Carbon fiber cloth-supported nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film and preparation method thereof

By using hydrothermal reaction to form a nickel-cobalt bimetallic selenide nanoneedle array film on carbon fiber cloth, the problem of transition metal selenide material agglomeration and low-dimensional array structure preparation was solved, achieving efficient electron transmission and catalytic performance, and improving Supercapacitor performance and stability.

CN113023665BActive Publication Date: 2024-10-11ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110244978.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-05
Publication Date
2024-10-11
Estimated Expiration
2041-03-05

AI Technical Summary

Technical Problem

Most of the existing transition metal selenide materials are powders, which are prone to agglomeration, leading to performance degradation. Research on double transition metal selenide crystal films with low-dimensional array structures is relatively rare, and there is a lack of efficient preparation methods.

Method used

Carbon fiber cloth is used as the substrate, and a nickel-cobalt bimetallic selenide crystal array film is formed on the surface through hydrothermal reaction. Hydrazine hydrate is used to introduce the selenium element into the ionic state, optimizing the ratio and reaction parameters of nickel and cobalt, and promoting the nanoneedle-like morphology. The nucleation and growth, combined with heat treatment, form a dense low-dimensional array structure.

Benefits of technology

The realization of a high specific surface area thin film material improves electron transmission efficiency and catalytic ability, significantly improves the electrochemical performance and cycle stability of supercapacitors, simplifies the preparation process, and reduces energy consumption and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113023665B_ABST
    Figure CN113023665B_ABST
Patent Text Reader

Abstract

This invention discloses a carbon fiber cloth-supported nanoneedle-shaped nickel-cobalt bimetallic selenide crystal array thin film and its preparation method. The preparation method mainly includes the following steps: First, using soluble nickel salt, soluble cobalt salt, and selenium powder as raw materials and activated carbon fiber cloth as a substrate, a nanoneedle-shaped nickel-cobalt bimetallic selenide thin film precursor is prepared by hydrothermal method. Then, the precursor is heat-treated under inert gas protection to obtain the nanoneedle-shaped nickel-cobalt bimetallic selenide crystal array thin film. The needle-shaped crystal array thin film disclosed in this invention has the advantages of simple process and easy operation; the nickel-cobalt bimetallic selenide crystal film is directly bonded to the activated carbon fiber cloth through the endpoints of the low-dimensional array, which is beneficial to increase the active sites and improve the conductivity and stability of the material. The nanoneedle-shaped nickel-cobalt bimetallic selenide crystal array thin film has broad application prospects in energy storage and catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a compound semiconductor film, in particular to a carbon fiber cloth-loaded nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film and a preparation method thereof. Background Art

[0002] Nano-selenides are a class of semiconductor materials with excellent performance and have broad application prospects in the fields of optics, electromagnetism, optoelectronics, nonlinear optics, nonlinear thermal science, biomedicine and other functional materials. As a non-stoichiometric transition metal selenide, M x Se (M=Ni,Co,Mn) has a special electronic configuration, abundant unsaturated bonds and a stable phase at room temperature. It shows a large number of electrochemically active sites and high-speed charge transfer channels, making it a potential energy storage and catalytic material.

[0003] At present, most transition metal selenides are in the form of powder materials. Zhao et al. used a simple two-step solvothermal method to prepare nickel cobalt selenide nanoparticles as an electrocatalyst for water decomposition. This inexpensive and easy-to-prepare electrocatalyst has a high current density of 10 mV / cm 2 The electrocatalyst showed excellent OER activity when the catalyst was heated to 100 ℃ and then heated to 200 ℃. The electrocatalyst also showed excellent durability under the chronoamperometry test, which could last for 10 hours. [NiCo-selenide as a novel catalyst for water oxidation[J].Journal of Materials Science, 2016, 51(8):3724-3734.]

