Trimetallic layered double hydroxide complex

By using a layered double hydroxide catalyst composed of cobalt, iron and chromium in the water splitting process, the problem of instability of existing catalysts under strongly acidic conditions is solved, and efficient catalytic oxidation of water to generate oxygen under low overpotential is achieved. Reduced energy and cost requirements.

CN112888810BActive Publication Date: 2024-10-08NEWSOUTH INNOVATIONS PTY LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980068635.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-08-16
Filing Date
2019-08-16
Publication Date
2024-10-08
Estimated Expiration
2039-08-16

AI Technical Summary

Technical Problem

Existing water splitting catalysts are unstable under strongly acidic conditions and have poor kinetic properties, which requires additional energy input during the water splitting process, making them costly and difficult to apply industrially.

Method used

A layered double hydroxide (LDH) material containing cobalt, iron and chromium was developed as a catalyst to form a CoFeCr composite material through electrodeposition. Chromium was used as an oxygen scavenger to maintain the catalytically active form of cobalt and reduce the overpotential.

Benefits of technology

It achieves a significant improvement in the catalytic activity of oxidizing water to generate oxygen at low overpotential, which is superior to chromium-free cobalt-iron composite materials, reduces the energy demand and cost of the water splitting process, and improves the stability and efficiency of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112888810B_ABST
    Figure CN112888810B_ABST
Patent Text Reader

Abstract

The present invention relates to layered double hydroxide (LDH) materials and methods for catalyzing oxygen evolution reaction (OER) using the LDH materials in a water splitting process. The present invention also provides compositions, catalytic materials, electrodes and electrolyzers comprising the LDH materials. In particular, the LDH materials include metal composite materials comprising cobalt, iron, chromium and optionally nickel materials, interspersed with hydroxide layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a layered double hydroxide (LDH) material and a method for catalyzing an oxygen evolution reaction (OER) using the LDH material in a water splitting process. The invention also provides a composite, a catalytic material, an electrode and an electrolytic cell comprising the LDH material. Background Art

[0002] The water splitting process is considered a sustainable method for hydrogen production and storage because it can exploit abundant available water resources and low carbon intensive energy sources, such as renewable energy (e.g., solar energy), as inputs. Water splitting can be performed in an electrolyzer to produce hydrogen at the cathode via the hydrogen evolution reaction (HER). Oxygen can be produced at the anode via the oxygen evolution reaction (OER).

[0003] In practice, water splitting is usually carried out in a strongly alkaline electrolyte, because most transition metal-based electrodes cannot be stably present under strongly acidic conditions. The performance of water splitting catalysts is limited by the relatively slow kinetics of the OER half-reaction. The OER involves a four-electron transfer process. Therefore, in addition to the theoretically defined electrolysis potential value of 1.23V, additional energy input is required to achieve the decomposition of water molecules. This additional energy requirement is called the overpotential (η) because a potential greater than the theoretical potential is required to drive the electrolysis reaction.

[0004] Although noble metal-based materials such as IrO2 and RuO2 can effectively oxidize water to oxygen within an acceptable overpotential range, the high cost of such noble metals still hinders the industrial application of water splitting.

[0005] Recent research efforts have been devoted to developing water splitting catalysts based on earth-abundant metals. Earth-abundant metals do not include Re, Ru, Os, Rh, Ir, Pd, Pt, Ag, and Au. Layered double hydroxides (LDHs) are a promising class of electrocatalysts based on earth-abundant metals. In general, LDHs include layers of positively charged metal-containing materials interspersed with negatively charged anions in spatial regions. An example of an LDH is Ni-Fe LDH, which contains Ni 2+ and Fe 3+ cations, interspersed with counter-charged anions. Ni-Fe LDHs have been shown to be effective OER catalysts under alkaline conditions. However, the complex structure of Ni-Fe LDHs has led to a poor understanding of the catalytic sites and action mechanisms, making it more difficult to further develop them as electrocatalysts.

[0006] Therefore, there is a continuing need to further develop catalytic materials made from earth-abundant elements. Summary of the invention

[0007] The inventors have developed a ternary composite material comprising cobalt, iron and chromium interspersed with hydroxide layers capable of catalyzing OER with low overpotential (η). Surprisingly, the OER catalytic performance of the CoFeCr composite is superior to that of a composite comprising cobalt and iron without chromium.

[0008] In one aspect, the present invention provides a layered double hydroxide (LDH) material comprising a metal composite material comprising cobalt, iron, and chromium species interspersed with hydroxide layers.

[0009] In another aspect, the present invention provides a catalytic material comprising the LDH material of the present invention.

[0010] In another aspect, the present invention provides an electrode, comprising a conductive substrate and a catalytic material coated on the surface of the conductive substrate, wherein the catalytic material comprises the LDH material of the present invention.

[0011] In another aspect, the present invention provides a method for releasing oxygen by splitting water, the method comprising providing an electrochemical cell comprising an anode, a cathode, an electrolyte solution and optionally a reference electrode, contacting water with the anode and the cathode, and applying a voltage between the anode and the cathode, wherein the anode comprises the layered double hydroxide material of the present invention.

[0012] In another aspect, the present invention provides an electrolytic cell comprising an anode, a cathode, a power supply and optionally a reference electrode, wherein the anode comprises the LDH material of the present invention.

[0013] In another aspect, the present invention provides a method for preparing the catalytic material or electrode of the present invention, which comprises contacting a conductive substrate with a solution comprising cobalt ions, iron ions and chromium ions, and applying a voltage to the substrate and a counter electrode through the solution to electrodeposit a composite material comprising cobalt, iron and chromium substances on the substrate.

[0014] In another aspect, the present invention provides a method for preparing the catalytic material of the present invention, which comprises treating a mixture comprising cobalt ions, iron ions and chromium ions at a temperature of about 150°C to about 220°C for about 8 hours to about 20 hours, cooling the mixture and collecting the product.

[0015] Before describing the present invention in detail, it is to be understood that this invention is not limited to specific exemplary embodiments, methods of manufacture or use, as such may vary.

[0016] The invention described and claimed has many features and embodiments, including but not limited to those listed, described or referenced in the Summary of the Invention section of this application, which is not exhaustive. The invention described and claimed is not limited to the features or embodiments identified in the Summary of the Invention section, which are for illustrative purposes only and are not intended to limit the invention.

[0017] All publications, patents and patent applications cited in this application, whether supra or infra, are hereby incorporated by reference in their entirety.

[0018] It should be appreciated that if this application refers to any prior art publication, this reference does not constitute an admission that the publication forms part of the common general knowledge.

[0019] BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention is further described below by way of examples and with reference to the accompanying drawings, in which:

[0021] Figure 1 In ad, (a) is a scanning electron microscope (SEM) image showing the microsphere morphology of the CoFeCr composite material on the nickel foam (NF) matrix, and the inset shows an enlarged image; (b) is a transmission electron tomography (TEM) image of the CoFeCr composite material, and the inset shows the lattice fringes; (c) is a selected area electron diffraction (SAED) pattern; (d) is an element distribution diagram of the CoFeCr composite material (O [upper left], Co [upper right], Fe [lower left], Cr [lower right]).

