as heat-cured flexible PU foam) will appropriately select the material required for each corresponding purpose, such as isocyanate, polyol, stabilizer, surfactant, etc., in order to obtain the required polyurethane type, particularly polyurethane foam type in each case. Other details of available starting materials, catalysts and auxiliary agents and additives can be found in, for example, Kunststoffhandbuch [Plastics Handbook], Volume 7, Polyurethane [Polyurethanes], Carl-Hanser-Verlag Munich, First Edition 1966, Second Edition 1983 and Third Edition 1993. The following compounds, components and additives are mentioned by way of example only and may be replaced and / or supplemented by other substances known to the person skilled in the art.

[0082] The isocyanate component used is preferably one or more organic polyisocyanates having two or more isocyanate functional groups. The polyol component used is preferably one or more polyols having two or more isocyanate-reactive groups.

[0083] Suitable isocyanates as isocyanate component for the purposes of the present invention are all isocyanates containing at least two isocyanate groups. In general, all aliphatic, cycloaliphatic, arylaliphatic and preferably aromatic polyfunctional isocyanates known per se can be used. The isocyanates are preferably used in the range of 60 to 350 mol %, more preferably in the range of 60 to 140 mol %, relative to the sum of the isocyanate-consuming components.

[0084] Specific examples are: alkylene diisocyanates having 4 to 12 carbon atoms in the alkylene radical, for example dodecane 1,12-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, tetramethylene 1,4-diisocyanate and preferably hexamethylene 1,6-diisocyanate (HMDI); cycloaliphatic diisocyanates, such as cyclohexane 1,3-diisocyanate and cyclohexane 1,4-diisocyanate and any mixtures of these isomers, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate or IPDI for short), hexahydrotolylene 2,4-diisocyanate and hexahydrotolylene 2,6-diisocyanate (HMDI); 2,6-diisocyanate) and corresponding isomer mixtures; and preferably aromatic diisocyanates and polyisocyanates, such as toluene 2,4-diisocyanate and toluene 2,6-diisocyanate (TDI) and corresponding isomer mixtures, mixtures of diphenylmethane 2,4'-diisocyanate and diphenylmethane 2,2'-diisocyanate (MDI) and polyphenyl polymethylene polyisocyanate (crude MDI) and mixtures of crude MDI and toluene diisocyanate (TDI). Organic diisocyanates and polyisocyanates can be used alone or in the form of mixtures thereof.

[0085] Isocyanates which have been modified by incorporation of urethane, uretdione, isocyanurate, allophanate, and other groups (referred to as modified isocyanates) may also be used.

[0086] Particularly suitable organic polyisocyanates which are therefore particularly preferably used are the various isomers of toluene diisocyanate (toluene 2,4-diisocyanate and toluene 2,6-diisocyanate (TDI), in pure form or as isomer mixtures of various compositions), diphenylmethane 4,4′-diisocyanate (MDI), “crude MDI” or “polymeric MDI” (comprising the 4,4′ isomer as well as the 2,4′ and 2,2′ isomers of MDI, and products having more than two rings) and bicyclic products (which are referred to as “pure MDI” and consist predominantly of a mixture of 2,4′ and 4,4′ isomers), and prepolymers derived therefrom. Examples of particularly suitable isocyanates are described in detail, for example, in EP 1 712 578, EP 1 161 474, WO 00 / 58383, US 2007 / 0072951, EP 1 678 232 and WO 2008 / 010466. 2005 / 085310, which are incorporated herein by reference in their entirety.

[0087] Suitable polyols as polyol component for the purposes of the present invention are all organic substances having two or more isocyanate-reactive groups, preferably OH groups, and preparations thereof. Preferred polyols are: all polyether polyols and / or hydroxyl-containing aliphatic polycarbonates, especially polyether polycarbonate polyols and / or filled polyols (polymer polyols), such as SAN, PHD and PIPA polyols, which contain solid organic fillers in dispersed form with a solids content of up to 40% or more; and / or autocatalytic polyols, which contain catalytically active functional groups, especially amino groups; and / or natural polyols known as "natural oil-based polyols" (NOP). The polyols used for heat-curing flexible PU foams preferably have a functionality of 1.8 to 8 and a number-average molecular weight in the range of 500-4000 g / mol. Polyols with a hydroxyl number in the range of 25-400 mg KOH / g are usually used. The number-average molecular weight is usually determined by gel permeation chromatography (GPC), in particular using polypropylene glycol as reference substance and tetrahydrofuran (THF) as eluent. The hydroxyl number can be determined in particular according to DIN standard DIN 53240:1971-12. Depending on the desired properties of the foam produced, suitable polyols as described, for example, in the following documents can be used: US 2007 / 0072951 A1, WO 2007 / 111828, US 2007 / 0238800, US 6359022 or WO 96 / 12759. Other polyols are known to those skilled in the art and can be found, for example, in EP-A-0380993 or US-A-3346557.

[0088] In a preferred embodiment of the invention, in particular for the production of flexible slabstock foams, polyether alcohols are used whose number of secondary hydroxyl groups is preferably greater than 50%, more preferably greater than 90%, in particular those having propylene oxide blocks or random propylene oxide and ethylene oxide blocks at the chain ends or those based exclusively on propylene oxide blocks. Such polyether alcohols preferably have a functionality of 2 to 8, more preferably 2 to 4, have a number average molecular weight in the range of 500-4000 g / mol, preferably 800-4000 g / mol, more preferably 2500-4000 g / mol, and generally have a hydroxyl number in the range of 20-100 mg KOH / g, preferably 40-60 mg KOH / g.

[0089] In a further preferred embodiment of the invention, use is additionally made of difunctional and / or trifunctional polyetherols which comprise primary hydroxyl groups in an amount of preferably greater than 50%, more preferably greater than 80%, in particular those which have ethylene oxide blocks at the chain ends. Polyols for cold-curing flexible PU foams ("HR polyols") form part of this class if the molar mass is at the same time >4000 g / mol. Depending on the desired properties of this embodiment, which is preferred according to the invention, in particular for the production of the above-mentioned heat-curing flexible PU foams, preference is given to using not only the polyetherols described here, but also other polyetherols having primary hydroxyl groups and being predominantly based on ethylene oxide and having an ethylene oxide block ratio of >70%, preferably >90%. All polyetherols described in the context of this preferred embodiment preferably have a functionality of 2 to 8, more preferably 2 to 5, a number-average molecular weight in the range of 500-8000 g / mol, preferably 500-7000 g / mol, and generally have a hydroxyl number in the range of 5-100 mg KOH / g, preferably 20-60 mg KOH / g. In a preferred embodiment, in the case of the heat-curing flexible PU foams of the invention, polyols having primary hydroxyl functions are used here, not alone but in combination with polyols having secondary OH groups. In a preferred embodiment, polyols having primary hydroxyl functions are used here only to an extent of <50% in the combination.

[0090] In another preferred embodiment of the present invention, autocatalytic polyols are used.

[0091] In another preferred embodiment of the invention, in particular for the production of viscoelastic flexible PU foams, preference is given to using mixtures of various, preferably two or three, polyfunctional polyetherols. The polyol combination used here usually consists of low molecular weight "crosslinker" polyols with high functionality, preferably with hydroxyl numbers of 100-400 mg KOH / g and / or conventional high molecular weight flexible slabstock polyols or HR polyols and / or "supersoft" polyether polyols, preferably with hydroxyl numbers of 20-40 mg KOH / g, with a high proportion of ethylene oxide and with open-cell properties. If HR polyols are also used in the viscoelastic foam formulation, their mass proportion in the polyol mixture is <50%.

