Curable resin composition, cured product and sheet-like molded body
By adjusting the composition of polyether polyol resin and epoxy resin, and combining it with trifunctional or above epoxy resin, it solves the problem that the curable resin in the existing technology cannot meet the requirements of transparency, bending resistance and heat resistance of foldable OLED displays. It achieves a balanced improvement in heat resistance and bending resistance and is suitable for materials in the electrical/electronic field.
Patent Information
- Application Number
- CN201980066445.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-10-11
AI Technical Summary
In the existing technology, curable resin compositions cannot meet the simultaneous requirements of transparency, bending resistance and heat resistance of foldable OLED display films, and the glass transition temperature is not sufficient to meet the heat resistance requirements.
Using specific polymer polyether polyol resin, trifunctional or above epoxy resin and epoxy resin curing agent, by adjusting the aromatic and alicyclic structure ratio of the polyether polyol resin, combined with the appropriate epoxy equivalent and number average molecular weight to produce a curable resin composition with excellent heat resistance and balanced bending resistance.
The curable resin composition achieves a balanced improvement in heat resistance and bending resistance. It is suitable for materials in the electrical/electronic field such as foldable OLED displays and has excellent transparency and mechanical properties.
Smart Images

Figure CN112823175B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a curable resin composition having excellent heat resistance and also excellent bending resistance, and can be used in various fields requiring heat resistance and toughness, especially in electrical / electronic fields such as sensors and displays. In addition, the present invention relates to a cured product and a sheet-like molded body obtained by curing the curable resin composition. Background Art
[0002] Epoxy resins are used in various fields due to their excellent heat resistance, adhesion, water resistance, mechanical strength, and electrical properties.
[0003] In recent years, various electronic devices have been used for applications such as requiring light weight / thin film or freedom of shape, and flexibility has attracted attention. In the flexibility of electronic devices, plastic films are used to replace glass that has been used as substrates in the past. This plastic film is required to have excellent bending resistance. In addition, in order to encapsulate semiconductor materials, heat resistance that can withstand the reflow process is required. Furthermore, in order to use it as a substrate for a display, transparency is also required.
[0004] In the flexibility of electronic devices, in recent years, the trend of using organic light-emitting diodes (OLEDs) in displays for foldable smartphones or foldable tablets has accelerated, and foldable OLED displays have been developed. Foldable OLED displays include a multi-layer film, generally speaking, including a layer called a front panel on the surface, a sensing layer below it, and a back film layer below it in this order. Since the functions or characteristics of the films used for each layer are different, it is important to select the material of the film according to the required characteristics when developing a foldable OLED display. Among them, in addition to transparency or bending resistance (flexibility), the sensing layer or the back film layer also needs heat resistance that can withstand high temperatures because it is close to the heat source.
[0005] Patent Document 1 discloses a polyether polyol resin having a high glass transition temperature and containing a specific amount of aromatic structure and alicyclic structure in the main chain, and a curable resin composition obtained by mixing a bifunctional or higher-functional epoxy resin, an epoxy resin curing agent, and a curing accelerator with the polyether polyol resin.
[0006] However, the cured product provided in Patent Document 1 has an insufficient glass transition temperature and cannot satisfy the above-mentioned requirement for heat resistance.
[0007] Furthermore, the curable resin composition described in Patent Document 1 cannot satisfy all of the transparency, bending resistance (flexibility), and heat resistance required of a film for a foldable OLED display in a balanced manner.
[0008] Prior art literature
[0009] Patent Literature
[0010] [Patent Document 1] Japanese Patent Application Publication No. 2006-176658 Summary of the invention
[0011] [Problems to be Solved by the Invention]
[0012] As described above, the object of the present invention is to provide a curable resin composition, a cured product obtained by curing the curable resin composition, and a sheet-like molded body. The curable resin composition has excellent heat resistance and balanced bending resistance, and can be used in various fields requiring heat resistance and toughness, especially in the electrical / electronic fields, and can be used as a material for a film used in foldable OLED displays that have been rapidly developed in recent years.
[0013] The present inventors have found that a cured product having excellent heat resistance and also excellent bending resistance can be obtained by using a specific high molecular weight polyether polyol resin, a trifunctional or higher epoxy resin, and an epoxy resin curing agent.
[0014] In the above-mentioned Patent Document 1, only bifunctional epoxy resin is used as the epoxy resin to be formulated with the polyether polyol resin, and only bisphenol A novolac resin is used as the curing agent. In Patent Document 1, phenol novolac type epoxy resin and cresol novolac type epoxy resin are described for trifunctional or higher epoxy resins, but no detailed description is clearly described.
[0015] The present inventors have found that, in the epoxy resin and curing agent described in Patent Document 1, the original heat resistance of the polyether polyol resin cannot be fully utilized, and the transparency of the obtained cured product is also insufficient. However, by changing the epoxy resin used in combination with the polyether polyol resin to a trifunctional or higher epoxy resin, excellent heat resistance can be achieved, and further, the flex resistance can be improved in a balanced manner.
[0016] The gist of the present invention is as follows.
[0017] [1] A curable resin composition comprising: a polyether polyol resin represented by the following general formula (1) having an epoxy equivalent of 7,000 g / equivalent to 100,000 g / equivalent, a trifunctional or higher-functional epoxy resin, and an epoxy resin curing agent.