[0022] Figure 2 Shown is the SEM image of the CoFe composite on NF obtained in the chromium-free electrolyte.

[0023] Figure 3 Shown are current-time curves (Jt curves) measured during electrodeposition of CoFe composites (top) and CoFeCr composites (bottom) on NFs.

[0024] Figure 4 ah shows a series of SEM images of CoFe composites on NF at different deposition times: (a) 30 s; (b) 60 s; (c) 120 s; (d) 300 s; (e) 900 s; (f) 1800 s; (g) 3600 s; and (h) 7200 s.

[0025] Figure 5ah shows a series of SEM images of CoFeCr composites on NF at different deposition times: (a) 30 s; (b) 60 s; (c) 120 s; (d) 300 s; (e) 900 s; (f) 1800 s; (g) 3600 s; and (h) 7200 s.

[0026] Figure 6 Schematic diagram comparing the growth of CoFe nanosheets and CoFeCr microsphere composites is shown.

[0027] Figure 7 Raman spectra of CoFeCr composite (top) and CoFe (bottom) composite on NF are shown.

[0028] Figure 8 ad show the X-ray photoelectron spectroscopy (XPS) spectra of the CoFeCr composite electrode before (top) and after (bottom) OER test in 1 M KOH solution, where: (a) O1s, (b) Co2p, (c) Fe2p, (d) Cr2p.

[0029] Fig. 9 Co2p XPS spectra of fresh CoFe (top) and CoFeCr (bottom) composites on NF are shown.

[0030] Fig.10 XPS spectra of Co2p of CoFe (top) and CoFeCr (bottom) composites after OER test in 1 M KOH are shown.

[0031] Fig.11 ad are linear sweep voltammetry (LSV) curves showing the OER performance of different LDH materials in 1 M KOH electrolyte at a scan rate of 5 mV·s -1 , using 95% iR compensation, the CoFeCr composites on NF synthesized with different precursor additives and different deposition times were tested, where: (a) Co 2+ :0mM to 48mM, (b)Fe 3+ :0mM to 48mM, (c)Cr 3+ : 0 mM to 24 mM, (d) at 12 mM Co 2+ , 3mM Fe 3+ and 6 mM Cr 3+ The deposition time under these conditions ranged from 60s to 7200s.

[0032] Fig.12 ad show (a) LSV curves of different OER catalytic reactions in 1 M KOH electrolyte at a scan rate of 5.0 mV·s -1, with 95% iR compensation; (b) LSV curves of the OER performance of CoFeCr composites before (black) and after (red) long-term durability testing in 1 M KOH electrolyte at a scan rate of 5.0 mV·s -1 , with 95% iR compensation, the inset shows the chronopotentiometry in 1 M KOH electrolyte at a current density of 100 mA cm -2 , time is 24 h, without iR compensation; (c) LSV curve of CoFeCr composite material in 1M KOH electrolyte, scan rate is 0.1mV·s -1 , with 95% iR compensation, the inset shows the derived Tafel slope simulation; (d) Electrochemical impedance spectroscopy (EIS) of CoFeCr (gray) and CoFe (black) composites on NF in 1 M KOH electrolyte with an applied potential of 1.48 V and without iR compensation relative to RHE: circles represent measured plots; curves represent calculated results.

[0033] Fig.13 af show the cyclic voltammetry curves at different scan rates in 1 M KOH electrolyte and the corresponding calculation of the electrochemical surface areas (a and b: NF; c and d: CoFe / NF; e and f: CoFeCr / NF).

[0034] Fig.14 LSV curves of CoFe (top) and CoFeCr (bottom) composites on copper foam (CF) before OER in 1 M KOH electrolyte (first scan after electrodeposition) at a scan rate of 5.0 mV s -1 , no iR compensation.

[0035] Fig.15 Shown is the SEM image of the previously prepared CoFeCr composite on NF after long-term OER testing in 1 M KOH, and the inset shows the magnified SEM image.

[0036] Fig.16 A series of LSV curves are shown, comparing the OER performance of different catalysts on a copper foam (CF) substrate.

[0037] Fig.17 LSV curves of CoFe composite on NF matrix are shown at a scan rate of 0.1 mV·s -1 , with 95% iR compensation, the inset shows the derived Tafel slope simulation.

[0038] Fig.18Shown are the LSV curves of the NiCoFeCr composite LDH on CF matrix in 1 M KOH with 90% iR compensation, compared with those of the CoFeCr composite LDH or the NiFeCr composite on CF matrix.

[0039] Fig.19 Shown are the LSV curves of CoFeCr composite LDH nanodots on NF matrix in 1 M KOH without iR compensation, compared with the binary CoFe composite catalyst and the commercial IrC catalyst.

[0040] Fig. 20 TEM images of CoFeCr LDH nanodots at 20 nm (a) and 10 nm (c) scales are shown.

[0041] definition

[0042] In this application, the term "water splitting" refers to any process that generates elemental hydrogen or oxygen using water as a starting material. The water splitting processes described in this application are essentially electrolytic. These electrolytic processes generally include a hydrogen evolution reaction (HER) at the cathode and an oxygen evolution reaction (OER) at the anode.

[0043] In the present application, the term "oxidation scavenger" relates to any material capable of inhibiting the oxidation of catalytic sites.

[0044] As used in this application and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. For example, "a surface" may include a plurality of surfaces, may refer to one or more surfaces, and so on.

[0045] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those of ordinary skill in the art to which the invention belongs. Any materials and methods similar or equivalent to those described in this application can be used to practice or test the present invention; the best embodiments of various materials and methods are described.

[0046] "(s)" after a noun includes the singular or plural form, or both.

[0047] The term "and / or" can mean "and" or "or".

[0048] Unless the context requires otherwise, all percentages mentioned in this application are percentages by weight of the material.

[0049] The various characteristics of the present invention are described with reference to certain values ​​or ranges of values. These values ​​are related to the results of various appropriate measurement techniques and should therefore be interpreted as including the error range inherent in any particular measurement technique. Some of the values ​​mentioned in this application are represented by the term "approximately", thereby at least partially illustrating their variability. When the term "approximately" is used to describe a certain value, the amount represented can be within ±25%, ±10%, ±5%, ±1% or ±0.1% of the value.

[0050] Unless the context requires otherwise due to linguistic expression or necessary meaning, the term "comprising" (or its variations, such as "comprise" or "comprises") used in the specification is an open-ended expression, which means that the required features are present, but does not exclude the existence of other features or the addition of other features in different embodiments of the invention. DETAILED DESCRIPTION

[0051] The present invention provides a layered double hydroxide material, which includes a metal composite material, wherein the metal composite material contains cobalt, iron and chromium substances.

[0052] Advantageously, the LDH materials of the present invention exhibit a surprising improvement in OER catalytic activity compared to LDH materials comprising cobalt and iron composites. Without being bound by theory, the inventors believe that the inclusion of chromium in the metal composite acts as an oxygen scavenger for cobalt ions, which are catalytic sites for OER. The results for the CoFeCr LDH material indicate that the chromium and iron species work synergistically to keep the cobalt in the composite in a catalytically active form.