[0092] In a further preferred embodiment of the present invention, recycled polyols are used.

[0093] The shaped thermosetting flexible PU foam articles obtained by the additional use of recycled polyols accordingly correspond to a preferred embodiment of the present invention. The use of recycled polyols leads to problems with shape recovery after roll compression. In the context of the present invention, it has surprisingly been found that the combined use of at least one compound of formula (1a) as detailed above with at least one compound of formula (1b) enables this problem to be alleviated.

[0094] Recycled polyols are polyols obtained from PU foam waste. This can be production waste from the production of heat-cured flexible PU foam or from heat-cured flexible PU foam waste after consumer use (e.g. old mattresses). In both cases, the PU foam is liquefied by chemical methods. Various methods are useful here, such as glycolysis, hydrolysis or acidolysis. The liquid recycled polyol obtained can then be used again to produce heat-cured flexible PU foam. However, a notable feature of such heat-cured flexible PU foams is often unfavorable mechanical properties, such as resistance to roll compression. One source of additional information on the use of recycled polyols in heat-cured flexible PU foams is the following BMBF research report: https: / / www.cleaner-production.de / fileadmin / assets / bilder / BMBF-Projekte / 01RI 05070-075_-_Abschlussbericht.pdf.

[0095] The additional use of regenerated polyols in the context of the present invention corresponds to a preferred embodiment of the invention for each of the claimed subject matter.

[0096] The preferred ratio of isocyanate to polyol (expressed as an index of the formulation, i.e. the stoichiometric ratio of isocyanate groups to isocyanate-reactive groups (e.g. OH groups, NH groups) multiplied by 100) is in the range of 50 to 140, preferably 70 to 130, more preferably 85 to 125. An index of 100 represents a molar reactive group ratio of 1:1.

[0097] Catalysts can also be used to produce the heat-curing flexible PU foams according to the invention. For the purposes of the present invention, the term "catalyst" includes all compounds known from the prior art which are capable of catalyzing isocyanate reactions and / or which are used as catalysts, cocatalysts or activators in the production of polyisocyanate reaction products, in particular polyurethane foams.

[0098] Suitable catalysts are known; these are in particular substances which catalyze the gel reaction (isocyanate-polyol), the blowing reaction (isocyanate-water) and / or the dimerization or trimerization of isocyanates. Such catalysts are preferably nitrogen compounds, in particular amines and ammonium salts, and / or metal compounds.

[0099] Examples of suitable nitrogen compounds as catalysts for the purposes of the present invention are the amines triethylamine, triethanolamine, diethanolamine, N,N-dimethylcyclohexylamine, N,N-dicyclohexylmethylamine, N,N-dimethylaminoethylamine, N,N,N',N'-tetramethylethane-1,2-diamine, N,N,N',N'-tetramethylpropane-1,3-diamine, N,N,N',N'-tetramethylbutane-1,4-diamine, N,N,N',N'-tetramethylhexane-1,6-diamine, N-[2-(dimethylamino)ethyl]-N,N',N'-trimethylethane-1,2-diamine, 2-[(2-(dimethylamino)ethyl]- ethyl)methylamino]ethanol, N',N'-dimethylpropane-1,3-diamine, N',N'-diethylpropane-1,3-diamine, 1-(2-aminoethyl)pyrrolidine, 1-(3-aminopropyl)pyrrolidine, 1-[3-(dimethylamino)propyl-(2-hydroxypropyl)amino]propan-2-ol, 2-[[3-(dimethylamino)propyl]methylamino]ethanol, 3-(2-dimethylamino)ethoxy)propylamine, N-[3-(dimethylamino)propyl]-N',N'-dimethylpropane-1,3-diamine, N'-[3-(dimethylamino)propyl]-N,N,N'-trimethylpropane-1,3-diamine, 1-[3-(dimethylamino)propyl]-N,N,N'-trimethylpropane-1,3-diamine [propyl] amino]-2-propanol, N,N-bis[3-(dimethylamino)propyl]-N',N'-dimethylpropane-1,3-diamine, 1,4-diazabicyclo[2.2.2]octane, 1,4-diazabicyclo[2.2.2]octane-2-methanol, 1,2-dimethylimidazole, N-(2-hydroxypropyl)imidazole, 2-methyl-1-(2-methylpropyl)imidazole, N-(3-aminopropyl)imidazole, N-methylimidazole, 1-(3-aminopropyl)-2-methyl-1H-imidazole, N-ethylmorpholine, N-methylmorpholine, 2,2,4-trimethyl-2-silamorpholine, N-ethyl-2,2-dimethyl-2-silamorpholine, N-(2- 1-(2-hydroxyethyl)pyrrolidine, 3-dimethylamino-1-propanol, 1-(3-hydroxypropyl)pyrrolidine, 2-[2-(dimethylamino)ethoxy]ethanol, 2-[2-(diethylamino)ethoxy]ethanol, bis(2-dimethylaminoethyl)ether, 2-[[2-(2-(dimethylamino)ethoxy)ethyl]methylamino]ethanol, N-[2-[2-(dimethylamino)ethoxy]ethyl]-N-methylpropane-1,3-diamine, 1,3,5- Tris[3-(dimethylamino)propyl]hexahydro-1,3,5-triazine, 1,8-diazabicyclo[5.4.0] undec-7-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, N-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1,4,6-triazabicyclo[3.3.0]oct-4-ene, 1,1,3,3-tetramethylguanidine, 2-tert-butyl-1,1,3,3-tetramethylguanidine, guanidine, 1,1'-[(3-{bis[3-(dimethylamino)propyl]amino} propyl)imino]bispropan-2-ol, (3-aminopropyl)bis[3-(dimethylamino)propyl]amine, 3-(dimethylamino)propaneurea, 1,3-bis[3-(dimethylamino)propyl]urea, 3-dimethylamino-N,N-dimethylpropionamide, 6-(dimethylamino)hexane-1-ol and 2,4,6-tris[(dimethylamino)methyl]phenol.

[0100] Catalysts and / or mixtures of this type are commercially available, for example, under the following names: ZF-10, DMEA, API, RX 20 and RX 21, RP202, RP 204, NE 300, NE 310, NE 400, NE 500, NE 600, NE 650, NE 660, NE 740, NE 750, NE 1060, NE 1080, NE 1082 and NE 2039, EF 860, EF 890, EF 700, EF 705, EF 708, EF 600, EF 602, 54. EF and ZE1.

