Condensed ring compound and preparation method thereof, organic electroluminescent device and electronic device
By using specific fused ring compounds as electron transport layer materials in OLED devices, the problems of unbalanced carrier transfer rates and insufficient film formation are solved, the luminous efficiency and lifespan of OLED devices are improved, and the driving voltage is reduced.
Patent Information
- Application Number
- CN202011264477.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-27
- Filing Date
- 2020-11-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-11-12
AI Technical Summary
The carrier transfer rates of hole transport materials and electron transport materials in existing OLED devices are unbalanced, resulting in a decrease in device performance, and the film-forming properties and thermal stability of the electron transport materials are insufficient, affecting device efficiency and lifespan.
Specific fused ring compounds are used as electron transport layer materials of OLED devices, and planar structures are introduced through oxygen, sulfur or nitrogen heterocycles to increase the HOMO energy level and connect through specific groups to enhance the triplet energy level to meet the exciton binding requirements and reduce Risk of crystallization.
The luminous efficiency and service life of the OLED device are improved, while the driving voltage is reduced, and the heat resistance of the organic layer and the Joule thermal stability between the electrodes are enhanced.
Smart Images

Figure CN113045558B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic light-emitting materials, and in particular to a condensed ring compound and a preparation method thereof, and an organic electroluminescent device and an electronic device. Background Art
[0002] Organic light emitting diodes (OLEDs) are self-emitting devices, have advantages such as wide viewing angles, excellent contrast, fast response, high brightness, and excellent driving voltage characteristics, and can provide color images.
[0003] The basic structure of OLED is a thin and transparent semiconductor indium tin oxide (ITO), connected to the positive electrode of electricity, and then another metal cathode, forming a sandwich structure. The entire structure includes a hole transport layer (HTL), a light-emitting layer (EL), and an electron transport layer (ETL). When electricity is supplied to an appropriate voltage, the positive holes and the cathode charges will combine in the light-emitting layer to generate light, and the three primary colors of red, green, and blue RGB will be generated according to different formulas, forming the basic colors.
[0004] Among them, the requirements that electron transport materials should meet are: (1) good electron transport properties, that is, high electron mobility; (2) high electron affinity, easy to inject electrons from the cathode; (3) relatively high ionization energy, which is conducive to blocking holes; (4) unable to form an excited radical complex with the light-emitting layer; (5) good film-forming properties and thermal stability, and not easy to crystallize.
[0005] At present, the hole mobility of hole transport materials in existing OLED devices is generally much greater than the electron mobility of electron transport materials, which is 100 times that of electron transport materials, about 10-3cm 2 / Vs. This unbalanced carrier transfer rate will lead to a significant decrease in device performance. Therefore, only with good electron mobility can electrons be effectively transferred to the recombination area far away from the cathode. In addition, the electron transport material must have good film-forming properties, otherwise it will not form a uniform film during evaporation, and it is easy to crystallize, which will seriously affect the efficiency and life of the device. At present, the most commonly used electron transport materials such as Alq 3 However, due to the influence of material properties, the driving voltage or luminous efficiency of the device is not ideal.
[0006] In view of the current industrial application requirements of OLED devices, as well as the different functional film layers of OLED devices and the photoelectric characteristics of the devices, it is necessary to select more suitable OLED functional materials or material combinations with high performance to achieve the comprehensive characteristics of high efficiency, long life and low voltage of the devices. As far as the actual needs of the current OLED display lighting industry are concerned, the current development of OLED materials is far from enough and lags behind the requirements of panel manufacturers. It is particularly important for material companies to develop higher performance organic functional materials. KR1020150111271A and KR1020160076357A respectively disclose an organic light-emitting compound. Summary of the invention
[0007] In order to overcome the above-mentioned defects of the prior art, the purpose of the present invention is to provide a condensed ring compound and a preparation method thereof, and an organic electroluminescent device and an electronic device containing the same. The condensed ring compound of the present invention is used as a luminescent host material or an electron transport layer material of an OLED device, which can effectively improve the luminous efficiency and service life of the OLED device.