[0053] LDH materials include metal composites that include cobalt, iron, and chromium species. In some embodiments, the metal composite is a ternary composite material (TCM) consisting primarily of cobalt, iron, and chromium. These ternary composites may contain trace amounts of impurity metals, such as nickel, copper, or other transition metal impurities. Trace amounts typically refer to up to 0.01 wt % of the composite material.

[0054] In some embodiments, the metal composite material may further comprise one or more other metal substances in addition to cobalt, iron and chromium. The other metal substances may be other substances capable of catalyzing OER, or may be other metal substances capable of acting as scavengers. In some embodiments, the one or more other metal substances are nickel. In the present embodiment, the metal composite material is a quaternary composite material comprising cobalt, iron, chromium and nickel.

[0055] Cobalt is a typical cationic substance, such as Co 2+ and / or Co 3+ .

[0056] Iron is a typical cationic substance, such as Fe 2+ and / or Fe 3+ .

[0057] Chromium is a typical cationic substance, such as Cr 3+ and / or Cr 6+ .

[0058] When present in quaternary composites, nickel is the typical cationic species, such as Ni 2+ and / or Ni 3+ .

[0059] The inventors found that when the CoFeCr LDH material is formed by electrolytic deposition, the composite material contains chromium in the +3 oxidation state. After OER catalysis, the CoFeCr LDH material contains chromium in the +3 and +6 oxidation states. The inventors believe that Cr 3+ is sacrificially oxidized to help maintain the cobalt species in a catalytically active form. The inventors also believe that Cr 6+ It can act as an oxygen scavenger, further helping to maintain the cobalt species in a catalytically active form.

[0060] The concentration of each substance present in the metal composite can be determined by inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0061] The cobalt content in the metal composite material can be determined by dissolving the electrode in 0.5M H2SO4 and performing ICP-OES testing. The metal composite material may contain cobalt at a concentration of about 0.0001 to about 24 mmol / L, in particular about 0.001 to about 10 mmol / L, such as about 0.01 mmol / L to about 0.06 mmol / L, or about 0.015 mmol / L to about 0.05 mmol / L, or about 0.03 mmol / L to about 0.05 mmol / L. The concentration of cobalt may remain substantially unchanged after oxidation.

[0062] The electrode is dissolved in 0.5M H2SO4 and tested by ICP-OES, and the iron content in the metal composite can be determined. The concentration of iron contained in the metal composite can be from about 0.0001mmol / L to about 24mmol / L, especially from about 0.001mmol / L to about 10mmol / L, for example, from about 0.005mmol / L to about 3mmol / L or 0.005mmol / L to about 0.06mmol / L, or from about 0.015mmol / L to about 0.05mmol / L or 0.03mmol / L to about 0.04mmol / L. After use as an OER catalyst, the concentration of iron may be lower than the concentration of iron measured immediately after the preparation of the metal composite. In some embodiments, the iron concentration after oxidation may be from about 0.005mmol / L to about 0.03mmol / L.

[0063] The electrode is dissolved in 0.5M H2SO4 and tested by ICP-OES to determine the chromium content in the metal composite material. The concentration of chromium contained in the metal composite material can be about 0.0001 to about 24mmol / L, in particular about 0.001 to about 10mmol / L, for example, about 0.005mmol / L to about 0.06mmol / L, or about 0.015mmol / L to about 0.05mmol / L, or about 0.03mmol / L to about 0.04mmol / L. After use as an OER catalyst, the concentration of chromium may be lower than the concentration of chromium measured immediately after the preparation of the metal composite material. In some embodiments, the concentration of chromium after oxidation may be about 0.005mmol / L to about 0.03mmol / L.

[0064] The metal content in the quaternary composite material can also be determined by dissolving the electrode in 0.5M H2SO4 and performing ICP-OES testing. The concentration of nickel contained in the quaternary composite material can be from about 0.0001mmol / L to about 24mmol / L, in particular from about 0.001mmol / L to about 10mmol / L, for example from about 0.01mmol / L to about 8mmol / L, or from about 0.1mmol / L to about 7mmol / L or from about 0.1mmol / L to about 6mmol / L. The concentration of nickel will change greatly after oxidation.

[0065] The metal composite material may include cobalt and iron in a ratio of about 1:1 to about 10:1. For example, before being used as an OER catalyst, the ratio of cobalt to iron (Co:Fe) is about 1.5:1 by weight, and after being used as an OER catalyst, the ratio of cobalt to iron (Co:Fe) is about 3.5:1 by weight.

[0066] The metal composite material may include cobalt and chromium in a ratio of about 1:1 to about 10:1. For example, before being used as an OER catalyst, the ratio of cobalt to chromium (Co:Cr) is about 1.5:1 by weight, and after being used as an OER catalyst, the weight ratio of cobalt to iron is about 2.5:1 by weight.

[0067] The metal composite material may include iron and chromium in a ratio of about 0.5:1 to about 1:0.5. In some embodiments, before use as an OER catalyst, the ratio of iron to chromium (Fe:Cr) is about 1:1 by weight, and after use as an OER catalyst, the ratio of iron to chromium (Fe:Cr) is about 0.7:1 by weight.

[0068] The ratio of cobalt, iron and chromium contained in the prepared metal composite material may be about 1.5:1:1, and the ratio of cobalt, iron and chromium after being used as an OER catalyst is about 3:1:1.

[0069] The prepared quaternary metal composite material may contain cobalt, iron, chromium and nickel in a ratio of about 1.5: 1.5: 1: 1. This ratio may change after OER oxidation.

[0070] The composite material may contain cobalt, iron, chromium and optionally nickel in any combination of the above mentioned concentrations and / or ratios.

[0071] The LDH material of the present invention includes a metal composite material interspersed with a hydroxide layer. The hydroxide layer is usually formed simultaneously with the metal composite material. Typically, the hydroxide layer comprises an amorphous hydroxide. In addition, the hydroxide layer may also include cationic substances corresponding to the metal contained in the metal composite material, such as cobalt hydroxide and / or oxide, iron hydroxide and / or oxide, and chromium hydroxide and / or oxide, and when the composite material is a quaternary metal composite, it is nickel hydroxide and / or oxide. In some embodiments, the hydroxide layer may include a mixed phase of an amorphous hydroxide and a Co-based spinel oxide.

[0072] The LDH material can be in a spherical form. The inventors believe that the spherical form helps to enhance the OER catalytic activity because the layer it provides has an increased surface area. The spherical form may include a plurality of microspheres. The average diameter of the microspheres may be monodisperse. In some embodiments, the average diameter of the microspheres is from about 100 nm to about 500 nm, for example, from about 100 nm to about 300 nm or about 200 nm. The average diameter of the microspheres can be determined by scanning electron microscopy (SEM).

[0073] In some embodiments, the amorphous oxide / hydroxide material prepared by hydrothermal treatment is drop-coated to form the LDH material into nanodots. In some embodiments, the diameter of the nanodots may be less than 200 nm, for example, from about 1 nm to about 200 nm, especially from about 3 nm to 100 nm. In some embodiments, the diameter may be from 3 nm to 10 nm.