[0101] Suitable metal compounds as catalysts can be selected, for example, from the group consisting of metal organic or organometallic compounds, metal organic or organometallic salts, organometallic salts, inorganic metal salts and from the group consisting of coordination compounds containing charged or uncharged metals, in particular metal chelates. The term "metal organic or organometallic compound" in the context of the present invention particularly includes the use of metal compounds with direct carbon-metal bonds, which are also referred to here as metal organics (e.g. tin organics) or organometallic compounds (e.g. organotin compounds). The term "organometallic or metal organic salt" in the context of the present invention particularly includes the use of metal organic or organometallic compounds with salt characteristics, i.e. ionic compounds in which the anion or cation has a metal organic nature (e.g. organotin oxides, organotin chlorides or organotin carboxylates). The term "organic metal salt" in the context of the present invention particularly includes the use of metal compounds which do not have any direct carbon-metal bonds and are at the same time metal salts, wherein the anion or the cation is an organic compound (e.g. tin(II) carboxylates). The term "inorganic metal salt" in the context of the present invention particularly includes the use of metal compounds or the use of metal salts in which both the anion and the cation are not organic compounds, such as metal chlorides (e.g. tin(II) chloride), pure metal oxides (e.g. tin oxide) or mixed metal oxides (i.e. comprising a plurality of metals), and / or metal silicates or aluminosilicates. The term "coordination compound" in the context of the present invention particularly includes the use of metal compounds which are formed from one or more central particles and one or more ligands, the central particles being charged or uncharged metals (e.g. metal or tin amine complexes). The term "metal chelate" in the context of the present invention particularly includes the use of metal coordination compounds, the ligands of which have at least two coordination or bonding sites for the metal center (e.g. metal or tin polyamines or metal or tin polyether complexes). Suitable metal compounds as catalysts in the sense of the present invention, in particular as defined above, can be selected, for example, from all metal compounds including lithium, sodium, potassium, magnesium, calcium, scandium, yttrium, titanium, zirconium, vanadium, niobium, chromium, molybdenum, tungsten, manganese, cobalt, nickel, copper, zinc, mercury, aluminum, gallium, indium, germanium, tin, lead and / or bismuth, in particular sodium, potassium, magnesium, calcium, titanium, zirconium, molybdenum, tungsten, zinc, aluminum, tin and / or bismuth, more preferably tin, bismuth, zinc and / or potassium.

[0102] Suitable metal-containing coordination compounds include, for example, any metal acetylacetonate, such as nickel(II) acetylacetonate, zinc(II) acetylacetonate, copper(II) acetylacetonate, molybdenum dioxyacetylacetonate, any iron acetylacetonate, any cobalt acetylacetonate, any zirconium acetylacetonate, any titanium acetylacetonate, any bismuth acetylacetonate, and any tin acetylacetonate. Particularly suitable metal organic salts and organometallic salts as defined above as catalysts in the context of the present invention are, for example, organotin, tin, zinc, bismuth and potassium salts, in particular the corresponding metal carboxylates, alcohol oxides, mercaptides and thioglycolates, for example dibutyltin diacetate, dimethyltin dilaurate, dibutyltin dilaurate (DBTDL), dioctyltin dilaurate (DOTDL), dimethyltin dineodecanoate, dibutyltin dineodecanoate, dioctyltin dineodecanoate, dibutyltin dioleate, dibutyltin bis-n-laurylmercaptide, dimethyltin bis-n-laurylmercaptide, monomethyltin tris-2-ethylhexylmercaptoacetate, dimethyltin dimethyl tin dioleate, dibutyltin dioleate, dibutyltin dioleate, dimethyl ... bismuth acetate, bismuth 2-ethylhexanoate, bismuth octanoate, bismuth isononanoate, bismuth neodecanoate, tin(II) acetate, tin(II) 2-ethylhexanoate (tin(II) octanoate), tin(II) isononanoate (3,5,5-trimethyltin(II) hexanoate), tin(II) neodecanoate, tin(II) ricinoleate, zinc(II) acetate, zinc(II) 2-ethylhexanoate (zinc(II) octanoate), zinc(II) isononanoate (3,5,5-trimethyltin(II) hexanoate), zinc(II) neodecanoate, zinc(II) ricinoleate, bismuth acetate, bismuth 2-ethylhexanoate, bismuth octanoate, bismuth isononanoate, bismuth neodecanoate, potassium formate, potassium acetate, potassium 2-ethylhexanoate (potassium octanoate), potassium isononanoate, potassium neodecanoate and / or potassium ricinoleate. It is generally preferred to select suitable metal catalysts such that they are free of any inherent offensive odor, are essentially toxicologically unobjectionable and impart to the resulting polyurethane system, in particular the polyurethane foam, as low a level of catalyst-induced emissions as possible.

[0103] Besides amines and metal compounds, it is also possible to use ammonium salts as catalysts. Suitable examples are ammonium formate and / or ammonium acetate.

[0104] Suitable catalysts are mentioned, for example, in DE 102007046860, EP 1985642, EP 1985644, EP1977825, US 2008 / 0234402, EP 0656382 B1 and US 2007 / 0282026 A1 and the patent literature cited therein.

[0105] Suitable catalyst amounts are guided by the catalyst type and are preferably in the range of 0.01 to 10.0 pphp, more preferably in the range of 0.02 to 5.00 pphp (=parts by weight based on 100 parts by weight of polyol).

[0106] The optional additives used may be all substances known in the prior art and used for the production of polyurethanes, in particular heat-curing flexible PU foams, such as blowing agents (preferably for forming CO 2 of water and, if desired, other physical blowing agents), crosslinkers and chain extenders, stabilizers against oxidative degradation (known as antioxidants), flame retardants, surfactants, biocides, cell-improving additives, cell openers, solid fillers, antistatic additives, nucleating agents, thickeners, colorants, pigments, color pastes, fragrances, emulsifiers, buffer substances and / or catalytically active substances, in particular as defined above.

[0107] In the production of heat-curing flexible PU foams, water is usually used as a blowing agent. Preference is given to using such an amount of water that the water concentration is 0.10 to 10.0 pphp (pphp=parts by weight based on 100 parts by weight of polyol).

[0108] Suitable physical blowing agents may also be used. These physical blowing agents are, for example, liquefied CO 2 and volatile liquids, such as hydrocarbons having 3, 4 or 5 carbon atoms (preferably cyclopentane, isopentane and n-pentane), oxygenates such as methyl formate, acetone and dimethoxymethane, or chlorinated hydrocarbons (preferably dichloromethane and 1,2-dichloroethane).

[0109] Besides water and physical blowing agents, it is also possible to use other chemical blowing agents which react with isocyanates to release gas, for example formic acid.

[0110] The optional crosslinking agent and the optional chain extender are low molecular weight polyfunctional compounds reactive toward isocyanates. Suitable compounds are, for example, hydroxyl or amine-terminated substances such as glycerol, neopentyl glycol, 2-methyl-1,3-propanediol, triethanolamine (TEOA), diethanolamine (DEOA) and trimethylolpropane. Based on 100 parts of polyol, the use concentration is generally in the range of 0.1 to 5 parts, but it can also deviate from this range depending on the formulation.

[0111] Suitable optional stabilizers against oxidative degradation (so-called antioxidants) preferably include all commonly used free radical scavengers, peroxide scavengers, UV absorbers, light stabilizers, complexing agents for metal ion contaminants (metal deactivators). Preference is given to using compounds of the following classes of substances or classes of substances containing the following functional groups, where the substituents on the corresponding parent molecule are preferably substituents, especially groups reactive toward isocyanates: 2-(2′-hydroxyphenyl)benzotriazole, 2-hydroxybenzophenone, benzoic acid and benzoates, phenols (especially including tert-butyl and / or methyl substituents on the aromatic entity), benzofuranones, diarylamines, triazines, 2,2,6,6-tetramethylpiperidine, hydroxylamines, alkyl and aryl phosphites, sulfides, zinc carboxylates, diketones.

[0112] Suitable optional flame retardants in the context of the present invention are all substances which are considered suitable for this purpose according to the prior art. Preferred flame retardants are, for example: liquid organophosphorus compounds, such as halogen-free organophosphates (e.g. triethyl phosphate (TEP)), halogenated phosphates (e.g. tris(1-chloro-2-propyl) phosphate (TCPP) and tris(2-chloroethyl) phosphate (TCEP)), and organophosphonates (e.g. dimethyl methylphosphonate (DMMP), dimethyl propylphosphonate (DMPP)); or solids, such as ammonium polyphosphate (APP) and red phosphorus. Suitable flame retardants also include halogenated compounds (e.g. halogenated polyols) and solids (such as expandable graphite and melamine).