[0008] In order to achieve the above object, the present invention adopts the following technical scheme:
[0009] In a first aspect, the present invention provides a condensed ring compound represented by Formula 1, Formula 2 or Formula 3:
[0010]
[0011] In formula 1 to formula 3, R 1 To R 6 Each is the same or different and is independently selected from hydrogen or C1-C6 alkyl;
[0012] Y 1 Selected from O, S or N (R 11 ), R 11 Selected from C6-C18 substituted or unsubstituted aryl, C3-C15 substituted or unsubstituted heteroaryl;
[0013] Y 2 is N;
[0014] A1 is a benzene ring;
[0015] M is a group represented by formula 4:
[0016]
[0017] In formula 4, X 1 , X 2 , X 3 At least 2 of them are N, and the rest are N or CH;
[0018] L is selected from C12-C60 substituted or unsubstituted arylene, C6-C60 substituted or unsubstituted heteroarylene;
[0019] Ar 1 and Ar 2 are the same or different, and are each independently selected from C6-C40 substituted or unsubstituted aryl, and C3-C40 substituted or unsubstituted heteroaryl.
[0020] In a second aspect, the present invention provides a method for preparing the condensed ring compound, comprising the following steps:
[0021] (1) under nitrogen protection, raw material Ia, xylene, raw material Ib, potassium carbonate, cuprous bromide and 18-crown ether-6 are added, and then the temperature is raised to reflux state for reaction, and after the liquid phase monitoring reaction is complete, the reaction liquid is cooled, and then the inorganic salt in the reaction is washed with water, and the liquid is separated, and the obtained organic phase is dried over anhydrous sodium sulfate, filtered, and the filtrate is concentrated to dryness and recrystallized from toluene to obtain intermediate Id;
[0022] (2) Under nitrogen protection, add intermediate Id, bipyraclostrobin, potassium acetate and 1,4-dioxane, add [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride at 30-80°C, continue heating to reflux state to react for 3-9 hours, cool the reaction solution, pour water and toluene into the solution under stirring, extract the solution after standing, separate the solution, extract the aqueous phase with toluene once more, separate the solution, combine the organic phases, add anhydrous sodium sulfate into the organic phases, stir and dry, and obtain intermediate Ie;
[0023] (3) under nitrogen protection, toluene, raw material Ic, intermediate Ie, potassium carbonate, tetrabutylammonium bromide, ethanol and water are added, tetrakistriphenylphosphine palladium is added at 30-100°C, and the reaction is continued to be heated to reflux state, and the reaction is kept warm until the reaction is complete after liquid phase monitoring, and the reaction liquid is cooled, poured into water with stirring, and allowed to stand for separation, and the aqueous phase is extracted with toluene, and the organic phases are combined, dried with anhydrous sodium sulfate and filtered, and the filtrate is concentrated until no solvent is distilled off, and then recrystallized from toluene to obtain the condensed ring compound;
[0024] The raw material Ib is Br-L-Cl, and the raw material Ic is in,
[0025] The raw material Ia is And the intermediate ID is
[0026] Intermediate Ie is The obtained condensed ring compound is shown in Formula 1; or
[0027] The raw material Ia is And the intermediate ID is
[0028] Intermediate Ie is The obtained condensed ring compound is shown in Formula 2; or
[0029] The raw material Ia is And the intermediate ID is
[0030] Intermediate Ie is The obtained condensed ring compound is shown in Formula 3.
[0031] In a third aspect, the present invention provides an organic electroluminescent device comprising an anode, a cathode and an organic layer deposited between the anode and the cathode, wherein the organic layer comprises a hole transport layer, an electron blocking layer, a light-emitting layer and an electron transport layer, wherein the electron transport layer or the light-emitting layer contains the condensed ring compound.
[0032] In a fourth aspect, the present invention provides an electronic device comprising the electroluminescent device.