[0074] Also provided is a catalytic material comprising the LDH material described herein. The catalytic material optionally comprises a matrix. Any suitable matrix that does not interfere with the OER catalytic activity of the LDH material can be used. Suitable matrixes include conductive metal matrices (e.g., metal matrices, such as foamed metals) and conductive non-metal matrices (e.g., carbon fiber paper matrices). In some embodiments, the catalytic material is in the form of nanodots.

[0075] Also provided is an electrode comprising an LDH material and a conductive matrix. Any conductive matrix that does not interfere with the OER catalytic activity of the LDH material can be used. Preferably, the conductive matrix has a high surface area, such as a metal foam. Suitable foam metals include nickel foam and copper foam. Preferably, the conductive matrix is ​​nickel foam. In some embodiments, the LDH material is present in the electrode in the form of nanodots.

[0076] Preparation method

[0077] The LDH material of the present invention can be prepared by any method known in the art as long as a metal composite containing cobalt, iron and chromium species is formed.

[0078] In some embodiments, the catalytic materials and / or electrodes of the present invention can be prepared by a facile electrodeposition process.

[0079] Thus, the present application describes a method for preparing a composite material comprising cobalt, iron and chromium species on a substrate, the method comprising electrolyzing a solution comprising a cobalt salt, an iron salt and a chromium salt in a solution in contact with the substrate. Suitable salts include nitrates, sulfates or chlorides. In a specific embodiment, the salt is a nitrate.

[0080] The method generally comprises contacting a conductive substrate with a solution comprising cobalt ions, iron ions and chromium ions and applying a voltage through the solution to the substrate and a counter electrode to electrodeposit a composite material comprising cobalt, iron and chromium species on the substrate.

[0081] In these preparation methods, cobalt salt, iron salt and chromium salt can be nitrate.Solution can include cobalt salt of about 100mM at most (for example, cobalt salt of about 75mM or about 50mM at most).The solution can include iron salt of about 100mM at most (for example, iron salt of about 75mM or about 50mM at most).The solution can include chromium salt of about 50mM at most (for example, chromium salt of about 40mM or about 30mM at most).Alternatively, the solution includes nickel salt of about 500mM at most (for example, nickel salt of about 6mM or about 100mM at most).Usually, the solution is an aqueous solution.

[0082] The solution may further comprise one or more electrolytes. Suitable electrolytes include salts such as potassium chloride (KCl). The electrolyte may be present at a concentration of about 1M.

[0083] In some embodiments, in the case of a three-electrode system and a constant potential input, the potential applied between the substrate and the reference electrode is about -0.6 V to -2.0 V relative to the reference value, particularly about -1.0 V relative to the reference value.

[0084] In some embodiments, a constant current electroplating method is used, where a constant current is applied to a two-electrode system. A suitable constant current is about 1 mA cm 2 to about 3mAcm 2 .

[0085] In this process, -OH ions are generated by the electrolysis of water in the electroplating bath and these ions are co-precipitated on the substrate with Co ions, Fe ions and Cr ions to form a double hydroxide layer.

[0086] In some embodiments, the method further comprises a substrate pretreatment step, wherein the substrate is washed with a strong acid (eg, 4M HCl) and sonicated. The pretreatment step typically removes oxides and other impurities from the substrate surface prior to electrodeposition of the LDH material.

[0087] In some embodiments, the method further involves introducing a reference electrode into the electrolytic cell, and the reference electrode is also in contact with the solution. Suitable reference electrodes include Ag / AgCl, reference hydrogen electrode, Ag / Ag2SO4 electrode, calomel electrode, Hg / Hg2SO4 electrode and Hg / HgO electrode. In a specific embodiment, when a reference electrode is used, the reference electrode is an Ag / AgCl electrode.

[0088] The conductive matrix may be a metal foam, such as copper or nickel foam, preferably nickel foam. After electrodeposition, the metal foam may have a mass loading of LDH material of about 1 mg / cm 2 To about 5mg / cm 2 , for example about 2 mg / cm 2 .

[0089] In another embodiment, the ternary or quaternary metal composite LDH material can be prepared by a hydrothermal method, and the obtained solid product can be ground into a powder. For example, a mixture of cobalt salts, iron salts, chromium salts and optionally nickel salts is suspended in an alcohol aqueous solution, such as a methanol aqueous solution, and heated in an autoclave at about 180 ° C for about 12 hours. The suspension is then cooled, washed with water, collected, and dried under vacuum, optionally at high temperature. The dried product can be ground into a powder.

[0090] The powder can be mixed with an alcohol aqueous solution (e.g., an ethanol aqueous solution or a methanol aqueous solution) and a binder (e.g., ) to form a uniform suspension to prepare nanodots. The uniform suspension can be obtained by thorough mixing by any suitable mixing procedure such as ultrasonic treatment.

[0091] The uniform suspension can be drop coated on a substrate such as an electrode or a conductive substrate. Suitable substrates include, but are not limited to, glassy carbon electrodes or metal foams, such as nickel foam or copper foam.

[0092] In another aspect of the present invention, a method for preparing the catalytic material of the present invention is provided, which comprises treating a mixture of cobalt ions, iron ions and chromium ions at a temperature between about 150°C and about 220°C, in particular at a temperature between about 150°C and about 220°C, for about 8 hours to about 50 hours, in particular for about 8 hours to about 20 hours, cooling the mixture, and collecting the product.

[0093] In a specific embodiment, the temperature is between about 170° C. and about 190° C., in particular about 180° C. In a specific embodiment, the heating time is about 10 hours to about 15 hours, in particular about 12 hours.

[0094] In some embodiments, the mixture may also include other metal ions, such as nickel ions.

[0095] In some embodiments, the product is ground into a powder suitable for drop coating.

[0096] How to use

[0097] The present invention provides a method for releasing oxygen from water splitting. The method is performed in an electrochemical cell comprising an anode, a cathode, an electrolyte solution and an optional reference electrode. The method comprises contacting water with the anode and cathode of the electrochemical cell and applying a voltage between the anode and the cathode. Since the OER half-reaction typically occurs at the anode, the anode comprises the LDH material of the present invention, for example in the form of an electrode. In some embodiments, the electrolyte solution is an aqueous electrolyte solution. The aqueous electrolyte solution can also be a source of water. Typically, water has an alkaline pH, for example, a pH of at least 8, 9 or 10 or higher. In some embodiments, water comprises a strong base, for example, a hydroxide base, such as NaOH or KOH, and the concentration of the base is, for example, 0.1M to about 10M or higher.

[0098] Typically, the cathode used in these methods includes a hydrogen evolution reaction (HER) catalyst such as Pt / C or nickel.

[0099] When used in these methods, the LDH materials of the present invention provide catalytic activity comparable to that of current leading OER catalysts. Surprisingly, the LDH materials of the present invention are able to provide similar catalysis when using earth-abundant metals. Also surprisingly, the LDH materials are able to provide improved catalytic activity and require lower overpotentials than other known earth-abundant metal-based OER catalysts, including corresponding CoFe LDHs (i.e., LDH materials prepared by similar routes, but without chromium).