[0113] In order to stabilize the rising foam mixture and to influence the foam properties of the polyurethane foam, organic modified siloxanes are usually used in the production of heat-cured flexible PU foams. (Organo modified) siloxanes suitable for this purpose are described in, for example, the following documents: EP 0839852, EP 1544235, DE 102004001408, EP 0839852, WO 2005 / 118668, US 20070072951, DE 2533074, EP 1537159, EP 533202, US 3933695, EP 0780414, DE 4239054, DE 4229402, EP 867465. These compounds can be prepared as described in the prior art. Suitable examples are described in, for example, US 4147847, EP 0493836 and US 4855379. Foam stabilizers for heat-cured flexible PU foams are characterized by having a large siloxane structure with more than 50 Si units and side polyethers. These foam stabilizers are also referred to as polydialkylsiloxane-polyoxyalkylene copolymers. The structure of these compounds is preferably such that, for example, a long-chain copolymer of ethylene oxide and propylene oxide is bonded to a polydimethylsiloxane free radical. The connection between the polydialkylsiloxane and the polyether portion can be through a SiC connection or a Si-OC bond. In terms of structure, the polyether or different polyethers can be bonded to the polydialkylsiloxane in a terminal or lateral position. The alkyl group of the siloxane can be aliphatic, alicyclic or aromatic. The methyl group is very particularly advantageous. The organic modified polydialkylsiloxane can be linear or contain branches. Suitable stabilizers, in particular foam stabilizers, are described in particular in US 2834748, US 2917480 and US 3629308. The function of the foam stabilizer is to ensure the stability of the foaming reaction mixture. The contribution to the foam stability is related to the siloxane chain length here. In the absence of a foam stabilizer, collapse is observed, so that no uniform foam is obtained. In the case of certain soft PU foam types that are not according to the present invention, which have higher stability and are therefore not prone to collapse, low molecular weight polyether siloxanes can also be used. These low molecular weight polyether siloxanes have a siloxane chain length much shorter than 50. For example, in the case of cold-curing soft PU foams or ester foams, unmodified or modified short-chain siloxanes are used. In contrast, when long-chain and therefore more effective siloxane stabilizers are used, excessive stability and therefore shrinkage after foam production will be observed in such foam types.

[0114] In the context of the present invention, the foam stabilizer can in principle be selected as desired, as long as the combination of compounds of the formula (1a) and (1b) is used according to the invention in the heat-curing flexible PU foam. As already explained, these are used in particular to increase the dimensional stability of the foam after compression, in particular after roll compression.

[0115] The compounds of formula (1a) and (1b) can be used, for example, together with suitable solvents and / or other additives. As optional solvents, all suitable substances known from the prior art can be used. Depending on the application, aprotic non-polar, aprotic polar and protic solvents can be used. Suitable aprotic non-polar solvents can be selected, for example, from the following categories of substances or substances comprising the following functional groups: aromatic hydrocarbons, aliphatic hydrocarbons (alkanes (chain alkanes) and polyolefins), carboxylates (for example isopropyl myristate, propylene glycol dioleate, decyl coconut oil or other fatty acid esters) and polyesters, (poly) ethers and / or halogenated hydrocarbons with low polarity. Suitable aprotic polar solvents can be selected, for example, from the following categories of substances or substances comprising the following functional groups: ketones, lactones, lactams, nitrile, formamide, sulfoxides and / or sulfones. Suitable protic solvents can be selected, for example, from the following classes of substances or classes of substances comprising the following functional groups: alcohols, polyols, (poly)alkylene glycols, amines, carboxylic acids, in particular fatty acids and / or primary and secondary amides. Particular preference is given to solvents which can be readily employed in the foaming operation and which do not adversely affect the properties of the foam. For example, isocyanate-reactive compounds are suitable, since they are incorporated into the polymer matrix by reaction and do not generate any emissions in the foam. Examples are OH-functional compounds such as (poly)alkylene glycols, preferably monoethylene glycol (MEG or EG), diethylene glycol (DEG), triethylene glycol (TEG), 1,2-propylene glycol (PG), dipropylene glycol (DPG), propylene glycol (propane-1,3-diol, PDO), tetramethylene glycol (butanediol, BDO), butyl diethylene glycol (BDG), neopentyl glycol, 2-methylpropane-1,3-diol (Ortegol CXT) and their higher homologues, for example polyethylene glycols (PEG) having an average molecular weight between 200 g / mol and 3000 g / mol. Particularly preferred OH-functional compounds also include polyethers having an average molecular weight of 200 to 4500 g / mol, in particular 400 to 2000 g / mol, among these preferably water-, allyl-, tert-butyl- or nonyl-initiated polyethers, in particular those based on propylene oxide (PO) and / or ethylene oxide (EO) blocks.

[0116] When the compounds of formula (1a) and (1b) are used according to the invention or the compounds of formula (1a) and (1b) are used in a premixed silicone combination with an additional carrier in dissolved form or in combination with a solvent, the mass ratio of the sum of all silicone components to the solvent is preferably 0.1:1 to 9:1, preferably 0.25:1 to 5:1 and more preferably 0.5:1 to 4:1.

[0117] In a preferred embodiment of the present invention, the two siloxane components - ie the compounds of formula (1a) and (1b) - can each be added to the foam mixture separately in pure form, or admixed with a solvent, or mixed with each other before addition.

[0118] Preferably, a sufficient amount of the compound of formula (1a) can be added to the composition for producing heat-cured flexible PU foam, and its mass proportion in the finished polyurethane foam is 0.1% to 5% by weight, preferably 0.25% to 3.0% by weight, more preferably 0.5% to 2.0% by weight. The compound of formula (1b) is preferably used in a mass proportion of 0.1% to 5% by weight, preferably 0.1% to 2.0% by weight, more preferably 0.1% to 1.5% by weight in the finished polyurethane foam.

[0119] It can be advantageous to produce and / or use and react a composition comprising at least the inventive compounds of formula (1a) and (1b), at least one polyol component, optionally at least one isocyanate component and optionally one or more blowing agents in the production of heat-cured flexible PU foams.

[0120] It is preferred when the compounds of formula (1a) and (1b) are each used in a total amount corresponding to a mass fraction of 0.1 to 5.0 parts (pphp), preferably 0.1 to 3.0 parts and more preferably 0.3 to 2.0 parts, based on 100 parts (pphp) of the polyol component.

[0121] The heat-cured flexible PU foam according to the invention can be produced by any method familiar to those skilled in the art, for example by manual mixing or preferably with the aid of a foaming machine, in particular a low-pressure or high-pressure foaming machine. Batch methods or continuous methods can be used here.

[0122] Any method known to those skilled in the art can be used to produce the heat-cured flexible PU foam. For example, the foaming operation can be carried out in a batch-operated device or a continuous-operated device in a horizontal direction or in a vertical direction. The composition used according to the invention can be used similarly for CO 2Technology. It can be used in low-pressure and high-pressure machines, in which the composition to be treated can be metered directly into the mixing chamber or even mixed before the mixing chamber with one of the components that subsequently enters the mixing chamber. Mixtures in raw material tanks are also possible.

