Method for joining and cooling sheet metal parts
By stacking and heating high-strength steel sheet parts in self-piercing riveting equipment, and performing quenching treatment during the cooling process, the problem of difficulty in joining high-strength materials with the existing technology is solved, the joint strength is improved, and the resistance to fatigue is enhanced. Resistance.
Patent Information
- Application Number
- CN201911300130.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-12-17
AI Technical Summary
Existing self-piercing riveting equipment is difficult to effectively join high-strength materials with a tensile strength greater than 680Mpa, such as welded aluminum steel, and high-frequency wave heating causes the intermetallic compound produced by the material melting reaction to have poor strength and is prone to material fatigue.
By stacking the first metal sheet piece (the melting point is higher than the second metal sheet piece) and the second metal sheet piece, and heating it to the softening temperature of the first metal sheet piece, inserting the self-piercing rivet and then cooling it to the second metal sheet piece The quenching temperature uses the original equipment for bonding and quenching to improve the bonding strength.
It achieves effective joining and strength improvement of high-strength steel sheet parts, avoids material melting reaction, and enhances the resistance of the joined metal sheet parts to fatigue.
Smart Images

Figure CN112974714B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for joining and cooling sheet metal parts, and in particular to a method for joining and cooling sheet metal parts, wherein the workpiece is heated to soften before self-piercing rivets are punched in, and in-die quenching is performed after the rivets are punched in. Background Art
[0002] In many fields (such as transportation), lightweighting is always a topic that must be considered. Aluminum alloys and advanced high-strength steel are both important materials for lightweight components. Dissimilar metals such as steel / aluminum have complementary effects. By introducing low-density materials such as aluminum and magnesium composite materials (composite body) into all-steel bodies, it has become a global trend for lightweighting of automobile bodies. Therefore, the technical field of body manufacturing is a major challenge for dissimilar metal joining technology.
[0003] For mechanical joining methods, such as self-piercing riveting, it is a high-strength mechanical joining method. Multiple layers of materials are connected by hard rivets. There is no need to drill holes in the sheet metal in advance. Very little sound is generated during construction, and no heat is required to enter the parts during joining. The rivet is penetrated by the upper material by applying pressure through the equipment, and the rivet is expanded and deformed by the supporting mold below to achieve the mechanical joining effect. Since the lower material is not penetrated by the rivet, the sealing of the joint surface is also improved. And since self-piercing riveting does not require melting and has no heat-affected zone, it has higher fatigue strength than traditional resistance welding, and the quality of the joint is good and can be automated, so it is suitable for the application of dissimilar metal joining in vehicles. However, when welding high-strength materials such as aluminum steel and high-strength steel, if the tensile strength of the material is greater than 680Mpa, the existing self-piercing riveting equipment is difficult to penetrate, and it is necessary to spend a huge amount of money to upgrade the existing equipment before it can be penetrated.
[0004] Japanese Patent Application No. 2016-055291 discloses a joining technology that applies self-piercing riveting and high-frequency wave heating to multiple resin parts. The joining device uses a punch to drive a self-piercing rivet into multiple resin parts arranged on a mold for joining. The joining device includes: a mold, which supports the resin member and the foot of the self-piercing rivet; a mold support member, which is used to support the mold and is formed by an insulator; a high-frequency electromagnetic induction coil, which is arranged in the mold support member; a front clamp, which is used to fix the resin part on the mold and is formed by an insulator; a high-frequency electromagnetic induction coil, which is wound around the front clamp; and a punch, which is used to drive the self-piercing rivet and is formed by an insulator. The high-frequency electromagnetic induction coil is used to preheat the self-piercing rivet, and the heated self-piercing rivet is driven into multiple resin parts to form a riveted joint. The high-frequency electromagnetic induction coil is used to heat and melt the riveted joint, so that the foot and multiple resin parts are melted and joined to each other, and because the multiple softened resin parts are riveted, cracks in the resin parts due to riveting can be avoided. High-frequency wave heating will cause the material to melt. If it is applied to dissimilar metal sheets, it may cause a large amount of intermetallic compounds to be produced due to the melting reaction of the material when the dissimilar materials are connected. Because the structure of the intermetallic compound is needle-shaped, its strength is relatively poor and it is not easy to resist external forces, causing the metal sheets after the connection to easily experience material fatigue during use and fail to effectively resist fatigue. Summary of the invention
[0005] The invention provides a method for joining and cooling sheet metal parts, which can be used to join steel sheet metal parts with higher strength by using existing self-piercing riveting equipment, and can recover the strength of the material by quenching after joining.