[0033] Compared with the prior art, the present invention has the following beneficial technical effects:
[0034] The condensed ring compound of the present invention includes a condensed ring core represented by any one of the structures in Formula 1, Formula 2 and Formula 3, and a condensed ring compound is obtained by introducing oxygen or sulfur or nitrogen heterocycles, and their planar structure improves the HOMO energy level of the material and increases the charge transfer efficiency. At the same time, by connecting a special group (i.e., M of Formula 1 to Formula 3) with an ortho-substituted connection of a specific linking group (L), the triplet energy level can be made to meet the requirements of exciton binding, and at the same time, due to the effect of steric hindrance, the corresponding compound is not easy to crystallize. The condensed ring compound of the present invention is successfully applied to organic light-emitting devices, so that the device has higher efficiency and brightness, while meeting a lower driving voltage. Therefore, it can have the heat resistance of improving the Joule heat generated in the organic layer of the organic light-emitting device and between the organic layer and the electrode, and the organic light-emitting device including the condensed ring compound represented by Formula 1-Formula 3 can maintain a long service life during storage and driving. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic structural diagram of an organic electroluminescent device according to an embodiment of the present invention.
[0036] Figure 2 is a schematic diagram of an electronic device according to an embodiment of the present invention.
[0037] Description of Reference Numerals
[0038] 100, anode; 200, cathode; 300, functional layer; 310, hole injection layer; 320, hole transport layer; 321, first hole transport layer; 322, second hole transport layer; 330, organic electroluminescent layer; 340, hole blocking layer; 350, electron transport layer; 360, electron injection layer; 370, electron blocking layer; 500, mobile phone screen. DETAILED DESCRIPTION
[0039] In a first aspect, the present invention provides a condensed ring compound represented by any one of Formula 1, Formula 2 and Formula 3:
[0040]
[0041] In formula 1 to formula 3, R 1 To R 6 The same or different, each independently selected from hydrogen or C1-C6 alkyl;
[0042] Y 1 Selected from O, S or N (R 11 ), R 11 Selected from C6-C18 substituted or unsubstituted aryl, C3-C15 substituted or unsubstituted heteroaryl;
[0043] Y 2 is N;
[0044] A1 is a benzene ring;
[0045] M is a group represented by formula 4:
[0046]
[0047] In formula 4, X 1 , X 2 , X 3 At least 2 of them are N, and the rest are N or CH;
[0048] L is selected from C12-C60 substituted or unsubstituted arylene, C6-C60 substituted or unsubstituted heteroarylene;
[0049] Ar 1 and Ar 2 are the same or different, and are each independently selected from C6-C40 substituted or unsubstituted aryl, and C3-C40 substituted or unsubstituted heteroaryl.
[0050] In the present invention, aryl refers to an optional functional group or substituent derived from an aromatic hydrocarbon ring. The aryl group can be a monocyclic aryl group or a polycyclic aryl group. In other words, the aryl group can be a monocyclic aryl group, a condensed ring aryl group, two or more monocyclic aryl groups connected by conjugation of carbon-carbon bonds, monocyclic aryl groups and condensed ring aryl groups connected by conjugation of carbon-carbon bonds, and two or more condensed ring aryl groups connected by conjugation of carbon-carbon bonds. That is, two or more aromatic groups connected by conjugation of carbon-carbon bonds can also be regarded as aryl groups of the present disclosure. Among them, the aryl group does not contain heteroatoms such as B, N, O, S, P, and Si. For example, biphenyl, terphenyl, etc. are aryl groups. Specific examples of aryl groups include, but are not limited to, phenyl, naphthyl, fluorenyl, spiro-fluorenyl, anthracenyl, phenanthrenyl, biphenyl, terphenyl, quaterphenyl, pentaphenyl, benzo[9,10]phenanthrenyl, pyrenyl, benzofluoranthenyl, Ji et al.
[0051] Substituted aryl means that one or more hydrogen atoms in the aryl are replaced by other groups (i.e., substituents), for example, at least one hydrogen atom is replaced by a deuterium atom, a -halogen group, -CN, an alkyl group (e.g., a C1-C6 alkyl group), a cycloalkyl group (e.g., a C3-C10 cycloalkyl group), an alkoxy group (e.g., a C1-C6 alkoxy group), a silane group (e.g., a C3-C10 silane group), or other substituents. It should be understood that the number of carbon atoms in the substituted aryl refers to the total number of carbon atoms in the aryl group and the substituents on the aryl group; for example, a substituted C6-C40 aryl means that the total number of carbon atoms in the aryl group and the substituents on the aryl group is 6-40.
