Multilayer Ceramic Capacitors
By using barium titanate-based side edge material in a multi-layer ceramic capacitor, containing an appropriate amount of lanthanide rare earth element terbium, the problems of dielectric thickness reduction and insufficient sintering driving force are solved, and mechanical strength and moisture resistance are improved. The bonding force between the electrode and the dielectric layer is enhanced, and high capacitance and high reliability ceramic capacitors are achieved.
Patent Information
- Application Number
- CN202010762364.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-08
- Filing Date
- 2020-07-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-31
AI Technical Summary
During the manufacturing process, the existing multi-layer ceramic capacitors have problems such as local reduction in dielectric thickness, resulting in a drop in withstand voltage, and insufficient sintering driving force in the edge area leads to insufficient mechanical strength and moisture resistance.
A barium titanate-based side edge material, containing lanthanide rare earth element terbium (Tb), whose content is 0.110≤Tb/RE≤2.333, is used to form a dielectric composition different from the ceramic body to Improve the sintering driving force and interface bonding force, and fill the interface gap at high temperatures.
The mechanical strength and high temperature and humidity resistance of the multi-layer ceramic capacitor are significantly improved, the reduction of interface adhesion and void generation are reduced, the uniformity of the electrode and dielectric layer is enhanced, and the capacitance characteristics and reliability are improved.
Smart Images

Figure CN112786311B_ABST
Abstract
Description
[0001] This application claims the benefit of priority from Korean Patent Application No. 10-2019-0142465 filed on November 8, 2019, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0002] The present disclosure relates to a multilayer ceramic capacitor and a method for manufacturing the same, and more particularly, to a multilayer ceramic capacitor and a method for manufacturing the same that can improve mechanical strength and can improve high temperature resistance and moisture resistance. Background Art
[0003] Generally, an electronic component using a ceramic material, such as a capacitor, an inductor, a piezoelectric element, a varistor, or a thermistor, includes a ceramic body formed using the ceramic material, an internal electrode formed inside the ceramic body, and an external electrode mounted on a surface of the ceramic body to be connected to the internal electrode.
[0004] Recently, as electronic products have become miniaturized and multifunctional, chip components have also been miniaturized and highly functionalized, and thus, high capacitance products such as multilayer ceramic capacitors having a small size and high capacitance are required.
[0005] In order to achieve miniaturization and high capacitance of multilayer ceramic capacitors, it is necessary to ensure a dielectric material having good dielectric properties and excellent withstand voltage characteristics.
[0006] In addition, it is necessary to thin the dielectric and significantly increase the electrode active area (increasing the effective volume fraction required to achieve capacitance).
[0007] However, due to dielectric thinning and edge step differences, a local reduction in dielectric thickness may occur, and therefore, structural design changes are necessary to significantly reduce the withstand voltage drop phenomenon caused by such local reduction.
[0008] In order to realize a multilayer ceramic capacitor with a small size and high capacitance as described above and to prevent the withstand voltage drop phenomenon, when manufacturing the multilayer ceramic capacitor, there is a method of exposing the inner electrode in the width direction of the body, thereby significantly increasing the inner electrode area in the width direction through an edgeless design, and in an operation before firing after the sheet is manufactured as described above, a separate edge portion is attached to the electrode exposed surface of the sheet in the width direction.
[0009] However, when the multilayer ceramic capacitor is manufactured as described above, the dielectric composition of the ceramic body is used as it is without distinguishing the dielectric composition of the side edge from the dielectric composition of the ceramic body.
[0010] Therefore, there is a problem that the interface gap between the electrode end and the edge joint surface is not filled. The interface gap is inevitably generated due to the problem of reducing the density of the side edge and the sintering drive mismatch between the dielectric at the side edge and the internal electrode during sintering.
[0011] Furthermore, since in the prior art, a ceramic dielectric sheet used as an edge is attached to a green sheet cut body without an edge by physical pressing, and then a sintered body having a rigid body is formed by high-temperature heat treatment. Therefore, in this case, when the adhesive force between the electrode exposed surface and the sheet for forming the edge portion is insufficient in the operation before sintering, a poor appearance due to the removal of the edge and a serious defect causing interface cracks may occur.
[0012] In addition, when the volume changes inside the sheet due to the shrinkage of the internal electrode during high-temperature heat treatment, voids are generated between the electrode end and the edge interface, serving as a starting point for crack generation or a moisture penetration path, thereby causing a decrease in moisture resistance reliability.
[0013] Furthermore, to solve the above problems, when a material with a high sintering driving force is applied as a general method, aggregation of the outermost inner electrode near the interface intensifies due to excessive grain growth, resulting in an increase in the decrease in withstand voltage due to uneven electrodes and dielectric layers.
[0014] Therefore, the dielectric in the edge region should have excellent sintering driving force so that the same sintered body density as that of the ceramic main body can be ensured even at a low physical packing density, thereby significantly reducing the reduction in strength of the multilayer ceramic capacitor.
[0015] Furthermore, the dielectric used in the edge region should be able to more actively mobilize materials at high temperatures to fill the interfacial voids.
[0016] In addition, an oxide layer should be formed on the end joint surface through reaction with the internal electrode to improve the interface bonding strength. Summary of the invention
[0017] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.
[0018] An aspect of the present disclosure is to provide a high-capacitance multilayer ceramic capacitor having improved mechanical strength and high temperature and humidity resistance and a method of manufacturing the same.
[0019] According to one aspect of the present disclosure, a multilayer ceramic capacitor includes: a ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface; a plurality of internal electrodes disposed inside the ceramic body, exposed from the first surface and the second surface, and each internal electrode having one end exposed from the third surface or the fourth surface; and a first side edge and a second side edge, respectively disposed on the first surface and the second surface from which the ends of the plurality of internal electrodes are exposed. The first side edge and the second side edge include a barium titanate-based base material and a subcomponent. The subcomponent includes a first subcomponent including a lanthanide rare earth element, the first subcomponent including terbium (Tb), and a content ratio of terbium (Tb) to a content of a portion (RE) of the first subcomponent other than terbium (Tb) satisfies 0.110≤Tb / RE≤2.333.
[0020] According to one aspect of the present disclosure, a multilayer ceramic capacitor includes: a ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface; a plurality of internal electrodes disposed inside the ceramic body, exposed from the first surface and the second surface, and each internal electrode having one end exposed from the third surface or the fourth surface; and a first side edge and a second side edge, respectively disposed on the first surface and the second surface from which the ends of the plurality of internal electrodes are exposed. The first side edge and the second side edge include a barium titanate-based base material and a subcomponent. The subcomponent includes a first subcomponent including a lanthanide rare earth element, the first subcomponent including terbium (Tb). The content ratio of terbium (Tb) to the content of a portion (RE) of the first subcomponent other than terbium (Tb) satisfies 0.110≤Tb / RE≤2.333. The dielectric composition included in the first side edge and the second side edge is different from the dielectric composition included in the ceramic body, and the content of terbium (Tb) included in the first side edge and the second side edge is greater than the content of terbium (Tb) included in the ceramic body. A content ratio of the content of the terbium (Tb) included in the first side edge and the second side edge to the content of the matrix material included in the first side edge and the second side edge is greater than a content ratio of the content of the terbium (Tb) included in the ceramic body to the content of the barium titanate-based matrix material included in the ceramic body.