[0018] [Chemistry 1]
[0019]
[0020] In the general formula (1), n is an integer greater than 1. A1 and A2 may be the same or different from each other and are divalent organic groups having an aromatic structure and / or an alicyclic structure. Among them, either A1 or A2 contains an aromatic ring structure and an alicyclic ring structure. B is a hydrogen atom or a group represented by the following formula (2). At least one of the two Bs is a group represented by the following formula (2).
[0021] [Chemistry 2]
[0022]
[0023] [2] The curable resin composition according to [1], wherein the polyether polyol resin contains 35% to 55% by mass of an aromatic structure and 8% to 25% by mass of an alicyclic structure in the main chain.
[0024] [3] The curable resin composition according to [1] or [2], wherein the number average molecular weight of the polyether polyol resin is 9,000 to 40,000.
[0025] [4] The curable resin composition according to any one of [1] to [3], wherein the solid content of the curable resin composition contains 45% by mass or more of the polyether polyol resin.
[0026] [5] The curable resin composition according to any one of [1] to [4], wherein A1 and A2 in the general formula (1) are groups represented by the following general formula (3).
[0027] [Chemistry 3]
[0028]
[0029] In the general formula (3), R1 may be the same as or different from each other and is a group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a halogen atom. X is a divalent group selected from a single bond, a divalent hydrocarbon group having 1 to 7 carbon atoms, a divalent organic group having a cyclohexane ring structure or a trimethylcyclohexane ring structure, -O-, -S-, -SO2-, and -C(O)-. Among them, X of at least one of A1 and A2 is a divalent group having a cyclohexane ring structure or a trimethylcyclohexane ring structure.
[0030] [6] The curable resin composition according to any one of [1] to [5], wherein the aromatic structure is a benzene ring structure, and the alicyclic structure is a cyclohexane ring structure or a trimethylcyclohexane ring structure.
[0031] [7] A method for producing a curable resin composition, which is the method for producing a curable resin composition according to any one of [1] to [6], comprising: reacting a bifunctional epoxy resin with bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane to produce the polyether polyol resin.
[0032] [8] A cured product obtained by curing the curable resin composition according to any one of [1] to [7].
[0033] [9] A sheet-like formed body comprising the cured product described in [8].
[0034]
[10] The sheet-like molded article according to [9], wherein Tg is 140° C. or higher.
[0035] Effects of the Invention
[0036] According to the present invention, a curable resin composition, a cured product obtained by curing the curable resin composition, and a sheet-like molded body are provided. The curable resin composition has excellent heat resistance and also has excellent balanced bending resistance, and can be applied to various fields requiring heat resistance and toughness, especially electrical / electronic fields such as various interfaces of sensors and displays, among which the curable resin composition is most suitable as a material for a film used in foldable OLED displays that have been rapidly developed in recent years.
[0037] The curable resin composition of the present invention, its cured product, and the sheet-like molded article including the cured product can be suitably used as optical materials in addition to insulating materials, sealing materials, substrates, etc. of electric / electronic parts. DETAILED DESCRIPTION
[0038] Hereinafter, embodiments of the present invention will be described in detail.
[0039] In the present invention, "solid content" refers to the content after removing the solvent, and includes not only solid epoxy resin but also semi-solid or viscous liquid.
[0040] The “total epoxy resin components” refers to the total of the polyether polyol resin of the present invention shown below, the trifunctional or higher-functional epoxy resin, and other epoxy compounds described below.
[0041] In the present invention, "sheet" and "film" have the same meaning. Among sheets, those with relatively thin thickness are called films, and sheets include films.
[0042] The sheet-like formed article of the present invention includes a film-like formed article.
[0043] [1] Curable resin composition
[0044] The curable resin composition of the present invention is characterized by comprising: a polyether polyol resin represented by the following general formula (1) having an epoxy equivalent of 7,000 g / equivalent to 100,000 g / equivalent (hereinafter sometimes referred to as "the polyether polyol resin of the present invention"), a trifunctional or higher epoxy resin, and an epoxy resin curing agent.
[0045] [Chemistry 4]
[0046]
[0047] In the general formula (1), n is an integer greater than 1. A1 and A2 may be the same or different from each other and are divalent organic groups having an aromatic structure and / or an alicyclic structure. Among them, either A1 or A2 contains an aromatic ring structure and an alicyclic ring structure. B is a hydrogen atom or a group represented by the following formula (2). At least one of the two Bs is a group represented by the following formula (2).
[0048] [Chemistry 5]
[0049]
[0050] [1-1] Polyether polyol resin
[0051] The polyether polyol resin of the present invention is represented by the above-mentioned general formula (1). From the viewpoint of heat resistance, A1 and A2 in the general formula (1) are preferably groups represented by the following general formula (3).
[0052] [Chemistry 6]
[0053]
[0054] In the general formula (3), R1 may be the same as or different from each other and is a group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, or a halogen atom. X is a divalent group selected from a single bond, a divalent hydrocarbon group having 1 to 7 carbon atoms, a divalent organic group having a cyclohexane ring structure or a trimethylcyclohexane ring structure, -O-, -S-, -SO2-, and -C(O)-. Among them, X in at least one of A1 and A2 is a divalent group having a cyclohexane ring structure or a trimethylcyclohexane ring structure.
[0055] In the general formula (3), X is particularly preferably a trimethylcyclohexane ring structure. R1 is preferably a group selected from a hydrogen atom, a hydrocarbon group having 1 to 2 carbon atoms, or a halogen atom.
