Sustained and easily separable cathode products from molten carbonate electrolysis

By controlling the electrolysis conditions and using a compression process to separate carbon nanomaterials during the molten carbonate electrolysis process, the problem of separation of solid carbon formed at the cathode from the electrolyte is solved, an efficient and sustainable separation effect is achieved, and waste of heat and electrolyte is avoided. High-quality carbon nanomaterials are provided.

CN112955586BActive Publication Date: 2024-10-29C2CNT LLC
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN201980071441.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-29
Publication Date
2024-10-29
Estimated Expiration
2039-10-29

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively separate the solid carbon nanomaterials formed at the cathode from the electrolyte during the molten carbonate electrolysis process, resulting in waste of heat and electrolyte, and the separation method is not sustainable and cost-effective.

Method used

By controlling electrolysis conditions, carbon nanomaterials are deposited on the cathode, and a compression process is used to separate the solid carbon product and the electrolyte mixture at a temperature higher than the melting point of the electrolyte. Vacuum and an interface with holes are used for electrolyte removal to ensure that the structure of the carbon nanomaterials is not destroyed. .

Benefits of technology

Effective separation of solid carbon products is achieved, reducing heat and electrolyte waste, providing cleaner and more useful nanomaterials, and improving the sustainability and economic benefits of the separation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112955586B_ABST
    Figure CN112955586B_ABST
Patent Text Reader

Abstract

A method for separating electrolyte from carbon in a solid carbon / electrolyte cathode product formed at the cathode during molten carbonate electrolysis. The method allows for easy separation of the solid carbon product from the electrolyte without any observed detrimental effects on the structure and / or stability of the resulting solid carbon nanomaterial.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application No. 62 / 752,141, filed on October 29, 2018, the entire contents of which are incorporated herein by reference. Field of the Invention

[0003] The present invention relates to an improved method for separating electrolyte from carbon in a solid carbon / electrolyte cathode product formed at the cathode during molten carbonate electrolysis. The method described herein allows for easy separation of the solid carbon product from the electrolyte without any observed detrimental effects on the structure and / or stability of the resulting solid carbon product. Background of the Invention

[0005] A method of improving the adverse consequences of elevated carbon dioxide levels is to convert carbon dioxide into useful products. Various methods of converting carbon dioxide into carbon nanomaterials such as carbon nanotubes, carbon nanofibers, carbon nano-onions, carbon scaffolds, carbon sheets and graphene (see, for example, cited documents 1-6 listed herein) have been described by electrolysis of molten carbonate. For example, carbon nanotubes can be formed by electrolysis in molten lithium carbonate (melting point 723°C) or in a related mixture (including alkali or alkaline earth carbonates, with or without oxides, borates, phosphates, sulfates, nitrates, chlorides or other inorganic salts). During the electrolysis, carbon nanomaterials are usually deposited on the electrolysis cathode, but are bound to the cathode with an excess of electrolyte.

[0006] Some methods explored for separating carbon from carbonate electrolytes in the resulting product include various water washes or drawing the molten electrolyte through a mesh with BNZ (calcium aluminum silicate) refractory bricks (see, for example, Reference 2). The water wash method requires cooling and heat is reversibly lost from the electrolytic cell. Aqueous and molten refractory brick extractions consume large amounts of material, which is detrimental to the sustainability of the overall carbon dioxide removal process. For example, aqueous separation can be achieved by adding large amounts of water and additives such as ammonium sulfate or formic acid or hydrochloric acid to promote the dissolution of carbonates into the aqueous phase for separation from the solid carbon product. For the (molten) solid carbon / electrolyte product, the refractory bricks act by drawing the molten carbon electrolyte through a chemical reaction with the aluminate or silicate components of the refractory bricks. These refractory brick components are consumed during the separation, for example, without being bound by any theory or specific equation, the reaction of the refractory brick material that consumes lithium carbonate is exemplified by the consumption of alumina and silica, respectively, to produce lithium aluminate and lithium orthosilicate or lithium metasilicate:

[0007] Li2CO3+Al2O3→2LiAlO2+CO2(releases gas) (1)

[0008] 2Li2CO3+SiO2→Li4SiO4+2CO2(releases gas) (2a)

[0009] Li2CO3+SiO2→Li2SiO3+CO2(releases gas) (2b)

[0010] Carbon nanotubes are flexible and have the highest tensile strength of any material measured to date (see, e.g., citations 7 and 8 listed herein). Recently, it has been observed that the carbon product of molten carbonate electrolysis can consist of a matrix of incorporated carbon nanotubes (see, e.g., citation 2 listed herein).

[0011] Therefore, new and efficient methods are needed to separate electrolyte from solid carbon nanomaterials formed at the cathode during electrolysis, thereby providing more sustainable (e.g., preventing heat and electrolyte waste), more cost-effective methods and providing cleaner, more useful nanomaterials. Summary of the invention

[0012] The present invention relates to an improved method for separating carbon products from a solid carbon / molten electrolyte mixed product (carbonate gel) formed, for example, at a cathode during a carbonate electrolysis reaction.

[0013] Various carbon nanomaterials can be deposited on the cathode by controlling the electrolysis conditions. During deposition, the carbon formed at the cathode shows a strong affinity for the electrolyte, and the cathode product contains a mixture of solid carbon and molten electrolyte. The deposited cathode product is a paste or gel at a temperature above the melting point of the electrolyte, or when the cathode is removed and cooled to room temperature, the cathode product is a solid mixture of carbon and condensed electrolyte. In either case, compared with carbon, the cathode deposition contains most of the electrolyte by mass. During electrolysis, a solid carbon product / electrolyte mixture is spontaneously formed on the cathode in real time, rather than after solid carbon is formed. The solid product is not removed from the cathode and then forms a slurry with the electrolyte. The paste is black (and red hot) and is clearly distinguished from the transparent molten electrolyte between the electrodes and in the electrolysis chamber. The product is a thick paste layer on the cathode that grows as the electrolysis continues. Depending on the electrolysis conditions, the percentage of electrolyte in the slurry containing the cathode product is 70% to 97% by weight, and typically 90% to 97% by weight.

[0014] The present inventors unexpectedly discovered that a solid carbon product can be separated from a solid carbon / molten electrolyte mixed product (carbonate gel) by a compression process, and that the carbonate gel formed on the cathode during a molten carbon carbonate electrolysis reaction can be repeatedly compressed without any observed deleterious effect on the structure and / or stability of the resulting solid carbon nanomaterial, thereby allowing the desired solid carbon product to be effectively separated.

[0015] Typically, individual carbon nanomaterials have a diameter of less than 500 nm. The inventors have also unexpectedly found that carbon nanotubes (whose height is greater than, for example, 500 nm) comprising a matrix of highly porous, intermingled carbon nanotubes can be repeatedly compressed to a fraction of their initial volume without destroying the structure of the carbon nanomaterial (see, for example, citations 9-11 listed herein).