[0021] According to one aspect of the present disclosure, a multilayer ceramic capacitor includes: a ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface; a plurality of internal electrodes disposed inside the ceramic body, exposed from the first surface and the second surface, and each internal electrode having one end exposed from the third surface or the fourth surface; and a first side edge and a second side edge, respectively disposed on the first surface and the second surface from which the ends of the plurality of internal electrodes are exposed. The first side edge and the second side edge include a barium titanate-based matrix material and a secondary component. The secondary component includes terbium (Tb) and one or more other lanthanide rare earth elements as a first secondary component. The content ratio of the terbium (Tb) included in the first side edge and the second side edge to the content of the matrix material included in the first side edge and the second side edge is greater than the content ratio of the terbium (Tb) included in the ceramic body to the content of the barium titanate-based matrix material included in the ceramic body. The content of the terbium (Tb) satisfies 0.15 mol≤Tb≤1.35 mol with respect to 100 mol of the base material included in the first and second side edges. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The above and other aspects, features and advantages of the present disclosure will be more clearly understood through the following detailed description in conjunction with the accompanying drawings, in which:
[0023] Figure 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment;
[0024] Figure 2 is along Figure 1 A cross-sectional view taken along line II';
[0025] Figure 3 is along Figure 1 A cross-sectional view taken along line II-II';
[0026] Figure 4 It shows the composition Figure 1 A top plan view of one dielectric layer of a multilayer ceramic capacitor is shown; and
[0027] FIG. 5A to FIG. 5F are cross-sectional views and perspective views schematically illustrating a method of manufacturing a multilayer ceramic capacitor according to another embodiment. DETAILED DESCRIPTION
[0028] The following detailed description is provided to help the reader gain a comprehensive understanding of the methods, devices and / or systems described herein. However, various changes, modifications and equivalents of the methods, devices and / or systems described herein will be apparent to those of ordinary skill in the art. The order of operations described herein is merely exemplary and is not limited to the order of operations set forth herein, but may be changed, as will be apparent to those of ordinary skill in the art, except for operations that must occur in a particular order. In addition, descriptions of functions and configurations known to those of ordinary skill in the art may be omitted for clarity and brevity.
[0029] The features described herein may be implemented in different forms and should not be construed as limited to the examples described herein. Rather, the examples described herein have been provided so that this disclosure will be thorough and complete, and will fully convey the scope of the disclosure to those skilled in the art.
[0030] Here, it should be noted that use of the term "may" with respect to an example or embodiment (e.g., with respect to what an example or embodiment may include or implement) means that there is at least one example or embodiment that includes or implements such features, while all examples and embodiments are not limited thereto.
[0031] Throughout the specification, when an element (such as a layer, a region, or a substrate) is described as being “on”, “connected to”, or “coupled to” another element, it may be directly “on”, “connected to”, or “coupled to” another element, or one or more other elements may be present between them. Conversely, when an element is described as being “directly on”, “directly connected to”, or “directly coupled to” another element, there may be no other elements present between them.
[0032] As used herein, the term "and / or" includes any one of the associated listed items and any combination of any two or more.
[0033] Although terms such as "first", "second", and "third" may be used herein to describe various members, components, regions, layers, or portions, these members, components, regions, layers, or portions are not limited by these terms. Specifically, these terms are only used to distinguish one member, component, region, layer, or portion from another member, component, region, layer, or portion. Therefore, without departing from the teachings of the examples described herein, the first member, first component, first region, first layer, or first portion mentioned in the examples may also be referred to as the second member, second component, second region, second layer, or second portion.
[0034] For ease of description, spatially relative terms such as "above", "upper", "below", and "lower" may be used herein to describe the relationship of one element to another element as shown in the figure. Such spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation depicted in the figure. For example, if the device in the accompanying drawings is turned over, an element described as being "above" or "upper" relative to another element will be "below" or "lower" relative to the other element. Therefore, depending on the spatial orientation of the device, the term "above" includes both the upper orientation and the lower orientation. The device can also be oriented in other ways (e.g., rotated 90 degrees or in other orientations), and the spatially relative terms used herein will be interpreted accordingly.
[0035] The terms used herein are only used to describe various examples and are not used to limit the present disclosure. Unless the context clearly indicates otherwise, the singular form is also intended to include the plural form meaning. The terms "include", "comprising" and "having" list the existence of the stated features, numbers, operations, components, elements and / or their combinations, but do not exclude the existence or addition of one or more other features, numbers, operations, components, elements and / or their combinations.
[0036] Variations in the shapes shown in the drawings may occur due to manufacturing techniques and / or tolerances. Therefore, the examples described herein are not limited to the specific shapes shown in the drawings but include variations in shapes that occur during manufacturing.
[0037] The features of the examples described herein may be combined in various ways as will be apparent after understanding the disclosure of the present application. In addition, although the examples described herein have various configurations, other configurations as will be apparent after understanding the disclosure of the present application are possible.
[0038] The drawings may not be drawn to scale, and the relative size, proportions, and depiction of elements in the drawings may be exaggerated for clarity, illustration, and convenience.
[0039] Subsequently, examples are described in more detail with reference to the accompanying drawings.
[0040] Figure 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment.
[0041] Figure 2 is along Figure 1 A cross-sectional view taken along line II'.
[0042] Figure 3 is along Figure 1 A cross-sectional view taken along line II-II'.
[0043] Figure 4 It shows the composition Figure 1A top plan view of one dielectric layer of a multilayer ceramic capacitor is shown.
[0044] FIG. 5A to FIG. 5F are cross-sectional views and perspective views schematically illustrating a method of manufacturing a multilayer ceramic capacitor according to another embodiment.
[0045] Reference Figures 1 to 4 , the multilayer ceramic capacitor according to the embodiment includes a ceramic body 110 , a plurality of internal electrodes 121 and 122 formed in the ceramic body 110 , and external electrodes 131 and 132 formed on an outer surface of the ceramic body 110 .
[0046] The ceramic body 110 has first and second surfaces 1 and 2 opposing each other, third and fourth surfaces 3 and 4 connecting the first and second surfaces to each other, and fifth and sixth surfaces 5 and 6 as upper and lower surfaces.
[0047] The first surface 1 and the second surface 2 may be defined as surfaces opposite to each other in the width direction (W direction) of the ceramic body 110, and the third surface 3 and the fourth surface 4 may be defined as surfaces opposite to each other in the length direction (X direction). The fifth surface 5 and the sixth surface 6 may be defined as surfaces opposite to each other in the thickness direction (Z direction).
[0048] The shape of the ceramic body 110 is not particularly limited, but may be a rectangular parallelepiped shape as shown in the drawings.
[0049] One end of each of the plurality of internal electrodes 121 and 122 formed in the ceramic body 110 is exposed to the third surface 3 or the fourth surface 4 of the ceramic body.
[0050] The internal electrodes ( 121 and 122 ) may be provided as a pair of first and second internal electrodes 121 and 122 having different polarities.
[0051] One end of the first internal electrode 121 may be exposed to the third surface 3 , and one end of the second internal electrode 122 may be exposed to the fourth surface 4 .
[0052] The other end of the first internal electrode 121 and the other end of the second internal electrode 122 are formed to be a predetermined distance from the third surface 3 or the fourth surface 4 , which will be described in more detail later.
[0053] The first and second external electrodes 131 and 132 may be formed on the third and fourth surfaces 3 and 4 of the ceramic body, respectively, to be electrically connected to the internal electrodes.
[0054] According to an embodiment, the multilayer ceramic capacitor includes: a plurality of internal electrodes 121 and 122, which are arranged inside the ceramic body 110 and exposed to the first surface 1 and the second surface 2, and each of the plurality of internal electrodes 121 and 122 has one end to the third surface 3 or the fourth surface; and a first side edge 113 and a second side edge 114, which are arranged on the ends of the internal electrodes 121 and 122 exposed to the first surface 1 and the second surface 2.
[0055] A plurality of internal electrodes 121 and 122 are formed in the ceramic body 110, and respective ends of the plurality of internal electrodes 121 and 122 are exposed to the first surface 1 and the second surface 2, which are surfaces in a width direction of the ceramic body 110. The first side edge 113 and the second side edge 114 are disposed on the first surface 1 and the second surface 2, respectively.
[0056] The thickness d1 of the first side edge 113 and the thickness d2 of the second side edge 114 may be 18 μm or less.
[0057] According to an embodiment, the ceramic body 110 may include a stacked body 111 in which a plurality of dielectric layers 112 are stacked, and first and second side edges 113 and 114 formed on both sides of the stacked body.
[0058] The plurality of dielectric layers 112 constituting the stacked body 111 are in a sintered state and may be integrated so that the boundaries between adjacent dielectric layers cannot be recognized.