[0123] Particularly preferred heat-cured flexible PU foams for the purposes of the present invention have in particular the following composition:

[0124] Table 1:

[0125]

[0126] The present invention also provides the use of a combination of at least one compound of formula (1a) and at least one compound of formula (1b) (wherein formula (1a) and (1b) are each as defined above) in the production of a shaped heat-cured flexible PU foam article, wherein the shaped heat-cured flexible PU foam article is obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one blowing agent to provide a shaped heat-cured flexible PU foam article having improved dimensional recovery after compression for a period of at least 20 hours.

[0127] The present invention also provides the use of a combination of at least one compound of formula (1a) and at least one compound of formula (1b) (wherein formula (1a) and (1b) are each as defined above) to improve the dimensional recovery of a shaped heat-cured flexible PU foam article after it has been compressed for a period of at least 20 hours, wherein the shaped heat-cured flexible PU foam article can be obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one blowing agent and in the presence of at least one compound of formula (1a) and at least one compound of formula (1b).

[0128] The present invention also provides for the use of a flexible heat-cured PU foam in a mattress and / or a cushion, in particular a mattress, wherein the flexible heat-cured PU foam is obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of the formula (1a) and at least one compound of the formula (1b), wherein the formulae (1a) and (1b) are each as defined above. In this regard, reference may be made in particular to the above, which also applies to this subject matter.

[0129] The use according to the invention enables the provision of a mattress and / or cushion having improved dimensional recovery after being compressed for a period of at least 20 hours. The use according to the invention allows a mattress and / or cushion having improved dimensional recovery after it has been compressed for a period of at least 20 hours.

[0130] The invention also provides a method for storing and / or transporting shaped PU foam articles, preferably mattresses and / or cushions,

[0131] in

[0132] (a) in a first step, providing a shaped heat-cured flexible PU foam article by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b) as well as at least one blowing agent and at least one catalyst, wherein formula (1a) and (1b) are each as defined above,

[0133] (b) in an optional subsequent step, the obtained heat-cured flexible PU foam can optionally be further processed to prepare it for an application,

[0134] (c) and wherein in the last step, the shaped thermosetting flexible PU foam article (optionally prepared for application) is compressed by at least 20%, preferably at least 30%, in particular at least 40%, based on its initial volume, and optionally vacuum-packed and kept in compressed form by an auxiliary device, in particular a packaging device, and stored and / or transported.

[0135] The present invention also provides a process for producing a heat-curable flexible polyurethane foam by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b) as well as at least one blowing agent and at least one catalyst, in particular by additional use of a regenerated polyol, wherein the heat-curable flexible polyurethane foam has a porosity of 1 to 6 scfm, preferably 1.5 to 4.5 scfm, in particular 1.75 to 4.25 scfm.

[0136] The present invention also provides a mixture comprising at least one compound of formula (1a) and at least one compound of formula (1b), and / or diols, polyethers, organic esters and / or other solvents suitable for the purpose of producing heat-cured flexible PU foam, wherein formula (1a) and (1b) are each as defined above. DETAILED DESCRIPTION

[0137] Example

[0138] Physical properties of soft PU foam:

[0139] The produced flexible PU foams were evaluated according to the following physical properties a) to g):

[0140] a) Rise time: The period between the end of mixing of the reaction components and the release of the polyurethane foam.

[0141] b) Rise height or foam height: The height of the free-rising foam formed after 3 minutes. The foam height is reported in centimeters (cm).

[0142] c) Foam settling at the end of the rising phase (=fallback): The settling is found from the difference between the foam height immediately after release and 3 minutes after the foam release. The foam height is measured at the maximum in the middle of the foam peak by means of a needle fixed to a centimeter scale. Negative values ​​here describe the settling of the foam after release; positive values ​​accordingly describe a further rise of the foam.

[0143] g) Number of holes per centimeter (hole count): This is determined visually on the cut surface (measured in accordance with DIN EN 15702).

[0144] e) Foam density (FD): Determined by measuring the core density according to Test A as described in ASTM D 3574-11. Foam density is expressed in kg / m 3 Report for the unit.

[0145] f) Porosity determined by flow method: In the airflow method according to ASTM D 3574 (2011-00), the volume of air that flows through a defined foam sample over a specific period of time when a pressure difference is applied is determined. For this purpose, 12 test samples with dimensions of 5 cm×5 cm×2.5 cm are cut from each finished foam transverse to the direction of rise of the foam and inserted successively into an analytical instrument constructed for this method. The construction of the instrument is described in ASTM D 3574 (2011-00). The analytical instrument keeps the air pressure difference constant by sucking just enough air through the test sample to produce an air pressure difference of 125 Pa between the inside of the instrument and the surrounding atmosphere. The airflow through the test sample is therefore a measure of the porosity of the foam. Values ​​in the range of 0-6.5 scfm (standard cubic feet per minute) are measured, where lower values ​​in the interval depict relatively closed foams and higher values ​​depict relatively open foams.

[0146] g) Roll-up test results: This specific test is described in detail below.

[0147] For the sake of completeness, the measuring principle of DIN EN ISO 16000-9:2008-04 is also explained below.

[0148] These materials are described here with respect to the type and amount of organic matter that can be outgassed from the materials. Analytical methods are used to determine emissions from materials used in furniture and mattresses. This is done by measuring emissions using a test chamber.

[0149] analyze

[0150] Test samples: sample preparation, sampling and sample size

[0151] The reaction mixture is placed in a PE plastic bag, which has an opening at the top. After the foam rises and releases, the PE bag is closed 3 minutes after the release. In order to make the complete reaction possible, but at the same time to prevent VOC from escaping prematurely, the foam is stored at room temperature for 12 hours in this way. Subsequently, the PE bag is opened, a 7cm×7cm×7cm cube is taken from the center of the foam block and immediately wrapped in aluminum foil and sealed in a PE bag airtightly. It is then transported to the analytical laboratory, and the foam cube is placed in a cleaned 30l glass test chamber. The conditions in the test chamber are controlled climate conditions (temperature 21°C, air humidity 50%). Half of the test chamber volume is replaced every hour. After 24 hours, a sample is taken out from the test chamber air. The Tenax adsorption tube is used to absorb VOC. The Tenax tube is then heated, and the released volatile substances are cold-collected in the cold trap of the temperature programmable evaporator by means of an inert gas stream. After the heating phase is over, the cold trap is quickly heated to 280°C. The concentrated substances evaporate in the process. These substances are subsequently separated in a gas chromatography column and detected by mass spectrometry. Calibration using reference substances allows a semi-quantitative assessment of emissions in terms of -μg / m 3 " indicates. The quantitative reference substance for VOC analysis (VOC value) is toluene. The signal peaks can be assigned to these substances using their mass spectra and retention indices. The following equipment was used for the analysis: Gerstel, D-45473 Mühlheim an der Ruhr, Eberhard-Gerstel-Platz 1, TDS-3 / KAS-4, Desorption tube, Agilent Technologies 7890A (GC) / 5975C (MS), column: HP Ultra2 (50 m, 0.32 mm, 0.52 μm), carrier gas: helium. A more detailed description of the procedure can be found in DIN EN ISO 16000-9: 2008-04.

[0152] The roll-up deformation test is described below, which makes it possible to test the dimensional recovery after compression in the context of the present invention.

[0153] Rolling deformation test (abbreviated as “rolling test”)

[0154] Target:

[0155] This test, for its purpose, must simulate the conditions of a rolled-up mattress in the laboratory. Since there is no meaningful industry standard for this, a novel test was developed which simulates the rolling-up of a mattress foam on a small scale.