[0016] Typically, during the electrolysis reaction, the desired carbon product forms a thick paste on the cathode (not released into the free circulating electrolyte). The paste includes solid carbon products and bound electrolyte. In the method described herein, the paste containing the solid carbon product is separated from the bound electrolyte. The electrolyte in the paste is fixed and separated from the free electrolyte located in the electrolysis chamber.

[0017] In one aspect, the present invention relates to a method for preparing a solid carbon product. In one embodiment, the method comprises separating electrolyte from a solid carbon / molten electrolyte mixed product ("carbonate gel") formed during carbonate electrolysis. In one embodiment, the method comprises:

[0018] (i) applying force to the solid carbon / molten electrolyte mixed product to remove the electrolyte;

[0019] (ii) removal force; and

[0020] (iii) optionally, isolating the solid carbon product.

[0021] In one embodiment of any of the methods described herein, steps (i) and (ii) are repeated one or more times, such as two, three or four times, prior to step (iii).

[0022] In certain embodiments of any of the methods described herein, the force (compression) is applied manually, pneumatically, or hydraulically.

[0023] In certain embodiments of any of the methods described herein, the force (compression) is performed at a pressure of about 10 psi to about 100,000 psi, such as about 50 psi to about 50,000 psi, or about 100 psi to about 1,000 psi.

[0024] In certain embodiments of any of the methods described herein, the electrolyte is removed through an interface having pores, such as a filter, porous carbon felt, graphite felt, metal mesh, porous or sieved ceramic, or any combination thereof.

[0025] In one embodiment, the pore size of the interface is smaller than the solid carbon matrix product size. For example, the pore size of the interface may be from about 10 μm to about 10 mm, such as from about 50 μm to about 5 mm or from about 70 μm to about 3 mm.

[0026] In one embodiment of any of the methods described herein, the method is performed in a vacuum (ie, by applying a vacuum during the separation / extraction process). In one embodiment, the vacuum enhances the removal of the electrolyte and the separation of the solid carbon product.

[0027] In one embodiment of any of the methods described herein, the applied vacuum is from about 0.1 to about 0.9 atmospheres.

[0028] In another embodiment of any of the methods described herein, the applied vacuum is greater than about 0.8 atmospheres, or greater than about 0.9 atmospheres, such as from about 0.8 to about 0.999 atmospheres, or from about 0.9 to about 0.99 atmospheres.

[0029] In another embodiment of any of the methods described herein, the method is performed at a pressure of about 0.1 to about 0.9 atmospheres, such as about 0.2 to about 0.9 atmospheres.

[0030] In another embodiment of any of the methods described herein, the method is performed at a pressure of less than about 0.1 atmospheres, such as less than about 0.01 atmospheres.

[0031] In one embodiment of any of the methods described herein, the applied vacuum is from about 0.01 MPa to about 0.1 MPa, such as from about 0.05 MPa to about 0.1 MPa, such as about 0.09 MPa.

[0032] In another embodiment of any of the methods described herein, the method is carried out in the absence of oxygen, such as under a blanket of a gas that is free of or substantially free of oxygen (a gas excluding oxygen). For example, in one embodiment, a gas excluding oxygen blankets the mixed product to protect the solid carbon product from oxidation.

[0033] In certain embodiments, the oxygen-excluding gas is an inert non-oxidizing gas, such as nitrogen, carbon dioxide, argon; or a reducing gas, such as methane, ammonia, hydrogen, and hydrogen sulfide, and any combination of any of the foregoing.

[0034] In another embodiment of any of the methods described herein, the method is carried out at a temperature of about 399° C. to about 900° C., such as about 700° C. to about 900° C. In another embodiment of any of the methods described herein, the method is carried out at a temperature of about 399° C., about 723° C., or about 891° C., which correspond to the melting points of eutectic lithium sodium potassium carbonate, lithium carbonate, and pure potassium carbonate, respectively.

[0035] In another embodiment of any of the methods described herein, the mixed product is cooled below freezing point, such as below 700° C., after being formed by electrolysis and then reheated / melted prior to one or more compression steps in the methods described herein.

[0036] In other embodiments of any of the methods described herein, the solid carbon / molten electrolyte mixed product is compressed directly on a cathode in an electrolysis chamber.

[0037] In one embodiment of any of the methods described herein, the solid carbon / molten electrolyte mixed product is removed from the cathode.

[0038] In another embodiment of any of the methods described herein, the solid carbon / molten electrolyte mixed product is removed from the cathode in the electrolysis chamber, e.g., without pumping, into a separate extraction compression chamber, prior to separation of the solid product.

[0039] In another embodiment of any of the methods described herein, the method does not involve flowing electrolyte.

[0040] In another embodiment of any of the methods described herein, the method does not involve a recirculation loop.

[0041] In another embodiment of any of the methods described herein, the resulting solid carbon product has an average thickness greater than 10 μm, eg, greater than 0.3 mm, greater than 1 mm, or greater than 3 mm.

[0042] In another embodiment of any method described herein, the solid carbon product obtained comprises greater than about 80% carbon nanomaterial, such as greater than about 85%, greater than about 90%, or greater than about 95% carbon nanomaterial. In a preferred embodiment, the carbon nanomaterial is a carbon nanotube, a carbon nanoonion, a carbon nanosheet, a carbon nanoscaffold, a graphene, or any combination thereof.

[0043] In another embodiment of any of the methods described herein, no morphological template is present on the cathode during the formation and / or separation (compression) of the solid carbon / molten electrolyte mixed product.

[0044] In another aspect, the invention relates to a chamber for performing any of the methods described herein.

[0045] In one embodiment, the present invention relates to an extraction chamber for separating electrolyte from a solid carbon / molten electrolyte mixed product formed during carbonate electrolysis, the extraction chamber comprising

[0046] (i) solid carbon / molten electrolyte mixed products formed during carbonate electrolysis;

[0047] (ii) a compression device for compressing the solid carbon / molten electrolyte mixed product;

[0048] (iii) a removal device configured to remove the compression;

[0049] (iv) an interface having pores through which electrolyte separated from the mixed product during compression is collected; and

[0050] (v) Optionally, a vacuum is applied to the extraction chamber.

[0051] In one embodiment, the extraction chamber is rectangular or circular.

[0052] In one embodiment, the extraction chamber is operated in vertical mode.

[0053] In one embodiment, the extraction chamber is operated in horizontal mode.

[0054] In one embodiment, the extraction chamber is operated in angle mode.

[0055] In one embodiment, the extraction chamber operates within a kiln.

[0056] In one embodiment, the extraction chamber is located together with the electrolysis chamber. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1A is a block diagram showing separation of solid carbon from a solid carbon / electrolyte cathode product of an electrolyte and a molten carbonate electrolysis reaction at a cathode in an electrolysis chamber.

[0058] Figure 1B is a block diagram showing the separation of electrolyte from the solid carbon in the solid carbon / electrolyte cathode product of the molten carbonate electrolysis reaction in an extraction chamber (not at the cathode in the electrolysis chamber).