[0059] The length of the stack 111 corresponds to the length of the ceramic body 110, and the length of the ceramic body 110 corresponds to the distance from the third surface 3 to the fourth surface 4 of the ceramic body 110. For example, the third surface 3 and the fourth surface 4 of the ceramic body 110 may be understood as the third surface and the fourth surface of the stack 111.
[0060] The laminated body 111 is formed by stacking a plurality of dielectric layers 112 , and the length of the dielectric layer 112 forms the distance between the third surface 3 and the fourth surface 4 of the ceramic body.
[0061] Although not particularly limited, according to an embodiment, the length of the ceramic body may be 400 μm to 1400 μm. In more detail, the length of the ceramic body may be 400 μm to 800 μm or 600 μm to 1400 μm.
[0062] The internal electrodes 121 and 122 may be formed on the dielectric layer, and the internal electrodes 121 and 122 may be formed in the ceramic body 110 through sintering with one dielectric layer 112 interposed therebetween.
[0063] Reference Figure 4, the first internal electrode 121 is formed on the dielectric layer 112. The first internal electrode 121 is not formed in the entire length direction of the dielectric layer. For example, one end of the first internal electrode 121 may be formed to be a predetermined distance d2 from the fourth surface 4 of the ceramic body 110, and the other end of the first internal electrode 121 may be formed to the third surface 3 to be exposed to the third surface 3.
[0064] The other end of the first internal electrode exposed to the third surface 3 of the stacked body is connected to the first external electrode 131 .
[0065] One end of the second internal electrode 122 is formed to be a predetermined distance away from the third surface 3 compared to the first internal electrode, and the other end of the second internal electrode 122 is exposed to the fourth surface 4 to be connected to the second external electrode 132 .
[0066] The dielectric layer 112 may have the same width as that of the first internal electrode 121. For example, the first internal electrode 121 may be formed in the entire width direction of the dielectric layer 112.
[0067] Although not particularly limited, according to an embodiment, the width of the dielectric layer and the width of the internal electrode may be 100 μm to 900 μm. In more detail, the width of the dielectric layer and the width of the internal electrode may be 100 μm to 500 μm or 100 μm to 900 μm.
[0068] As the ceramic body becomes smaller, the thickness of the side edge may affect the electrical characteristics of the multilayer ceramic capacitor. According to an embodiment, the side edge may have a thickness of 18 μm or less, thereby improving the characteristics of the miniaturized multilayer ceramic capacitor.
[0069] In an embodiment, the inner electrode and the dielectric layer are formed by being cut at the same time, and the width of the inner electrode and the width of the dielectric layer may be the same as each other. More details about this will be described later.
[0070] In the present embodiment, the width of the dielectric layer is formed to be the same as the width of the internal electrode, and thus the ends of the internal electrodes 121 and 122 may be exposed to the first and second surfaces of the ceramic body 110 in the width direction.
[0071] The first and second side edges 113 and 114 may be formed on both side surfaces in the width direction at which the ends of the internal electrodes 121 and 122 of the ceramic body 110 are exposed.
[0072] The thickness of the first and second side edges 113 and 114 may be 18 μm or less. When the thickness of the first and second side edges 113 and 114 is smaller, an overlap area of internal electrodes formed in the ceramic body may be further increased.
[0073] The thickness of the first and second side edges 113 and 114 is not particularly limited as long as they have a thickness that can prevent short circuits of internal electrodes exposed to the sides of the stacked body 111. For example, the thickness of the first and second side edges 113 and 114 may be 2 μm or more.
[0074] If the thickness of each of the first side edge and the second side edge is less than 2 μm, the mechanical strength against external impact may be reduced. If the thickness of each of the first side edge and the second side edge is greater than 18 μm, the overlapping area of the inner electrodes may be relatively reduced, and thus, it may be difficult to ensure high capacitance of the multilayer ceramic capacitor.
[0075] In order to significantly increase the capacitance of a multilayer ceramic capacitor, a method of thinning a dielectric layer, a method of highly stacking the thinned dielectric layer, a method of increasing the coverage of an internal electrode, and the like have been considered.
[0076] Furthermore, a method of increasing an overlapping area of internal electrodes forming a capacitor has been considered.
[0077] In order to increase the overlapping area of the internal electrodes, the edge area in which the internal electrodes are not formed should be significantly reduced.
[0078] In detail, as the multilayer ceramic capacitor becomes smaller, the edge area should be significantly reduced to increase the overlapping area of the internal electrodes.
[0079] According to the present embodiment, the internal electrodes are formed in the entire width direction of the dielectric layer, and the thickness of the side edges is set to 18 μm or less, so that the overlapping area of the internal electrodes is relatively wide.
[0080] Generally, the more the dielectric layers are stacked, or the thinner the dielectric layers and the inner electrodes are, the more frequently the inner electrode short circuit may occur. In addition, when the inner electrode is formed only on a portion of the dielectric layer, a step difference may occur due to the inner electrode, thereby reducing the accelerated life of the insulation resistance.
[0081] However, according to the present embodiment, even when the internal electrodes and the dielectric layer are formed as thin films, since the internal electrodes are formed in the entire width direction of the dielectric layer, the overlapping area of the internal electrodes can be increased to increase the capacitance of the multilayer ceramic capacitor.
[0082] In addition, the multilayer ceramic capacitor can have excellent capacitance characteristics and excellent reliability by reducing the step difference caused by the inner electrode to improve the accelerated life of the insulation resistance.
[0083] On the other hand, in the related art, when manufacturing a multilayer ceramic capacitor, a dielectric composition of a ceramic body is used without distinguishing a dielectric composition for forming a side edge from the dielectric composition of the ceramic body.
[0084] Therefore, in this case, the physical filling density of the dielectric in the side edge is relatively low, resulting in the problem of reduced densification of the side edge, and due to the sintering-driven mismatch phenomenon between the inner electrode and the dielectric at the side edge during the sintering process, the interface gap between the electrode end and the edge joint surface that is inevitably generated may not be filled.
[0085] In addition, a ceramic dielectric sheet used as a side edge is attached to a green sheet cut without an edge portion by physical pressing, and then a sintered body having a rigid body is formed by high-temperature heat treatment. Therefore, in the operation before sintering, in the case where the adhesive force between the electrode exposed surface and the sheet for forming the edge is insufficient, a poor appearance due to the removal of the side edge and a serious defect causing interface cracks may occur.
[0086] In addition, when the volume changes inside the sheet due to the shrinkage of the internal electrode during high-temperature heat treatment, voids are generated between the electrode end and the edge interface, serving as a starting point for crack generation or a moisture penetration path, thereby causing a decrease in moisture resistance reliability.
[0087] Therefore, the dielectric in the edge region should have excellent sintering driving force so that the same sintered body density as that of the ceramic main body can be ensured even at a low physical packing density, thereby significantly reducing the reduction in strength of the multilayer ceramic capacitor.
[0088] Furthermore, the dielectric used in the edge region should be able to more actively mobilize materials at high temperatures to fill the interfacial voids.
[0089] In addition, an oxide layer should be formed on the end joint surface through reaction with the internal electrode to improve the interface bonding strength.
[0090] According to an embodiment of the present disclosure, the dielectric composition included in the first and second side edges 113 and 114 and the dielectric composition included in the ceramic body 110 are different from each other.
[0091] The first side edge 113 and the second side edge 114 include a barium titanate matrix material and a subcomponent, and the subcomponent includes a first subcomponent including a lanthanide rare earth element, and the first subcomponent includes terbium (Tb). The content ratio of terbium (Tb) to the content of the portion (RE) other than terbium (Tb) of the first subcomponent satisfies 0.110≤Tb / RE≤2.333. In one example, the content ratio of the present disclosure may refer to a molar ratio.
[0092] The first side edge 113 and the second side edge 114 include a barium titanate matrix material and a subcomponent, and the subcomponent includes terbium (Tb) as a first subcomponent including a lanthanide rare earth element, and the above problem can be solved by adjusting the content ratio of terbium (Tb) to the content of a portion (RE) of the first subcomponent other than terbium (Tb) to satisfy 0.110≤Tb / RE≤2.333.
[0093] In detail, according to the embodiment, reduction in interface adhesiveness between the internal electrode and the edge portion may be prevented, and generation of a void between the internal electrode and the edge portion may be prevented, thereby improving reliability.