[0052] In the present invention, the heteroaryl group may be a heteroaryl group including at least one of B, O, N, P, Si and S as a heteroatom. The heteroaryl group may be a monocyclic heteroaryl group or a polycyclic heteroaryl group. In other words, the heteroaryl group may be a single aromatic ring system or a plurality of aromatic ring systems conjugated by carbon-carbon bonds, and any aromatic ring system may be an aromatic monocyclic ring or an aromatic condensed ring. Specific examples of heteroaryl groups include, but are not limited to, thienyl, furyl, pyrrolyl, imidazolyl, thiazolyl, oxazolyl, oxadiazolyl, triazolyl, pyridyl, bipyridyl, pyrimidyl, triazine, acridinyl, pyridazinyl, pyrazinyl, quinolyl, quinazolinyl, quinoxalinyl, phenoxazinyl, phthalazinyl, pyridopyrimidinyl, pyridopyrazinyl, pyrazinopyrazinyl, isoquinolyl, indolyl, carbazolyl, N-arylcarbazolyl (e.g., N-phenyl) The invention also includes benzoxazolyl, benzimidazolyl, benzothiazolyl, benzocarbazolyl, benzothiophenyl, dibenzothiophenyl, thienothiphenyl, benzofuranyl, phenanthrolinyl, isoxazolyl, thiadiazolyl, benzothiazolyl, phenothiazinyl, dibenzosilyl, dibenzofuranyl, phenyl-substituted dibenzofuranyl, dibenzofuranyl-substituted phenyl, etc. Among them, thienyl, furanyl, phenanthrolinyl, etc. are heteroaryl groups of a single aromatic ring system, and N-arylcarbazolyl, N-heteroarylcarbazolyl, phenyl-substituted dibenzofuranyl, dibenzofuranyl-substituted phenyl, etc. are heteroaryl groups of multiple aromatic ring systems conjugated by carbon-carbon bonds.
[0053] Substituted heteroaryl means that one or more hydrogen atoms in the heteroaryl are replaced by other groups (i.e., substituents) other than heteroaryl, for example, at least one hydrogen atom is replaced by a deuterium atom, a halogen group, -CN, an alkyl group (e.g., a C1-C6 alkyl group), a cycloalkyl group (e.g., a C3-C10 cycloalkyl group), an alkoxy group (e.g., a C1-C6 alkoxy group), a silyl group (e.g., a C3-C10 silyl group), or other substituents. It should be understood that the number of carbon atoms in the substituted heteroaryl refers to the total number of carbon atoms in the heteroaryl group and the substituents on the heteroaryl group. For example, a substituted C3-C40 heteroaryl means that the total number of carbon atoms in the heteroaryl group and the substituents on the heteroaryl group is 3-40.
[0054] In the present invention, the non-positioned connecting bond refers to a single bond extending from the ring system. It means that one end of the connecting bond can be connected to any position in the ring system that the bond passes through, and the other end is connected to the rest of the compound molecule. For example, as shown in the following formula (X'), the phenanthryl group represented by formula (X') is connected to other positions of the molecule through a non-positional connecting bond extending from the middle of one side of the benzene ring, and the meaning represented by it includes any possible connection mode shown in formula (X'-1) to formula (X'-4).
[0055]
[0056] The non-positioning substituent in the present invention refers to a substituent connected by a single bond extending from the center of the ring system, which means that the substituent can be connected to any possible position in the ring system. For example, as shown in the following formula (Y), the substituent R' represented by formula (Y) is connected to the quinoline ring through a non-positioning connecting bond, and the meaning represented includes any possible connection mode shown in formula (Y-1) to formula (Y-7).