[0059] FIG. 2A to FIG. 2E Various shapes of suitable extraction chambers for use in the methods described herein are shown.

[0060] Figure 3A An exemplary rectangular extraction chamber for use in the methods described herein is shown.

[0061] Figure 3B An exemplary circular extraction chamber for use in the methods described herein is shown.

[0062] Figure 3C An exemplary extraction chamber for use in the methods described herein is shown operating in a vertical mode.

[0063] Figure 3D An exemplary extraction chamber for use in the methods described herein is shown operating in horizontal mode.

[0064] FIG. 4A to FIG. 4E An exemplary extraction chamber for collecting coarse material from an electrode according to the methods described herein is shown, wherein the extraction chamber is positioned at an angle and directly engages an electrolysis chamber.

[0065] Figure 5 An exemplary extraction chamber for use in the methods described herein is shown, which can be operated with or without a vacuum system to separate the electrolyte in a vacuum.

[0066] FIG. 6A to FIG. 6C The pressure applied to the extraction chamber used in the method described herein by mechanical, pneumatic or hydraulic pressure is shown.The extraction unit is inside the kiln.

[0067] 7A to 7E An exemplary product extractor and extraction process located within an electrolysis chamber is shown. DETAILED DESCRIPTION

[0068] When describing the exemplary, non-limiting embodiments of the present invention shown in the accompanying drawings, specific terms will be used for the sake of clarity. However, the present invention is not intended to be limited to the specific terms so selected, and it should be understood that each specific term includes all technical equivalents that operate in a similar manner to achieve similar purposes. Several embodiments of the present invention are described for illustrative purposes, and it should be understood that the present invention can be implemented in other forms not specifically shown in the accompanying drawings.

[0069] U.S. Publication Nos. 2019 / 0039040 and 2018 / 0044183, which are incorporated herein by reference in their entireties, describe the synthesis of carbon nanomaterials via electrolysis in a molten electrolyte containing a carbonate.

[0070] As used herein, the term "carbonate gel" refers to a product similar to an aerogel, wherein the air in the aerogel is replaced by molten carbonate. For example, a carbonate gel contains a majority of molten carbonate and a solid matrix component admixed therewith. For sustainable and efficient carbon dioxide decomposition, it is necessary to separate the electrolyte trapped in the carbonate gel product of molten carbonate electrolysis so that it can be further used in electrolysis.

[0071] As used herein, a gas that is "substantially free of oxygen" means a gas that contains less than about 1000 ppm of oxygen, e.g., less than about 500 ppm, less than about 400 ppm, less than about 300 ppm, less than about 200 ppm, less than about 100 ppm, less than about 50 ppm, less than about 25 ppm, less than about 10 ppm, less than about 5 ppm, or less than about 1 ppm of oxygen.

[0072] Figure 1A 1 is a diagram of an exemplary extraction system 100 for separating electrolyte from solid carbon in a solid carbon / electrolyte product formed at a cathode during a molten carbonate electrolysis reaction. System 100 includes a force applicator 102, a solid carbon / electrolyte product 104, a cathode 106, a filter or interface having pores 108, and electrolyte 110 pressed from the solid carbon / electrolyte product. Figure 1A In one embodiment, the interface 108 with holes is shown on the side of the solid carbon electrolyte product 104, but it should be understood that if the cathode includes a porous material, the interface 108 with holes can also be an integral part of the cathode, in which case the squeezed electrolyte 110 is then pushed through the back side of the cathode 106 and pushed out the back side of the cathode 106.

[0073] More specifically, the system 100 can be a chamber, such as an extraction chamber. The chamber 100 can be formed as a single shell or container 101 having an interior. As shown, the container 101 can be elongated, having a bottom, two lateral sides or walls, and two longitudinal sides or walls, which have a substantially rectangular cross-section and define a central longitudinal axis (extending along the length of the container 101), although any suitable shape and size can be used. The top of the container 101 is open, although a cover with a hole can be optionally placed on at least two side sections 101a, 101c of the container 101. The lateral walls extend substantially orthogonal to the longitudinal axis, while the longitudinal sides extend substantially parallel to the longitudinal axis.

[0074] One or more partitions or separators, such as filters, membranes or interfaces, are received inside the container 101. Here, the first interface 108a has a first side and a second side opposite to the first side. The first side of the first interface 108a faces one lateral side of the container 101 to define a first section 101a inside the container 101 between the first side of the first interface 108a and the lateral side of the container 101. The second interface 108b has a first side and a second side opposite to the first side. The first side of the second interface 108b faces the second side of the first interface 108a to define a second section 101b inside the container 101 between the first side of the second interface 108b and the second side of the first interface 108a. The second side of the second interface 108b faces the other lateral side of the container 101 to define a third section 101c inside the container 101 between the second side of the second interface 108b and the other lateral side of the container 101. The central section 101b forms an extraction chamber or container, and the two side sections 101a, 101c each form a collection chamber or container.

[0075] As shown, each segment 101a, 101b, 101c can have a substantially square cross-section, although any suitable shape and size can be used. The interface 108 is relatively thin and can form a plate with two relatively flat and planar opposite sides (or two plates with filter material therebetween), and can have a plurality of holes that allow material to reach one of the two outer segments 101a, 101c from the center segment 101b through the interface 108. The interface 108 extends substantially transversely to the longitudinal axis of the container over the entire width and height, and is parallel to the lateral sides of the container 101, so that the material in the center segment 101b cannot be transferred to the outer segments 101a, 101c, unless through one of the two interfaces 108a, 108b. The interface 108a, 108b can be any suitable device for separating materials. Each segment 101a, 101b, 101c has a corresponding internal space inside the container 101.

[0076] The middle or center section 101b of the container 101 receives the force applicator 102, the cathode 106 and the material 104, such as the carbon / electrolyte product. The size and shape of the force applicator 102 match the center section 101b, shown here as a compressor formed by a flat square plate or a rectangular plate, which extends the entire space between the two interfaces 108a, 108b and the two longitudinal sides of the container 101. The cathode 106 can also be a flat square plate or a rectangular plate, which extends the entire space between the two interfaces 108a, 108b and the two longitudinal sides of the container 101. The cathode 106 can be located at the bottom of the interior space of the center section 101b, for example.

[0077] like Figure 1AAs shown by the large arrow in , the cathode 106 and the material 104 are placed in the central section 101b. The compressor 102 is located above the central section 101b and is forced downward into the central section 101b, for example by pneumatic operation. As the compressor 102 moves downward, it forces the product 104 to separate. The first interface 108a can have a first filtering mechanism (e.g., a first porous material) that filters a first product (i.e., a gas, liquid, or material), and the second interface 108b can have a second filtering mechanism (e.g., a second porous material) that filters a second product (e.g., a gas, liquid, or material) that is the same as or different from the first product. Here, the first interface 108a and the second interface 108b both filter carbon so that only the electrolyte 110 can enter the first section 101a and the second section 101c through the interfaces 108a and 108b, respectively. As described, the size and shape of the compressor 102 matches the size and shape of the center section 101b so that the material 104 does not escape around the sides of the compressor 102 as the compressor 102 compresses downwardly, but rather the material 104 is squeezed through the interfaces 108a, 108b.