[0056] The polyether polyol resin of the present invention is represented by the general formula (1), and preferably contains 35% to 55% by mass of an aromatic structure and 8% to 25% by mass of an alicyclic structure in the main chain. The content of the aromatic structure is more preferably 40% to 50% by mass. The content of the alicyclic structure is more preferably 10% to 20% by mass.
[0057] From the viewpoint of heat resistance and hygroscopicity, the aromatic structure contained in the main chain of the polyether polyol resin of the present invention is preferably a benzene ring structure, and the alicyclic structure is a cyclohexane ring structure or a trimethylcyclohexane ring structure. The alicyclic structure may include both a cyclohexane ring structure and a trimethylcyclohexane ring structure.
[0058] The molecular weight of the polyether polyol resin is preferably a predetermined value or more suitable for film formation and a predetermined value or less excellent in operability without being too high in viscosity. From the perspectives of both film formation and the operability of the resin, the number average molecular weight of the polyether polyol resin of the present invention is preferably in the range of 9,000 to 40,000, and particularly preferably in the range of 9,000 to 30,000.
[0059] The polyether polyol resin of the present invention may adopt a chemical form that has an epoxy terminal (B is a glycidyl group represented by formula (2)) as an essential component and contains a phenol terminal (B is a hydrogen atom). For the purpose of curing reaction, the polyether polyol resin of the present invention must have an epoxy group. The epoxy equivalent of the polyether polyol resin of the present invention is 7,000 g / equivalent to 100,000 g / equivalent.
[0060] When the epoxy equivalent is less than 7,000 g / equivalent, the reactivity is sufficient, but the molecular weight becomes too low for the polyether polyol resin, and film formation cannot be obtained. When the epoxy equivalent exceeds 100,000 g / equivalent, the epoxy group almost disappears, so curing reactivity cannot be expected substantially. The epoxy equivalent of the polyether polyol resin of the present invention is particularly preferably 7,000 g / equivalent to 30,000 g / equivalent.
[0061] The number average molecular weight (Mn) of the polyether polyol resin of the present invention is a value in terms of polystyrene measured by gel permeation chromatography.
[0062] In the present invention, “epoxy equivalent” is defined as “the mass of an epoxy resin containing 1 equivalent of epoxy groups” and can be measured in accordance with JIS K7236.
[0063] The polyether polyol resin of the present invention can be produced by a common method for producing polyether polyol resins. The polyether polyol resin of the present invention can be obtained, for example, by combining a dihydric phenol compound having an aromatic structure and an alicyclic structure with a bifunctional epoxy resin and subjecting the resultant to a heating addition reaction in the presence of a catalyst.
[0064] The diphenol compound used is not particularly limited as long as it has an aromatic structure and an alicyclic structure, and preferably 1,1-bis(4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, etc. can be used. Among them, bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane is particularly preferred. The bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane used may have a purity of 96% or more, particularly 98% or more. When the purity of bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane is less than 96%, it is sometimes impossible to fully achieve a high molecular weight.
[0065] As the raw material diphenol compound, other diphenol compounds can be used together with the diphenol compound having an aromatic structure and an alicyclic structure. In this case, as other diphenol compounds, any compound can be used as long as two hydroxyl groups are bonded to the aromatic ring. For example, bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, biphenol, catechol, resorcinol, hydroquinone, dihydroxynaphthalene, etc. can be listed. In addition, substances formed by substitution of these compounds with non-interfering substituents such as alkyl, aryl, ether, ester, etc. can also be used. Among these diphenol compounds, bisphenol A, bisphenol F, bisphenol S, 4,4'-biphenol, and 3,3',5,5'-tetramethyl-4,4'-biphenol are preferred.
[0066] The other dihydric phenol compounds may be used alone or in combination of two or more.
[0067] When other diphenol compounds are used in combination, their usage is preferably 30% by mass or less of all diphenol compounds used as raw materials, that is, 70% to 100% by mass of the raw material diphenol compounds are diphenol compounds having an aromatic structure and an alicyclic structure.
[0068] The raw material bifunctional epoxy resin may be any compound as long as it is a compound having two epoxy groups in the molecule, and examples thereof include bisphenol-type epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin, biphenol-type epoxy resins, alicyclic epoxy resins, diglycidyl ethers of monocyclic dihydric phenols such as catechol, resorcinol, and hydroquinone, diglycidyl ethers of dihydroxynaphthalene, diglycidyl ethers of diols, and diglycidyl esters of dicarboxylic acids such as phthalic acid, isophthalic acid, tetrahydrophthalic acid, and hexahydrophthalic acid. Furthermore, those obtained by substituting these compounds with non-interfering substituents such as alkyl groups, aryl groups, ether groups, and ester groups may also be used.
[0069] Among these bifunctional epoxy resins, epoxy resins obtained by a condensation reaction of bisphenol A, bisphenol F, bisphenol S, bisphenol AF, hydrogenated bisphenol A, 4,4′-biphenol, 3,3′,5,5′-tetramethyl-4,4′-biphenol and epihalohydrin are preferred.
[0070] These raw material bifunctional epoxy resins may be used alone or in combination of two or more.
[0071] The equivalent ratio of the bifunctional epoxy resin and the divalent phenol compound in the reaction is preferably set to epoxy group:phenolic hydroxyl group = 1: 0.90 to 1.10. If the equivalent ratio is less than 0.90 or greater than 1.10, the molecular weight may not be sufficiently increased.