[0004] However, nanopowders will agglomerate during the preparation, separation, processing and storage process, which leads to the decline of the performance of nanopowder materials. Making nanoparticles into low-dimensional array materials is an effective way to solve the agglomeration problem. Therefore, researchers began to pay attention to the development of transition metal selenide thin film materials. Gong et al. used nickel foam as a substrate and synthesized high-performance Ni on its surface by hydrothermal method. 0.85Se electrode material, under 1 A / g charge and discharge conditions, the specific capacity can reach up to 1115 F / g, and after 1000 cycles of charge and discharge, the specific capacitance only decreases by 8.3%. [Gong C, Huang M, Zhang J, et al. Facilesynthesis of Ni0.85Se on Ni foam for high-performance asymmetric capacitor[J]. Rsc Advances, 2015, 5(99):81474-81481.]. Abhik Banerjee et al. synthesized Co with dense self-woven structure on conductive carbon fiber paper. 0.85 Se hollow nanowires, with area specific capacitance values ​​of 929.5 mF / c and 600 mF / cm 2 , the retention rate reaches 60% [Abhik, Banerjee, Sumit, et al. Hollow Co0.85Se Nanowire Array onCarbon Fiber Paper for High Rate Pseudocapacitor[J]. ACS Applied Materials &Interfaces, 2014, 6(21):18844-18852.].

[0005] Compared with single metal selenides, selenides containing two or more transition metals show better electrochemical performance. Chen et al. prepared NiSe-CoSe nanoparticles with different Ni / Co ratios through hydrothermal reaction. The specific capacitance can reach 584 F / g at a current density of 1 A / g, and its capacity can still be maintained at about 77.3% at a current density of 20 A / g.

[0006] At present, there are few research reports on double transition metal selenide crystal films with low-dimensional array structures. Directly growing low-dimensional array structures on the surface of substrate materials eliminates the mixing and coating process steps in the traditional electrode preparation process, and also avoids the use of binders and conductive agents. The low-dimensional array structure film provides a high-speed conduction channel for ions and electrons; at the same time, the gaps between the nanoarrays provide sufficient space for volume changes during the charge and discharge process, which is beneficial to maintain the stability of the structure on the one hand, and on the other hand, it also helps to fully infiltrate the electrolyte and improve the utilization rate of active substances. Many factors make double transition metal selenide crystal film materials have better electrochemical properties than traditional materials. Summary of the invention

[0007] In order to solve the problems in the background technology, the present invention provides a carbon fiber cloth-loaded nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film and a preparation method thereof. The preparation method makes full use of the porous surface of activated carbon fiber to provide a large number of nucleation centers for heterogeneous nucleation and crystallization of crystals on the surface of activated carbon fiber; utilizes the strong reduction effect of hydrazine hydrate to introduce selenium element into the reaction in an ionic state to improve the reaction efficiency of the selenium source; optimizes the ratio of nickel to cobalt to form a single-phase bimetallic selenide; combines the adjustment of reactant concentration, reaction time, and heat treatment parameters to make the nickel-cobalt bimetallic selenide crystals crystallize preferentially on the surface of activated carbon fiber, and then grows anisotropically to form a nano-needle-shaped morphology.

[0008] The present invention designs a stable hydrothermal reaction system, and through comprehensive optimization of reaction parameters, a one-step method is used to promote the formation of a dense and uniform needle array of selenium-containing nickel-cobalt bimetallic compounds on the surface of activated carbon fibers, and then a subsequent heat treatment is performed to strengthen the regularity of atomic arrangement to obtain a nickel-cobalt bimetallic selenium compound. The reaction system and parameters precisely control the crystal growth process and promote the formation of anisotropic low-dimensional nano-needle crystal morphology.

[0009] The technical solution adopted by the present invention is as follows:

[0010] A carbon fiber cloth-loaded nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film: the carbon fiber cloth is loaded with nickel-cobalt bimetallic selenide crystals; the nickel-cobalt bimetallic selenide crystals are needle-shaped, with a length of 5 to 10 microns and a diameter of 200 to 300 nanometers, and are densely and evenly grown on the carbon fiber.