[0100] In some embodiments, the Tafel slope of the oxygen evolution process is as high as 40 mV dec -1 , e.g. up to 39mV dec -1 、38mV dec -1 、37mV dec -1 、36mV dec -1 、35mV dec -1 or 32mV dec -1 .

[0101] The voltage applied to the anode should be chosen to match or exceed the overpotential of the LDH material to drive the OER.

[0102] The LDH materials of the present invention require a relatively low overpotential at the anode to drive OER. In some embodiments, the LDH materials catalyze OER with an overpotential of about 270 mV to provide about 100 mA cm -2The onset potential of OER is only about 1.43 V relative to the reference reversible hydrogen electrode (RHE), which is advantageous compared to the theoretical minimum onset potential of OER of 1.23 V relative to the reference reversible hydrogen electrode. Therefore, in some embodiments, the voltage applied to the solution is at least 1.43 V, for example, 1.43 V to about 10 V, about 1.5 V to about 10 V, about 1.43 V to about 5 V, about 1.43 V to about 3 V or about 1.5 V to about 3 V relative to RHE.

[0103] In some embodiments, the LDH material is present on the electrode in the form of nanodots.

[0104] An electrolyzer is also provided, comprising an anode, a cathode, a power source and optionally a reference electrode. Typically, the anode comprises the LDH material of the present invention. In certain embodiments, the power source provides electricity from a low carbon intensive power source. The power source can be a renewable power source, such as one or more solar panels or wind turbines, or a non-renewable power source, such as a nuclear reactor.

[0105] Example

[0106] The present invention will be further described by way of non-limiting examples. It will be appreciated by those skilled in the art that many modifications may be made without departing from the spirit and scope of the present invention.

[0107] Example 1

[0108] experiment

[0109] Materials Synthesis All chemicals were purchased from suppliers and used without further purification. The nickel foam (NF, 1.5 mm thick, 110 ppm) or copper foam (CF, 1.5 mm thick, 110 ppm) substrates were washed and ultrasonically treated in 4.0 M hydrochloric acid (HCl, 32.0%, RCI LABSCAN) for 10 min to remove surface oxides. The substrates were then washed with Mill-Q water (18.2 MΩ cm -1 ) and dried under nitrogen flow. The matrix material was cut into a certain size and sealed with Teflon tape, with an exposed geometric surface area of ​​1×1 cm 2. Thereafter, the substrate was used as the working electrode of a standard three-electrode system, in which the graphite plate and Ag / AgCl (1.0M KCl) were the counter electrode and the reference electrode, respectively. The deposition bath contained 0-48mM cobalt nitrate (Co(NO3)2·6H2O, Chem-Supply), 0-48mM iron nitrate (Fe(NO3)3·9H2O, Chem-Supply), and 0-24mM chromium nitrate (Cr(NO3)3·9H2O, Jax Chemicals). Electrodeposition was performed for 0-7200s at an applied potential of -1.0V (relative to Ag / AgCl (1.0M KCl)) using a CHI760D potentiostat. The prepared electrode was slowly removed from the electrolyte and used To prepare a commercial catalytic electrode as a control sample, 20 mg of Ir / C catalyst (20% Ir on Vulcan XC-72, Premetek Co.) was dispersed in a solvent and mixed with 480 μL H2O, 480 μL anhydrous ethanol (C2H5OH, Chem-Supply) and 40 μL The suspension was sonicated for 20 min to obtain a homogenous ink, which was then drop-coated and dried onto NF or CF substrates with a mass loading of 2.0 mg cm -2 .

[0110] Material characterization The microscopic morphology of the prepared materials was observed using a scanning electron microscope (SEM, JSM7001F) and a high-resolution transmission electron microscope (HRTEM, Philips CM200). The element distribution was studied using an X-ray energy dispersive spectrometer (EDS) attached to the TEM. Raman spectra were recorded using a Renishaw spectrometer with a laser λ = 532 nm. The chemical environment and composition were analyzed by X-ray photoelectron spectroscopy (XPS, Thermo ESCALAB250i). The atomic weight of the elements on the electrode surface before and after the long-term OER test was measured by an inductively coupled plasma emission spectrometer (ICP-OES, 7300 PerkinElmer). The obtained electrode (0.5×0.5cm 2 ) were immersed in 15 mL of 0.5 M H2SO4 aqueous solution and sonicated for 20 minutes. The solution was then collected and tested in an ICP-OES system.

[0111] Electrochemical Measurements The electrodes were placed in a 1.0 M potassium hydroxide solution (KOH, Chem-Supply) in a standard three-electrode system. The counter electrode and the reference electrode were graphite plate and Ag / AgCl (1.0 M KCl), respectively. The prepared electrodes were first subjected to cyclic voltammetry (CV, -0.2 V to 0.6 V, relative to the reference value, 10 mV·s-1 ) for more than 20 cycles to achieve stable performance. Then, the linear sweep voltammetry (LSV, 5.0 mV·s -1 , 95% iR compensation) and chronopotentiometry to demonstrate its performance at 100 mA cm -2 The recorded potential values ​​were calibrated with reference to the reversible hydrogen electrode (RHE) according to the following formula:

[0112] E RHE =E 参比电极 +0.222+0.059×pH (1)

[0113] At 0.1mV s -1 The Tafel slope was recorded and derived from the near-static LSV under the conditions of scan rate and 95% iR compensation. It is worth noting that only the LSV tests in this work were iR corrected. At the same time, the electrochemically active surface area (ECSA) was calculated based on the charge / discharge process of the double layer capacitance in a non-Faraday process. The charge / discharge current (IC) is related to the scan rate (ν) and the electrochemical double layer capacitance (Cdl), which can be expressed by formula (2):

[0114] IC=ν×C dl (2)

[0115] Therefore, the ECSA can be calculated by measuring CVs at different scan rates. The electrochemical impedance spectra were collected in a 1M KOH solution in a standard three-electrode system as described above using an electrochemical potentiostat (Metrohm). At the specific applied potential, the frequency range of the input sinusoidal signal was 100 KHz to 0.01 KHz with an amplitude of 10 mV. The measured graphs were further simulated by Zimpwin software. The double layer capacitance (C) can be calculated from the simulated constant phase element (Q) value according to formula (3): dl ):

[0116] C dli =[Qi / (Rs-1+Ri-1)(1-ni)]1 / ni (3)

[0117] Where R s and R i are the solution resistance and charge transfer resistance in the simulated circuit respectively, and n represents the phase angle value.

[0118] The conversion efficiency (TOF) is calculated by formula (4):

[0119] TOF = j × A / (4F × m) (4)

[0120] where j, A, F, and m are the current density, electrode area, Faraday constant (96,485 C / mol), and the number of moles of active material on the substrate at a certain overpotential, respectively, which can be determined by the weight difference before and after electrodeposition.

