Cathode active material with silicon carbide additive
By adding silicon carbide particles to the cathode material of the lithium battery to form a conductive path, the problem of insufficient energy density and magnification capacity of the cathode material after the thickness increases in the prior art is solved, and the electrochemical performance and diffusion characteristics of the lithium battery are significantly improved.
Patent Information
- Application Number
- CN202011058698.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-04
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-09-30
AI Technical Summary
It is difficult for existing lithium battery cathode materials to achieve high energy density and high magnification capabilities at the same time after increasing the thickness, and the electronic conductivity and lithium ion diffusion efficiency are insufficient.
Using a composite material of lithium transition metal-based particles and silicon carbide particles, the silicon carbide particles reside at the grain boundary of the lithium transition metal particles to form a conductive pathway to improve ions and electron diffusion in the cathode.
The electrochemical performance of lithium batteries is improved, the electron and ion conductivity is enhanced, the rate performance and diffusion characteristics are achieved, and the dense microstructure is maintained after high-temperature heat treatment.
Smart Images

Figure CN112909225B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a cathode active material for a lithium battery, the cathode active material including a silicon carbide additive. Background Art
[0002] Lithium batteries use cathode active materials to release and store cations during charging and discharging operations, respectively. Such cathode active materials may include transition metal oxides and phosphates, which are generally used to exchange lithium cations with electrolytes. However, transition metal oxides and phosphates with excellent performance as cathode active materials are increasingly reaching their performance limits. Increasing cathode thickness is one of the most effective ways to develop lithium batteries with improved energy density. It has been found that thick cathodes increase battery cell polarization and underutilize active materials. The former is affected by electronic conductivity, while the latter is affected by lithium ion diffusion in active materials. Therefore, it is still necessary to develop cathode materials that meet the requirements of high energy density and high rate capability while meeting thick cathodes (5um-50um for solid electrolytes) and ultra-thick cathodes (greater than 150um for liquid electrolytes). Summary of the invention
[0003] Disclosed herein is a specific implementation of a cathode material for a lithium battery, the cathode material comprising lithium transition metal-based particles and silicon carbide particles, the lithium transition metal-based particles being selected from lithium transition metal oxides and lithium transition metal phosphates, the silicon carbide particles residing at grain boundaries of the lithium transition metal-based particles, thereby forming conductive pathways along the grain boundaries.
[0004] The silicon carbide particles can each have a longest dimension of less than 100 nm.
[0005] The silicon carbide particles may be less than 10% by weight of the cathode material.
[0006] The silicon carbide particles may be less than 1% by weight of the cathode material.
[0007] The silicon carbide particles may have an aspect ratio of 1 to 25.
[0008] The silicon carbide particles may be nanofiber particles.
[0009] The silicon carbide nanofiber particles may have an aspect ratio between 5 and 25, inclusive.
[0010] The cathode materials disclosed herein may have an internal pore volume of 0-50%.
[0011] Also disclosed herein is a lithium battery comprising the cathode material disclosed herein. The lithium battery may be a lithium metal battery having one or more lithium metal battery cells. The lithium battery may be a lithium ion battery having one or more lithium ion battery cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The following detailed description is best understood in conjunction with the accompanying drawings when reading this disclosure. It should be emphasized that, according to convention, the various features of the drawings are not to scale. On the contrary, the sizes of the various features may be arbitrarily enlarged or reduced for clarity.
[0013] Figure 1A is a high-resolution TEM image showing bulk grains of LCO and crystal grain boundaries containing silicon carbide located between the bulk grains.
[0014] Figure 1B for Figure 1A A magnified image of a portion of .
[0015] Figure 1C for Figure 1A A magnified image of another portion of the .
[0016] Figure 2A High-resolution SEM image of the LCO cathode material after heat treatment.
[0017] Figure 2B is a high resolution SEM image of LCO and 0.5 wt. % SiC after heat treatment as disclosed herein.
[0018] Figure 3A The discharge curve of a lithium battery cell using LCO cathode material.
[0019] Figure 3B : The discharge curve of a lithium battery cell using LCO and 1.0 wt % SiC as cathode materials.
[0020] Figure 4 is a plan view of a lithium battery cell according to an embodiment.
[0021] Figure 5 For use Figure 4 Schematic diagram of a side view of the layers of a lithium battery cell.
[0022] Fig. 6A is a perspective view of a solid-state battery cell according to an embodiment.