[0156] Sample preparation:

[0157] Test samples of dimensions 12 cm (width), 16 cm (length) and 2.5 cm (thickness) were cut out from a soft PU foam block such as obtained from manual foaming using a band saw. The center position in the foam block from manual foaming was selected. The test samples were cut out so that the rising direction of the foam during production was at right angles to the length and width of the test samples. The test samples were marked with a watercolor pen.

[0158] Test procedure:

[0159] The test sample is compressed at the 12 cm edge with a thin metal rod (e.g. a metal ballpoint pen) with a diameter of 5-8 mm. The foam test sample is then rolled up by hand around the metal rod. This significantly compresses the foam, thereby forming a roll with a diameter of about 3-4 cm. The roll is held in this compressed state by hand and pushed completely into the cardboard tube. The cardboard tube has an inner diameter of 4 cm and a length of at least 13 cm. Once the rolled foam is completely inserted into the tube, the metal rod is removed. In order to minimize friction during removal, the metal rod can be slightly greased before the foam is rolled up. The foam then fills the volume of the tube. The compression of the foam is more severe in the center than at the edges of the tube. The roll is then stored under controlled constant conditions (temperature: 21° C., atmospheric humidity: 60%) for 7 days. After 168 hours, the foam is removed from the tube by hand and placed on a flat surface, and the expansion of the foam is observed. The expansion of the foam must not be disturbed or influenced.

[0160] evaluate:

[0161] The molded soft PU foam products are expanded for 10 minutes. The test samples are then evaluated. The most important criterion is whether the foam has completely recovered its original thickness or - especially at the edges where the compression is more severe - whether there are still compressed areas. In some cases, the grooves from the compression are still obvious on the surface of the test sample. Very poor test samples remain rolled up at one end. Slight bends in the test samples after expansion are normal and are not taken into account in the evaluation. The following grades are used for evaluation:

[0162] +++: The test specimen is fully expanded, with no visible compression lines or compression whatsoever, expansion occurs rapidly and is complete after 5 minutes.

[0163] ++: The test sample recovered a thickness of 2.5 cm at all locations. No dents or grooves were visible on the surface (especially at the end where compression was more severe) after 10 minutes.

[0164] +: The test sample recovered a thickness of 2.5 cm at all locations. However, slight dents and grooves were still visible on the surface (especially at the end where the compression was more severe).

[0165] 0: The test sample shows slight compression at the end where the compression is more serious. The thickness at this end is greater than 2.0 cm but less than 2.5 cm. A dent is clearly visible at this end.

[0166] -: The test sample shows slight compression at the end where the compression is more serious. The thickness of the sample at this end is greater than 1 cm but still significantly less than 2.0 cm.

[0167] --: The test sample shows severe compression at the end where the compression is more severe. The thickness of the sample at this end is less than 1 cm. The sample is still partially rolled up at this end.

[0168] ---: The test specimen is still rolled up and compressed at the end where the compression is more serious.

[0169] The evaluation is preferably performed by at least two persons. The results are recorded. In the context of the present invention, the evaluation is performed by four persons who reach a consensus result.

[0170] Disadvantages and limitations of the test: The correct size and uniform rolling of the test specimens must be ensured during the test. The foam test specimens must have constant cell structure parameters, i.e. in particular constant cell size and constant air permeability. The metal rod must not be overly greased so that grease does not penetrate into the specimen. Constant storage conditions must be maintained. The test specimens assigned the various evaluation levels must remain available for comparison.

[0171] Test accuracy:

[0172] Evaluation by two or more people will often produce consistent assessments. And in repeated measurements, the same results will often be confirmed. The test is therefore proven to be reliable.

[0173] Thermal Curing Soft PU Foam - Foaming Example

[0174] Example 1: Production of heat-cured flexible PU foam (flexible block foam)

[0175] For the performance testing of the inventive compounds of formula (1a) and (1b), the heat-cured flexible PU foam formulations detailed in Table 2 were used.

[0176] Table 2: Formulation 1 for the production of heat-cured flexible PU foam.

[0177]

[0178] 1)Polyol 1: Available from Dow Chemical CP 3322, a polyether polyol based on glycerol, having a hydroxyl number of 48 mg KOH / g and having predominantly secondary OH groups, average molar mass=3500 g / mol.

[0179] 2) 29, available from Evonik Industries: Tin(II) salt of 2-ethylhexanoic acid.

[0180] 3) DMEA: Dimethylethanolamine, available from Evonik Industries. Amine catalyst used in the production of polyurethane foams.

[0181] 4) Polyether-modified polysiloxane of the following structure:

[0182] Foam stabilizer 1 (corresponding to the compound of formula 1a):

[0183] Polyether siloxanes of the following structure:

[0184] [R 1 Me 2 SiO 1 / 2 ] a [Me 2 SiO 2 / 2 ] b [R 2 MeSiO 2 / 2 ] c [MeSiO 3 / 2 ] d [SiO 4 / 2 ] e

[0185] in

[0186] a=2

[0187] b=70

[0188] c=4

[0189] d=0

[0190] e=0

[0191] in:

[0192] a+b+c+d+e=76

[0193] R 1 =Me

[0194] R 2= the same or different polyethers of the general formula (e), obtainable from the polymerization of ethylene oxide and propylene oxide,

[0195] Formula (e):

[0196]

[0197] in:

[0198] 37.5 mol% polyether 1, wherein

[0199] f=3

[0200] g=37

[0201] h=38

[0202] in

[0203] g+h=75, statistical structure

[0204] R 3 =Methyl

[0205] as well as

[0206] 62.5 mol% polyether 2, of which

[0207] f=3

[0208] g=14

[0209] h=0

[0210] in

[0211] g+h=14, statistical structure

[0212] R 3 =Methyl.

[0213] In the inventive experiments, short-chain siloxane components were added to heat-cured flexible PU foam formulations containing high molecular weight silicone components (of Formula 1a) as foam stabilizers. The three selected silicone additives (each corresponding to a compound of Formula 1b) are characterized as follows:

[0214] 5) Silicone Additives1

[0215] Unmodified silicone oil of the following composition:

[0216] [R 4 Me 2 SiO 1 / 2 ] i [Me 2 SiO 2 / 2 ] j [R 5 MeSiO 2 / 2 ]k [MeSiO 3 / 2 ] l [SiO 4 / 2 ] m

[0217] in

[0218] i=2

[0219] j = distributed from 2 to 15, with a maximum at 9

[0220] k=0

[0221] l=0

[0222] m=0

[0223] in:

[0224] i+j+k+l+m=distributed from 4 to 17, with the largest value at 11

[0225] R 4 =Me

[0226] Silicone Additives 2

[0227] Polyether-modified siloxanes with the following structural parameters:

[0228] [R 4 Me 2 SiO 1 / 2 ] i [Me 2 SiO 2 / 2 ] j [R 5 MeSiO 2 / 2 ] k [MeSiO 3 / 2 ] l [SiO 4 / 2 ] m

[0229] in

[0230] i=2

[0231] j=4.0

[0232] k = 2.0

[0233] l=0

[0234] m=0

[0235] in:

[0236] i+j+k+l+m=8

[0237] R 4 =Me

[0238] R 5 =Polyether 1 of formula f:

[0239]

[0240] in:

[0241] n=3

[0242] o=3.5

[0243] p=2.0

[0244] in

[0245] o+p=5.5

[0246] R 6 =OH

[0247] Silicone Additives 3

[0248] Heptamethyltrisiloxane modified with n-octene. The structural parameters are as follows:

[0249] [R 4 Me 2 SiO 1 / 2 ] i [Me 2 SiO 2 / 2 ] j [R 5 MeSiO 2 / 2 ] k [MeSiO 3 / 2 ] l [SiO 4 / 2 ] m

[0250] in

[0251] i=2

[0252] j=0

[0253] k=1

[0254] l=0

[0255] m=0

[0256] in:

[0257] i+j+k+l+m=3

[0258] R 4 =Me

[0259] R 5 =n-octyl

[0260] 6)Toluene diisocyanate T 80 from Covestro (80% 2,4 isomer, 20% 2,6 isomer), 3 mPa·s, 48% NCO, functionality 2.