[0011] A method for preparing a carbon fiber cloth-supported nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film comprises the following steps:

[0012] (1) Dissolving a soluble nickel salt and a soluble cobalt salt in deionized water and stirring to obtain a uniform solution A;

[0013] (2) dissolving selenium powder in hydrazine hydrate solution and stirring by ultrasonic to obtain a uniform solution B;

[0014] (3) Stir solution A with a magnetic stirrer, add solution B dropwise into the vigorously stirred solution A with a dropper, and continue stirring for 30 min to obtain a uniform solution C;

[0015] (4) immersing the activated carbon fiber cloth in solution C of step (3) for 5 hours;

[0016] (5) The solution obtained after immersion in step (4) is transferred together with the activated carbon fiber cloth into a stainless steel reactor lined with polytetrafluoroethylene, and reacted together at 150° C. to 180° C. for 12 to 24 hours in a sealed state;

[0017] (6) After the reaction is completed, wait for the reactor to cool naturally to room temperature, take out the activated carbon fiber cloth, wash it with distilled water and ethanol in turn, and then vacuum dry it at 60℃~90℃ for 8 h;

[0018] (7) Under the protection of argon or nitrogen, the activated carbon fiber cloth obtained by drying in step (6) is heat-treated at 300° C. to 350° C. for 1 h to obtain a nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film on its surface.

[0019] In the step 1), the soluble nickel salt is one of nickel nitrate, nickel chloride or nickel acetate; the soluble cobalt salt is one of cobalt nitrate, cobalt chloride or cobalt acetate.

[0020] In the step 1), the total molar concentration of nickel ions and cobalt ions is 0.10-0.20 mol / L, and the molar concentration ratio of nickel ions to cobalt ions is 1:1.

[0021] The selenium content in the solution B in step 2) is 0.2 mol / L.

[0022] In the step 2), the hydrazine hydrate solution is a mixed solution of hydrazine hydrate (the volume percentage of hydrazine hydrate is 85%) and deionized water in a volume ratio of 1:1.

[0023] In the step 3), the rotation speed of the magnetic stirrer is 2000 r / min.

[0024] In the step 4), the activated carbon fiber cloth is obtained by heat treating natural cotton fiber cloth at 1000° C. for 1 hour in a nitrogen atmosphere.

[0025] The beneficial effects of the present invention are:

[0026] 1) The film of the present invention has a high specific surface area characteristic of low-dimensional materials, and is combined with a conductive substrate in a binder-free manner, effectively improving the electron transmission efficiency, greatly improving the application value of the film material in energy storage devices. On the other hand, the degeneracy of the double transition metal d orbital plays a key role in the process of electron gain and loss and bonding, and plays a positive role in improving its catalytic ability.

[0027] 2) The carbon fiber cloth loaded with nano-needle-shaped nickel-cobalt bimetallic selenide crystal array thin film electrode material prepared by the present invention is applied to supercapacitors. Test results show that the electrode materials of the present invention all exhibit efficient pseudocapacitive performance and specific capacitance, especially the electrode material prepared under the conditions of nickel-cobalt ratio of 1:1 and hydrothermal reaction at 180°C for 12 hours has the best electrochemical performance.

[0028] 3) The present invention utilizes the high temperature and high pressure wet chemical environment formed by the hydrothermal reaction system, and adjusts the reaction parameters to achieve the formation of nano-needle morphology of nickel-cobalt bimetallic selenide, and densely arranges in array form on the surface of activated carbon fiber cloth to form a continuous film. Hydrazine hydrate is selected to reduce the selenium source to ion form and enter the solution system. The nitrogen on the hydrazine molecule coordinates with the empty orbital of the nickel-cobalt ion d zone using the lone pair of electrons, and guides the formation of low-dimensional needle-like morphology. The porous structure on the surface of the activated carbon fiber provides a large number of nucleation micro-regions for crystallization, reduces the activation energy of the crystal nucleation reaction, and makes the crystal preferentially heterogeneously nucleate to form a film. The hydrothermal reaction temperature is adjusted to 170°C to control the crystal growth rate, which is conducive to the low-dimensional heterogeneous growth of the crystal to micron-level length. The amount of nickel-cobalt substances is reasonably proportioned, and the heat treatment parameters are finely adjusted to form a single-phase nickel-cobalt bimetallic selenide.