[0094] Furthermore, uniform oxide layers and insulating layers may be ensured on the ends of the inner electrodes to reduce short circuit defects, and the density of the edge portions may be increased, and the mechanical strength and high temperature / humidity reliability of the multilayer ceramic capacitor may be improved.
[0095] If the content ratio (Tb / RE) of the content of terbium (Tb) to the content of the portion (RE) other than terbium (Tb) of the first subcomponent is less than 0.110, the content of terbium (Tb) is relatively small, and thus, a gap generated between the internal electrode and the edge portion may not be effectively filled, thereby reducing reliability.
[0096] If the content ratio (Tb / RE) of the content of terbium (Tb) to the content of the portion (RE) other than terbium (Tb) of the first subcomponent exceeds 2.333, the content of terbium (Tb) is excessive, which has a side effect of reducing the insulation resistance of the dielectric layer accompanied by an increase in leakage current due to the electron emission phenomenon through the reaction formula.
[0097] According to an embodiment, the content of terbium (Tb) included in the first and second side edges 113 and 114 may satisfy 0.15 mol≦Tb≦1.35 mol with respect to 100 mol of the base material included in the first and second side edges 113 and 114 .
[0098] Since the content of terbium (Tb) included in the first side edge 113 and the second side edge 114 satisfies 0.15 mol≤Tb≤1.35 mol relative to 100 mol of the base material included in the first side edge 113 and the second side edge 114, the reduction in interface adhesion between the inner electrode and the edge portion can be prevented, and the reliability can be improved by preventing the generation of gaps between the inner electrode and the edge.
[0099] Furthermore, a uniform oxide layer and an insulating layer may be ensured on the end portions of the inner electrodes to reduce short circuit defects, increase the density of the edge portions, and improve the mechanical strength of the multilayer ceramic capacitor and improve high temperature / humidity reliability.
[0100] If the content of terbium (Tb) is less than 0.15 mol relative to 100 mol of the base material, the content of terbium (Tb) may be relatively small, so that the gap between the inner electrode and the edge may not be effectively filled and reliability may be deteriorated.
[0101] If the content of terbium (Tb) exceeds 1.35 mol relative to 100 mol of the base material, the content of terbium (Tb) is excessive and leakage current increases due to electron emission caused by defect chemical reaction formula, which has a side effect of reducing the insulation resistance of the dielectric layer.
[0102] According to an embodiment of the present disclosure, the subsidiary components include magnesium (Mg) and barium (Ba), and a content ratio of the content of magnesium (Mg) to the content of barium (Ba) may satisfy 0.125≤Mg / Ba≤0.500.
[0103] The auxiliary components include magnesium (Mg) and barium (Ba). By adjusting the content ratio of magnesium (Mg) to barium (Ba) to satisfy 0.125≤Mg / Ba≤0.500, the interface adhesion between the inner electrode and the edge can be prevented from being reduced, and the reliability can be improved by preventing the formation of gaps between the inner electrode and the edge.
[0104] Furthermore, uniform oxide layers and insulating layers may be ensured on the ends of the inner electrodes to reduce short circuit defects, increase density of edge portions, and improve mechanical strength of the multilayer ceramic capacitor and high temperature / humidity reliability.
[0105] If the content ratio (Mg / Ba) of magnesium (Mg) to barium (Ba) is less than 0.125, problems such as edge density degradation, generation of interface voids, and uneven thickness of dielectric and internal electrode ends occur, and reliability may be reduced.
[0106] If the content ratio (Mg / Ba) of the content of magnesium (Mg) to the content of barium (Ba) exceeds 0.500, dielectric properties may be degraded.
[0107] The content of magnesium (Mg) may satisfy 0.25 mol ≤ Mg ≤ 1.0 mol relative to 100 mol of the base material.
[0108] By adjusting the content of magnesium (Mg) to satisfy 0.25 mol ≤ Mg ≤ 1.0 mol relative to 100 mol of the base material, degradation of interface adhesion between the inner electrode and the edge portion can be prevented, and generation of voids between the inner electrode and the edge portion can be prevented, thereby improving reliability.
[0109] Furthermore, it is possible to ensure uniform oxide layers and insulating layers on the ends of the inner electrodes, reduce short circuit defects, increase density of edge portions, and improve mechanical strength of the multilayer ceramic capacitor and high temperature / humidity reliability.
[0110] If the content of magnesium (Mg) is less than 0.25 mol relative to 100 mol of the base material, problems such as edge density degradation, generation of interface voids, and uneven thickness of dielectric and internal electrode ends may occur, thereby reducing reliability.
[0111] If the content of magnesium (Mg) exceeds 1.0 mol relative to 100 mol of the base material, dielectric properties may be degraded.
[0112] As described above, the inner electrode is exposed in the width direction of the body, thereby significantly increasing the inner electrode area in the width direction by the edgeless design. In this case, after manufacturing the sheet, in an operation before firing, in the case of manufacturing a multilayer ceramic capacitor by a method of attaching the edge portion alone to the electrode exposed surface of the sheet in the width direction, during the cutting process of the inner electrode exposed surface, the upper electrode and the lower electrode may be connected by a slip phenomenon of the inner electrode exposed surface, which may cause a short circuit and a decrease in withstand voltage.
[0113] Furthermore, at the interface when heterojunction of metal and ceramic is performed, a physical / chemical phenomenon of interface opening may occur due to a spontaneous reaction toward lower surface energy caused by a reduction in specific surface area during sintering.
[0114] Therefore, in order to solve these problems, it is necessary to select an element that can form a uniform oxide layer without forming a secondary phase and that has a high affinity with nickel (Ni) used as an internal electrode and can thus be easily solid-solved.
[0115] According to an embodiment of the present disclosure, Mg oxide having the same structure as NiO (NiO is constituted as a NaCl structure, wherein the ratio of cations to anions is 1:1) is utilized, and at the same time, by controlling the absolute content ratio of Mg oxide having high oxygen affinity, in addition to uniformly forming an insulating layer on the nickel (Ni) electrode terminal, the bonding strength with the side edge ceramic can be increased by generating an oxide layer.
[0116] In this case, in the case where the content ratio of Mg exceeds the optimum composition ratio, sinterability may be reduced due to excessive Mg addition, or withstand voltage may be reduced due to generation of a secondary phase. Therefore, selection of the content ratio may be significantly important.
[0117] In addition, in order to further improve the withstand voltage of moisture-proof multilayer ceramic capacitors and suppress crack generation, the density of the side edges should be ensured and the gaps at the electrode ends should be effectively filled. To this end, it is necessary to increase the sintering driving force and induce active material migration at high temperatures.
[0118] The content of barium (Ba) may satisfy 0.5 mol ≤ Ba ≤ 3.0 mol relative to 100 mol of the base material.
[0119] A detailed description of the content of barium (Ba) will be described later.
[0120] According to an embodiment of the present disclosure, the subcomponent may include a second subcomponent and a third subcomponent, the second subcomponent being an oxide or carbonate containing Mg, and the third subcomponent including at least one of a carbonate or oxide containing at least one of silicon (Si), barium (Ba) or aluminum (Al), or a glass compound containing Si. The content ratio of magnesium (Mg) to the total content of barium (Ba) and silicon (Si) may satisfy 0.09≤Mg / (Ba+Si)≤0.19.
[0121] By adjusting the content ratio of magnesium (Mg) to the total content of barium (Ba) and silicon (Si) to satisfy 0.09≤Mg / (Ba+Si)≤0.19, formation of voids between the inner electrode and the edge can be prevented, thereby improving reliability.
[0122] Furthermore, a uniform oxide layer and an insulating layer may be ensured on the end portions of the inner electrodes to reduce short circuit defects, increase the density of the edge portions, and improve the mechanical strength of the multilayer ceramic capacitor and improve high temperature / humidity reliability.
[0123] If the content ratio (Mg / (Ba+Si)) of magnesium (Mg) to the total content of barium (Ba) and silicon (Si) is less than 0.09, problems such as edge density degradation and interface void generation occur, and reliability may be reduced.