[0121] Results and Discussion

[0122] CoFeCr LDH electrodes were prepared by electrodeposition in a nitrate-based electrolyte at a potential of -1.0 V relative to Ag / AgCl (1 M KCl). Under these conditions, the OH generated by the electrolysis of H2O - Ions and local Co in solution 2 + , Fe 3+ and Cr 3+ The ions were co-precipitated on nickel foam (NF) substrate (denoted as CoFeCr / NF). After deposition, a brown film was observed on the NF, which was different from the green CoFe composite material (denoted as CoFe / NF) as a control. The morphology of the samples was characterized by SEM. Figure 1 As shown in a, the obtained CoFeCr composite material shows a layer of monodispersed microspheres with a diameter of about 200 nm (see Figure 1 a), which is similar to Figure 2 The nanosheet array structures of the CoFe composites grown on NFs are obviously different. To understand the morphological transformation from CoFe nanosheets to CoFeCr microspheres, the crystal nucleation and growth details were further investigated. Figure 3 The dynamic crystal growth process of CoFe and CoFeCr on NF is shown (the relationship between electrodeposition current and time). For CoFe, after applying a negative potential of -1.0 V (reference Ag / AgCl), the current density increases from about 5.0 mA cm to 1.5 mA cm in the first 20 s. -2 It dropped sharply to 3.5 mA cm -2 , indicating a rapid nucleation and crystal growth process. As shown by the SEM over time ( Figure 4 a), a large number of nanosheet cores are formed, and CoFe grows continuously on the preformed nanosheet cores and maintains the original nanosheet structure ( Figure 4 bh). However, when Cr is present, its deposition it curve undergoes a different nucleation path ( Figure 3 ): The electrodeposition curve is first shown in the first 30s, the current density is from 8mA·cm -2 Dropped sharply to 6 mA cm -2 , indicating the formation of nuclei on the substrate. Interestingly, another slow drop in current was observed over the next 30 s to 150 s, suggesting that secondary nucleation occurred immediately due to the “modulating effect” of Cr. Figure 5 Figure 2 shows the morphology of CoFeCr over time. Initially, a thin layer of nanosheet cores is formed on the matrix with almost no nanosphere structure ( Figure 5 a). As the deposition time increases, more and more nanospheres begin to appear and become the main features ( Figure 5 bc), and eventually lead to the formation of uniform CoFeCr microspheres covering the NF electrode ( Figure 5 dh and Figure 6 ).

[0123] Figure 1 In b, the crystal structure of the aggregated nanosheets from the CoFeCr composite microspheres was further characterized by high-resolution TEM (HRTEM). As shown in the HRTEM image, two lattice fringes were measured to be about 0.25 nm and about 0.15 nm, corresponding to the (311) plane of the CoCr2O4 (PDF#22-1084) spinel phase and the (440) plane of the CoFe2O4 (PDF#22-1086) spinel phase, respectively. Figure 1 The selected area electron diffraction (SAED) pattern in c shows halos around the two rings, confirming the mixture of amorphous CoFeCr hydroxide composite and crystalline spinel phase. Figure 1 d shows the element distribution map obtained by energy dispersive spectroscopy (EDS) on TEM, indicating the uniform distribution of O, Co, Fe and Cr elements. Figure 7 The Raman spectrum also shows the presence of a spinel phase, with a peak at about 554 cm -1 and about 688cm -1 The two strong peaks appearing nearby are octahedral (OH) and tetrahedral (Td) MO stretching. As chromium is introduced into the CoFe composite, the OH peak corresponding to LDH becomes broader, indicating the formation of more defects. The Td peak is stronger than that of the CoFe composite, confirming the formation of the para-spinel phase in the CoFeCr composite.

[0124] The chemical composition and electronic structure of the prepared CoFeCr / NF electrode before and after OER were studied by XPS. Figure 8 As shown in a, in the core-level O1s XPS, three fitting peaks were observed at ~533.1eV, ~531.5eV and ~529.8eV, corresponding to the O bond, M-OH bond and MO bond of liquid water, respectively. In particular, the presence of M-OH and MO is related to hydroxide or (oxy)hydroxide

[28] . After the OER test, the O intensity in liquid water decreased, and the peak corresponding to the MO bond became stronger. The intensity change before and after OER can be attributed to the residual intermediate MOOH phase. For Figure 8Fe2p XPS spectrum in b, from the satellite peak (~716.9 eV) and Fe 3+ Peak (~712.0eV) shows that before and after the OER test, Fe 3+ The oxidation state remains constant. Figure 8 The core-level Cr2p XPS spectrum in c shows that before OER, there is a strong broad peak at ~577.0 eV, corresponding to the Cr in Cr-OH and Cr-O. 3+

[19] . However, after OER testing, the broad peak split into two peaks, and a new peak appeared at ~579.7 eV, corresponding to a higher degree of chromium oxidation state Cr 6+ . Figure 8 d shows the high-resolution XPS of Co2p in the CoFeCr composite. The two peaks at ∼803.2 eV and ∼787.1 eV correspond to Co2p, respectively. 1 / 2 and Co2p 3 / 2 Satellite peak characteristics. Co2p 1 / 2 (~796.8eV) and Co2p 3 / 2 The fitting peak of (~781.2eV) shows that the cobalt in the composite is mainly in the form of Co 2+ The oxidation states of Fig. 9 As shown in Figure 2, the Co oxidation state of the freshly prepared sample remains almost Co 2+ It is well known that for water oxidation electrolysis involving cobalt, after applying the OER potential, part of the Co 2+ It is converted to a higher oxidation state in the CoOOH intermediate phase and is considered to be an active site. However, there are β-CoOOH and γ-CoOOH phases in the CoOOH intermediate, and their oxidation states are between 3+ and 4+. According to DFT calculations, Co in a relatively low oxidation state in the β-CoOOH state is the most active site, rather than Co in a higher valence state in γ-CoOOH. (Similarly, this relatively low valence state of Ni in the NiOOH active phase is also found in β-NiOOH for water oxidation.) In addition, the active β-MOOH can be degraded to the less active γ-MOOH (higher oxidation state) by overcharging

[36] . Therefore, maintaining a relatively low oxidation state of Co in β-CoOOH is key to improving OER performance. Therefore, similar to the oxidation state changes widely observed when a positive potential is applied, the cobalt in CoFeCr is also oxidized to a higher valence state, at least on the surface, to catalyze water to produce O2 bubbles. However, after OER, Fig.10 The Co2p XPS of CoFeCr in the medium shows that the long-term oxidation of CoFe(Co 2+ / Co 3+ =1.1), the residual Co 3+State (Co 2+ / Co 3+ =1.8) is even less. This phenomenon indicates that although the Co in the CoFeCr composite 2+ can be converted to a CoOOH active intermediate phase with a higher oxidation state, but the average Co oxidation state is lower than that in CoFe because fewer Co oxidation states are observed after water oxidation. 3+ The reason for this unique phenomenon may be that during the water oxidation process, the chromium in the composite material is partially oxidized to a high-valent state Cr 6+ The electrons generated by this oxidation reaction can be transferred to the cobalt site to maintain the cobalt in a relatively low oxidation state (in the case of Co 2+ and Co 3+ This synergistic effect can effectively prevent the deactivation of β-CoOOH by overcharging, thereby enhancing the OER performance. In addition, the chemical composition of the CoFeCr composite was detected by ICP-OES measurement. As shown in Table 1, the atomic ratio of Co, Fe and Cr is about 3:2:2.