[0006] The method for joining and cooling sheet metal parts provided by the present invention comprises: providing a first metal sheet and a second metal sheet, the melting point of the first metal sheet being higher than the lowest heating softening temperature of the second metal sheet; sequentially stacking the second metal sheet and the first metal sheet on a concave mold to form a superimposed sheet metal part; heating the superimposed sheet metal part to a first temperature and then stopping the heating, the first temperature being the sheet metal softening temperature of the first metal sheet; driving a self-piercing rivet from the first metal sheet of the superimposed sheet metal part toward the second metal sheet metal part, so that the rivet foot of the self-piercing rivet pierces the first metal sheet metal of the upper layer and stays inside the second metal sheet metal of the lower layer, and the bottom surface of the second metal sheet metal corresponding to the position of the self-piercing rivet is turned outward and plastically deformed to form a riveted joint to join the first metal sheet metal part and the second metal sheet metal part; cooling the superimposed sheet metal part to a second temperature, the second temperature being the quenching temperature relative to the material of the first metal sheet metal part; opening the mold and taking out the superimposed sheet metal part.
[0007] In the above embodiment, the materials of the first metal plate and the second metal plate are steel, the first temperature is above 400° C., and the second temperature is above 250° C.
[0008] In one embodiment, the step of heating the laminated sheet metal also includes a workpiece heating device, which uses a moving mechanism to move to an initial position to stop heating and a heating position to heat, and the heating position corresponds to the area of the first metal sheet where the self-piercing rivet is predetermined to be punched into.
[0009] In one embodiment, the workpiece heating device uses electromagnetic induction coil heating.
[0010] In one embodiment, the step of cooling the laminated sheet metal further comprises a workpiece cooling device, wherein a water channel is arranged in the die, and liquid circulates in the cooling water channel to cool the laminated sheet metal in the die.
[0011] The present invention provides another embodiment of a method for joining and cooling sheet metal parts, comprising: providing a first metal sheet and a second metal sheet, wherein the melting point of the first metal sheet is lower than the lowest heating softening temperature of the second metal sheet; placing the second metal sheet on a die, heating the second metal sheet to a softening temperature and then stopping the heating, wherein the softening temperature is the sheet material softening temperature of the second metal sheet; stacking the first metal sheet on the second metal sheet to form a composite sheet metal part; driving a self-piercing rivet into the composite sheet metal part from the first metal sheet toward the second metal sheet metal part, so that the rivet foot of the self-piercing rivet pierces the first metal sheet metal of the upper layer and stays inside the second metal sheet metal of the lower layer, and the bottom surface of the second metal sheet metal corresponding to the rivet position is plastically deformed outward to form a riveted joint to join the first metal sheet metal and the second metal sheet metal; cooling the composite sheet metal part to a quenching temperature, wherein the quenching temperature is the quenching temperature relative to the material of the second metal sheet metal; and opening the die to take out the composite sheet metal part.
[0012] In the above embodiment, the material of the first metal sheet is aluminum alloy, the material of the second metal sheet is steel, the softening temperature is above 400° C., and the quenching temperature is above 250° C.
[0013] In the above embodiment, the step of heating the overlapped sheet metal also includes a workpiece heating device, which uses a moving mechanism to move to an initial position to stop heating and a heating position to heat, and the heating position corresponds to the area of the first metal sheet where the self-piercing rivet is predetermined to be punched into.
[0014] In the above-mentioned embodiment, the workpiece heating device includes electromagnetic induction coil heating.
[0015] In one embodiment, the step of cooling the laminated sheet further comprises a workpiece cooling device, wherein a cooling water channel is arranged in the die, and liquid flows in the cooling water channel to cool the laminated sheet in the die.
[0016] Based on the above description, the present invention includes a softening treatment of the workpiece before self-piercing joining, so the original equipment can be used to perform higher-strength steel sheet joining. The present invention can use the original equipment to add a heating device and a quenching device for cooling the die (i.e., the lower die), and has high feasibility. The present invention can perform higher-strength steel sheet joining than the original equipment. The present invention has a strength-enhancing effect on both the workpiece and the rivet due to the application of quenching in the self-piercing range, and can further strengthen the self-piercing riveted joint. The joining method of the present invention is not easy to contaminate the workpiece because there is no oil or water on the surface of the workpiece. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A flow chart of an embodiment of a method for joining and cooling a sheet metal part according to the present invention;
[0018] Figures 2 to 6 for Figure 1 A structural flow chart of a method for joining and cooling a sheet metal part according to an embodiment of the present invention;
[0019] Figure 7 A flow chart of another embodiment of the method for joining and cooling a sheet metal part according to the present invention;
[0020] Figure 8 To Fig.13 for Figure 7 The illustrated embodiment is a structural flow chart of the method for joining and cooling sheet metal parts of the present invention.