[0057]
[0058] In the present invention, C1-C6 alkyl includes C1-C6 straight-chain alkyl and C3-C6 branched-chain alkyl; the number of carbon atoms in the alkyl is, for example, 1, 2, 3, 4, 5, 6, and specific examples of the alkyl include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl, n-hexyl, etc.
[0059] In the present invention, the C3-C10 cycloalkyl group can be used as a substituent for the aryl group or the heteroaryl group, and specific examples include but are not limited to cyclohexyl, adamantyl, and the like.
[0060] In the present invention, the halogen group may include -F, -Cl, -Br, -I.
[0061] In the present invention, when R 11 , L, Ar 1 and Ar 2 When there is a substituent in, according to an exemplary embodiment, R 11 , L, Ar 1 and Ar 2 The substituents in are each independently selected from deuterium, halogen, -CN, C1-C6 alkyl, C3-C10 silyl, and C3-C10 cycloalkyl.
[0062] Specific examples of the substituent in L include, but are not limited to, deuterium, fluorine, -CN, methyl, ethyl, n-propyl, isopropyl, tert-butyl, trimethylsilyl, cyclohexyl, adamantyl, and the like.
[0063] In the present invention, specifically, the structures of the condensed ring compounds are shown in Formula 5 to Formula 13:
[0064]
[0065]
[0066] Optionally, R 11is selected from hydrogen, C6-C10 substituted or unsubstituted aryl, C3-C14 substituted or unsubstituted heteroaryl. The C6-C10 substituted or unsubstituted aryl may be, for example, phenyl, alkyl-substituted phenyl or halogen-substituted phenyl, and the C3-C14 substituted or unsubstituted heteroaryl may be, for example, pyridyl, quinolyl, dibenzofuranyl, dibenzothiophenyl, etc.
[0067] According to an exemplary embodiment, R 1 To R 6 can be selected from hydrogen, or R 1 To R 6 One or more than two of them are selected from C1-C6 alkyl groups.
[0068] According to one embodiment, X 1 , X 2 , X 3 Both are N.
[0069] According to another implementation, X 1 , X 2 , X 3 Two of them are N.
[0070] According to one embodiment, L is selected from a C18-C40 substituted or unsubstituted arylene group, a C15-C40 substituted or unsubstituted heteroarylene group. According to a more specific exemplary embodiment, when L is selected from a C18-C40 substituted or unsubstituted arylene group, L may include at least 3 benzene rings in its structure; when L is selected from a C15-C40 substituted or unsubstituted heteroarylene group, L may include at least 2 benzene rings in its structure.
[0071] Optionally, L is selected from the group represented by formulae 4-1 to 4-29:
[0072]
[0073]
[0074] In formulas 4-1 to 4-29, Z 1 To Z 3 Each is independently selected from hydrogen, deuterium, a halogen group (such as F), a cyano group, an alkyl group (such as a C1-C4 alkyl group), a cycloalkyl group (such as a C3-C10 alkyl group); or selected from substituted or unsubstituted aryl groups, substituted or unsubstituted heteroaryl groups, wherein the substituent is a halogen group, a cyano group, an alkyl group (such as a C1-C4 alkyl group), a cycloalkyl group (such as a C5-C10 alkyl group), preferably a deuterium, a halogen group, a cyano group, a methyl group, a tert-butyl group, a cyclohexyl group, and an adamantyl group.
[0075] When Z 1 To Z3 When selected from aryl, optionally, Z 1 To Z 3 At least one of them is fused to the connected benzene ring (ie Z 1 To Z 3 At least one of the two rings may be fused or not fused to the benzene ring to which it is connected).
[0076] Preferably, in Z 1 To Z 3 wherein the aryl group is phenyl, biphenyl, terphenyl, naphthyl, anthracenyl, fluorenyl, spiro-fluorenyl (e.g., spirobifluorenyl), 9,9-diphenylfluorenyl;
[0077] Preferably, in Z 1 To Z 3 In the above, the heteroaryl group is represented by: R-Ar 3 -L 2 -,in,
[0078] R is phenyl or hydrogen,
[0079] L 2 represents a single bond or a phenylene group;
[0080] Ar 3 Selected from pyridylene, pyrazinylene, pyrimidinylene, benzopyrimidinylene, benzothiazolylene, pyridazinylene, quinolylene, isoquinolylene, quinoxalylene, quinazolinylene, carbazolylene, triazinylene, piperazinylene, dibenzothienylene, dibenzofuranylene, thienylene, phenanthrolineylene, benzimidazolylene.