[0261] 400 g of polyol were used in each foaming operation; the other formulation ingredients were recalculated accordingly. For example, 1.00 part of a component means 1.00 g of that substance per 100 g of polyol.

[0262] Foaming is performed by so-called manual mixing. Use preparation 1 as detailed in Table 2. For this reason, polyol, corresponding amine catalyst mixture, tin catalyst 2-ethylhexanoate tin (II), water, foam stabilizer and optional additional low molecular weight silicon additive (compound of formula (1b)) are loaded into a paper cup, and the contents are mixed at 1000rpm for 60 seconds with a disc stirrer. After the first stirring, isocyanate (TDI) is added to the reaction mixture and stirred at 2500rpm for 7s, then immediately transferred to a paper-lined box (30cm×30cm bottom area and 30cm height). After pouring, the foam rises in the foaming box. Ideally, the foam will release when reaching the maximum rise height, and then fall back slightly. This opens the pore film of the foam bubble and obtains the open-cell pore structure of the foam. In order to evaluate the properties, the following characteristic parameters are determined: rise time, rise height and fall back (=sedimentation) of the foam after the end of the rise phase.

[0263] Defined foams were cut out from the resulting heat-cured flexible PU foam blocks and these foams were further analyzed. The following physical properties were determined from the test samples: cell count, porosity determined by flow method, foam density (FD) and roll-up deformation at room temperature.

[0264] The results of the effects of the compounds according to the invention on foaming and the physical properties of the resulting heat-curing flexible PU foams are compiled in the table below. By way of comparison, heat-curing flexible PU foams were first produced with only a standard flexible foam stabilizer (foam stabilizer 1) and only with silicone additives (silicone additive 1, silicone additive 2 and silicone additive 3). The foams without foam stabilizer collapsed completely, so that no foams of significance were obtained. According to the invention, combinations of foam stabilizer 1 with silicone additives 1, 2 and 3 were then used.

[0265] Table 3:

[0266]

[0267] Table 4:

[0268]

[0269] Table 5:

[0270]

[0271] Table 6:

[0272]

[0273] Table 7:

[0274]

[0275] In the evaluation of the results, it must be taken into account that the results of the roll-up test depend greatly on the porosity of the foam. Foams with a relatively closed pore structure are generally inferior here to those with an open-pore structure. Since the porosity in the foaming operation varies to a certain extent due to a number of different influencing factors (temperature, air pressure, etc.), the results of the roll-up test must be evaluated in each case in conjunction with the porosity in order to make a meaningful analysis.

[0276] For this purpose, Figures 1 to 3 In Figure 1, the results of the roll-up test are plotted against the porosity. In each case, the curves are plotted for the reference (heat-cured flexible PU foam with only foam stabilizer 1) and the values ​​for the reference + 1 part of silicone additive. In order to obtain heat-cured flexible PU foams with different porosities, the same foaming operation was repeated on different days, varying the amount of stabilizer and varying the amount of tin catalyst (Kosmos 29). Especially the variation of the tin catalyst showed an ideal wide range of porosity values.

[0277] It was found that for the reference foam, the result of the roll-up test was observed to be greatly dependent on the porosity. Non-inventive foams with porosities up to 2.3 scfm are usually very poor in the roll-up test. On the contrary, when non-inventive heat-cured soft PU foams are very open (scfm>4.5), they are very good in the roll-up test. However, most industrial heat-cured soft PU foams are between 1.5 and 4.5 scfm. Within this range, for all foams according to the present invention in the roll-up test, significantly improved results have been surprisingly found. Since both the measurement of porosity and the measurement of the roll-up test results are susceptible to change, there is usually a certain degree of dispersion in these values. However, significant improvement can be seen.

[0278] It can be seen that the inventive combination of the compound of formula (1a) and the compound of formula (1b) shows significant advantages in the roll-up deformation test on heat-cured flexible PU foams compared to the use of a single high molecular weight silicone component as a foam stabilizer. The recovery of the original shape of the test specimen after the roll-up deformation is improved to a very important extent. The use of a low molecular weight silicone additive (compound of formula (1b)) alone leads to collapse in the heat-cured flexible PU foam formulation. The combination of a high molecular weight foam stabilizer (compound of formula (1a)) and a low molecular weight silicone component (compound of formula (1b)) shows more sufficient stability (settling of less than 2.0 cm), a constant pore count (14 to 15 pores per cm) and a clear advantage in the roll-up test.

[0279] It was also found that the heat-cured flexible PU foam according to the invention has low emissions if emission-optimizing additives are used. This can be seen in the VOC test according to DIN EN ISO 16000-9:2008-04. It was found here that in the low-emission formulation, the total emissions increased slightly (from 40 μg / m 3 (See Table 8) Increased to 130 μg / m 3 (See Table 9), but still well below the typical limit of TVOC 500 μg / m 3 Silicone Additive 1 is therefore also very suitable for low-emission formulations.

[0280] The overall advantages of the invention have also been demonstrated in the case of viscoelastic flexible foams.

[0281] Table 8: VOC test according to DIN EN ISO 16000-9:2008-04: (reference to thermosetting PU flexible foam)

[0282]

[0283] Table 9: VOC test according to DIN EN ISO 16000-9:2008-04: (reference to thermosetting PU flexible foam + 1.0 part of silicone additive 1)

[0284]

Claims

1. A mattress, which is a shaped thermosetting soft PU foam product, wherein the thermosetting soft PU foam is obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b), at least one blowing agent and at least one catalyst, in [R 1 Me2SiO 1 / 2 a [Me2SiO 2 / 2 b [R 2 MeSiO 2 / 2 c [MeSiO 3 / 2 d [SiO 4 / 2 e Formula (1a) wherein​​​​​ a=2 to 10, b = 25 to 200, c = 2 to 40, d = 0 to 10, e = 0 to 5, in: a+b+c+d+e>48 R 1 =Me or R 2 R 2 =same or different polyethers obtained from the polymerization of ethylene oxide, propylene oxide and / or other alkylene oxides, and among them [R 4 Me2SiO 1 / 2 i [Me2SiO 2 / 2 j [R 5 MeSiO 2 / 2 k [MeSiO 3 / 2 l [SiO 4 / 2 m Formula (1b) wherein​​​​​ i=2 to 10, j = 0 to 20, k = 0 to 20, l = 0 to 10, m = 0 to 5, in: i+j+k+l+m<20 R 4 =Me or R 5 R 5 =same or different polyethers obtained from the polymerization of ethylene oxide, propylene oxide and / or other alkylene oxides, Characterized in that the catalyst is a tin catalyst, and the tin catalyst is present in an amount of from 0.20 parts to 0.28 parts by mass based on 100 parts by mass of the polyol.