[0072] Although it depends on the reaction conditions, etc., when the epoxy group:phenolic hydroxyl group ratio is less than 1:1, the probability of the terminal being an epoxy group becomes high, and when the epoxy group:phenolic hydroxyl group ratio is greater than 1:1, the probability of the terminal being a phenolic hydroxyl group becomes high.
[0073] The catalyst used in the production of the polyether polyol resin of the present invention may be any compound as long as it has a catalytic ability to promote the reaction between epoxy groups and phenolic hydroxyl groups, alcoholic hydroxyl groups or carboxyl groups, for example, alkali metal compounds, organic phosphorus compounds, tertiary amines, quaternary ammonium salts, cyclic amines, imidazoles, etc.
[0074] Specific examples of alkali metal compounds include alkali metal hydroxides such as sodium hydroxide, lithium hydroxide, and potassium hydroxide; alkali metal salts such as sodium carbonate, sodium bicarbonate, sodium chloride, lithium chloride, and potassium chloride; alkali metal alcoholates such as sodium methoxide and sodium ethoxide; alkali metal phenolates; alkali metal hydrides such as sodium hydride and lithium hydride; and alkali metal salts of organic acids such as sodium acetate and sodium stearate.
[0075] Specific examples of the organophosphorus compound include tri-n-propylphosphine, tri-n-butylphosphine, triphenylphosphine, tetramethylphosphonium bromide, tetramethylphosphonium iodide, tetramethylphosphonium hydroxide, trimethylcyclohexylphosphonium chloride, trimethylcyclohexylphosphonium bromide, trimethylbenzylphosphonium chloride, trimethylbenzylphosphonium bromide, tetraphenylphosphonium bromide, triphenylmethylphosphonium bromide, triphenylmethylphosphonium iodide, triphenylethylphosphonium chloride, triphenylethylphosphonium bromide, triphenylethylphosphonium iodide, triphenylbenzylphosphonium chloride, and triphenylbenzylphosphonium bromide.
[0076] Specific examples of the tertiary amine include triethylamine, tri-n-propylamine, tri-n-butylamine, triethanolamine, and benzyldimethylamine.
[0077] Specific examples of the quaternary ammonium salt include tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium hydroxide, triethylmethylammonium chloride, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium iodide, tetrapropylammonium bromide, tetrapropylammonium hydroxide, tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium iodide, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylammonium hydroxide, benzyltributylammonium chloride, and phenyltrimethylammonium chloride.
[0078] Specific examples of imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole.
[0079] Specific examples of the cyclic amines include 1,8-diazabicyclo(5,4,0)undec-7-ene and 1,5-diazabicyclo(4,3,0)non-5-ene.
[0080] These catalysts may be used alone or in combination of two or more.
[0081] The amount of the catalyst used is usually 0.001 wt% to 1 wt% in the reaction solid component. When the amount of the catalyst used is less than 0.001 wt%, it is difficult to achieve high molecular weight. When the amount of the catalyst used is greater than 1 wt%, there is a risk of gelation. The reaction solid component refers to the total amount of the reaction matrix other than the solvent in the reaction system.
[0082] In the process of the synthesis reaction when manufacturing the polyether polyol resin of the present invention, a solvent can be used. As the solvent, any solvent can be used as long as it dissolves the polyether polyol resin. For example, aromatic solvents, ketone solvents, amide solvents, glycol ether solvents, etc. can be listed.
[0083] Specific examples of aromatic solvents include benzene, toluene, xylene, etc. Specific examples of ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, 4-heptanone, 2-octanone, cyclohexanone, acetylacetone, dioxane, etc.
[0084] Specific examples of the amide solvent include formamide, N-methylformamide, N,N-dimethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, 2-pyrrolidone, and N-methylpyrrolidone.
[0085] Specific examples of the glycol ether-based solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol mono-n-butyl ether, and propylene glycol monomethyl ether acetate.
[0086] These solvents may be used alone or in combination of two or more.
[0087] The solvent is preferably used to make the solid content concentration of the reaction system in the synthesis reaction during the manufacture of the polyether polyol resin be 35% to 95% by mass. When a highly viscous product is produced during the reaction, the solvent can be added to continue the reaction. After the reaction is completed, the solvent can be removed as needed or further added.
[0088] The polymerization reaction during the production of the polyether polyol resin of the present invention is carried out at a reaction temperature that does not decompose the catalyst used. The reaction temperature is preferably 50° C. to 230° C., more preferably 120° C. to 200° C. When a low boiling point solvent such as acetone or methyl ethyl ketone is used, the reaction temperature can be ensured by using an autoclave to carry out the reaction under high pressure.
[0089] The polyether polyol resin of the present invention can also be used after its epoxy group or hydroxyl group is modified by other compounds. For example, acrylic acid or methacrylic acid is used as a modifier and is added to a part of the epoxy group to modify it, or an isocyanate compound is added to the hydroxyl group to modify it.
[0090] The curable resin composition of the present invention may contain only one kind of the polyether polyol resin of the present invention, or may contain two or more kinds of polyether polyol resins having different organic groups and the like in the general formula (1).