[0078] In another embodiment, an oxygen-excluded gas (e.g., a gas containing no or substantially no oxygen) 112 may optionally be used to cover (e.g., completely cover) the system 100, for example, to prevent oxidation of the solid carbon during separation of the electrolyte from the solid carbon / electrolyte product 104. In this embodiment, the system 100 may include a main housing that encloses the compressor 102 and the container 101, for example, as FIG. 2A to FIG. 2C As shown (see, for example, main housing 201). Gas 112 may be pumped into the main housing surrounding container 101 to contact product 104 and / or electrolyte 110 in any of segments 101a, 101b, 101c.

[0079] Figure 1A The chamber 100 has segments 101a, 101b, 101c arranged in a side-by-side relationship, and the electrolyte is filtered into the two outer segments 101a, 101c. However, the segments 101 can be arranged in any suitable manner, and only a single segment (or compartment) is required to accommodate the product 104, and another segment (or compartment or container) is required to receive the filtered electrolyte 110.

[0080] Figure 1B is a diagram of an exemplary system 200 for separating electrolyte from solid carbon in a solid carbon / electrolyte product in an extraction chamber. Figure 1A. The solid carbon / electrolyte product 104 is first removed from the cathode of the electrolysis chamber (not shown) and placed as a gel (hot) or initially solid (frozen gel and then heated to a molten gel) into an extraction reservoir or chamber 210 for extruding the electrolyte. As another embodiment, an optional vacuum 220 can be applied to the extrusion chamber to provide a pulling force for the electrolyte through the interface 108 having holes.

[0081] More specifically, the extraction chamber 200 has a housing 202 having four sides or walls 204 forming a container having an interior space and a square or rectangular cross-section. The housing 202 has an open top and an open bottom. The interface 108 is disposed at the bottom of the housing 202 and closes the open bottom of the housing 202. The product 104 is placed inside the housing 202. A lower container or extraction chamber 210 is located below the housing 202 and the interface 108. The size and shape of the compressor 102 matches the size and shape of the interior of the housing 202 and pushes down on the product 104, forcing the electrolyte through the interface 108 and into the extraction reservoir, such as the square or rectangular chamber 210. In addition, an optional vacuum 220 may be provided with or in place of the compressor 102 to further facilitate the passage of the electrolyte through the interface 108; although it is also noted that some electrolytes can pass through the interface 108 under gravity without the use of the compressor 102 and / or the vacuum 220. Vacuum 220 may also operate as a drain to collect separated electrolyte, or a separate drain (eg, hose or line) may be provided. Interface 108 prevents carbon from passing through, so only electrolyte enters extraction chamber 210. Although not shown, cathode 106 may also be located in housing 202.

[0082] Figures 2 to 6 show other embodiments of the invention. The system may be of any suitable size or shape and may be configured vertically, horizontally or at an angle. Figure 2A , Figure 3D , a horizontal configuration of an extractor system 300 is shown. The system 300 has an extraction container or chamber 302, an electrolyte collection chamber 310, and a filter 308 between the container 302 and the collection chamber 310. The extraction chamber 302 has a top, a bottom, and at least two sides or walls, shown here as longitudinal walls extending along the length of the chamber 302. One side can be open to receive a plate of a compressor 102. In the illustrated embodiment, the chamber 302 is elongated, and the compressor 102 is received at the open proximal lateral end of the chamber 302. The compressor 102 extends from the proximal end of the chamber 302 along the longitudinal axis of the chamber 302. The crude product 304 can enter through an opening in the side wall or the top.

[0083] The interface or filter 308 is located at the open distal lateral end of the extraction chamber 302, and the collection chamber 310 is connected to the distal lateral end of the extraction chamber 302. The heating zone 306 can be set at a portion of the container 300, such as at the proximal portion, and is adjacent to the interface or filter 308. The compressor 102 pushes inward from the proximal end to the distal end so that the heated product passes through the filter 308 and enters the electrolyte collection reservoir or chamber 310. The vacuum 320 can be connected to the electrolyte collection reservoir 310 to facilitate the electrolyte to pass through the filter 308 into the reservoir 310. The vacuum 320 can be connected to the side of the reservoir 310 opposite the filter 308. The vacuum is used both to pull the electrolyte out of the carbon nanogel and to protect it from oxidation.

[0084] like Figure 2B , Figure 2C , Figure 3B As shown, the compressor 102 and the container 202 may be circular, and Figure 2B , Figure 2C , Figure 3C The compressor 102 is shown as being coupled or attached to the main housing 201. Figure 2D , Figure 2E , the container 202 can have a support shelf or protrusion 205 extending inwardly from one or more side walls 204. A steel support plate 212 can be placed on the protrusion 205. The support plate 212 has a plurality of openings, such as forming a honeycomb pattern. The plate 212 can support an interface 208 placed on top of the plate 212 (e.g., a filter membrane, a mesh, a felt material, etc.).

[0085] Figure 3A A chamber 202 is shown for use with a molten paste from an electrode containing a carbon product and an electrolyte. The paste is on top of a mesh screen 208 on a porous support 212. A compressor pushes the paste downward and the electrolyte passes through the mesh screen 208 into the bottom of a separate container or chamber. The chamber 202 can be airtight and an oxygen-free gas (e.g., Ar, N2, CO2) or a vacuum can be applied around the paste within the container.

[0086] Figure 3B It is shown that instead of the internal support tabs 205, a grid support may be provided to support the porous mesh support 212. In addition, a mesh screen 208 may be provided on top of the mesh support 212, and the sample placed on top of the mesh screen 208. A heater may be provided to heat the system, for example the system may be inside a kiln or connected to a kiln.

[0087] Figure 2B , Figure 2CIt is shown that the compressor 102 can be formed as a plate and a screw. The screw can extend through a threaded opening in the top plate of the main housing 201, and the screw can be rotated in the opening to extend the rod and the plate further into the container 202. Figure 3C Another embodiment is shown in which the compressor 102 has a pressure plate and a scissor-type hydraulic jack mounted to the pressure plate. The jack presses against the top plate of the main housing 201, and the screw in the jack can be rotated to extend the jack and move the pressure rod or bar and the pressure plate further into the container 202. Figure 3C Also shown is a molten paste product from the electrode in a container 202. The molten paste product contains a carbon product and an electrolyte. The press plate forces the electrolyte out of the paste product, through a mesh screen 208 located on a porous support 212, and into a collection reservoir at the bottom of the container 202. In addition, a separator 207 is provided in the main housing 207. The separator 207 is a plate extending across the main housing 201 and surrounding the compressor 102 (e.g., a rod of the compressor 102). The separator 207 forms an airtight seal and closes the container 202. An oxygen-free gas can be introduced into the sealed enclosure. When the paste product from the electrode is introduced before the press plate is placed, or during any leak in the seal between the press plate and the paste product from the electrode, the gas contacts the product.