2. The mattress according to claim 1, characterized in that: R 2 = the same or different polyethers of the general formula (c), in f=0-6, g = 0 to 150, h = 0 to 150, in g+h>0 R 3 =OH, alkyl or acetyl, and R 5 = the same or different polyethers of general formula (d), or alkyl C3 to C 15 , in n=0-6, o = 0 to 100, p = 0 to 100, in o+p>0 R 6 =OH, alkyl or acetyl.

3. The mattress according to claim 1, characterized in that: The porosity of the heat-cured flexible polyurethane foam is 1-6 scfm.

4. The mattress according to claim 1 or 2, characterized in that: The heat-cured flexible polyurethane foam has a rebound resilience of 1% to 50% measured according to DIN EN ISO 8307:2008-03, and / or a strength of 5 to 150 kg / m 3 The foam density is 1-6 scfm and / or the porosity is 1-6 scfm.

5. The mattress according to claim 1 or 2, characterized in that: The heat-cured flexible polyurethane foam has a compressive strength of 0.1 to 8.0 kPa at CLD 40% according to DIN EN ISO 3386-1:2015-10.

6. The mattress according to claim 1 or 2, characterized in that: The heat-cured flexible polyurethane foam has a compressive strength of 2.0-8.0 kPa at CLD 40% according to DIN EN ISO 3386-1:2015-10, and / or a rebound resilience of 15-50% measured according to DIN EN ISO 8307:2008-03, and / or a spring rate of 8-80 kg / m 3 Foam density of 1-6 scfm, and / or porosity of 1-6 scfm.

7. The mattress according to claim 1 or 2, characterized in that: The heat-cured flexible polyurethane foam is a viscoelastic flexible polyurethane foam and has a glass transition temperature between -20°C and +15°C, and / or a compressive strength of 0.1-5.0 kPa at CLD 40% according to DIN EN ISO 3386-1:2015-10, and / or a rebound resilience of <10% measured according to DIN EN ISO 8307:2008-03, and / or a strength of 30-130 kg / m 3 Foam density of 1-6 scfm, and / or porosity of 1-6 scfm.

8. The mattress according to claim 1 or 2, characterized in that the mattress has a height from 1 cm to 50 cm and a width from 20 cm to 300 cm, and a length from 20 cm to 300 cm.

9. The mattress according to claim 1 or 2, characterized in that, based on its initial volume, the mattress is compressed by at least 20% and maintained in the compressed form for at least 20 hours by an auxiliary device.

10. The mattress of claim 9, wherein the mattress is in a compressed state.

11. The mattress according to claim 1 or 2, characterized in that: It is obtained by the additional use of recycled polyols.

12. Use of a combination of at least one compound of formula (1a) and at least one compound of formula (1b) for improving the dimensional recovery of a mattress after it has been compressed for a period of at least 20 hours, wherein formula (1a) and (1b) are each as defined in claim 1, wherein the mattress is a shaped thermosetting flexible PU foam article obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one blowing agent and at least one catalyst and in the presence of at least one compound of formula (1a) and at least one compound of formula (1b), The porosity of the heat-cured flexible polyurethane foam is 1-6 scfm, The catalyst is a tin catalyst, and the tin catalyst is present in an amount of from 0.20 parts to 0.28 parts by mass based on 100 parts by mass of the polyol.

13. A method for storing and / or transporting a mattress, the mattress being a shaped thermosetting soft PU foam product, in (a) in a first step, providing a shaped heat-cured flexible PU foam article by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b) as well as at least one blowing agent and at least one catalyst, wherein formula (1a) and (1b) are each as defined in claim 1, (b) in an optional subsequent step, optionally further processing the obtained shaped thermosetting flexible PU foam article to prepare it for application, (c) and wherein in the last step, the shaped heat-cured flexible PU foam article, optionally prepared for the application, is compressed by at least 20% based on its initial volume, and optionally vacuum-packed and kept in compressed form by auxiliary devices, and stored and / or transported, The porosity of the heat-cured flexible polyurethane foam is 1-6 scfm, The catalyst is a tin catalyst, and the tin catalyst is present in an amount of from 0.20 parts to 0.28 parts by mass based on 100 parts by mass of the polyol.

14. The method according to claim 13, characterized in that In step (a), a sufficient amount of a compound having formula (1a) is added, and its mass proportion in the molded heat-cured flexible PU foam product is 0.1 wt %-5 wt %, and in step (a), a sufficient amount of a compound having formula (1b) is added, and its mass proportion in the molded heat-cured flexible PU foam product is 0.1 wt %-5 wt %.

15. A method for producing a mattress by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b), at least one blowing agent and at least one catalyst, wherein the mattress is a shaped thermosetting flexible polyurethane foam product, the thermosetting flexible polyurethane foam having a porosity of 1-6 scfm, Wherein formula (1a) and (1b) are defined as follows: [R 1 Me2SiO 1 / 2 a [Me2SiO 2 / 2 b [R 2 MeSiO 2 / 2 c [MeSiO 3 / 2 d [SiO 4 / 2 e Formula (1a)​​​​​ in a=2 to 10, b = 25 to 200, c = 2 to 40, d = 0 to 10, e = 0 to 5, in: a+b+c+d+e>48 R 1 =Me or R 2 R 2 =same or different polyethers obtained from the polymerization of ethylene oxide, propylene oxide and / or other alkylene oxides, and among them [R 4 Me2SiO 1 / 2 i [Me2SiO 2 / 2 j [R 5 MeSiO 2 / 2 k [MeSiO 3 / 2 l [SiO 4 / 2 m Formula (1b)​​​​​ in i=2 to 10, j = 0 to 20, k = 0 to 20, l = 0 to 10, m = 0 to 5, in: i+j+k+l+m<20 R 4 =Me or R 5 R 5 =same or different polyethers obtained from the polymerization of ethylene oxide, propylene oxide and / or other alkylene oxides, The catalyst is a tin catalyst, and the tin catalyst is present in an amount of from 0.20 parts to 0.28 parts by mass based on 100 parts by mass of the polyol.

16. The method according to claim 15, characterized in that R 2 = the same or different polyethers of the general formula (c), in f=0-6, g = 0 to 150, h=0 to 150, in g+h>0 R 3 =OH, alkyl or acetyl, and R 5 = the same or different polyethers of general formula (d), or alkyl C3 to C 15 , in n=0-6, o = 0 to 100, p = 0 to 100, in o+p>0 R 6 =OH, alkyl or acetyl.

17. Use of a heat-cured flexible polyurethane foam in a mattress, wherein the heat-cured flexible polyurethane foam is obtained by reacting at least one polyol component with at least one isocyanate component in the presence of at least one compound of formula (1a) and at least one compound of formula (1b), at least one blowing agent and at least one catalyst, wherein formula (1a) and (1b) are each as defined in claim 1, for providing a compressed mattress having improved dimensional recovery after being compressed for a period of at least 20 hours, The porosity of the heat-cured flexible polyurethane foam is 1-6 scfm, The catalyst is a tin catalyst, and the tin catalyst is present in an amount of from 0.20 parts to 0.28 parts by mass based on 100 parts by mass of the polyol.

18. A mixture comprising at least one compound of formula (1b) and at least one compound of formula (1a), a catalyst, and / or diols, polyethers, organic esters and / or other solvents suitable for mattress production purposes, wherein formulas (1a) and (1b) are each as defined in claim 1, the mattress is a shaped thermosetting flexible polyurethane foam product, the catalyst is a tin catalyst, and the tin catalyst is present in an amount of from 0.20 to 0.28 parts by mass based on 100 parts of polyol.