[0021] Explanation of symbols in the accompanying drawings:
[0022] 1 Self-piercing riveting equipment;
[0023] 11. Concave die;
[0024] 12 punches;
[0025] 2. Workpiece heating device;
[0026] 3. Workpiece cooling device;
[0027] 31 Water channel;
[0028] 4, 4' self-piercing rivets;
[0029] 41, 41' nail foot;
[0030] 5, 5' riveted joint;
[0031] L Liquid;
[0032] L1, L1' initial position;
[0033] L2, L2' heating positions;
[0034] W1, W1' first metal sheet;
[0035] W2, W2' second metal sheet;
[0036] S11 to S16 are steps of a method for joining and cooling a sheet metal part according to an embodiment of the present invention;
[0037] S21-S27 are steps of a method for joining and cooling sheet metal parts according to another embodiment of the present invention. DETAILED DESCRIPTION
[0038] The embodiments of the present invention are described in detail as follows with the help of the accompanying drawings. The accompanying drawings are mainly simplified schematic diagrams, which only illustrate the basic structure of the present invention in a schematic manner. Therefore, only components related to the present invention are marked in these drawings, and the components shown are not drawn in terms of the number, shape, size ratio, etc. during implementation. The specifications and dimensions during actual implementation are actually a selective design, and the component layout form may be more complicated.
[0039] The following descriptions of the embodiments are made with reference to the attached drawings to illustrate specific embodiments in which the present invention may be implemented. The directional terms mentioned in the present invention, such as "upper", "lower", "front", "back", "left", "right", "inner", "outer", "side", etc., are only with reference to the directions of the attached drawings. Therefore, the directional terms used are used to illustrate and understand the present application, rather than to limit the present application. In addition, in the specification, unless explicitly described to the contrary, the words "include" or "comprise" should be interpreted as meaning to include the component, but not to exclude any other components.
[0040] First, please refer to Figure 1 and Figures 2 to 6 The method of sheet metal joining and cooling in this embodiment comprises the following steps:
[0041] Step S11, providing a first metal sheet W1 and a second metal sheet W2, wherein the melting point of the first metal sheet W1 is higher than the lowest heating softening temperature of the second metal sheet W2, for example, the first metal sheet W1 and the second metal sheet W2 are both made of high-strength steel;
[0042] Step S12, sequentially stacking the second metal sheet W2 and the first metal sheet W1 on a die 11 (e.g., a die 11 of a self-piercing riveting device 1), and appropriately fixing the first metal sheet W1 and the second metal sheet W2, for example, by clamping the first metal sheet W1 and the second metal sheet W2, to form a stacked sheet member;
[0043] Step S13, heating the laminated sheet to a first temperature and then stopping the heating, the first temperature being the softening temperature of the first metal sheet W1. Figure 2 and Figure 3 As shown;
[0044] In step S14, a self-piercing rivet 4 is driven from the first metal sheet W1 of the stacked sheet metal toward the second metal sheet W2 (for example, a punch 12 of the self-piercing riveting device 1 is used to apply a punching force to the self-piercing rivet 4), so that the nail foot 41 of the self-piercing rivet 4 pierces the first metal sheet W1 of the upper layer and stays inside the second metal sheet W2 of the lower layer, and the bottom surface of the second metal sheet W2 corresponding to the position of the self-piercing rivet 4 is plastically deformed outward due to the action of the punch 12 and the die 11 to form a riveted joint 5 to connect the first metal sheet W1 and the second metal sheet W2, as shown in FIG. Figure 4 and Figure 5 As shown;
[0045] Step S15, cooling the laminated sheet to a second temperature, the second temperature being the quenching temperature of the first metal sheet W1 material, such as Figure 5 As shown;
[0046] Step S16, opening the mold and taking out the joined superimposed sheet metal parts, such as Figure 6 shown.
[0047] In an example of the present invention, the first metal sheet W1 and the second metal sheet W2 are made of high-strength steel, the first temperature (ie, the softening temperature of the high-strength steel) is above 400° C., and the second temperature (ie, the quenching temperature of the high-strength steel) is above 250° C.