[0091] The curable resin composition of the present invention preferably contains 45% or more of the polyether polyol resin of the present invention in the solid content of the curable resin composition of the present invention. If the content of the polyether polyol resin of the present invention is less than 45% by mass, it is sometimes impossible to fully obtain the film forming properties and bending resistance of the film by using the polyether polyol resin of the present invention. However, from the perspective of obtaining a good cured product by ensuring the preferred content of the trifunctional or higher epoxy resin or the preferred content of the epoxy resin curing agent described later, the content of the polyether polyol resin of the present invention in the curable resin composition of the present invention is preferably 99% by mass or less relative to the solid content. The content of the polyether polyol resin of the present invention is particularly preferably 50% to 99% by mass, and particularly preferably 60% to 97% by mass relative to the solid content in the curable resin composition of the present invention.
[0092] [1-2] Epoxy resins with three or more functional groups
[0093] The epoxy resin used together with the polyether polyol resin of the present invention is a trifunctional or higher epoxy resin, for example, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, dicyclopentadiene phenol type epoxy resin, terpene phenol type epoxy resin, phenol aralkyl type epoxy resin, biphenyl aralkyl type epoxy resin, naphthol novolac type epoxy resin, triglycidylaminophenol type epoxy resin, tetraglycidyl diamino diphenylmethane type epoxy resin, etc. can be used. , glycidyl ether type epoxy resins such as trisphenol methane epoxy resins and tetraphenol ethane epoxy resins, heterocyclic epoxy resins such as triglycidyl isocyanurate, polyphenol resins obtained by condensation reaction with various aldehydes such as hydroxybenzaldehyde, crotonaldehyde, glyoxal, etc., epoxy resins made from various phenol compounds and epihalohydrins such as modified phenol resins obtained by condensing petroleum-based heavy oils or asphalts, formaldehyde polymers and phenols in the presence of an acid catalyst, and various epoxy resins such as straight-chain aliphatic epoxy resins and alicyclic epoxy resins.
[0094] Among these, from the viewpoint of heat resistance, bisphenol A novolac epoxy resin, trisphenol methane epoxy resin, and tetrakisphenol ethane epoxy resin are preferred, and trisphenol methane epoxy resin and tetrakisphenol ethane epoxy resin are particularly preferred.
[0095] The curable resin composition of the present invention may contain only one of these trifunctional or higher-functional epoxy resins, or may contain two or more of them.
[0096] The curable resin composition of the present invention preferably contains 1% to 54% by mass, particularly 2% to 50% by mass of a trifunctional or higher epoxy resin relative to the solid content. The curable resin composition of the present invention preferably contains 1% to 55% by mass, particularly 3% to 50% by mass of a trifunctional or higher epoxy resin relative to 100% by mass of the total of the polyether polyol resin of the present invention and the trifunctional or higher epoxy resin.
[0097] By setting the content of the trifunctional or higher epoxy resin to be equal to or greater than the lower limit, the effect of improving heat resistance brought about by using the trifunctional or higher epoxy resin in combination with the polyether polyol resin of the present invention can be sufficiently obtained. By setting the content of the trifunctional or higher epoxy resin to be equal to or less than the upper limit, the content of the polyether polyol resin of the present invention is sufficient, and the original heat resistance and bending resistance effects of the polyether polyol resin can be sufficiently obtained.
[0098] [1-3] Epoxy resin curing agent
[0099] In the present invention, the epoxy resin curing agent refers to a substance that contributes to the cross-linking reaction and / or chain growth reaction between epoxy groups of the epoxy resin. In the present invention, even a substance commonly referred to as a "curing accelerator" is regarded as a curing agent as long as it contributes to the cross-linking reaction and / or chain growth reaction between epoxy groups of the epoxy resin.
[0100] The epoxy resin curing agent used in the present invention is not particularly limited, and examples thereof include polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, cationic polymerization initiators, and organic phosphines.
[0101] Among these, polyfunctional phenols and imidazole compounds are preferred from the viewpoint of pot life, and imidazole compounds are most preferred.
[0102] Examples of the polyfunctional phenols include bisphenol A, bisphenol F, 4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenyl ether, 1,4-bis(4-hydroxyphenoxy)benzene, 1,3-bis(4-hydroxyphenoxy)benzene, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, phenol novolac, bisphenol A novolac, o-cresol novolac, m-cresol novolac, p-cresol novolac, xylenol novolac, polyparahydroxystyrene, hydroquinone, resorcinol, catechol, Tert-butylcatechol, tert-butylhydroquinone, pyrogallol, pyrogallol, tert-butylpyrogallol, allylated pyrogallol, polyallylated pyrogallol, 1,2,4-pyrogallol, 2,3,4-trihydroxybenzophenone, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,4-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,8-dihydroxynaphthalene, allylated or polyallylated products of the dihydroxynaphthalenes, allylated bisphenol A, allylated bisphenol F, allylated phenol novolac, allylated pyrogallol, and the like.
[0103] Examples of the imidazole compound include 2-phenylimidazole, 2-ethyl-4(5)-methylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl] -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resins and the above-mentioned imidazoles, etc.
[0104] These epoxy resin curing agents may be used alone or in combination of two or more.
[0105] The content of the epoxy resin curing agent in the curable resin composition of the present invention is preferably 0.1 to 100 parts by mass, more preferably 80 parts by mass or less, further preferably 60 parts by mass or less, and particularly preferably 40 parts by mass or less, relative to 100 parts by mass of all epoxy resin components as solid components in the curable resin composition of the present invention. If the content of the epoxy resin curing agent is within the above range, it is not easy to leave unreacted epoxy groups or functional groups of the curing agent, so it is preferred.