[0088] FIG. 4A to FIG. 4E A collection chamber 450 is shown, which is positioned relative to the electrolysis chamber 400 and operates to remove the product. Figure 4A , an electrolysis chamber 400 is shown having a cathode electrode surrounded by an electrolyte positioned between two anode electrodes. A collection chamber 450 is integrally formed with or coupled to the electrolysis chamber 400. The collection chamber 450 is above the level of the electrolyte in the electrolysis chamber 400. A transport device is coupled to the cathode, such as by a wire, a rod, or a solid bar, and is configured to move the cathode from the electrolysis chamber 400 to the collection chamber 450. Here, the transport device includes a conveyor device located above the electrolysis chamber 400 and the collection chamber 450. When carbon adheres to the cathode, one or more transport motors are operated to vertically lift the cathode out of the electrolysis chamber 400, such as Figure 4B As shown, the cathode is then moved horizontally above the collection chamber 450, as shown in FIG. Figure 4C The compressor 452 is withdrawn from the collection chamber 450 and the cathode is lowered into an opening in the collection chamber 450 by a conveyor.

[0089] The crude product is then released from the cathode into a collection chamber. For example, the collection chamber 450 may have one or more scrapers 454 positioned in an opening of the collection chamber 450. A scraper channel or opening is formed between the one or more blades 454. The cathode descends into the scraper channel between the scrapers 454, which forces the crude product to leave the cathode and enter the collection chamber 450. The compressor then extends into the collection chamber and compresses the crude product. The electrolyte from the product passes through the interface of the collection chamber and returns directly to the electrolysis chamber, while the carbon remains in the collection chamber. The extracted carbon product is removed with the collection chamber. It should also be noted that FIGS. 1 to 3, Figure 5 Any of the systems in Figure 7 can be used to FIG. 4A to FIG. 4E In addition, although the collection chamber 450 is shown as being angled relative to the electrolysis chamber 400, the collection chamber 450 can be positioned vertically or horizontally relative to the electrolysis chamber 400.

[0090] Figure 5 A vertically arranged product extractor or collection chamber 450 and a vacuum system 456 are shown. The vacuum system 456 may be optionally attached to the collection chamber 450. The collection chamber 450 may be a container with walls, shown here as a cube with rectangular or square sides and an open bottom. The vacuum system 456 includes an extraction chamber 410, a gasket or sealant 412, and a vacuum line 420. The extraction chamber 410 may be a container or reservoir for accommodating electrolytes extracted from the extractor 450. The extraction chamber 410 is shown as a cube with square or rectangular sides and an open top. The seal 412 is disposed at the top edge of the extraction chamber 410 and the bottom edge of the collection chamber 450 to form an airtight seal between the collection chamber 450 and the extraction chamber 410. The vacuum line 420 is coupled to the extraction chamber 410 and is in gas communication with it. Once a seal is formed, the vacuum line 420 may generate a vacuum or negative pressure in the extraction chamber 410, which in turn pulls the electrolyte out of the product contained in the collection chamber 450. The extraction chamber 410 may then be removed, emptied of electrolyte, and replaced. Figure 5 The vacuum system 456 shown in FIG. 4 may be used with any of the systems 100, 200, 300 of FIG. 1 to FIG. 4. A drain or conduit 458 drains away the accumulation of excess electrolyte that has separated from the paste product from the electrode.

[0091] Fig. 6A , Figure 6B , Figure 6C The extraction chamber 200 is shown as having a vertical configuration. Figure 3C As described, the extraction chamber 200 may be enclosed in the main housing 201 , which forms a complete enclosure around the extraction chamber 200 . Fig. 6A , Figure 6B , Figure 6CThe main housing 201 is shown as a frame 203 extending above the extraction chamber 200. The frame 203 has two elongated vertical support members and a horizontal cross member connecting the two vertical members. The vertical members can be fixed to the ground or a horizontal base or platform 209. The extraction chamber 200 can be located on the base 209. Figure 6B As further shown in FIG. 1 , the extraction chamber 200 may be located within a kiln to control the temperature within the extraction chamber 200 . Fig. 6A , Figure 6C A compressor 102 is shown having a screw and a pressure plate attached to a frame cross member, Figure 6B A compressor 102 is shown having a scissor-type jack mechanism connected to a cross member of a frame 203 . Figure 6C Also shown is a circular electrolyte from the product extraction unit.

[0092] Figures 7A-7H Yet another embodiment of the present invention is shown. Here, an extraction system 500 is shown. System 500 includes an electrolysis and extraction chamber 502, a transport assembly 520, a housing 530, and a compressor and collection assembly 550. The electrolysis and extraction chamber 502 is a container having one or more vertical side walls 504, a bottom, and an at least partially open top. The container receives an anode electrode, a cathode electrode, and a liquid electrolyte surrounding the anode and cathode. An opening 506 is disposed along at least one wall 504 at a position above the level of the electrolyte in the chamber 502.

[0093] The housing 530 at least partially encloses the electrolysis chamber 502. Here, the housing 530 can be a frame having an elongated support frame member extending horizontally above the electrolysis chamber 502. The support frame member can be connected to other frame features, such as vertical support beams connected to the base, such as Fig. 6A , Figure 6B shown.

[0094] The conveyor assembly 520 is used to lift the cathode out of the electrolyte to remove the crude product, and then lower the cathode back into the electrolyte after removing the crude product. This can be achieved by any suitable mechanism, such as a motor, gear or wheel, and wire. The motor and rotating wheel can be connected to the horizontal support frame 530. The wire is connected to the wheel and the cathode. The motor runs to rotate the wheel, and the wheel raises and lowers the cathode again. The anode can also be individually connected to the conveyor assembly 520 by a separate wire and wheel, and has a separate or shared motor.

[0095] The compressor and collection assembly 550 has an extension rod 552, a pressure plate 554, an extrusion wall 556, and a collection device 560. The extraction assembly 550 is received in an opening 506 in one or more side walls of the electrolysis chamber 500, and the entire extraction assembly 550 is positioned above the electrolyte in the electrolysis chamber 500. The pressure plate 554 is vertically positioned inside the electrolysis chamber 500, and the rod 552 extends horizontally through the wall opening 506 to the outside of the electrolysis chamber 500. The extrusion wall 556 is a vertical plate or wall having a proximal end that is coupled to and extends downward from the horizontal support frame member 530. The wall 556 has a distal end that extends downward into the electrolysis chamber 500. In the embodiment shown, the distal end of the wall 556 stops above the electrolyte so that the wall does not contact the electrolyte at the bottom of the electrolysis chamber 500. The extrusion wall 556 may have other support members, such as a horizontal beam connected to the frame at the bottom end of the wall 556. The extrusion wall 556 has two sides, each with a respective surface facing outward. The first wall surface faces the compressor 550, and the second wall surface faces away from the compressor 550. The first wall surface is aligned with and faces the inwardly facing surface of the pressure plate 554. The rod 552 moves the pressure plate 554 horizontally forward and inward into the container 502 toward the extrusion wall 556. Of course, other suitable mechanisms may be provided to move the pressure plate forward, such as a scissor-like jack located on the wall of the container 502.