[0125] Table 1 Inductively coupled plasma optical emission spectroscopy (ICP-OES) data

[0126] sample Co Cr Fe Ni S Fresh CoFeCr(mg / L) 2.63 1.77 1.70 17.60 14925 Fresh CoFeCr(mmol / L) 0.0446 0.0339 0.0305 0.3001 531 Oxidized CoFeCr(mg / L) 2.66 0.80 1.07 41.30 15112 Oxidized CoFeCr(mmol / L) 0.0451 0.0154 0.0192 0.7034 538

[0127] The OER performance of the prepared CoFeCr composites and other control samples such as CoFe, CoCr, FeCr composites (represented as CoFe / NF, CoCr / NF and FeCr / NF, respectively) and commercial Ir / C were evaluated in 1 M KOH electrolyte. To optimize the OER electrode, we first varied the preparation conditions, including adjusting the addition amount of ion precursors and the deposition time ( Fig.11 ), and then in the presence of 12 mM Co 2+ , 3 mM Fe 3+ and 6 mM Cr 3+ The optimized CoFeCr / NF was prepared by electrodeposition in an electrolyte of for 900 s. Fig.12 The linear sweep voltammetry (LSV) curve of the CoFeCr / NF electrode in a shows the most active capacity: the onset potential value is only ∼1.43 V vs. RHE, while that of CoFe / NF is ∼1.47 V (which can be seen from Fig.12 c and Fig.13 The Tafel slope (dashed line) in the figure is used to calculate the intersection of the Tafel slope (dashed line) and the y-axis (x=0). In detail, in order to achieve 10 mA cm -2 and 100mA·cm -2The current density was 2.37 V and 1.50 V respectively, with the potential fed back being only ~1.46 V and ~1.50 V relative to RHE. The OER performance of the resulting ternary CoFeCr composite was superior to the combination of binary composites of CoFe, CoCr or FeCr. The OER performance of the CoFeCr / NF electrode was even better than that of the commercial Ir / C catalyst on NF, as well as the benchmark NiFe LDH (referred to as NiFe / NF) electrode. By measuring the weight difference after electrodeposition on NF, ~1.22 mg of the composite was obtained on the substrate. Referring to the above element ratios in ICP, the stoichiometry can be determined to be Co3Fe2Cr2(OH) 18 Therefore, at an overpotential of 250 mV, the TOF value of the CoFeCr composite material was calculated to be 0.046 s -1 In comparison, the TOF of the CoFe composite material at 250 mV is only 0.008 s -1 , indicating a faster response in the OER reaction with the introduction of chromium. It is worth noting that Figure 4 The small peak at about 1.33 V to 1.36 V (relative to RHE) in a is due to the oxidation of the nickel matrix. Fig.14 The first LSV scan of the composite on copper foam shown above shows that, free from the influence of the nickel matrix, the anodic peaks around 1.15 V (vs. RHE) on the CoFe and CoFeCr composites indicate the formation of an intermediate CoOOH phase. The weaker peaks for the CoFeCr composite also indicate that less CoOOH is formed in the presence of Cr protection. 2+ Oxidized to a higher valence state.

[0128] Long-term stability is another key issue in practical applications. -2 The long-term stability of the electrode was measured by chronopotentiometry. Fig.12 As shown in the insert in b, the feedback potential is well maintained at ∼1.58 V (vs. RHE) for more than 24 h without degradation. The robustness of the CoFeCr electrode after chronopotentiometry is also demonstrated by retesting its LSV curve and comparing it to the initial LSV to reflect the unchanged OER performance ( Fig.12 b). In addition, after more than 24 hours of OER testing, the structural morphology of CoFeCr / NF ( Fig.15) still maintains the microspherical structure, indicating the structural stability of the composite material in alkaline medium. In order to quantify the composition of the post-electrode, the ICP-OES data of the CoFeCr / NF electrode after long-term oxidation were also measured. As shown in Table 1, the atomic ratio of Co, Fe and Cr is about 3:1:1, which indicates that excess Fe and Cr are dissolved during the oxidation process, but the durability of the electrode is not sacrificed. It should be noted that this simple synthesis method is also suitable for depositing highly active materials on other conductive substrates such as copper foam (CF) to eliminate the strong synergistic effect of the nickel substrate. Fig.16 As shown in Figure 2, the CoFeCr composite on CF still shows the best OER performance, however, the performance of FeCr / CF is much worse than that of FeCr / NF ( Fig.12 a).

[0129] To understand the mechanism of enhanced OER performance, the ECSA values ​​of NF, CoFe / NF, and CoFeCr / NF electrodes were measured by CVs capacitance technique ( Fig.13 ), the ECSA values ​​of NF, CoFe / NF and CoFeCr / NF were simulated to be 37.58 cm 2 、64.28cm 2 and 51.86cm 2 . From the above data, it can be seen that the ECSA of CoFeCr / NF is smaller than that of CoFe / NF electrode. The reduced ECSA of CoFeCr composite is due to the formation of aggregated microspheres, compared with the formation of nanosheet structure of CoFe / NF composite. The above results suggest that, on the one hand, the improvement in OER performance may not be due to ECSA; on the other hand, other factors, such as different reaction kinetics or electron transfer rates, may contribute to the improved OER performance of CoFeCr electrode. To confirm our hypothesis, we used a much slower scan rate of 0.1 mV·s -1 Another LSV was measured ( Fig.12 c) to reach a near-equilibrium reaction state at the electrode. The Tafel slope ( Figure 8 c), and the Tafel slope is obtained from this near-equilibrium LSV to be 32 mV·dec -1 The intersection of the Tafel slope (dashed line) and the y-axis (x=0) indicates an onset potential value of ~1.43 V (vs. RHE). Theoretically, the Tafel slope value is 40 mV·dec -1 , corresponding to M-O+OH as RDS - →M-OOH+e - The third charge transfer. Here, Fig.17The Tafel slope of the CoFe composite material is 40 mV·dec -1 In comparison, the smaller Tafel slope value is 32mV·dec -1 Indicates that the RDS process has been accelerated.

[0130] In order to further confirm the mechanism of the OER process, Fig.12 In d, the electrochemical impedance spectroscopy (EIS) was measured under an applied potential of ∼1.48 V (vs. RHE). A small semicircle ( Fig.12 d) and a large semicircle in the low-frequency region. s (Q1R1)(R2Q2) model is used to simulate the equivalent circuit of the OER process. s The value represents the resistance from the working electrode to the reference electrode solution, and the R1 and R2 values ​​are the resistances of charge transfer. It is worth noting that the double layer capacitor is simulated based on the constant phase elements (Q1, Q2), which is more accurate on the rough surface of the NF matrix. In this application, the intersection on the x-axis in the high frequency region represents the R of the CoFe and CoFeCr composites. s The values ​​are 2.59Ω and 2.48Ω, respectively, representing the solution resistance between the working electrode and the reference electrode. The small semicircle in the high-frequency region (Q1R1 in the simulation model) represents the formation of the active CoOOH intermediate phase, while the large semicircle in the low-frequency region (Q2R2) corresponds to the charge transfer of the rate-determining step in the OER process. The simulation parameters are listed in detail in Table 2. Specifically, the resistance (R1) of the charge transfer process of the intermediate phase in the CoFeCr composite is larger than that of the CoFe composite, which indicates that under the overcharge potential of 250mV, Co 2+ There is less conversion to higher oxidation states. Afterwards, there is less degradation of β-CoOOH during the OER process and a faster charge transfer process (smaller R2 value) in CoFeCr / NF compared with CoFe / NF, indicating that the RDS process is accelerated on the CoFeCr / NF electrode.

