A mold and growth method for growing gallium oxide single crystal by guided mode method
Through multiple partition molds arranged in mirror symmetry and using multiple slits to supply materials to increase surface tension, the problem of growing gallium oxide single crystal thin sheets by the guided mold method is solved, and efficient production and high-quality single crystals in the thickness direction are achieved. grow.
Patent Information
- Application Number
- CN202011644809.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-12-31
AI Technical Summary
The products of the existing guided mode method for growing gallium oxide single crystals are usually thin plates, resulting in a small number of blanks that can be processed at one time and low production efficiency.
Design a multi-part separator mold arranged in mirror symmetry. There are slits between two adjacent partitions. Materials are fed through multiple slits to increase surface tension, ensure the stable rise and growth of the gallium oxide melt, and achieve thickness Efficient production in the direction.
Feeding through multiple slits increases the amount of gallium oxide melt supplied per unit time, ensures the growth of single crystals with a thickness of more than 10 mm, improves production efficiency, and reduces the temperature difference at the crystallization interface, improving single crystal quality. crystal quality.
Smart Images

Figure CN112831832B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of crystal growth equipment, and in particular to a mold and a growth method for growing a gallium oxide single crystal using a guided mold method. Background Art
[0002] The monoclinic gallium oxide (β-Ga2O3) crystal is a new type of direct bandgap ultra-wide bandgap semiconductor. Its bandgap width is about 4.9eV and its breakdown voltage is as high as 8MV / cm, which is more than 20 times that of Si and more than 2 times that of SiC and GaN. 3 , relative to Si) is as high as 3214.1, which is about 10 times that of SiC and 4 times that of GaN. This shows that the devices developed using β-Ga2O3 have smaller conduction losses and higher power conversion efficiency, and are expected to have good applications in high-voltage and high-power devices.
[0003] At present, gallium oxide single crystals are the only new generation wide bandgap semiconductors that can be grown by melt method. Large-sized single crystals can be prepared at low cost and high quality by standard single crystal preparation techniques such as floating zone method, descent method, Czochralski method, guided mold method, etc. Among them, the guided mold method for growing gallium oxide single crystals is the most promising growth method at present because it is easier to control the volatilization of gallium oxide raw materials in the growth of large-sized gallium oxide due to the introduction of mold limitation and crucible sealing.
[0004] However, the gallium oxide single crystals grown by the existing guided mold method are generally relatively thin plates, which means that the number of processable blanks in the thickness direction of the single crystals grown by this method is small, and the single-time output efficiency of columnar single crystals is low compared to the pulling method, the descending method, etc.
[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a mold and a growth method for growing gallium oxide single crystals by a guided mold method, aiming to solve the problem that the currently grown gallium oxide single crystals are relatively thin plates, and the number of blanks that can be processed at one time is small, resulting in low production efficiency.
[0007] The technical solution of the present invention is as follows:
[0008] A mold for growing gallium oxide single crystals using a guided mold method, wherein the mold comprises a plurality of partitions arranged in mirror symmetry, the plurality of partitions being fixed together by a fixing portion, and a slit being provided between two adjacent partitions; wherein the plurality of partitions refers to more than three.
[0009] Optionally, the plurality of partitions are fixed together by a plurality of rivets, and a coil is wound around the rivets between two adjacent partitions or an annular gasket is sleeved thereon, and the coil or annular gasket is used to control the width of the slit. Further optionally, the coil is an iridium wire coil or an iridium-containing alloy coil. Further optionally, the annular gasket is an annular iridium gasket or an annular iridium alloy gasket.
[0010] Optionally, the width of the slit between two adjacent partitions is 0.1-0.5 mm.
[0011] Further optionally, the widths of any two slits are the same.
[0012] Optionally, the ratio of the thickness of any single partition to the width of any slit is 2:1-20:1.
[0013] Optionally, among the plurality of partitions, except for the two outermost partitions, the remaining partitions have the same thickness.
[0014] Optionally, among the multiple partitions, any two partitions have the same thickness.
[0015] Optionally, two adjacent partitions are fixed by welding.
[0016] Optionally, a notch is provided at the bottom end of each partition plate for allowing the raw material to flow into the slit.
[0017] Optionally, each separator is an iridium separator or an alloy separator containing iridium.