[0023] Figure 6B for Fig. 6A An exploded view of a solid-state battery cell. DETAILED DESCRIPTION
[0024] Electrochemically active cathode materials in their pure form (e.g., commercially available LiCoO2) may not provide sufficiently high lithium ion diffusion and electronic conductivity. Improved cathode performance of both pure and composite cathodes requires, in part, a high effective diffusion coefficient inside the cathode. During cell discharge, mass and charge transport inside the cathode allows as much electrochemically active material (ions and electrons) as possible to be inserted into the cathode in the shortest possible time and into the cathode location farthest from the cathode-electrolyte interface. Fast ion grain boundary conduction can effectively provide ions to and from the locations of the electrochemical reactions responsible for capacity and energy storage, which are located inside the grain bulk. The cathode material for a lithium battery disclosed herein improves ion and electron diffusion within the cathode by providing a silicon carbide additive that provides paths around and between bulk grains of the cathode active material.
[0025] The small grain size of the active cathode material is beneficial to shorten the migration path of lithium ions and electrons during lithiation / delithiation, and thus improve the electrochemical performance. The lithium battery cathode material disclosed herein includes a silicon carbide additive that inhibits grain growth and provides a very dense cathode microstructure.
[0026] The lithium battery cathode material disclosed herein comprises a lithium transition metal-based material and crystalline silicon carbide, wherein the lithium transition metal-based material is selected from lithium transition metal oxides and lithium transition metal phosphates, and the crystalline silicon carbide resides at the grain boundaries of the lithium transition metal-based material, thereby forming a conductive path along the grain boundaries.
[0027] The lithium transition metal based material may be a lithium ion intercalation compound such as LiMO2 and LiM x O y Lithium transition metal oxides, and lithium transition metal phosphates having the general formula LiMPO4, wherein M is one or more transition metal cations. As non-limiting examples, the lithium transition metal-based materials may include: layered materials such as LiCoO2, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 and LiNi 0.8 Co 0.15 Al 0.05 O2; olivine type materials, such as LiFePO4; spinel type materials, such as LiMn2O4; and other similar materials.
[0028] The crystalline silicon carbide resides at the grain boundaries of the lithium transition metal-based material, thereby forming a conductive path along the grain boundaries. Figures 1A to 1CAs can be seen in FIG. 1 , LiCoO 2 (LCO) is used as the lithium transition metal-based material and contains 0.5 wt % silicon carbide, which is annealed at 800° C. Figure 1A is a high resolution TEM image showing crystalline silicon carbide 10 along the grain boundaries between bulk LCO 12. The silicon carbide resides at the grain boundaries and surrounds the grains at the nanometer scale. Figure 1B and Figure 1C yes Figure 1A The width between bulk particles of the silicon carbide conductive path is about 20 nm or less, 10 nm or less, and may be 5 nm or less.
[0029] Silicon carbide is mixed with lithium transition metal based materials or their precursors and processed to form a cathode film. The silicon carbide does not decompose even after high temperature heat treatment and is incorporated into active materials such as Figures 1A to 1C After annealing of the cathode material, the crystalline silicon carbide is located between bulk grains of the lithium transition metal-based material, thereby surrounding the grains of the lithium transition metal-based material and providing a conductive path through the cathode material.
[0030] The silicon carbide facilitates compaction of the cathode material without causing significant grain growth, which typically occurs during high temperature compaction.It has been found that heat treatments as low as 700°C can produce very dense microstructures. Figure 2A and Figure 2B High-resolution SEM images of LCO without SiC and LCO with 0.5 wt.% SiC, respectively. Figure 2A The pure LCO in the annealing is at 850 ° C, while the LCO with silicon carbide is annealed at 800 ° C. The density of the LCO with SiC additive is greater than 95% of the theoretical density, while the LCO without additive is less than 90% of the theoretical density, and the LCO with SiC additive has a grain size of 500nm or less, while the LCO without SiC additive has a grain size of greater than 2000nm.
[0031] The silicon carbide particles in the disclosed cathode material can be any particle shape having a longest dimension less than 100 nm. The silicon carbide particles can be spherical or filamentous or fibrous with an aspect ratio (L / D) of 1 to 25. In some embodiments, the silicon carbide particles are nanofibers having an aspect ratio between 5 and 25, inclusive.
[0032] Silicon carbide is not electrochemically active, so the amount used should be sufficient to provide nanoscale conductive pathways around the bulk active material. The silicon carbide may be less than 10% by weight of the cathode material. In some embodiments, the silicon carbide may be less than 1% by weight of the cathode material.
[0033] Lithium batteries using the cathode materials disclosed herein achieve better rate capabilities and improved diffusion characteristics. Figure 3A is the discharge curve of a battery cell formed with a 10 μm thick LCO wafer, and Figure 3B 1 is the discharge curve of a cell formed with a 10 μm thick LCO wafer and 1 wt% SiC. The mixture of LCO and SiC was deposited on a solid electrolyte or substrate by dry spraying. The as-deposited film was then annealed at high temperature. The cathode film was then cycled against metallic lithium at 0.2C (cycles 1 and 2), 0.5C (cycle 3), 1C (cycle 4), and 2C (cycle 5). Figure 3B The relatively flat discharge curves and minimal voltage drop at different discharge rates shown in indicate enhanced electronic and ionic conductivity in cells using the cathode materials disclosed herein.