[0096] The collecting device 560 is located at the bottom end of the pressing plate 554. As shown, the collecting device 560 can be a shelf extending horizontally outward from the bottommost edge of the pressing plate 560, substantially orthogonal to the inwardly facing surface of the pressing plate 560. The size of the collecting device 560 is suitable for collecting the carbon (graphene) removed from the cathode. The collecting device 560 can be received in a channel formed in the bottom end of the pressing plate 560, or attached to the bottom edge of the pressing plate 560. However, other suitable collecting devices can also be provided, such as the collecting device 560 does not need to be connected to the pressing plate 554, but can be connected to at least one chamber wall 504 of the electrolysis chamber 502, and extends outward from the chamber wall 504 and inwardly toward the extrusion wall 556.

[0097] from Fig. 7E Initially, operation of the extraction system 500 begins with the anode and electrode being lowered by the transport mechanism 520 into the electrolyte within the electrolysis and extraction chamber 502. The compression rod 552 is fully retracted so that the pressure plate 554 is retracted and can rest against one or more walls 504. At this point, electrolysis begins. Figure 7F In the process, gases are expelled from the reaction at the anode and products begin to accumulate at the cathode. Figures 7G to 7H The reaction continues and more and more pasty products are formed on the cathode.

[0098] exist Figure 7HIn the process, the cathode is saturated with the paste product. Therefore, the motor of the transport assembly 520 is operated, and the cathode is lifted out of the electrolyte, as Fig. 7A As shown. At this point, the cathode and the paste product are substantially aligned and parallel to the first surface of the extrusion wall 556 facing the pressing plate 554. The extrusion wall 556 is located between the cathode and the anode. Therefore, the paste product is mainly gathered on the cathode side facing the extrusion wall 556. Once the cathode is fully raised, the pressing rod 552 is operated to move the pressing plate 554 inwardly toward the extrusion wall 556, as shown by the arrow. Figure 7B In the embodiment, the pressing plate 556 is in contact with the cathode, which in turn applies pressure to the paste product, forcing the paste product downward along the extrusion wall 556 between the extrusion wall 556 and the cathode.

[0099] The discharged product reaches the collection device 560. The collection device 560 can be a plate with openings or holes, and can have a mesh screen or other filtering mechanism located on the porous plate. The distal end of the collection device 560 can contact the extrusion wall 556 and / or extend below the extrusion wall 556. The paste product discharged by compression enters the collection device 560, which collects the clean product (such as carbon or graphene) and allows the clean electrolyte to pass through and return to the bottom of the electrolysis chamber 502. When pressed, the electrolyte is pressed and separated from the paste by the supported screen. Figure 7C In , the clean electrolyte has returned to the electrolysis chamber 502, and the clean products are in the collection device 560. Fig.7D In the embodiment of the present invention, the pressing rod 552 is operated to retract the pressing plate 554 outward from the pressing wall 556 and return it to its initial position adjacent to the chamber wall 504. Then, the transport device lowers the cathode back into the electrolyte for further electrolysis, and removes the cleaned product from the collection device 560.

[0100] It should also be noted that when the paste product is removed from the electrolyte, Fig. 7A As shown, it will begin to cool and possibly solidify. Heat can be applied during compression, such as Figure 7B As shown, to promote the separation of carbon and electrolyte. In addition, a scraper can be used to completely remove the product from the press plate surface and the cathode surface, such as Fig.7D As shown, the solid carbon / molten electrolyte mixed product is compressed directly on the cathode in the electrolysis chamber. In addition, it is also noted that some products may exist on both sides of the cathode, in which case the products can also be compressed directly between the press plate and the cathode and separated and collected.

[0101] Therefore, as shown in various embodiments, and as implemented in any embodiment, unless otherwise specifically stated, the present invention relates to applying force to nanoscale products to separate materials macroscopically. The present invention is generally applied to pastes, and is particularly suitable for paste products formed at the cathode during electrolysis reactions, and includes solid carbon nanomaterial products combined with some liquid electrolytes reacting therewith (i.e., the paste is solid carbon plus liquid electrolyte). When the paste is compressed, the combined liquid electrolyte is separated from the desired solid carbon nanomaterial product. Due to the separation process, the electrolyte is not diluted, destroyed or otherwise becomes unavailable. Therefore, the electrolyte can be recycled (e.g., returned to the electrolysis chamber) or discarded, and the solid carbon product is retained. These electrolysis reactions are carried out in molten electrolytes at 700+ degrees Celsius. Compression can be carried out in the electrolysis chamber or outside the electrolysis chamber, and can be carried out while the paste is on the cathode or after the paste is removed from the cathode. If the compression / separation process is carried out in a separate extraction chamber (i.e., not in the electrolysis chamber in which the reaction is carried out), the product can be cooled to below the melting point of the electrolyte to form a solid carbon / solid electrolyte product that can be removed from the cathode and placed in a separate extraction chamber, and then heated to re-melt the electrolyte so that the liquid electrolyte can be removed from the desired solid carbon product in this separate chamber.

[0102] Although a compressive force is shown, other suitable forces such as torque, centripetal force, torsion or rotational force may also be applied. Also, although the present invention is described for use with a paste product to separate electrolyte and carbon products, the system may be used to separate other suitable materials. In addition, the system for applying force to the product may be of any suitable configuration, and the system shown in the accompanying drawings is for illustrative purposes only and does not limit the present invention. For example, the accompanying drawings show that any number of containers or chambers may be used. In FIG7 , a single chamber may be used for electrolysis, compression and separation. In FIG4 , a chamber for compression and separation is provided, which is separated from the chamber where electrolysis occurs. In FIG1 , three chambers may be used for compression and separation, and in FIG2 , two chambers may be used. The chambers may be arranged horizontally or vertically and may have any suitable shape, such as a rectangle, a square and a circle. Force may be applied pneumatically or manually by any suitable device, such as a platen and a rod or a hydraulic mechanism. In addition, the type and manner of applying force may be changed, such as applying, removing, and then applying (repeatedly applying) a compressive force again, or a compressive force may be applied, followed by applying a different force, such as a torque. Additionally, compression may be applied while the product is on the cathode, or after the product has been removed from the cathode.

[0103] It should be noted that it can be considered that the high temperature press exposes and oxidizes (burns) the carbon product. However, the inventors recognize that the electrolyte itself protects the product from burning during extrusion. In addition, the nano material is too small to be separated by the press because the press essentially depends on a filter greater than micron or greater than millimeter, so the nano material is too small to be separated by the filter. However, the inventors recognize that the agglomeration and aggregation of the carbon nanotube product during electrolysis allows the nano material to be filtered with a larger filter (e.g., a filter of micron and millimeter size). That is to say, a single carbon nano material product has nanometer size, but carbon agglomerates and agglomerate products have micron and millimeter sizes.