[0018] A method for growing a gallium oxide single crystal, wherein the mold of the present invention is placed in a crucible filled with a gallium oxide raw material, the crucible is heated, and the crystal is grown to obtain a thick gallium oxide single crystal.
[0019] Optionally, the gallium oxide single crystal has a thickness of more than 10 mm.
[0020] Beneficial effects: The present invention provides a mold for growing gallium oxide single crystals by a guided mold method, and more importantly, provides a mold suitable for growing thick gallium oxide single crystals. In this embodiment, the mold has multiple partitions arranged in a mirror-symmetrical manner, and there is a slit between two adjacent partitions, so that a mold with multiple slits is obtained, and the gallium oxide melt can rise to the top of the mold in parallel through the multiple slits. Since the surface tension is proportional to the length of the slits, multiple slits can increase the total surface tension by multiple times, so that the growth of thick gallium oxide single crystals remains stable, so that thicker wafers can be grown, so that a large number of blanks can be processed at one time in the thickness direction, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1A three-dimensional view of the mold assembled with four partitions.
[0022] Figure 2 for Figure 1 Side view of the mold in the thickness direction.
[0023] Figure 3 for Figure 1 Side view of the mold with steps on the two outer partitions.
[0024] Figure 4 This is a flow chart of processing a blank from a crystal blank in Example 1.
[0025] Figure 5 Side view of the mold assembled with eight baffles.
[0026] Figure 6 Top view of the mold assembled with eight partitions.
[0027] Figure 7 This is a flow chart of processing a blank from a crystal blank in Example 2. DETAILED DESCRIPTION
[0028] The present invention provides a mold and a growth method for growing gallium oxide single crystals by a guided mode method. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] The growth principle of the guided mold method: a mold with a slit is placed into a crucible filled with raw material melt. The melt in the crucible rises to the top of the mold along the slit due to capillary action. The seed crystal is then brought into contact with the liquid surface at the top of the mold. After the end of the seed crystal is melted, it merges with the melt at the top of the mold, and then is slowly pulled upward, followed by processes such as necking and shouldering, and finally the desired crystal grows with equal diameter. In this process, the surface tension of the melt provides the power for the capillary rise of the melt and maintains the meniscus liquid film between the mold and the crystal, ensuring the continuity and stability of the crystallization process. For thicker crystal growth, the total amount of melt that needs to be pulled upward by capillary action per unit time is greater, and the demand for surface tension is greater.
[0030] In the current technology of growing gallium oxide crystals by guided mold method, the mold is only opened with a narrow slit, and a single slit feeding method is adopted. If the thickness of the wafer exceeds 10mm, there will be problems such as uneven crystal thickness or difficulty in shoulder placement, which seriously affects the crystal growth speed and quality. Therefore, gallium oxide crystals grown by existing single slit molds are generally difficult to exceed 10mm in thickness.
[0031] Based on this, an embodiment of the present invention provides a mold for growing gallium oxide single crystals by a guided mode method, such as Figure 1As shown, the mold includes a plurality of partitions 1 ( Figure 1 Taking the mold consisting of four partitions as an example, the multiple partitions 1 are fixed together by a fixing part, and there is a slit 2 between two adjacent partitions 1; wherein the multiple partitions refer to more than 3 partitions. The multiple partitions can be three, four, five, six, seven or eight, but are not limited thereto, and can be determined according to actual needs.
[0032] In this embodiment, the mold is mainly assembled from a plurality of partitions arranged in mirror symmetry, and a slit is provided between two adjacent partitions, so that a mold with a plurality of slits is obtained, and the gallium oxide melt can rise to the top of the mold through the plurality of slits in parallel. Since the surface tension is proportional to the length of the slits, the plurality of slits can increase the total surface tension by multiples, so that the total amount of the gallium oxide melt pulled upward by capillary action per unit time is increased by multiples, thereby ensuring the continuity and stability of the growth process of thick-sized gallium oxide single crystals, thereby growing thicker wafers, and increasing the number of blanks that can be processed at one time in the thickness direction, thereby improving production efficiency.