[0131] Table 2 EIS simulation parameters

[0132]

[0133] This example describes a ternary cobalt-iron-chromium hydroxide composite on a nickel foam substrate prepared by a facile electrodeposition method. The prepared electrode showed excellent OER performance and electrochemical duration in alkaline media. By introducing chromium into the cobalt-iron composite, the nanoflakes gradually aggregated into microspheres with a mixed phase of amorphous hydroxide and Co-based spinel oxide. The nature of the electrocatalytic improvement was studied in detail: the chromium in the composite was partially oxidized to 6+, which can protect the active sites of cobalt and keep it in a lower oxidation state in β-CoOOH. It was then demonstrated by Tafel slope value and EIS curve simulation that it accelerated the M-O+OH - →M-OOH+e - RDS.

[0134] Example 2

[0135] NiCoFeCr composites

[0136] Active NiCoFeCr LDH electrodes were fabricated by electrodeposition. The electrodeposition bath contained 6 mM nickel nitrate, 6 mM cobalt nitrate, 3 mM iron nitrate and 6 mM chromium nitrate in aqueous solution.

[0137] For constant potential electrodeposition, a three-electrode system was used, where the working electrode, counter electrode, and reference electrode were copper foam, graphite plate, and Ag / AgCl, respectively. The applied potential was -1.0 V relative to the Ag / AgCl reference electrode.

[0138] For constant current electrodeposition, a two-electrode system was used, which had a working electrode and a counter electrode, which were copper foam (or nickel foam) and a graphite plate, respectively. The applied current density was -2-3 mA / cm 2 The constant current is 300s.

[0139] Slowly remove the electrode from the electrolyte and The electrode was then evaluated in a three-electrode system with a graphite plate, a counter electrode, and an Ag / AgCl reference electrode in a water splitting reaction. Its OER performance was compared with that of a CoFeCr / CF electrode and a NiFeCr / CF electrode. Fig.18 The quaternary NiCoFeCr electrode exhibits enhanced performance compared to the ternary CoFeCr and NiFeCr electrodes on the copper foam substrate.

[0140] Example 3

[0141] CoFeCr LDH nanodots

[0142] CoFeCr composite LDH nanodots were synthesized by hydrothermal method. The precursor solution contained 1mmol cobalt nitrate, 1mmol iron nitrate, 1mmol chromium nitrate, 60mL methanol and 12mL water. The solution was then transferred to a sealed autoclave. The reaction was carried out in a room at 180 °C for 12 hours. After cooling naturally to room temperature, the suspension was centrifuged and washed with water three times. The product was collected and dried at 60 °C overnight in a vacuum. The obtained material was ground into powder in an agate mortar.

[0143] 10 mg of catalyst powder was dispersed in a solution containing 480 μL of water, 480 μL of anhydrous ethanol (C2H5OH, Chem-Supply) and 40 μL of The suspension was sonicated in an ice-water bath for 1 hour for nano-drop coating.

[0144] The uniform suspension (2 μL) was drop-coated on a nickel foam (NF) substrate and dried overnight in a fume hood. The mass loading was 2 mg / cm 2 .

[0145] Nanodot electrodes were used in the OER in 1 M KOH solution. Fig.19 The performance of the ternary composite nanodots is better than that of the commercially available IrC catalyst and the CoFe binary catalyst.

[0146] Nanodots formed by CoFeCr composite LDH such as Fig. 20 shown.

Claims

1. A layered double hydroxide material comprising a metal composite material comprising cobalt, iron and chromium species interspersed with hydroxide layers; in, The metal composite material has a spherical morphology, the spherical morphology comprises a plurality of microspheres, and the average diameter of the microspheres is monodisperse; Wherein, the metal composite material comprises Co 2+ and / or Co 3+ , Fe 2+ and / or Fe 3+ , and Cr 3+ and / or Cr 6+ ; Wherein, the hydroxide layer is a mixed phase of amorphous hydroxide and Co-based spinel oxide.

2. The layered double hydroxide material according to claim 1, wherein The metal composite material comprises cobalt and iron in a ratio of (1.5-3.5):1 by weight.

3. The layered double hydroxide material according to claim 1, wherein The metal composite material comprises cobalt and chromium in a ratio of (1.5-2.5):1 by weight.

4. The layered double hydroxide material according to claim 1, wherein The metal composite material comprises iron and chromium in a ratio of (0.7-1):1 by weight.

5. The layered double hydroxide material according to claim 1, wherein The average diameter of the monodisperse microspheres is 100 nm to 300 nm.

6. The layered double hydroxide material according to claim 1, wherein The metal composite material also includes a nickel substance.

7. A catalytic material comprising the layered double hydroxide material according to any one of claims 1 to 6, and optionally a matrix.

8. The catalytic material according to claim 7, which is in the form of nanodots.

9. An electrode comprising a conductive substrate and a catalytic material coated on the surface of the conductive substrate, wherein the catalytic material comprises the layered double hydroxide material according to any one of claims 1 to 6.

10. The electrode according to claim 9, wherein The conductive matrix is ​​foamed metal.

11. The electrode according to claim 9 or 10, wherein The conductive matrix is ​​nickel foam.

12. A method for preparing the catalytic material of claim 7 or the electrode of any one of claims 9 to 11, the method comprising contacting a conductive substrate with a solution comprising cobalt ions, iron ions and chromium ions, and applying a voltage to the substrate and a counter electrode through the solution to electrodeposit a composite material comprising cobalt, iron and chromium substances on the substrate.

13. A method for preparing the catalytic material of claim 7 or 8, the method comprising treating a solution containing cobalt ions, iron ions and chromium ions at a temperature of 150°C to 220°C for 8 hours to 20 hours, cooling the mixture and collecting the product.

14. The method according to claim 12 or 13, wherein: The solution also includes nickel, and the catalytic material includes cobalt, iron, chromium and nickel species.

15. A method of releasing oxygen from water, the method comprising providing an electrochemical cell comprising an anode, a cathode and an electrolyte solution, contacting water with the anode and the cathode, and applying a voltage between the anode and the cathode, wherein: The anode comprises the layered double hydroxide material of any one of claims 1-6 or the catalytic material of claim 7 or 8 or the electrode of any one of claims 9-11.

16. The method according to claim 15, wherein: The anode voltage provides an overpotential of 200 mV to 500 mV.

17. The method according to claim 15, wherein: The electrochemical cell also includes a reference electrode.

18. An electrolytic cell comprising an anode, a cathode and a power supply, wherein: The anode comprises the layered double hydroxide material of any one of claims 1-6 or the catalytic material of claim 7 or 8 or the electrode of any one of claims 9-11.

19. The electrolytic cell of claim 16, further comprising a reference electrode.