[0104] In another embodiment of any of the methods described herein, the electrolyte is removed through an interface 108 having pores. In one embodiment, the interface 108 having pores comprises a foam, such as porous carbon felt, graphite felt, metal mesh, porous or mesh ceramic, or any combination thereof. In one embodiment, the pore size of the interface having pores is from about 10 μm to about 10 mm, such as from about 0.1 mm to about 5 mm or from about 0.3 mm to about 3 mm. In another embodiment, any of the methods described herein further comprises applying a vacuum, such as vacuum 220, during the separation / extraction process, for example to enhance the removal of the electrolyte and the separation of the solid carbon product.

[0105] In another embodiment, an oxygen-excluded gas (e.g., a gas that is free of oxygen or substantially free of oxygen), such as nitrogen, carbon dioxide, argon, or a reducing gas, such as methane, ammonia, hydrogen, and hydrogen sulfide, and any combination of the foregoing, is used to cover the carbon products during separation, for example, to minimize any loss of oxidized carbon products during exposure to oxygen at high temperatures.

[0106] In other embodiments of any of the methods described herein, the molten electrolyte cathode product mixture is compressed directly on the cathode in the electrolysis chamber.

[0107] In another embodiment of any of the methods described herein, the electrolyte cathode product mixture is removed from the cathode in the electrolysis chamber, such as without pumping, into a separate extraction compression chamber prior to separation of the solid product.

[0108] In a further embodiment of any method described herein, the mixed product is separated from the molten stage without cooling, for example, for inclusion in electrolysis without heat loss. In a further embodiment of any method described herein, the mixed product is cooled, and the cooled condensed product is reheated to a temperature higher than the electrolyte melting point before compression (separation). In either case, the molten mixture can be compressed by applying pressure and squeezed through an interface 108 having a hole smaller than the size of the carbon matrix. The macroscopic (greater than micron) pore size is larger than the nm size of the nanomaterial in the carbon product, but smaller than the carbon matrix size. The product compression extracts the electrolyte from the product, while the solid carbon is limited by the pores and retained in the product.

[0109] Example

[0110] Example 1: Using vacuum extraction

[0111] The cathode was removed from the brass cathode and passed through a molten alkali carbonate electrolyte at 750°C at 0.1 A cm -2 The solid carbon / molten electrolyte mixed product (carbonate gel) formed on the cathode during electrolysis between an Inconel anode and a brass cathode for 4 hours was used. Figure 2A The product extractor 300 shown in is separated into carbon nanotubes and clarified electrolyte. The carbon felt is placed on a 1 / 8" honeycomb steel plate, which is used as a support in the subsequent extrusion stage. On top of the carbon felt, layers of 200×200, 100×100 and finally 50×50 Monel mesh are placed respectively. Carbon dioxide flows into the top of the extractor to prevent oxidation of the carbonate gel and the subsequently separated carbon products. 50g of the carbonate gel product grown by electrolysis in pure lithium carbonate electrolyte, previously analyzed to contain 6% carbon nanomaterial and 94% electrolyte (containing 3g carbon and 47g electrolyte), was removed from the cathode and placed on top of the topmost (50 mesh) Monel layer at 770°C. Layers of 40×40 Inconel mesh and 200×200 Monel mesh are then placed above the carbonate gel. In Figure 2A The press plate shown on the left is placed on top of the uppermost web layer and applies 0.5 tons of pressure for 1.5 hours. Figure 2A The metal tube shown on the left applies a vacuum 304 of 0.08 MPa. A vacuum is applied in the electrolyte collection chamber at the bottom of the extractor. Finally, the extractor is cooled, the press plate is removed, the carbon product is retained, and the clarified extracted electrolyte is removed and weighed. 87.0% of the electrolyte in the carbonate gel is removed and recovered by this procedure.

[0112] Example 2: Extraction without vacuum

[0113] The cathode was removed from the brass cathode and heated to 0.1 A cm in a molten alkali carbonate electrolyte at 750 °C. -2 The solid carbon / molten electrolyte mixed product (carbonate gel) formed on the cathode during electrolysis between an Inconel anode and a brass cathode for 4 hours was used in Figure 2A The product extractor shown in the middle and on the right separates into carbon nanotubes and clarified electrolyte. No carbon felt is used. Using a larger press minimizes leakage at the platen edges and reduces pressing time, both of which increase extraction efficiency even without vacuum extraction.

[0114] On a honeycomb steel support plate are placed (1) a 40×40 Inconel mesh, (2 and 3) two layers of 200×200 monel mesh, and finally (4) another layer of 40×40 Inconel mesh. Carbon dioxide flows into the top of the extractor to prevent oxidation of the carbonate gel and the subsequently separated carbon product. 200g of the carbonate gel product grown by electrolysis in a 20wt.% sodium carbonate and 80wt.% lithium carbonate electrolyte, previously analyzed to contain 6% carbon nanomaterials and 94% electrolyte (including 3g carbon and 47g electrolyte), was removed from the cathode and placed on top of the topmost mesh layer at 770°C. Subsequent layers of 40×40 Inconel mesh and 200×200 monel mesh are placed above the carbonate gel. A press plate is placed on top of the topmost mesh layer and a pressure of 5 tons is applied for 0.5 hours. By Figure 2A The metal tube shown on the left applies a vacuum of 0.08 MPa. Vacuum suction is applied to the electrolyte collection chamber at the bottom of the extractor. Finally, the extractor is cooled, the press plate is removed, the carbon product is retained, and the clarified extracted electrolyte is removed and weighed. 93.9% of the electrolyte in the carbonate gel is removed and recovered by this procedure.

[0115] It should also be noted that the specification and claims use several geometric or relational terms, such as plane, elongated, circular, parallel, vertical, orthogonal, transverse, longitudinal and plane. In addition, the specification and claims use several directions or positioning terms, such as horizontal, vertical, top, bottom, left, right, upper, lower, distal and proximal. These terms are only for the convenience of description based on the embodiments shown in the accompanying drawings. Those terms are not intended to limit the present invention. Therefore, it should be appreciated that the present invention can be described in other ways without those geometric, relational, direction or positioning terms. In addition, geometric or relational terms may not be accurate. For example, due to, for example, the roughness of the surface, the tolerances allowed in the manufacture, etc., the walls may not be precisely perpendicular or parallel to each other, but are still considered to be substantially perpendicular or parallel. And, without departing from the spirit and scope of the present invention, other suitable geometric shapes and relationships can be provided.

[0116] The following documents are incorporated herein by reference.