[0033] In one embodiment, the plurality of partitions are fixed together through a plurality of rivets, and a coil is wound around the rivet between two adjacent partitions or a ring-shaped gasket is sleeved thereon, and the coil or the ring-shaped gasket is used to control the width of the slit. Furthermore, the coil is an iridium wire coil or an iridium-containing alloy coil. Furthermore, the ring-shaped gasket is an annular iridium gasket or an annular iridium-containing alloy gasket. The iridium-containing alloy may be an iridium-rhodium alloy or an iridium-platinum alloy. The coil or the ring-shaped gasket is used to separate the partitions so that a slit is formed between two adjacent partitions, and can be used to control the width of the slit. Some of the plurality of rivets may be two, three, four or five, etc., but are not limited thereto. The number of rivets may be determined specifically according to the actual width of the partition.
[0034] Combination Figure 1 As shown, with four partitions 1, six rivets ( Figure 1The rivet in the middle is not shown, and 3 is a through hole) as an example to introduce the fixing of the partition by rivets. The four partitions are: the first partition, the second partition, the third partition and the fourth partition, and the six rivets are: the first rivet, the second rivet, the third rivet, the fourth rivet, the fifth rivet and the sixth rivet. The first partition is provided with two rows of first through holes, second through holes, third through holes, fourth through holes, fifth through holes and sixth through holes symmetrically arranged in the width direction, the second partition is provided with a seventh through hole corresponding to the first through hole, an eighth through hole corresponding to the second through hole, a ninth through hole corresponding to the third through hole, a tenth through hole corresponding to the fourth through hole, an eleventh through hole corresponding to the fifth through hole, and a twelfth through hole corresponding to the sixth through hole, and so on, the third partition is provided with a through hole corresponding to the second partition, and the fourth partition is provided with a through hole corresponding to the third partition, wherein the first rivet passes through the first through hole and extends to the corresponding through hole on the second partition, the corresponding through hole on the third partition and the corresponding through hole on the fourth partition in sequence, and the second rivet passes through the first through hole and extends to the corresponding through hole on the second partition, the corresponding through hole on the third partition and the corresponding through hole on the fourth partition in sequence, and the second rivet passes through the second through hole and extends to the corresponding through hole on the second partition, the corresponding through hole on the third partition and the corresponding through hole on the fourth partition in sequence. The fourth rivet passes through the fourth through hole and extends to the corresponding through hole on the second partition, the corresponding through hole on the third partition and the corresponding through hole on the fourth partition in sequence. The fifth rivet passes through the fifth through hole and extends to the corresponding through hole on the second partition, the corresponding through hole on the third partition and the corresponding through hole on the fourth partition in sequence. The sixth rivet passes through the sixth through hole and extends to the corresponding through hole on the second partition, the corresponding through hole on the third partition and the corresponding through hole on the fourth partition in sequence. The four partitions are fixed together by six rivets.
[0035] In one embodiment, the width of the slit between two adjacent partitions is 0.1-0.5 mm. In other words, the width of any slit is within the range of 0.1-0.5 mm.
[0036] Further, in one embodiment, the widths of any two slits are the same. That is, the width of each slit is the same. For example, the widths of any two slits may be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm or 0.5 mm. The slits are used to feed by capillary action, and the widths of the slits are the same, which can ensure that the overall feeding capacity and feeding speed are relatively stable, thereby ensuring uniform growth of the single crystal.
[0037] In one embodiment, the ratio of the thickness of any single partition to the width of any slit is 2: 1-20: 1. If the partition is too thin, it is not conducive to processing; if the partition is too thick, the slit is narrower than the partition, which easily leads to insufficient feeding.
[0038] In one embodiment, among the plurality of partitions, except for the two outermost partitions, the remaining partitions have the same thickness, which can ensure that the overall feeding capacity and feeding speed are relatively stable, thereby ensuring uniform growth of the single crystal.
[0039] In one embodiment, any two of the plurality of partitions have the same thickness, which can further ensure the uniformity of single crystal growth.
[0040] In one embodiment, two adjacent partitions are fixed by welding, which can be done by directly welding the two adjacent partitions or by welding the two adjacent partitions through a thin iridium plate, in order to enhance the stability between the partitions and prevent the partitions from shifting during use.
[0041] In one embodiment, each partition has a notch at the bottom for raw materials to flow into the slit, which can effectively ensure that the gallium oxide melt in the crucible flows into the slit through the notch. Furthermore, the number of notches at the bottom of each partition may be one, two, three or four, etc., without limitation thereto.