[0106] [1-4] Other epoxy compounds
[0107] The curable resin composition of the present invention may contain other epoxy compounds other than the polyether polyol resin of the present invention and the trifunctional or higher epoxy resin. As other epoxy compounds, bifunctional epoxy resins, for example, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, biphenyl epoxy resin, glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, heterocyclic epoxy resin, etc., one or more of various epoxy resins.
[0108] When the curable resin composition of the present invention contains other epoxy compounds other than the polyether polyol resin of the present invention and the trifunctional or higher epoxy resin, the content of the other epoxy compounds is preferably 90% by mass or less, and more preferably 70% by mass or less relative to the total epoxy resin components as solid components in the curable resin composition of the present invention. By containing other epoxy compounds, the effects of improving physical properties such as water absorption and transparency can be obtained, but if the content is too much, there is a risk of damaging the effects of improving heat resistance and bending resistance brought about by the polyether polyol resin of the present invention and the trifunctional or higher epoxy resin.
[0109] [1-5] Solvent
[0110] In the curable resin composition of the present invention, in order to appropriately adjust the viscosity of the curable resin composition during the operation such as when forming a coating film, a solvent can be mixed for dilution. In the curable resin composition of the present invention, the solvent is used to ensure the operability and workability in the forming of the curable resin composition, and its usage amount is not particularly limited. In the present invention, the term "solvent" and the term "solvent" are used differently according to their usage, but the same word or different words may be used independently.
[0111] Examples of the solvent that may be contained in the curable resin composition of the present invention include acetone, methyl ethyl ketone, toluene, xylene, methyl isobutyl ketone, ethyl acetate, butyl acetate, propyl acetate, cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, etc. These solvents may be used as a mixed solvent of two or more thereof as appropriate.
[0112] [1-6] Other ingredients
[0113] The curable resin composition of the present invention may contain other components in addition to the components listed above. Other components may be used in appropriate combination according to the desired physical properties of the curable resin composition.
[0114] For example, in order to improve various properties such as the effect of reducing the cure shrinkage of the obtained cured product and the effect of reducing the thermal expansion coefficient, an inorganic filler is mixed into the curable resin composition of the present invention, thereby achieving expanded applications in the electrical / electronic fields, especially in liquid semiconductor sealing materials.
[0115] In order to impart toughness, an organic filler such as rubber particles or acrylic particles may be mixed into the curable resin composition of the present invention.
[0116] Examples of the inorganic filler include powdered reinforcing materials or filling materials, for example, metal oxides such as aluminum oxide and magnesium oxide, metal carbonates such as calcium carbonate and magnesium carbonate, diatomaceous earth powder, basic magnesium silicate, calcined clay, fine powdered silica, fused silica, silicon compounds such as crystalline silica, metal hydroxides such as aluminum hydroxide, kaolin, mica, quartz powder, graphite, molybdenum disulfide, etc.
[0117] The inorganic filler may be generally mixed in an amount of 10 to 900 parts by mass with respect to 100 parts by mass of the total of the epoxy resin component and the epoxy resin curing agent as solid contents.
[0118] Furthermore, a fibrous reinforcing material or a filling material may also be mixed. Examples of fibrous reinforcing materials or filling materials include glass fibers, ceramic fibers, carbon fibers, aluminum oxide fibers, silicon carbide fibers, boron fibers, etc. Furthermore, organic fibers or inorganic fibers may also be used as cloth or nonwoven fabrics.
[0119] The surfaces of these inorganic fillers, fibers, cloths, and nonwoven fabrics may be subjected to surface treatment such as treatment with a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, or primer treatment.
[0120] The curable resin composition of the present invention may contain the following components (1) and (2) as needed.
[0121] (1) Coupling agents, plasticizers, diluents, flexibility-imparting agents, dispersants, wetting agents, colorants, pigments, ultraviolet light absorbers, light stabilizers such as hindered amine light stabilizers, antioxidants, degassing agents, flow modifiers, etc. These compounds are usually mixed in an amount of 0.1 to 20 parts by mass relative to 100 parts by mass of the total of the epoxy resin component and the epoxy resin curing agent as solid components.
[0122] (2) Various curable monomers, oligomers and synthetic resins for the purpose of improving the properties of the resin in the final coating film, such as one or more of cyanate resins, acrylic resins, silicone resins and polyester resins.
[0123] When these resins are used, the mixing ratio is preferably within a range that does not impair the original properties of the curable resin composition of the present invention, that is, 50 parts by mass or less relative to 100 parts by mass of the total of the epoxy resin component and the epoxy resin curing agent as solid content.
[0124] In order to impart flame retardancy to the curable resin composition of the present invention, a non-halogen P-based, N-based, or Si-based flame retardant or the like may be added.
[0125] [2]Cured product
[0126] By curing the curable resin composition of the present invention, a cured product can be obtained. Here, "curing" means intentionally curing the epoxy resin by heat and / or light. The degree of curing can be controlled according to the desired physical properties and application.
[0127] The curing method of the curable resin composition of the present invention when curing the curable resin composition to form a cured product varies depending on the mixed components or mixed amounts in the curable resin composition and the shape of the mixture, and generally, a condition of heating at 23°C to 200°C for 5 minutes to 24 hours can be cited. In order to reduce the curing failure, the heating is preferably carried out by a secondary treatment of performing a primary heating at 23°C to 160°C for 5 minutes to 24 hours, a secondary heating at 80°C to 200°C which is 40°C to 177°C higher than the primary heating temperature for 5 minutes to 24 hours, and a tertiary treatment of performing a tertiary heating at 100°C to 200°C which is higher than the secondary heating temperature for 5 minutes to 24 hours.