[0117] (1)Ren et al.,One-pot synthesis of carbon nanofibers from CO2,Nano.Lett.,15,6142-6148(2015);(2)Johnson et al.,Carbon nanotube wools madedirectly from CO2 by molten electrolysis:Value driven pathways to carbondioxide greenhouse gas mitigation,Materials Today Energy,5,230-236(2017);(3)Ren et al.,Tracking airborne CO2mitigation and low-cost transformation intovaluable carbon Nanotubes,Scientific Reports,Nature,6,27760 1-10(2016);(4)Wuet al.,One-pot synthesis of nanostructured carbon material from carbondioxide via electrolysis in molten carbonate salts,Carbon,106,208-217(2016);(5)Wang et al.,Exploration of alkali cation variation on the synthesis ofcarbon nanotubes by electrolysis of CO2 in molten carbonates,J.CO2Utilization,34,303–312(2019);(6)Liu et al.,Carbon Nano-Onions MadeDirectly from CO2 by Molten Electrolysis for Greenhouse Gas Mitigation,Advanced Sustainable Systems,1900056,1-10(2019);(7)Yu et al.,Strength andBreaking Mechanism of Multiwalled Carbon Nanotubes Under Tensile Load,Science.287,637–640(2000);(8)Chang et al.,A New Lower Limit for the UltimateBreaking Strain of Carbon Nanotubes,ACS Nano,4,5095-5100(2010);(9)Gui et al.,Carbon nanotube sponges,Advanced Materials, 22, 617-621 (2010); (10) Wu et al., Carbon nanofiber aerogels for emergent cleanup of oil spillage and chemical leakage under harsh conditions, Scientific Reports, 4, 4079 1-6 (2014); (11) Kim et al., Graphene-Coated Carbon Nanotube Aerogels Remain Superelastic while Resisting Fatigue and Creep over-100to+500℃, Chemistry of Materials, 4, 2748-2755(2017).

[0118] The foregoing description and accompanying drawings should be considered as merely illustrations of the principles of the invention. The present invention can be constructed into various shapes and sizes and is not intended to be limited by the embodiments. Those skilled in the art will readily appreciate many applications of the present invention. Therefore, it is not desirable to limit the present invention to the disclosed specific embodiments or the precise structures and operations shown and described. On the contrary, all suitable modifications and equivalents may be adopted and fall within the scope of the present invention.

Claims

1. A system for separating electrolyte from a solid carbon / molten electrolyte mixed product of carbonate electrolysis, the system comprising: an electrolysis chamber having a cathode, an electrode, and said carbon / molten electrolyte, said cathode accumulating a paste product in response to said carbonate electrolysis; a compression device that applies compression to the cathode and paste product to produce a mixture of carbon and electrolyte; A filter removes carbon from the carbon and electrolyte mixture and delivers electrolyte to the electrolysis chamber.

2. A method for producing a solid carbon product by separating electrolyte from a solid carbon / molten electrolyte mixed product removed from a cathode of carbonate electrolysis using the system of claim 1, the method comprising: (i) applying force to compress the solid carbon / molten electrolyte mixed product to remove the electrolyte; (ii) removing the force; and (iii) separating the solid carbon product.

3. The method of claim 2, wherein step (i) and step (ii) are repeated two, three or four times before step (iii).

4. The method of claim 2, wherein the compression is performed at a pressure of 10 psi to 100,000 psi. The method according to claim 2 , wherein the electrolyte is removed through an interface having pores.

6. The method of claim 5, wherein the interface having pores comprises porous carbon felt, graphite felt, metal mesh, porous or meshed ceramic, or any combination thereof.

7. The method according to claim 6, wherein the pore size of the interface is 10 μm to 10 mm.

8. The method of claim 2, wherein the method is carried out at a temperature of 399°C to 900°C.

9. The method of claim 2, further comprising applying a vacuum during the separation process.

10. The process according to claim 9, wherein the process is carried out at a pressure of 0.1 to 0.9 atmospheres.

11. The method of claim 9, wherein the method is carried out at a pressure less than 0.1 atmosphere.

12. The method according to claim 2, wherein the method is carried out under an oxygen-free atmosphere.

13. The method according to claim 12, wherein the gas is selected from nitrogen, carbon dioxide, argon, methane, ammonia, hydrogen, hydrogen sulfide and any combination thereof.

14. The method of claim 2, wherein the mixed product is cooled after it is formed by electrolysis and is reheated prior to the compression step.

15. The method according to claim 2, wherein: The solid carbon / molten electrolyte mixed product is compressed directly on the cathode in the electrolysis chamber.

16. The method of claim 2, wherein the solid carbon / molten electrolyte mixed product is moved from the cathode of an electrolysis chamber to an extraction compression chamber prior to compression.

17. The method of claim 2, wherein the electrolyte is not a flowing electrolyte and the electrolyte is not recirculated via a recirculation loop.

18. The method of claim 2, wherein the solid carbon product has an average thickness greater than 1 mm.

19. The method of claim 2, wherein the solid carbon product comprises greater than 80% carbon nanomaterial.

20. The method of claim 2, wherein the solid carbon product comprises greater than 85% carbon nanomaterial.

21. The method of claim 2, wherein the solid carbon product comprises greater than 90% nanomaterial.

22. The method of claim 2, wherein the solid carbon product comprises greater than 95% carbon nanomaterial.

23. The method of any one of claims 19 to 22, wherein the nanomaterial comprises nanofibers.

24. The method of any one of claims 19 to 22, wherein the nanomaterial comprises nanotubes.

25. The method of any one of claims 19 to 22, wherein the nanomaterial comprises a nano-onion.

26. The method of any one of claims 19 to 22, wherein the nanomaterial comprises nanosheets.

27. The method of any one of claims 19 to 22, wherein the nanomaterial comprises a nanoscaffold.

28. The method of any one of claims 19 to 22, wherein the nanomaterial comprises graphene.

29. The method of claim 2, wherein the solid carbon product is formed from crude carbon nanomaterial agglomerated during the carbonate electrolysis, and the separating comprises filtering the solid carbon product with a filter having larger pores than the crude carbon nanomaterial.

30. The method of claim 2, wherein the solid carbon / molten electrolyte comprises a paste.

31. The method of claim 2, wherein: The solid carbon product is capable of being repeatedly compressed without deleteriously affecting the structure and / or stability of the resulting solid carbon product.

32. The method of claim 19, wherein: The carbon nanomaterial is carbon nanofiber, carbon nanotube, carbon nanoonion, carbon nanosheet, carbon nanoscaffold, graphene or any combination thereof.

33. The method of claim 22, wherein: The carbon nanomaterial is carbon nanofiber, carbon nanotube, carbon nanoonion, carbon nanosheet, carbon nanoscaffold, graphene or any combination thereof.

Citation Information

Patent Citations

  • Methods And Systems For Carbon Nanofiber Production

    US20180044183A1

  • Methods and systems for carbon nanofiber production

    US20190039040A1

  • Powder comprising carbon nanostructures and its method of production

    CN104321909A

  • Preparation method of graphene metal composite material

    CN106629680A

  • A battery or fuel cell system

    CN107275722A