[0048] like Figure 3 and Figure 4 As shown. The step of heating the laminated sheet (i.e., step S13) of the present invention further comprises a workpiece heating device 2, which uses a moving mechanism (since the moving mechanism can use a simple slider rail mechanism, a connecting rod mechanism, etc., which are all commonly used mechanical structures, no further explanation is given here and no diagram is shown) to move to an initial position L1 to stop heating and a heating position L2 to heat, and the heating position L2 corresponds to the area of the first metal sheet W1 where the self-piercing rivet is predetermined to be punched. The workpiece heating device 2 can use an electromagnetic induction coil heating method.
[0049] like Figure 4 and Figure 5 The step of cooling the superposed sheet metal parts (i.e., step S15) of the present invention further comprises a workpiece cooling device 3, wherein the workpiece cooling device 3 is provided with a water flow channel 31 in the die 11, and a liquid L circulates in the water flow channel 31, so as to cool the superposed sheet metal parts in the die 11 when the punch 12 presses the superposed sheet metal parts and closes the die 11.
[0050] In the above embodiment, the first metal sheet W1 and the second metal sheet W2 are made of the same material or their softening temperatures are close, that is, when the sheet is heated to the first temperature, it will not affect the mechanical properties of the other sheet. However, when the softening temperatures of the sheets of the workpieces are greatly different, for example, when the first metal sheet W1' to be processed is an aluminum alloy and the second metal sheet W2' is a steel sheet, it is not suitable and unnecessary to heat them together before riveting, because the original material of the aluminum alloy is softer than the self-piercing rivet, so it is not necessary to heat and soften it. The method of joining the sheets and cooling them in this case is as follows: Please refer to Figure 7 , and compare Figures 8 to 13 The method of sheet metal joining and cooling in this embodiment includes:
[0051] Step S21, providing a first metal sheet W1' and a second metal sheet W2', wherein the melting point of the first metal sheet W1' is lower than the lowest heating softening temperature of the second metal sheet W2', for example, the first metal sheet W1' is made of aluminum alloy, and the second metal sheet W2' is made of high-strength steel;
[0052] Step S22, placing the second metal sheet W2' on a die 11 of the self-piercing riveting device 1;
[0053] Step S23, heating the second metal sheet W2' to a softening temperature and then stopping the heating, the softening temperature being the softening temperature of the second metal sheet W2'. Fig. 9 As shown;
[0054] Step S24, stacking the first metal sheet W1' on the second metal sheet W2' to form a laminated sheet. Of course, before riveting, the laminated sheet will be properly fixed together, for example, by a pressing plate or a clamp to prevent sliding against each other. Fig.11 As shown;
[0055] Step S25, the self-piercing rivet 4 is driven from the first metal sheet W1' of the stacked sheet metal toward the second metal sheet W2', so that the nail foot 41' of the self-piercing rivet 4' pierces the first metal sheet W1' of the upper layer and stays inside the second metal sheet W2' of the lower layer, and the bottom surface of the second metal sheet W2' corresponding to the position of the self-piercing rivet 4 is turned outward and plastically deformed to form a riveted joint 5', so as to join the first metal sheet W1' and the second metal sheet W2'. Fig.11 , Fig.12 As shown;
[0056] Step S26, cooling the laminated sheet to a quenching temperature, the quenching temperature being a quenching temperature relative to the second metal sheet W2' material, such as Fig.12 As shown;
[0057] Step S27, opening the mold and taking out the joined superimposed sheet metal parts, such as Fig.13 shown.
[0058] The material of the first metal sheet W1 ′ is aluminum alloy, the material of the second metal sheet W2 ′ is steel, the softening temperature of the second metal sheet W2 ′ is above 400° C., and the quenching temperature is above 250° C.
[0059] In one embodiment, if Fig. 9 and Fig.10 As shown. In the step of heating the stacked sheet (i.e., step S23), a workpiece heating device 2 is also provided. The workpiece heating device 2 uses a moving mechanism (not shown) to move to an initial position L1' to stop heating and a heating position L2' to heat. The heating position L2' corresponds to the area of the first metal sheet W1' where the self-piercing rivet 4' is predetermined to be punched. The workpiece heating device 2 includes an electromagnetic induction coil heating method. Similarly, in one embodiment, see Fig.11 and Fig.12 The step of cooling the superposed sheet metal (i.e., step S26) further comprises a workpiece cooling device 3, wherein the workpiece cooling device 3 is provided with a water flow channel 31 in the die 11, and the liquid L circulates in the water flow channel 31 to cool the superposed sheet metal in the die 11 when the punch 12 presses the superposed sheet metal and closes the die 11.