[0124] If a content ratio (Mg / (Ba+Si)) of magnesium (Mg) to a total content of barium (Ba) and silicon (Si) exceeds 0.19, dielectric characteristics may be degraded due to excessive diffusion of magnesium (Mg) into an effective dielectric layer.
[0125] In detail, based on the eutectic line of the binary phase diagram in the two-element system, since barium (Ba) and silicon (Si) are important trace components that determine the densification at low temperature by liquid phase sintering or the solubility limit of terbium (Tb), magnesium (Mg), etc. in the BaTiO3 lattice, their relationship with the addition ratio of terbium (Tb) and magnesium (Mg) may be important.
[0126] According to an embodiment of the present disclosure, the dielectric composition included in the first and second side edges 113 and 114 is different from the dielectric composition included in the ceramic body 110. The dielectric composition included in the first and second side edges 113 and 114 will be described below.
[0127] a) Main components of matrix material
[0128] The dielectric ceramic composition included in the first and second side edges 113 and 114 according to the embodiment of the present disclosure may include a matrix material main component including barium (Ba) and titanium (Ti).
[0129] According to an embodiment, the main component of the matrix material is BaTiO3 or a main component represented by (Ba,Ca)(Ti,Ca)O3, (Ba,Ca)(Ti,Zr)O3, Ba(Ti,Zr)O3 or (Ba,Ca)(Ti,Sn)O3 in which Ca, Zr, Sn, etc. are partially dissolved. The main component of the matrix material may be contained in a powder form.
[0130] b) The first secondary component
[0131] According to one embodiment, the first subcomponent containing a lanthanide rare earth element includes terbium (Tb), and in addition, relative to 100 mol of the base material, the first subcomponent having a content greater than 0 mol and less than or equal to 4.0 mol may be included, which contains an oxide or carbonate of at least one of yttrium (Y), dysprosium (Dy), holmium (Ho), erbium (Er), gadolinium (Gd), cerium (Ce), neodymium (Nd), samarium (Sm), lanthanum (La), ytterbium (Yb) and praseodymium (Pr).
[0132] The content of the first subcomponent may be provided based on the content of at least one of Tb, Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, La, Yb, and Pr included in the first subcomponent without distinguishing an addition form such as oxide or carbonate.
[0133] For example, relative to 100 mol of the main component of the base material, the sum of the contents of at least one or more elements of Tb, Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, La, Yb and Pr contained in the first subcomponent may be less than or equal to 4.0 mol.
[0134] In one embodiment, the first subcomponent prevents reliability degradation of a multilayer ceramic capacitor to which the dielectric ceramic composition is applied.
[0135] If the content of the first subcomponent exceeds 4.0 mol relative to 100 mol of the main component of the base material, the high temperature withstand voltage characteristics may be deteriorated due to the pyrochlore (RE2Ti2O7) (wherein RE is one or more elements of Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, La, Yb and Pr) secondary phase.
[0136] c) Second subcomponent
[0137] According to an embodiment of the present disclosure, the dielectric ceramic composition may include a second subcomponent including one or more selected from the group consisting of oxides and carbonates including the Mg element.
[0138] The second subcomponent may be contained in an amount of 0.25 mol ≤ Mg ≤ 1.0 mol relative to 100 mol of the base material.
[0139] The content of the second subcomponent may be based on the content of the Mg element included in the second subcomponent without distinguishing an addition form such as oxide or carbonate.
[0140] When the second subcomponent is included in an amount of 0.25 mol≦Mg≦1.0 mol relative to 100 mol of the base material, high temperature withstand voltage characteristics may be improved.
[0141] d) The third subcomponent
[0142] According to an embodiment, the dielectric ceramic composition may include a third subcomponent including at least one of an oxide or a carbonate including at least one of Si, Ba, and Al, or a glass compound including Si.
[0143] The content of barium (Ba) may satisfy 0.5 mol≤Ba≤3.0 mol relative to 100 mol of the base material, and the content of the portion other than Ba of the third subcomponent may be greater than 0 mol and less than 4.5 mol.
[0144] The content of the third subcomponent may be based on the content of the Si element, the Ba element, or the Al element included in the third subcomponent without distinguishing an addition form such as glass, oxide, or carbonate.
[0145] If the part other than Ba of the third subcomponent is included in an amount of 4.5 mol or more relative to 100 mol of the base material, there may be problems such as reduction in sintering property and density, generation of a secondary phase, and the like.
[0146] A multilayer ceramic capacitor according to another embodiment includes: a ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface to each other; a plurality of internal electrodes disposed inside the ceramic body, exposed to the first surface and the second surface, and each of the internal electrodes has one end exposed to the third surface or the fourth surface; and a first side edge and a second side edge disposed on the ends of the internal electrodes exposed to the first surface and the second surface, respectively. The first side edge and the second side edge include a barium titanate matrix material and a subcomponent, and the subcomponent includes a first subcomponent including a lanthanide rare earth element, and the first subcomponent includes terbium (Tb). In the first side edge and the second side edge, a content ratio of terbium (Tb) content to a content of a portion (RE) of the first subcomponent other than terbium (Tb) satisfies 0.110≤Tb / RE≤2.333. The dielectric composition included in the first side edge and the second side edge is different from the dielectric composition included in the ceramic body. The content of terbium (Tb) included in the first side edge and the second side edge is greater than the content of terbium (Tb) in the ceramic body. For example, a content ratio of terbium (Tb) included in the first side edge and the second side edge to a content of the matrix material included in the first side edge and the second side edge may be greater than a content ratio of terbium (Tb) included in the ceramic body to a content of the matrix material (such as a barium titanate-based matrix material) included in the ceramic body.
[0147] According to another embodiment, the dielectric composition included in the first side edge 113 and the second side edge 114 is different from the dielectric composition included in the ceramic body 110. The first side edge 113 and the second side edge 114 include a barium titanate base material and a subcomponent, and the subcomponent includes a first subcomponent including a lanthanide rare earth element, the first subcomponent includes terbium (Tb), and a content ratio of terbium (Tb) to a content of a portion (RE) other than terbium (Tb) of the first subcomponent satisfies 0.110≤Tb / RE≤2.333, and a content ratio (Tb / RE) of terbium (Tb) included in the first side edge 113 and the second side edge 114 is greater than a content ratio (Tb / RE) of terbium (Tb) included in the ceramic body 110.
[0148] In the multilayer ceramic capacitor according to another embodiment, the dielectric composition included in the first side edge 113 and the second side edge 114 is different from the dielectric composition included in the ceramic body 110. The content ratio of terbium (Tb) included in the first side edge 113 and the second side edge 114 is adjusted to be higher than the content ratio of terbium (Tb) included in the ceramic body 110, thereby providing the effect according to the embodiment of the present disclosure.
[0149] In detail, according to another embodiment, the interface adhesion between the internal electrode and the edge portion may be prevented from being degraded, and a gap may be prevented from being formed between the internal electrode and the edge portion, thereby improving reliability.
[0150] Furthermore, a uniform oxide layer and an insulating layer may be formed on the end portions of the inner electrodes to reduce short circuit defects, increase density of edge portions, and improve mechanical strength of the multilayer ceramic capacitor and high temperature / humidity reliability.
[0151] Hereinafter, a method of manufacturing a multilayer ceramic capacitor according to another embodiment will be described.
[0152] FIG. 5A to FIG. 5F are cross-sectional views and perspective views schematically illustrating a method of manufacturing a multilayer ceramic capacitor according to another embodiment.
[0153] like Figure 5A As shown, a plurality of stripe-shaped first internal electrode patterns 221a are formed on the ceramic green sheet 212a at a predetermined interval d4. The plurality of stripe-shaped first internal electrode patterns 221a may be formed parallel to each other.
[0154] The predetermined interval d4 is the distance between the inner electrode and the outer electrode having different polarities and can be understood as Figure 4 The distance d2×2 shown in .
[0155] The ceramic green sheet 212 a may be formed using a ceramic paste including ceramic powder, an organic solvent, and an organic binder.