[0128] When a cured product is produced in the form of a semi-cured product, the curing reaction of the curable resin composition can be carried out to a degree that the shape can be maintained by heating, etc. When the curable resin composition contains a solvent, most of the solvent is removed by heating, decompression, air drying, etc., but less than 5% by mass of the solvent may remain in the semi-cured product.
[0129] [3] Sheet-shaped molded body
[0130] The sheet-like molded article of the present invention is a sheet-like molded article including the cured product of the present invention obtained by curing the curable resin composition of the present invention.
[0131] The sheet-like molded article of the present invention can be manufactured by curing the curable resin composition of the present invention in a state adjusted to a sheet of a predetermined thickness. Alternatively, the sheet-like molded article of the present invention can be manufactured by forming a semi-cured product obtained from the curable resin composition of the present invention into a sheet of a predetermined thickness and further curing it.
[0132] The thickness of the sheet-like molded product of the present invention is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.001 mm or more, further preferably 0.01 mm or more, particularly preferably 0.02 mm or more, and particularly preferably 0.05 mm or more.
[0133] In the sheet-like molded article of the present invention, the glass transition temperature (Tg) measured in the items of the examples described later is preferably 140°C or higher. If Tg is above the lower limit, heat resistance becomes high, so it is preferred. From this viewpoint, the Tg of the sheet-like molded article of the present invention is more preferably 150°C or higher, further preferably 160°C or higher, and particularly preferably 170°C or higher.
[0134] [4] Application
[0135] The curable resin composition of the present invention provides a cured product with excellent heat resistance and excellent bending resistance, and can be used for laminated plates, sealing materials, adhesives, coatings, and electrical insulating materials. In particular, the curable resin composition of the present invention can be used for various devices requiring bending resistance for interfaces such as sensors and displays, substrates supporting them or, sealing materials for semiconductor sealing, powder coatings for electrical insulation, resist inks, casting materials for electrical / electronic parts, adhesives for electrical / electronic parts, and insulating films. The curable resin composition of the present invention is also useful as a material for the film used in the foldable OLED display being developed in recent years.
[0136] Example
[0137] Hereinafter, the present invention will be described in more detail based on the examples, but the present invention is not limited by any of the following examples. The values of various manufacturing conditions or evaluation results in the following examples have the meaning of preferred values as the upper or lower limits in the embodiments of the present invention, and the preferred range may also be the range specified by the value of the upper or lower limit and the value of the following examples or the combination of the values of the examples. Hereinafter, "parts" all represent "parts by mass".
[0138] [Various analysis / evaluation / measurement methods]
[0139] The following analysis / evaluation / measurement methods of various physical properties or characteristics are as follows.
[0140] 1) Glass transition temperature (Tg)
[0141] For the cured film of the curable resin composition, the temperature was raised to 30°C to 200°C at 10°C / min using a differential scanning calorimeter "DSC 7020" manufactured by SII Nanotech Co., Ltd. The glass transition temperature was measured based on the "midpoint glass transition temperature: Tmg" described in JIS K7121 "Determination of transition temperature of plastics". Tg less than 140°C was evaluated as ×, and 140°C or more was evaluated as 0.
[0142] 2) Transparency
[0143] The obtained cured film was measured for YI (yellowness) using a colorimeter (ZE6000 manufactured by Nippon Denshoku Industries) in accordance with ASTM D1925. A YI of less than 14 was evaluated as 0, a YI of 14 or more and less than 30 was evaluated as Δ, and a YI of 30 or more or white turbidity was evaluated as ×.
[0144] 3)Flexibility
[0145] The obtained cured film was evaluated as 0 if it was not broken even when it was bent 180°, and was evaluated as × if it could not be bent.
[0146] [Production / Evaluation of Polyether Polyol Resin and Curable Resin Composition]
[0147] <Examples 1 to 3 and Comparative Examples 1 to 3>
[0148] 100 parts of a bifunctional epoxy compound (3,3',5,5'-tetramethyl-4,4'-biphenol type epoxy resin (trade name "YX 4000" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 186 g / equivalent)) and 80.9 parts of a dihydric phenol compound (bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (hydroxy equivalent 155 g / equivalent)), 0.37 parts of tetramethylammonium hydroxide (27% by mass aqueous solution) and methyl ethyl ketone (solid content: 70% by mass) were placed in a pressure-resistant reaction vessel equipped with a stirrer and reacted at 135° C. for 8 hours under a nitrogen atmosphere. After the reaction, methyl ethyl ketone was added to adjust the solid content concentration to 40% by mass.
[0149] The polyether polyol resin thus obtained had an epoxy equivalent of 8765 g / equivalent and a number average molecular weight of 9,968.
[0150] The polyether polyol resin was analyzed by the following method.
[0151] Number average molecular weight: measured as a polystyrene-equivalent value by gel permeation chromatography.
[0152] · Epoxy equivalent: measured by potentiometric titration in accordance with JIS K7236 and converted into a value in terms of resin solid content.