[0034] The cathode materials disclosed herein can be used with all-solid-state batteries having all solid components. The cathode materials disclosed herein can also be used in lithium-ion batteries having non-metallic lithium anodes containing liquid or solid electrolytes and lithium metal batteries containing liquid, solid or gel electrolytes.
[0035] A lithium battery can be prepared according to the following method. As a non-limiting example, the cathode can be prepared using the cathode material disclosed herein. The cathode current collector having a cathode active layer formed thereon can be prepared by directly coating the cathode active material composition on the cathode current collector using dry spraying and deposition such as PVD and CVD (as a non-limiting example), and the cathode current collector can be, for example, an aluminum sheet or aluminum foil. The cathode active layer can also be cast on a separate support to form a film, and then the cathode can be prepared by separating the film from the support and laminating the separated film on the cathode current collector.
[0036] Anodes can be prepared from available anode active materials and optional binders and / or solvents. The binder can be any suitable binder, such as one or more of the following: vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, poly(methyl methacrylate), polytetrafluoroethylene (PTFE) and styrene-butadiene rubber-based polymers. The solvent can be any suitable solvent, such as one or more of the following: N-methyl pyrrolidone (NMP), acetone and water.
[0037] Exemplary anode active materials include: elemental materials, such as lithium; alloys, including alloys of Si, Sn, Al, Ge, Pb, Bi and Sb or other lithium compounds; and embedded host materials, such as carbon-based materials. The carbon-based material may include one or more of crystalline carbon and amorphous carbon. The crystalline carbon may include one or more graphites, such as, for example, amorphous, plate-like, flaky, spherical or fibrous graphite, wherein the graphite may be natural graphite or artificial graphite. Amorphous carbon may include one or more of the following: soft carbon (e.g., low-temperature roasted carbon), hard carbon, mesophase pitch carbide and roasted coke. For example, the anode can be prepared by sputtering or evaporating a metal anode to form an anode active material composition on an anode current collector, which may be, for example, a copper sheet or copper foil. The anode can also be prepared by casting the anode active material composition on a separate carrier to form a film, then separating the film from the separate carrier, and laminating the separated film onto the anode current collector.
[0038] A separator, if used, may be inserted between the cathode and the anode. The separator is not particularly limited, and any separator may be used. A separator having a high moisture retention capacity for the electrolyte and / or a low resistance to electrolyte ion transfer may be used. The separator may include, for example, one or more of the following: glass fiber, polyester, Teflon, polyethylene, polypropylene, and polytetrafluoroethylene (PTFE). The separator may be a nonwoven fabric or a woven fabric type. The electrolyte is not particularly limited, and the electrolyte may be a liquid electrolyte, a gel, and / or a solid. For example, the liquid electrolyte may be in the form of a solution in which a lithium salt is dissolved in an organic solvent. The gel electrolyte may be in the form of a gel in which the above-mentioned liquid electrolyte is impregnated into a matrix polymer consisting of an ion-conducting polymer.
[0039] Figure 4A plan view of a lithium battery cell 100 according to an embodiment is illustrated; the lithium battery cell 100 includes a stack 102, which includes multiple layers including a cathode, a separator, an electrolyte, and an anode. These layers can remain flat in a planar configuration or can be wound into a winding configuration (e.g., a "jelly roll"), but other configurations are also possible. A flexible pouch is formed by folding a flexible sheet along a fold line 112. For example, the flexible sheet can be made of aluminum with a polymer film (such as polypropylene). After folding the flexible sheet, the flexible sheet can be sealed, for example, by applying heat along the side seal 110 and along the platform seal 108. The stack 102 also includes a set of conductive leads 106 coupled to the cathode and the anode. The conductive lead 106 can extend through the seal in the pouch to provide a terminal for the battery cell 100. Then, the conductive lead 106 can be used to electrically couple the battery cell 100 with one or more other battery cells to form a battery pack. The lithium battery can be combined in a battery pack in any configuration. For example, a battery pack may be formed by coupling battery cells in series, parallel, or a series-parallel configuration.
[0040] Figure 5 1 is a schematic diagram of a side view of the layers for the lithium battery cell 100 of Figure 1. The layers may include a cathode current collector 202, a cathode active coating 204, a separator 206, an anode active coating 208, and an anode current collector 210. The cathode current collector 202 and the cathode active coating 204 may form the cathode of the lithium battery cell, and the anode current collector 210 and the anode active coating 208 may form the anode of the lithium battery cell.