[0156] The ceramic powder is a material having a high dielectric constant. Although not particularly limited, barium titanate (BaTiO3)-based materials, lead composite perovskite-based materials, strontium titanate (SrTiO3)-based materials, etc. can be used as the ceramic powder. In detail, barium titanate (BaTiO3) powder can be used. When the ceramic green sheet 212a is fired, the ceramic green sheet 212a becomes the dielectric layer 112 constituting the ceramic body.
[0157] The stripe-shaped first internal electrode pattern 221a may be formed using an internal electrode paste containing a conductive metal. The conductive metal is not particularly limited, but may be nickel (Ni), copper (Cu), palladium (Pd), or an alloy thereof.
[0158] A method of forming the stripe-shaped first internal electrode pattern 221 a on the ceramic green sheet 212 a is not particularly limited, but may be formed by, for example, a printing method such as a screen printing method or a gravure printing method.
[0159] Although not shown, a plurality of stripe-shaped second internal electrode patterns 222a (in the ceramic green sheet 212a) may be formed at predetermined intervals on the other ceramic green sheet 212a. Figure 5B ).
[0160] Hereinafter, the ceramic green sheet having the first internal electrode pattern 221 a formed thereon may be referred to as a first ceramic green sheet, and the ceramic green sheet having the second internal electrode pattern 222 a formed thereon may be referred to as a second ceramic green sheet.
[0161] Next, if Figure 5B As shown, the first ceramic green sheets and the second ceramic green sheets may be alternately stacked such that the stripe-shaped first internal electrode patterns 221 a and the stripe-shaped second internal electrode patterns 222 a are alternately stacked.
[0162] Subsequently, the stripe-shaped first internal electrode patterns 221 a may form the first internal electrode 121 , and the stripe-shaped second internal electrode patterns 222 a may form the second internal electrode 122 .
[0163] Figure 5C is a cross-sectional view showing a ceramic green sheet laminate 210 in which a first ceramic green sheet and a second ceramic green sheet are stacked according to an embodiment, and Figure 5D is a perspective view of a ceramic green sheet stacked body 210 in which a first ceramic green sheet and a second ceramic green sheet are stacked.
[0164] Reference Figure 5C and Figure 5D , first ceramic green sheets having a plurality of parallel strip-shaped first internal electrode patterns 221 a printed thereon and second ceramic green sheets having a plurality of parallel strip-shaped second internal electrode patterns 222 a printed thereon are alternately stacked.
[0165] In more detail, the green sheets may be stacked in such a manner that the center of the stripe-shaped first internal electrode pattern 221 a printed on the first ceramic green sheet and the center of the interval d4 between the stripe-shaped second internal electrode patterns 222 a printed on the second ceramic green sheet overlap each other.
[0166] Next, if Figure 5D As shown, the ceramic green sheet laminate 210 may be cut to cross the plurality of stripe-shaped first internal electrode patterns 221a and the stripe-shaped second internal electrode patterns 222a. For example, the ceramic green sheet laminate 210 may be cut into rod-shaped laminates 220 along line C1-C1.
[0167] In more detail, the strip-shaped first and second internal electrode patterns 221a and 222a may be cut in a length direction and divided into a plurality of internal electrodes having a predetermined width. At this time, the stacked ceramic green sheets are also cut together with the internal electrode patterns. Therefore, the dielectric layer may be formed to have the same width as that of the internal electrode.
[0168] An end portion of the first internal electrode and an end portion of the second internal electrode may be exposed to a cut surface of the rod-shaped laminated body 220. The cut surfaces of the rod-shaped laminated body may be referred to as a first side and a second side of the rod-shaped laminated body, respectively.
[0169] The ceramic green sheet laminate may be fired, and then the ceramic green sheet laminate may be cut into a rod-shaped laminate. Alternatively, the ceramic green sheet may be cut into a rod-shaped laminate and then fired. Although not particularly limited, firing may be performed in an N2-H2 atmosphere at 1100°C to 1300°C.
[0170] Next, if Figure 5E As shown, a first side edge 213a and a second side edge 214a may be respectively formed on a first side surface and a second side surface of the rod-shaped stacked body 220. The second side edge 214a is not clearly shown but is outlined by a dotted line.
[0171] The first side edge 213 a and the second side edge 214 a may be provided by forming a ceramic slurry including ceramic powder on the rod-shaped laminated body 220 .
[0172] The ceramic slurry may include ceramic powder, an organic binder, and an organic solvent, and the amount of the ceramic slurry may be adjusted so that the first side edge 213 a and the second side edge 214 a have desired thicknesses.
[0173] The first and second side edges 213a and 214a may be formed by applying ceramic slurry to the first and second side surfaces of the rod-shaped stacked body 220. The method of applying the ceramic slurry is not particularly limited, and for example, the slurry may be applied by spraying or using a roller.
[0174] In addition, the rod-shaped stacked body may be dipped in the ceramic slurry to form the first and second side edges 213 a and 214 a on the first and second side surfaces of the rod-shaped stacked body.
[0175] As described above, the thickness of the first side edge and the second side edge may be 18 μm or less.
[0176] Next, if Figure 5E and 5F As shown, the rod-shaped laminated body 220 on which the first side edge 213a and the second side edge 214a are formed can be cut into individual pieces having desired sizes along the C2-C2 cutting line. Figure 5C To determine the location of the C2-C2 cutting line.
[0177] Since the rod-shaped laminated body 220 is cut into a sheet size, a ceramic body having the laminated body 111 and the first and second side edges 113 and 114 formed on both sides of the laminated body may be formed.
[0178] When the rod-shaped laminate 220 is cut along the C2-C2 cutting line, the central portions of the overlapped first and second internal electrodes and the predetermined interval d4 between the second internal electrodes may be cut by the same cutting line. From another perspective, the central portion of the second internal electrode and the predetermined interval between the first internal electrodes may be cut by the same cutting line.
[0179] Therefore, one end of the first inner electrode and one end of the second inner electrode may be alternately exposed to the cutting surface cut along the C2-C2 cutting line. The exposed surface of the first inner electrode may be understood as Figure 4 The third surface 3 of the ceramic body shown, and the surface exposed by the second internal electrode can be understood as Figure 4 The fourth surface 4 of the ceramic body is shown.
[0180] When the rod-shaped laminated body 220 is cut along the C2-C2 cutting line, the predetermined interval d4 between the strip-shaped first internal electrode patterns 221a is cut in half, so that one end of the first internal electrode 121 is spaced apart from the fourth surface by a predetermined interval d2. In addition, one end of the second internal electrode 122 is spaced apart from the third surface by a predetermined interval d2.
[0181] Thereafter, an external electrode may be formed on each of the third surface and the fourth surface to be connected to one end of the first internal electrode and one end of the second internal electrode.
[0182] As in the present embodiment, when the first side edge and the second side edge are formed on the rod-shaped laminated body 220 and cut into a sheet size, the side edges can be formed on a plurality of laminated bodies 111 through one process.
[0183] In addition, although not shown, a plurality of laminated bodies may be formed by cutting the rod-shaped laminated body into a sheet size before forming the first side edge and the second side edge.
[0184] For example, the rod-shaped laminated body may be cut so that the central portion of the overlapped first inner electrode and the predetermined interval between the second inner electrodes are cut by the same cutting line. Therefore, one end of the first inner electrode and one end of the second inner electrode may be exposed to different cutting surfaces, respectively.
[0185] Thereafter, first and second side edges made of the above-mentioned material may be formed on the first and second surfaces of the laminate. The method of forming the first and second side edges is as described above.
[0186] In addition, an external electrode may be formed on a third surface of the stacked body to which the first internal electrode is exposed, and another external electrode may be formed on a fourth surface of the stacked body to which the second internal electrode is exposed.
[0187] According to another embodiment, the end of the first inner electrode and the end of the second inner electrode are exposed through the first surface and the second surface of the laminate. A plurality of stacked first inner electrodes and second inner electrodes may be cut simultaneously, and thus the ends of the inner electrodes may be arranged in a straight line. Thereafter, a first side edge and a second side edge are formed together on the first surface and the second surface of the laminate. The ceramic body is formed by the laminate and the first side edge and the second side edge. For example, the first side edge and the second side edge are formed on the first side surface and the second side surface of the laminate, respectively.