[0042] In one embodiment, each partition is made of a precious metal material that is resistant to oxidation at high temperatures, such as an iridium partition or an iridium-containing alloy partition. The iridium-containing alloy may be an iridium-rhodium alloy or an iridium-platinum alloy.
[0043] In one embodiment, the outermost two partitions of the plurality of partitions are provided with steps 5 on the outer sides of the top ends of the two partitions and along the width direction. Figure 3 The step is used to place a sealing cover, which is used to seal the upper end of the crucible except for the mold opening to prevent the high-temperature gallium oxide melt from evaporating from the crucible and adhering to the components outside the crucible.
[0044] In one embodiment, along the thickness direction of the partition, the top end formed by the plurality of partitions is configured as a curved surface or inclined surface with a high outer side and a low center in a centrally symmetrical manner. Figure 2 As shown, Figure 2 The medium thick black line 4 is an iridium pin for penetrating and fixing. That is, the top end is set as a concave curved surface symmetrical with the center, or the top end is set as a concave inclined surface symmetrical with the center.
[0045] Since the temperature distribution of the mold top is: the temperature is higher towards the outside and lower towards the top, the present embodiment sets the existing horizontal top structure to a curved top structure or an inclined top structure, so that the temperature of the outer partition is always slightly higher than the temperature of the inner partition, reducing the temperature difference of the crystal interface in the thickness direction, thereby improving the quality of the gallium oxide single crystal.
[0046] Further in one embodiment, the angle between the tangent line at any point of the curved surface and the horizontal direction is between 0° and 30°;
[0047] Alternatively, the angle between the inclined surface and the horizontal direction is between 0° and 30°.
[0048] In this embodiment, the curved surface or inclined surface is too steep, which is not conducive to feeding, because the maximum height to which the raw material rises in the slit is inversely proportional to the width of the slit. If it is too steep, the slit becomes wider as it goes up, and it is not easy to spread the raw material. 0° is equivalent to horizontal, and the raw material is sucked up and directly spreads on the surface.
[0049] Further in one embodiment, the height difference between the highest point and the lowest point on the curved surface is ≤2 mm;
[0050] Alternatively, the height difference between the highest point and the lowest point on the inclined surface is ≤2 mm, so as to ensure that the raw material continues to rise to the top of the mold.
[0051] An embodiment of the present invention provides a method for growing a gallium oxide single crystal, wherein the mold described in the embodiment of the present invention is placed in a crucible filled with a gallium oxide raw material, the crucible is heated, and the crystal is grown to obtain a thick gallium oxide single crystal.
[0052] In this embodiment, the mold is a mold with multiple slits, and the gallium oxide melt can rise to the top of the mold through the multiple slits in parallel. Since the surface tension is proportional to the slit length, the multiple slits can increase the total surface tension exponentially, so that the total amount of gallium oxide melt pulled upward by capillary action per unit time is increased exponentially, ensuring the continuity and stability of the growth process of thick-sized gallium oxide single crystals, so that wafers with a thickness of more than 10 mm can be grown, and the number of blanks that can be processed at one time in the thickness direction is increased, thereby improving production efficiency.
[0053] In addition, the top structure of the mold in this embodiment can be set to a curved top structure or a sloped top structure, so that the temperature of the outer partition is always slightly higher than the temperature of the inner partition, reducing the temperature difference of the crystallization interface in the thickness direction, thereby growing high-quality gallium oxide single crystals.
[0054] The present invention will be further described below by means of specific examples.
[0055] Example 1
[0056] The mold structure of this embodiment is as follows Figure 1-2As shown, the three-slit feeding mold is composed of 4 partitions, the width of all partitions is 110mm, and there are 4 12mm×2mm feeding notches at the bottom of each partition. The thickness of each partition is 3.5mm, the width of the slit between two adjacent partitions is 0.5mm, the total thickness of the mold is 15.5mm, the height of the two outer partitions is 38-38.8mm, the height of the two inner partitions is 37.5-37.9mm, the maximum angle between the inclined surface of the mold and the horizontal plane is about arctan(0.8 / 3.5)=12.875°, and the angle between the two outermost partitions is about 154.25°.