[0041] Fig. 6A is a perspective view of an example of a solid-state lithium battery 300, and Figure 6B 300 is an exploded view of the layers of a solid-state lithium battery 300. The solid-state lithium battery 300 has an anode current collector 302, an anode 304, a solid electrolyte 306, a cathode 308, a cathode current collector 310, and an optional substrate 312. These layers may be sequentially deposited as thin layers on the substrate 312. These layers are encapsulated with an encapsulation material 314. Alternatively, the cathode 308 and / or the cathode current collector 310 may have sufficient mechanical strength to support these layers, so that a substrate 312 is not required. The cathode 308 is a cathode material disclosed herein. The anode material may be lithium metal or may be other materials listed above. As a non-limiting example, the solid electrolyte may be a sulfur-containing compound (e.g., argyrodite, LGPS, LPS, etc.), a garnet structure oxide (e.g., LLZO with various dopants), a NASICON-type phosphate glass ceramic (LAGP), a nitride oxide (e.g., lithium phosphorus oxynitride or LIPON), and a polymer (PEO).
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those of ordinary skill in the art to which the present disclosure belongs. Preferred methods, techniques, equipment, and materials are described, but any methods, techniques, equipment, or materials similar or equivalent to the described methods, techniques, equipment, or materials may be used in the practice or testing of the present disclosure. The structures described herein are also understood to refer to the functional equivalents of such structures.
[0043] It should be noted that, as used herein and in the appended claims, the singular forms "a", "an", and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "an element" refers to one or more elements and includes equivalents thereof known to those skilled in the art.
[0044] While the present disclosure has been described in conjunction with certain embodiments, it should be understood that the present disclosure is not limited to the disclosed embodiments, but on the contrary, it is intended to cover various modifications and equivalent arrangements included within the scope of the appended claims, which scope is to be given the broadest interpretation so as to encompass all such modifications and equivalent structures permitted by law.
Claims
1. A cathode material for a lithium battery, comprising: Lithium transition metal-based particles selected from lithium transition metal oxides and lithium transition metal phosphates; and Silicon carbide resides at grain boundaries of the lithium transition metal based particles to form conductive paths along the grain boundaries, wherein the silicon carbide does not decompose and does not bond with the lithium transition metal based particles, wherein the width of the conductive paths between the lithium transition metal based particles is 5 nm or less.
2. The cathode material of claim 1, wherein the silicon carbide particles each have a longest dimension less than 100 nm.
3. The cathode material of claim 1, wherein the silicon carbide is less than 10% by weight of the cathode material.
4. The cathode material of claim 1, wherein the silicon carbide is less than 1 wt% of the cathode material. 5 . The cathode material of claim 1 , wherein the silicon carbide particles have an aspect ratio of 1 to 25. The cathode material of claim 1 , wherein the silicon carbide is in the form of nanofiber particles.
7. The cathode material of claim 6, wherein the nanofiber particles have an aspect ratio between 5 and 25, inclusive.
8. The cathode material according to claim 1, which has a density greater than 95% of the theoretical density of LiCoO2 and a grain size less than 500 nm after high temperature heat treatment.
9. A lithium metal battery cell comprising: A cathode comprising the cathode material according to claim 1; an anode comprising a lithium compound; and Electrolytes.
10. The lithium metal battery cell of claim 9, wherein the cell is an all-solid-state cell.
11. A lithium-ion battery cell comprising: A cathode comprising the cathode material according to claim 1; an anode comprising one or more of: a metal and a metalloid capable of forming an alloy with lithium, an alloy thereof, or an oxide thereof, and a carbon material; and One or more of a liquid electrolyte, a gel electrolyte and a polymer electrolyte.
12. A lithium battery cathode material, comprising: Lithium transition metal-based particles selected from lithium transition metal oxides and lithium transition metal phosphates; and Crystalline silicon carbide, the crystallized silicon carbide residing at the grain boundaries of the lithium transition metal based particles to form a conductive path along the grain boundaries, the crystallized silicon carbide being less than 10 weight percent of the cathode material, wherein the crystallized silicon carbide does not decompose and does not bond to the lithium transition metal based particles, wherein the width of the conductive path between the lithium transition metal based particles is 5 nm or less.
13. The lithium battery cathode material of claim 12, wherein the crystalline silicon carbide is 1 wt% or less of the cathode material.
14. The lithium battery cathode material according to claim 12, wherein the crystalline silicon carbide is in the form of nanofibers.
15. The lithium battery cathode material of claim 12, wherein the crystalline silicon carbide material has a longest dimension less than 100 nm. 16 . The lithium battery cathode material of claim 12 , wherein the crystalline silicon carbide material has an aspect ratio of 1 to 25.
17. The lithium battery cathode material according to claim 12, which has a density greater than 95% of the theoretical density of LiCoO2 and a grain size less than 500 nm after high temperature heat treatment.