[0029] 4) The hydrothermal synthesis route disclosed in the present invention obtains a nano needle-shaped crystal array film through a one-step wet chemical reaction, and the preparation process is simple and the conditions are mild. The subsequent heat treatment at a lower temperature obtains a pure phase, which has low energy consumption and low cost and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is the XRD pattern of the product obtained in Example 1.

[0031] Figure 2 This is an electron microscope photograph of the product obtained in Example 1.

[0032] Figure 3 This is the X-ray energy dispersive spectrum (EDS) analysis chart of the product obtained in Example 1.

[0033] Figure 4 This is the cyclic voltammogram of the product obtained in Example 1.

[0034] Figure 5 This is a constant current charge and discharge curve picture of the product obtained in Example 1.

[0035] Figure 6 It is the AC impedance spectrum of the product obtained in Example 1.

[0036] Figure 7 This is a cyclic stability test diagram of the product obtained in Example 1.

[0037] Figure 8 This is an electron microscope photograph of the product obtained in Example 2.

[0038] Fig. 9 This is an electron microscope photograph of the product obtained in Example 3. DETAILED DESCRIPTION

[0039] The carbon fiber cloth of the present invention carries a nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film, wherein the nano-needle-shaped nickel-cobalt bimetallic selenide crystals have a diameter of 200-300 nanometers and a length of 5-10 micrometers, and are densely arranged in an array form to form a film. The nickel-cobalt bimetallic selenide crystal film is directly combined with the activated carbon fiber cloth through the endpoints of the low-dimensional array, which is conducive to increasing active sites and improving the conductivity and stability of the material. The nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film has broad application prospects in the fields of energy storage and catalysis.

[0040] Embodiment 1:

[0041] 0.4759 g CoCl2.6H2O and 0.4753 g NiCl2.6H2O were dissolved in 20 mL of deionized water and stirred to obtain a uniform mixed solution A, in which the total molar concentration of nickel ions and cobalt ions was 0.20 mol / L, and the molar concentration ratio of nickel ions to cobalt ions was 1:1. 0.3159 g of selenium powder was dissolved in 20 mL of hydrazine hydrate solution to obtain a mixed solution B, in which the selenium content was 0.2 mol / L, and the hydrazine hydrate solution was uniformly mixed by 10 mL (85%) hydrazine hydrate solution and 10 mL deionized water; the mixed solution B was slowly added dropwise to the vigorously stirred mixed solution A, and ultrasonicated for 30 minutes to obtain a uniform solution C; the activated carbon fiber cloth was immersed in the solution C for 5 hours; then the solution C, together with the activated carbon fiber cloth, was transferred into an 85 mL polytetrafluoroethylene-lined stainless steel autoclave, and sealed and reacted at 180°C for 12 hours; after the reaction was completed, the reactor was naturally cooled to room temperature, the activated carbon fiber cloth was taken out, washed with distilled water and ethanol in turn, and dried at 90°C for 8 hours; under argon protection, the dried activated carbon fiber cloth was heat treated at 350°C for 1 hour to obtain a nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film grown on the surface of the activated carbon fiber cloth.

[0042] Figure 1 This is the XRD spectrum of the product of Example 1. The characteristic diffraction peaks of the crystalline material on the spectrum match the standard XRD spectrum of CoNiSe2 (JCPDS No 70-2851). The diffraction peak intensity of the sample is relatively large and the half-peak width is relatively small, indicating that the prepared nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film sample has high crystallinity.

[0043] Figure 2 This is an electron microscope photograph of the product of Example 1. A NiCoSe2 nanoneedle crystal array film is formed on the surface of the activated carbon fiber. The needles are uniform in size, with a diameter of 200 nanometers to 300 nanometers and a length of 5-10 micrometers. They are densely arranged in an array on the fiber surface.

[0044] Figure 3The X-ray energy dispersive spectrum analysis (EDS) of the product of Example 1 shows that the atomic contents of Ni, Co and Se in the sample are 25.46%, 29.05% and 45.49% respectively, which is basically consistent with the ratio of the NiCoSe2 molecular formula.