[0057] Based on this mold, a thick gallium oxide single crystal with a width of 110 mm and a thickness of 15.5 mm was grown. Figure 4 As shown, 12 1mm blanks can be processed at one time in the thickness direction, and the growth rate ranges from 5 to 60 mm / h, which greatly improves the growth efficiency.
[0058] Example 2
[0059] The mold structure of this embodiment is as follows Figure 5-6 As shown, the 7-slit feeding mold is composed of 8 partitions, the width of all partitions is 60mm, and there are 4 12mm×2mm feeding gaps at the bottom of each partition. The thickness of the two outermost partitions is 4mm, the thickness of each middle partition is 2.5mm, and the width of the slit between two adjacent partitions is 0.5mm. The total thickness of the mold is 2×4+6×2.5+7×0.5=26.5mm, the height of the two outer partitions is 38-39mm, and the height of the multiple inner partitions is 37-37.9mm. The maximum angle between the inclined surface of the mold and the horizontal plane is about arctan(1 / 4)=14°. The angle between the two outermost partitions is about 152°.
[0060] Based on the mold, a gallium oxide single crystal was grown by pulling in the
[010] direction at a pulling speed of 5-40 mm / h, and a thick gallium oxide single crystal with a width of 60 mm and a thickness of 26.5 mm was grown. Figure 7 As shown, not only can more than 20 pieces be produced at a time in the thickness direction, but cross-sections can also be cut and processed to provide multiple (010) face single crystals (number of pieces = length / single piece thickness).
[0061] In summary, the present invention provides a mold and a growth method for growing gallium oxide single crystals by a guided mold method. In this embodiment, the mold is a mold with multiple slits. The material is fed through the multiple slits, which increases the material feeding amount per unit time, ensuring the continuity and stability of the thick-sized gallium oxide single crystal growth process, so that a wafer with a thickness of more than 10 mm can be grown, and then a large number of blanks can be processed at one time in the thickness direction, thereby improving production efficiency. In addition, the present invention sets the existing horizontal top structure as a curved top structure or an inclined top structure, so that the temperature of the outer partition is always slightly higher than the temperature of the inner partition, reducing the temperature difference of the crystallization interface in the thickness direction, thereby improving the quality of the gallium oxide single crystal.
[0062] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A mold for growing gallium oxide single crystals by a guided mold method, characterized in that: The mold comprises a plurality of partitions arranged in mirror symmetry, the plurality of partitions being fixed together by a fixing portion, and a slit being provided between two adjacent partitions; wherein the plurality of partitions refers to more than three partitions; The plurality of partitions are fixed together by a plurality of rivets, and a coil is wound around the rivet between two adjacent partitions or an annular gasket is sleeved thereon, and the coil or annular gasket is used to control the width of the slit; The ratio of the thickness of any single partition to the width of any slit is 2:1-20:
1.
2. The mold for growing gallium oxide single crystal by the guided mode method according to claim 1, characterized in that: The width of the slit between two adjacent partitions is 0.1-0.5 mm.
3. The mold for growing gallium oxide single crystal by the guided mode method according to claim 2, characterized in that: The width of any two slits is the same.
4. The mold for growing gallium oxide single crystal by the guided mode method according to claim 1, characterized in that: Among the plurality of partitions, except for the two outermost partitions, the remaining partitions have the same thickness; Alternatively, among the plurality of separators, any two separators have the same thickness.
5. The mold for growing gallium oxide single crystal by the guided mode method according to claim 1, characterized in that: Two adjacent partitions are fixed by welding.
6. The mold for growing gallium oxide single crystal by the guided mode method according to claim 1, characterized in that: A notch is provided at the bottom end of each partition plate for raw materials to flow into the slit.
7. A method for growing a gallium oxide single crystal, characterized in that: The mold according to any one of claims 1 to 6 is placed in a crucible containing a gallium oxide raw material, the crucible is heated, and crystals are grown to obtain a thick gallium oxide single crystal.
8. The method for growing a gallium oxide single crystal according to claim 7, characterized in that: The thickness of the gallium oxide single crystal is greater than 10 mm.
Citation Information
Patent Citations
Die for growing gallium oxide single crystal by edge-defined film-fed growth method