[0060] The above-mentioned embodiments are only used to illustrate the principles, features and effects of the present invention, and are not intended to limit the scope of the present invention. Anyone skilled in the art can modify and change the above-mentioned embodiments without violating the spirit and scope of the present invention. Any equivalent changes and modifications made by using the contents disclosed in the present invention should still be covered by the scope of the patent application claims. Therefore, the scope of protection of the present invention should be as listed in the scope of the patent application claims.
Claims
1. A method for joining and cooling sheet metal parts, characterized in that: Include: Providing a first metal sheet and a second metal sheet, wherein the melting point of the first metal sheet is higher than the lowest heating softening temperature of the second metal sheet; stacking the second metal sheet and the first metal sheet on a concave mold in sequence to form a stacked sheet member; The laminated sheet is heated to a first temperature and then stopped, wherein the first temperature is a softening temperature of the first metal sheet; A self-piercing rivet is driven from the first metal sheet toward the second metal sheet of the laminated sheet member, so that the nail leg of the self-piercing rivet pierces the first metal sheet of the upper layer and stays inside the second metal sheet of the lower layer, and the bottom surface of the second metal sheet corresponding to the position of the self-piercing rivet is turned outward and plastically deformed to form a riveted joint to join the first metal sheet and the second metal sheet; Cooling the laminated sheet to a second temperature, the second temperature being the quenching temperature of the first metal sheet material; and Opening the mold and taking out the superimposed sheet metal part; The step of heating the laminated sheet further comprises a workpiece heating device, which uses a moving mechanism to move to an initial position to stop heating and a heating position to heat, and the heating position corresponds to the area of the first metal sheet where the self-piercing rivet is predetermined to be punched; The step of cooling the laminated sheet also includes a workpiece cooling device, in which a cooling water channel is arranged in the die, and liquid circulates in the cooling water channel to cool the laminated sheet in the die.
2. The method for joining and cooling sheet metal parts according to claim 1, characterized in that: The first metal sheet and the second metal sheet are made of steel, the first temperature is above 400° C., and the second temperature is above 250° C.
3. The method for joining and cooling sheet metal parts according to claim 1, characterized in that: The workpiece heating device uses electromagnetic induction coil heating.
4. A method for joining and cooling sheet metal parts, characterized in that: Include: Providing a first metal sheet and a second metal sheet, wherein the melting point of the first metal sheet is lower than the lowest heating softening temperature of the second metal sheet; Placing the second metal sheet on a concave mold; After heating the second metal sheet to a softening temperature, the heating is stopped, and the softening temperature is the softening temperature of the second metal sheet; Stacking the first metal sheet material on the second metal sheet material to form a laminated sheet member; A self-piercing rivet is driven from the first metal sheet toward the second metal sheet of the laminated sheet member, so that the nail leg of the self-piercing rivet pierces the first metal sheet of the upper layer and stays inside the second metal sheet of the lower layer, and the bottom surface of the second metal sheet corresponding to the position of the self-piercing rivet is turned outward and plastically deformed to form a riveted joint to join the first metal sheet and the second metal sheet; Cooling the laminated sheet to a quenching temperature, the quenching temperature being the quenching temperature of the second metal sheet material; and Opening the mold and taking out the superimposed sheet metal part; The step of heating the laminated sheet further comprises a workpiece heating device, which uses a moving mechanism to move to an initial position to stop heating and a heating position to heat, and the heating position corresponds to the area of the first metal sheet where the self-piercing rivet is predetermined to be punched; The step of cooling the laminated sheet also includes a workpiece cooling device, wherein a cooling water channel is arranged in the die, and liquid circulates in the water channel to cool the laminated sheet in the die.
5. The method for joining and cooling sheet metal parts according to claim 4, characterized in that: The material of the first metal sheet is aluminum alloy, the material of the second metal sheet is steel, the softening temperature is above 400° C., and the quenching temperature is above 250° C.
6. The method for joining and cooling sheet metal parts according to claim 4, characterized in that: The workpiece heating device includes electromagnetic induction coil heating.
Citation Information
Patent Citations
Bonding device for resin member, joint structure and joint method
JP2016055291A
Self-piercing riveting method by locally heating magnesium alloy plate with laser
CN101879572A
Riveting method of ultrahigh strength steel plates or aluminum alloy plates
CN103600016A
Self-punching riveting device of ultrahigh strength steel plate and aluminum alloy plate
CN104607557A
Joining device for resin member, joining structure, and joining method