[0045] The three-electrode system test was performed on the nano-needle-shaped nickel-cobalt bimetallic selenide crystal array thin film supercapacitor electrode material prepared in this embodiment. Figure 4 The cyclic voltammogram is shown below. -1 In the KOH electrolyte, a pair of obvious redox peaks can be seen in the cyclic voltammetry curve of the electrode material, and with the increase of the scan rate, the oxidation peak moves to the positive potential and the reduction peak moves to the negative potential. This is mainly due to the potential jump caused by the electric double layer formed when the electronic conductor contacts the electrolyte at a high scan rate and the increase in the internal resistance of the active material, which leads to the separation of the redox peaks. -1 To 30 mV·s -1 It exhibits good pseudocapacitive behavior at a scan rate of 2.5 %. Figure 5 The constant current charge and discharge curve is shown in Figure 2. -1 The current density was 2, 5, 10, 20 and 50 mA·cm in KOH electrolyte. -2 When the composite electrode exhibited 1513.6, 1421.3, 1254.1, 1102.9 and 967.4 F·g -1 The high specific capacity shows good electrochemical performance. Figure 6 The AC impedance spectrum is shown in 2 mol·L -1 In the KOH electrolyte, the internal resistance of the composite electrode during the test was 0.5 Ω and the charge transfer resistance was 2.3 Ω. Figure 7 As the cycle stability test chart, we can see that at 10 mA·cm -2 Under the same current density, after 1000 charge and discharge cycles, the composite electrode still retained 84.3% of the original capacitance value, showing good cycle stability.

[0046] Embodiment 2:

[0047] 0.2379 g CoCl2 . 6H2O and 0.2377 g NiCl2 .6H2O was dissolved in 20 mL of deionized water and stirred to obtain a uniform mixed solution A, in which the total molar concentration of nickel ions and cobalt ions was 0.10 mol / L, and the molar concentration ratio of nickel ions to cobalt ions was 1:1. 0.3159 g of selenium powder was dissolved in 20 mL of hydrazine hydrate solution to obtain a mixed solution B, in which the selenium content was 0.2 mol / L, and the hydrazine hydrate solution was uniformly mixed by 10 mL (85%) hydrazine hydrate solution and 10 mL deionized water; the mixed solution B was slowly added dropwise to the vigorously stirred mixed solution A, and ultrasonicated for 30 minutes to obtain a uniform solution C; the activated carbon fiber cloth was immersed in the solution C for 5 hours; then the solution C, together with the activated carbon fiber cloth, was transferred into an 85 mL polytetrafluoroethylene-lined stainless steel autoclave, and sealed and reacted at 150°C for 24 hours; after the reaction, the reactor was naturally cooled to room temperature, the activated carbon fiber cloth was taken out, washed with distilled water and ethanol in turn, and dried at 60°C for 8 hours; the dried activated carbon fiber cloth was heat treated at 300°C for 1 hour under argon protection to obtain a nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film grown on the surface of the activated carbon fiber cloth.

[0048] Figure 8 This is an electron microscope photograph of the product of Example 2. The NiCoSe2 nanoneedle particles have a diameter of 100-150 nanometers and a length of 5-10 micrometers and are evenly distributed on the activated carbon fibers.

[0049] Embodiment 3:

[0050] 0.4759 g CoCl2.6H2O and 0.4753 g NiCl2.6H2O were dissolved in 20 mL of deionized water and stirred to obtain a uniform mixed solution A, in which the total molar concentration of nickel ions and cobalt ions was 0.20 mol / L, and the molar concentration ratio of nickel ions to cobalt ions was 1:1. 0.3159 g of selenium powder was dissolved in 20 mL of hydrazine hydrate solution to obtain a mixed solution B, in which the selenium content was 0.2 mol / L, and the hydrazine hydrate solution was uniformly mixed by 10 mL (85%) hydrazine hydrate solution and 10 mL deionized water; the mixed solution B was slowly added dropwise to the vigorously stirred mixed solution A, and ultrasonicated for 30 minutes to obtain a uniform solution C; the activated carbon fiber cloth was immersed in the solution C for 5 hours; then the solution C, together with the activated carbon fiber cloth, was transferred into an 85 mL polytetrafluoroethylene-lined stainless steel autoclave, and sealed and reacted at 165°C for 18 hours; after the reaction, the reactor was naturally cooled to room temperature, the activated carbon fiber cloth was taken out, washed with distilled water and ethanol in turn, and dried at 90°C for 8 hours; the dried activated carbon fiber cloth was heat treated at 350°C for 1 hour under nitrogen protection to obtain a nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film grown on the surface of the activated carbon fiber cloth.