[0188] Therefore, according to the present embodiment, the distances from the ends of the plurality of internal electrodes to the first and second surfaces of the ceramic body may be uniformly formed. In addition, the first and second side edges are formed by the ceramic paste and may have a relatively thin thickness.
[0189] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to experimental examples. However, the scope of the present disclosure is not limited by the experimental examples.
[0190] Experimental Example
[0191] BaTiO3 powder of 100 nm or less was used as the main component of the matrix material, and the subcomponent composition in this case was as shown in Table 1 below.
[0192] In preparing the slurry, the matrix material main component and sub-component powders are mixed with ethanol / toluene and a dispersant by using zirconia balls as a mixing / dispersion medium, followed by mechanical grinding, and then a binder for achieving dielectric sheet strength is added and a mixing process is performed.
[0193] The prepared slurry was made into a sheet having a thickness of 10 to 20 μm using an on-roll coater of the head discharge method to form a side edge.
[0194] In addition, a thin sheet was attached to a portion of the green sheet where the internal electrodes were exposed, wherein the internal electrodes were exposed in a width direction without edges, and the thin sheet was cut to have a size of 5 cm×5 cm to form side edges.
[0195] A multilayer ceramic capacitor green sheet of 0603 size (width×length×height: 0.6 mm×0.3 mm×0.3 mm) was manufactured by attaching the thin sheets to both sides of the green sheet by applying constant temperature and pressure under conditions that significantly reduced deformation of the green sheet.
[0196] The manufactured multilayer ceramic capacitor samples were subjected to calcination treatment at a temperature of 400°C or less in a nitrogen atmosphere, and then subjected to firing at a firing temperature of 1200°C or less and a hydrogen concentration of 0.5% H2 or less. Then, electrical characteristics, insulation resistance, sheet strength, adhesion at the interface between the side edge and the inner electrode and gap filling therebetween, the degree of formation of the insulating layer on the electrode end, density difference at the side edge, etc. were comprehensively confirmed.
[0197] The dielectric loss and room temperature capacitance of the multilayer ceramic capacitor (MLCC) of each composition were measured using an LCR meter at 1 kHz and AC 0.5 V, and 50 samples were taken to measure the breakdown voltage (BDV) causing breakdown.
[0198] The side edge hardness of the multilayer ceramic capacitor (MLCC) was measured using a Vickers hardness tester under a load of 5 kgf and a holding time of 5 seconds. The microstructures such as edge density and the degree of insulating layer generation of the fractured surface and the polished surface of the sheet were compared.
[0199] Table 1 below is a dielectric composition table of experimental examples (comparative examples and embodiments), and BaTiO3 is used as a main component of the matrix material. In this case, additional elements in the form of basic donors and acceptors constituting a multilayer ceramic capacitor (MLCC) and elements used as sintering aids including Ba-Si-Al are used as subcomponents.
[0200] At this time, in order to compare the density of the side edges, the formation of the oxide layer on the electrode end, the gap filling, and the interface adhesion between the examples according to the present invention and the comparative examples, the additive element content ratio was variously changed for each subcomponent.
[0201] Table 2 below summarizes the electrical characteristics and microstructural results for 0603 size multilayer ceramic capacitors (MLCCs) corresponding to the compositions specified in Table 1 above.
[0202] [Table 1]
[0203]
[0204] [Table 2]
[0205]
[0206] ◎: Excellent, ○: Good, △: Fair, ×: Poor
[0207] As shown in Tables 1 and 2, when the ratio of terbium (Tb) in the rare earth elements increases to a certain level or more, an interfacial void filling effect can be obtained by increasing the bulk density and bulk strength and increasing the driving force for material migration of the bulk. The content ratio of terbium (Tb) to the content of the portion (RE) other than terbium (Tb) of the first subcomponent can be as high as 9.0.
[0208] However, considering the high temperature and humidity resistance reliability of the multilayer ceramic capacitor, in the case of terbium (Tb) having a strong donor tendency, when the content ratio is too high, the leakage current increases due to the electron emission phenomenon generated by the defect chemical reaction formula. Since the side effect of the dielectric layer insulation resistance decreases, the content ratio of terbium (Tb) to the content of the portion (RE) other than terbium (Tb) of the first subcomponent may satisfy 0.110≤Tb / RE≤2.333 to simultaneously obtain the effects of densification of the main body and increase in insulation resistance of the dielectric layer.
[0209] In addition, a content ratio of the content of magnesium (Mg) to the content of barium (Ba) may satisfy 0.125≤Mg / Ba≤0.500.
[0210] By adjusting the content ratio of magnesium (Mg) to barium (Ba) to satisfy 0.125≤Mg / Ba≤0.500, degradation of interface adhesion between the inner electrode and the edge and generation of voids between the inner electrode and the edge can be prevented, thereby improving reliability.
[0211] Furthermore, a uniform oxide layer and an insulating layer on the end of the inner electrode can be ensured to reduce short circuit defects, improve the density of the edge portion, and improve the mechanical strength of the multilayer ceramic capacitor and improve high temperature / humidity resistance reliability.
[0212] In the case of samples 12, 16, and 17, the content ratio of the content of magnesium (Mg) to the content of barium (Ba) is outside the numerical range according to the embodiment of the present disclosure. In this case, the edge density is reduced, interface voids occur, and the thickness uniformity at the dielectric end and the inner electrode end may be reduced. In addition, a reduction in dielectric properties may occur.
[0213] On the other hand, a content ratio of the content of magnesium (Mg) to the total content of barium (Ba) and silicon (Si) may satisfy 0.09≤Mg / (Ba+Si)≤0.19.
[0214] In an embodiment where a content ratio of magnesium (Mg) to a total content of barium (Ba) and silicon (Si) satisfies 0.09≤Mg / (Ba+Si)≤0.19, generation of voids between the internal electrode and the edge portion can be prevented, and thus, it can be seen that reliability can be improved.
[0215] In addition, a uniform oxide layer and an insulating layer can be ensured on the end of the inner electrode to reduce short circuit defects, increase the density of the edge portion, and improve the mechanical strength of the multilayer ceramic capacitor. Therefore, it can be seen that the high temperature / humidity resistance reliability can be improved.
[0216] In the case of sample 13 in which the content ratio of magnesium (Mg) to the total content of barium (Ba) and silicon (Si) (Mg / (Ba+Si)) is less than 0.09, there are problems of reduced edge density, generation of interface voids, and reduced thickness uniformity at the inner electrode terminal, resulting in reduced reliability.
[0217] In the case of Sample 21 in which the content ratio (Mg / (Ba+Si)) of magnesium (Mg) to the total content of barium (Ba) and silicon (Si) exceeded 0.19, excessive diffusion of magnesium (Mg) into the active dielectric layer degraded dielectric properties.
[0218] In the case of Sample 22, the content of silicon (Si) is outside the numerical range according to the embodiment of the present disclosure, which may cause problems of reduced sintering performance and density and generation of a short circuit.
[0219] As described above, according to the embodiments, after a sheet is manufactured in such a manner that the inner electrode is exposed in the width direction of the body, a reduction in interface adhesion between the inner electrode and the edge that occurs during a manufacturing process of a multilayer ceramic capacitor in which the edge is separately attached to the electrode exposed surface of the sheet in the width direction in an operation before firing can be prevented.
[0220] In addition, in the multilayer ceramic capacitor manufactured through the above-described manufacturing process, a void may be prevented from being generated between the internal electrode and the edge portion, thereby improving reliability.
[0221] Furthermore, uniform oxide layers and insulating layers may be ensured on the ends of the internal electrodes, thereby reducing short circuit defects.
[0222] Furthermore, the density of the edge portion can be increased, thereby increasing the mechanical strength of the multilayer ceramic capacitor and improving high temperature / humidity resistance.
[0223] The inner electrodes are formed over the entire width direction of the dielectric layer and exposed to the sides of the body in the width direction, and then the edges are separately attached, thereby significantly increasing the overlap area between the inner electrodes to realize a high-capacitance multilayer ceramic capacitor and reducing the generation of step differences.