[0153] Using an applicator, a curable resin composition prepared by mixing an epoxy resin, an epoxy resin curing agent, and a solvent in the polyether polyol resin was applied to a separator (polyethylene terephthalate film treated with silicone) to form a coating film, which was dried at 100°C to 120°C for 1 hour and then heat-treated at 150°C to 170°C for 1 hour to obtain a cured film of the thickness required for each evaluation. The types and amounts of the epoxy resin and epoxy resin curing agent used, as well as the properties of the cured film obtained are shown in Table 1.
[0154] The epoxy resins and epoxy resin curing agents used in Examples and Comparative Examples are as follows.
[0155] [Epoxy resin]
[0156] <Trifunctional or higher epoxy resin>
[0157] (A-1) Trisphenol methane type epoxy resin (jER1032H60 manufactured by Mitsubishi Chemical Corporation)
[0158] (A-2) Bisphenol A novolac type epoxy resin (jER157S65 manufactured by Mitsubishi Chemical Corporation)
[0159] (A-3) Phenol novolac type epoxy resin (jER154 manufactured by Mitsubishi Chemical Corporation)
[0160] <Bifunctional epoxy resin>
[0161] (A-4) Bisphenol F type epoxy resin (jER806 manufactured by Mitsubishi Chemical Corporation)
[0162] (A-5) Bisphenol A type epoxy resin (YX4000 manufactured by Mitsubishi Chemical Corporation)
[0163] [Epoxy resin curing agent]
[0164] (B-1): 2-ethyl-4(5)-methylimidazole (EMI-24 manufactured by Mitsubishi Chemical Corporation)
[0165] (B-2): Bisphenol A novolac resin (YLH129 manufactured by Mitsubishi Chemical Corporation)
[0166] [Table 1]
[0167] Table 1. Mixing conditions and evaluation results of curable resin composition
[0168]
[0169] ※In the table, "-" in the curable resin composition formula indicates that the raw material was not used.
[0170] [Evaluation results]
[0171] According to the results in Table 1, the following can be known.
[0172] The cured products of Examples 1 to 3 obtained using the curable resin composition of the present invention containing the polyether polyol resin of the present invention and a trifunctional or higher epoxy resin have superior heat resistance (Tg) compared to the cured products of Comparative Examples 1 to 3 using a bifunctional epoxy resin instead of a trifunctional or higher epoxy resin.
[0173] In particular, the trifunctional epoxy resin used in Example 1 has structural restrictions on molecular motion compared to other resins, so the Tg in Example 1 is higher, which is practically preferred.
[0174] According to the curable resin composition of Examples 1 to 3, it can be seen that: compared with the curable resin composition of Comparative Examples 1 to 3, the transparency, flexibility and heat resistance can be improved in a balanced manner, and it is suitable as a film material used in foldable OLED displays that require transparency, heat resistance and bending resistance.
[0175] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made without departing from the spirit and scope of the present invention.
[0176] This application is based on Japanese Patent Application No. 2018-194395 filed on October 15, 2018, the entirety of which is incorporated herein by reference.
Claims
1. A curable resin composition comprising: a polyether polyol resin represented by the following general formula (1) having an epoxy equivalent of 7,000 g / equivalent to 100,000 g / equivalent, a trifunctional or higher epoxy resin, and an epoxy resin curing agent; the polyether polyol resin contains 40% to 55% by mass of an aromatic structure and 8% to 25% by mass of an alicyclic structure in the main chain; and the solid content contains 45% or more of the polyether polyol resin; The trifunctional or higher epoxy resin is a triphenol methane type epoxy resin and / or a tetraphenol ethane type epoxy resin; In the general formula (1), n is an integer greater than 1; A1 and A2 may be the same or different and are groups represented by the following general formula (3); B is a hydrogen atom or a group represented by the following formula (2); at least one of the two Bs is a group represented by the following formula (2); In the general formula (3), R1 may be the same as or different from each other and is a group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms or a halogen atom; X is a single bond, a divalent hydrocarbon group having 1 to 7 carbon atoms, a divalent organic group having a cyclohexane ring structure or a trimethylcyclohexane ring structure, -O-, -S-, -SO2- and -C(O)-; wherein, X in at least one of A1 and A2 is a divalent group having a cyclohexane ring structure or a trimethylcyclohexane ring structure.
2. The curable resin composition according to claim 1, wherein The number average molecular weight of the polyether polyol resin is 9,000 to 40,000 as a value in terms of polystyrene measured by gel permeation chromatography.
3. The curable resin composition according to claim 1, wherein The aromatic structure is a benzene ring structure, and the alicyclic structure is a cyclohexane ring structure or a trimethylcyclohexane ring structure.
4. The curable resin composition according to any one of claims 1 to 3, wherein The polyether polyol resin contains 10 to 20% by mass of an alicyclic structure in the main chain.
5. A method for producing a curable resin composition, which is the method for producing a curable resin composition according to any one of claims 1 to 4, comprising: A step of reacting a bifunctional epoxy resin with bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane to produce the polyether polyol resin. 6 . A cured product obtained by curing the curable resin composition according to claim 1 .
7. A sheet-like formed body comprising the cured product according to claim 6. 8 . The sheet-like molded product according to claim 7 , which has a Tg of 140° C. or higher as measured by a differential scanning calorimeter.
Citation Information
Patent Citations
Temperature detector
JP2018194395A
Polyether polyol resin, hardenable resin composition and hardened product thereof
JP2006176658A
Epoxy resin composition
JP2010111859A
Epoxy resin, epoxy resin composition, hardened product and laminate for electric / electronic circuit
JP2014001380A