[0051] Fig. 9 This is an electron microscope photograph of the product of Example 3. The NiCoSe2 nanoneedle particles have a diameter of 200-300 nanometers and a length of 5-8 micrometers and are evenly distributed on the activated carbon fibers.

Claims

1. A method for preparing a carbon fiber cloth-supported nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film, characterized in that: The carbon fiber cloth is loaded with nickel-cobalt bimetallic selenide crystals; the nickel-cobalt bimetallic selenide crystals are needle-shaped, 5 to 10 microns in length, 200 to 300 nanometers in diameter, and grow densely and evenly on the carbon fiber; Nano-needle-shaped nickel-cobalt bimetallic selenide crystal array thin film supercapacitor electrode material at 2 mol·L -1 The current density was 2, 5, 10, 20 and 50 mA·cm in KOH electrolyte. -2 When the composite electrode exhibited 1513.6, 1421.3, 1254.1, 1102.9 and 967.4 F·g -1 High specific capacity; The method for preparing the carbon fiber cloth-supported nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film comprises the following steps: (1) Dissolving a soluble nickel salt and a soluble cobalt salt in deionized water and stirring to obtain a uniform solution A; (2) dissolving selenium powder in hydrazine hydrate solution and stirring by ultrasonic to obtain a uniform solution B; (3) Stir solution A with a magnetic stirrer, add solution B dropwise into the vigorously stirred solution A with a dropper, and continue stirring for 30 min to obtain a uniform solution C; (4) immersing the activated carbon fiber cloth in solution C of step (3) for 5 hours; (5) The solution obtained after immersion in step (4) is transferred together with the activated carbon fiber cloth into a stainless steel reactor lined with polytetrafluoroethylene, and reacted together at 150° C. to 180° C. for 12 to 24 hours in a sealed state; (6) After the reaction is completed, wait for the reactor to cool naturally to room temperature, take out the activated carbon fiber cloth, wash it with distilled water and ethanol in turn, and then vacuum dry it at 60℃~90℃ for 8 h; (7) Under the protection of argon or nitrogen, heat-treating the activated carbon fiber cloth obtained by drying in step (6) at 300° C. to 350° C. for 1 h to obtain a nano-needle-shaped nickel-cobalt bimetallic selenide crystal array film on its surface; In the step (1), the total molar concentration of nickel ions and cobalt ions is 0.10-0.20 mol / L, and the molar concentration ratio of nickel ions to cobalt ions is 1:1; The selenium content in solution B in step (2) is 0.2 mol / L; In the step (2), the hydrazine hydrate solution is a mixed solution of hydrazine hydrate and deionized water in a volume ratio of 1:

1.

2. The method for preparing a carbon fiber cloth-supported nano-acicular nickel-cobalt bimetallic selenide crystal array thin film according to claim 1, characterized in that: In the step (1), the soluble nickel salt is one of nickel nitrate, nickel chloride or nickel acetate; the soluble cobalt salt is one of cobalt nitrate, cobalt chloride or cobalt acetate.

3. The method for preparing a carbon fiber cloth-supported nano-acicular nickel-cobalt bimetallic selenide crystal array thin film according to claim 1, characterized in that: In the step (3), the rotation speed of the magnetic stirrer is 2000 r / min.

4. The method for preparing a carbon fiber cloth-supported nano-acicular nickel-cobalt bimetallic selenide crystal array thin film according to claim 1, characterized in that: In the step (4), the activated carbon fiber cloth is obtained by heat treating natural cotton fiber cloth at 1000° C. for 1 hour in a nitrogen atmosphere.