[0224] Although the present disclosure includes specific examples, it will be apparent to those of ordinary skill in the art that various changes in form and detail may be made in these examples without departing from the spirit and scope of the claims and their equivalents. The examples described herein should be considered in a descriptive sense only, and not for limiting purposes. The description of the features or aspects in each example will be considered to be applicable to similar features or aspects in other examples. If the described techniques are performed in a different order, and / or if the components in the described systems, architectures, devices, or circuits are combined in different ways and / or replaced or supplemented by other components or their equivalents, suitable results may be achieved. Therefore, the scope of the present disclosure is not limited by specific embodiments, but by the claims and their equivalents, and all variations within the scope of the claims and their equivalents will be interpreted as included in the present disclosure.
Claims
1. A multilayer ceramic capacitor comprising: A ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface; a plurality of internal electrodes disposed inside the ceramic body, exposed from the first surface and the second surface, and each of the internal electrodes having one end exposed from the third surface or the fourth surface; and The first side edge and the second side edge are respectively disposed on the first surface and the second surface from which the ends of the plurality of inner electrodes are exposed, wherein the first side edge and the second side edge include a barium titanate-based matrix material and a secondary component, wherein the subcomponent includes a first subcomponent including a lanthanide rare earth element, the first subcomponent includes Tb, and a molar ratio of a content of Tb to a content of a portion RE of the first subcomponent excluding Tb satisfies 0.110≤Tb / RE≤2.333, The auxiliary components further include Mg and Ba, and a molar ratio of the content of Mg to the content of Ba in the auxiliary components satisfies 0.125≤Mg / Ba≤0.
500.
2. The multilayer ceramic capacitor according to claim 1, wherein The content of Tb satisfies 0.15 mol≤Tb≤1.35 mol relative to 100 mol of the base material.
3. The multilayer ceramic capacitor according to claim 1, wherein The content of Mg satisfies 0.25 mol≤Mg≤1.0 mol relative to 100 mol of the base material.
4. The multilayer ceramic capacitor according to claim 1, wherein The content of Ba as the auxiliary component satisfies 0.5 mol≤Ba≤3.0 mol relative to 100 mol of the base material.
5. The multilayer ceramic capacitor according to claim 1, wherein The auxiliary ingredients also include: A second subcomponent including a carbonate or an oxide containing Mg; and a third subcomponent containing at least one of an oxide or carbonate containing at least one of Si, Ba and Al and a glass compound containing Si, The molar ratio of the Mg content to the total content of Ba and Si satisfies 0.09≤Mg / (Ba+Si)≤0.
19.
6. The multilayer ceramic capacitor according to claim 1, wherein The subcomponent includes the first subcomponent in an amount greater than 0 mol and less than or equal to 4.0 mol relative to 100 mol of the base material, and the first subcomponent includes an oxide or carbonate of at least one of Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, La, Yb and Pr.
7. The multilayer ceramic capacitor according to claim 1, wherein: A dielectric composition included in the first side edge and the second side edge is different from a dielectric composition included in the ceramic body.
8. A multilayer ceramic capacitor comprising: A ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface; a plurality of internal electrodes disposed inside the ceramic body, exposed from the first surface and the second surface, and each of the internal electrodes having one end exposed from the third surface or the fourth surface; and The first side edge and the second side edge are respectively disposed on the first surface and the second surface from which the ends of the plurality of inner electrodes are exposed, wherein the first side edge and the second side edge include a barium titanate-based matrix material and a secondary component, Wherein, the auxiliary component includes a first auxiliary component including a lanthanide rare earth element, and the first auxiliary component includes Tb, The molar ratio of the content of Tb to the content of the part RE of the first auxiliary component other than Tb satisfies 0.110≤Tb / RE≤2.333, and Wherein, the molar ratio of the Tb content included in the first side edge and the second side edge to the content of the matrix material included in the first side edge and the second side edge is greater than the molar ratio of the Tb content included in the ceramic body to the content of the barium titanate-based matrix material included in the ceramic body.
9. The multilayer ceramic capacitor according to claim 8, wherein: The content of Tb included in the first side edge and the second side edge satisfies 0.15 mol≦Tb≦1.35 mol with respect to 100 mol of the base material included in the first side edge and the second side edge.
10. The multilayer ceramic capacitor according to claim 8, wherein The auxiliary component further includes Mg and Ba, and a molar ratio of a content of Mg to a content of Ba in the auxiliary component satisfies 0.125≤Mg / Ba≤0.
500.
11. The multilayer ceramic capacitor according to claim 10, wherein: The content of Mg satisfies 0.25 mol≤Mg≤1.0 mol with respect to 100 mol of the base material included in the first side edge and the second side edge.
12. The multilayer ceramic capacitor according to claim 10, wherein: The content of Ba satisfies 0.5 mol≤Ba≤3.0 mol with respect to 100 mol of the matrix material included in the first side edge and the second side edge.
13. The multilayer ceramic capacitor according to claim 10, wherein: The auxiliary ingredients also include: A second subcomponent including an oxide or a carbonate containing Mg; and a third subcomponent containing at least one of an oxide or carbonate containing at least one of Si, Ba and Al and a glass compound containing Si, The molar ratio of the Mg content to the total content of Ba and Si satisfies 0.09≤Mg / (Ba+Si)≤0.
19.
14. The multilayer ceramic capacitor according to claim 8, wherein: The subcomponent includes the first subcomponent in an amount greater than 0 mol and less than or equal to 4.0 mol relative to 100 mol of the base material included in the first side edge and the second side edge, and the first subcomponent contains an oxide or carbonate of at least one of Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, La, Yb and Pr.
15. A multilayer ceramic capacitor comprising: A ceramic body including a first surface and a second surface opposite to each other and a third surface and a fourth surface connecting the first surface and the second surface; a plurality of internal electrodes disposed inside the ceramic body, exposed from the first surface and the second surface, and each of the internal electrodes having one end exposed from the third surface or the fourth surface; and The first side edge and the second side edge are respectively disposed on the first surface and the second surface from which the ends of the plurality of inner electrodes are exposed, wherein the first side edge and the second side edge include a barium titanate-based matrix material and a secondary component, wherein the secondary component comprises Tb and one or more other lanthanide rare earth elements as the first secondary component, wherein a molar ratio of a content of Tb included in the first side edge and the second side edge to a content of the base material included in the first side edge and the second side edge is greater than a molar ratio of a content of Tb included in the ceramic body to a content of the barium titanate-based base material included in the ceramic body, and Wherein, the content of Tb included in the first side edge and the second side edge satisfies 0.15 mol≤Tb≤1.35 mol relative to 100 mol of the base material included in the first side edge and the second side edge.
16. The multilayer ceramic capacitor according to claim 15, wherein: The auxiliary component further includes Mg and Ba, and a molar ratio of a content of Mg to a content of Ba in the auxiliary component satisfies 0.125≤Mg / Ba≤0.
500.
17. The multilayer ceramic capacitor according to claim 16, wherein: The content of Mg satisfies 0.25 mol≤Mg≤1.0 mol with respect to 100 mol of the base material included in the first side edge and the second side edge.
18. The multilayer ceramic capacitor according to claim 16, wherein: The content of Ba satisfies 0.5 mol≤Ba≤3.0 mol with respect to 100 mol of the matrix material included in the first side edge and the second side edge.
19. The multilayer ceramic capacitor according to claim 16, wherein: The auxiliary ingredients also include: A second subcomponent including an oxide or a carbonate containing Mg; and a third subcomponent containing at least one of an oxide or carbonate containing at least one of Si, Ba and Al and a glass compound containing Si, The molar ratio of the Mg content to the total content of Ba and Si satisfies 0.09≤Mg / (Ba+Si)≤0.
19.
20. The multilayer ceramic capacitor according to claim 15, wherein The subcomponent includes the first subcomponent in an amount greater than 0 mol and less than or equal to 4.0 mol relative to 100 mol of the base material included in the first side edge and the second side edge, and the first subcomponent contains an oxide or carbonate of at least one of Y, Dy, Ho, Er, Gd, Ce, Nd, Sm, La, Yb and Pr.