[0081] Y 3 Selected from O, S, N (R 12 ) or C(R 13 R 14 ), R 12 To R 14 are the same or different, and are independently selected from C6-C12 aryl, C1-C10 alkyl; R 12 Preferably, phenyl, R 13 and R 14 Preferred is methyl.
[0082] L 1 represents a single bond or a phenylene group.
[0083] a 3 is an integer selected from 1 to 3, a 4 is an integer selected from 1 to 4, a 5 is an integer selected from 1 to 5, a 6 is an integer selected from 1 to 6, a 8 is an integer selected from 1 to 8, and * represents a binding site connected to an adjacent atom.
[0084] Optionally, L is selected from the group shown in Formula 4-2, Formula 4-23, Formula 4-27, Formula 4-28 or Formula 4-29.
[0085] In this application, Z 1 To Z 3 At least one of Z is fused to the benzene ring to which it is connected, 1 To Z 3 At least one of them shares an edge with the connected benzene ring; for example, when Z 2 When Z is phenyl, 2 The structure formed by the benzene ring connected to it is a naphthylene group. 2 When Z is pyridyl, 2 The structure formed with the attached benzene ring may include a quinolylene group.
[0086] According to one embodiment, L is a group represented by formula 4-2:
[0087]
[0088] And in formula 4-2, L 1 Z represents phenylene, 1 and Z 2 For hydrogen, two a 3 Both are 3, Y 2 Selected from O, S, N (R 12 ) or C(R 13 R 14 ), R 12 is phenyl, R 13 and R 14 All are methyl.
[0089] According to another embodiment, L is a group shown in formula 4-23:
[0090]
[0091] In formula 4-23, Z 1 is selected from substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl; wherein the substituent is selected from deuterium, fluorine, cyano, methyl, tert-butyl, cyclohexyl or adamantyl;
[0092] Z 1 In the above, the aryl group is phenyl, biphenyl, terphenyl, naphthyl, anthracenyl, fluorenyl, spirobifluorenyl, 9,9-diphenylfluorenyl;
[0093] Z 1 In the above, the heteroaryl group is represented by: R-Ar 3 -L 2 -,in,
[0094] L 2 represents a single bond or a phenylene group;
[0095] Ar 3 is selected from the group consisting of pyridylene, pyrazinylene, pyrimidinylene, benzothiazolylene, pyridazinylene, quinolylene, isoquinolylene, quinoxalylene, quinazolinylene, carbazolylene, triazinylene, dibenzothienylene, dibenzofuranylene, thienylene, phenanthrolineylene, and benzimidazolylene;
[0096] R is phenyl or hydrogen;
[0097] Z 2 is selected from hydrogen or aryl; the aryl is phenyl or naphthyl, optionally, Z 2 Fused with the benzene ring to which it is attached;
[0098] Two A's 4 are the same or different and are each independently selected from an integer from 1 to 4.
[0099] According to another embodiment, L is selected from the group shown in Formula 4-28 or Formula 4-29:
[0100]
[0101] In formula 4-28 to formula 4-29, Z 2 is selected from hydrogen, phenyl, pyridyl, dibenzofuranyl or dibenzothienyl, a 4 An integer selected from 1 to 4. When Z 2 When selected from phenyl or pyridyl, optionally, Z 2 Fused to the benzene ring to which it is attached.
[0102] Further optionally, L is selected from the group consisting of the following groups:
[0103]
[0104] According to one embodiment, in Formula 4, Ar 1 ,Ar 2 Each is independently selected from a C6-C25 substituted or unsubstituted aryl group and a C6-C25 substituted or unsubstituted heteroaryl group. The C6-C25 substituted or unsubstituted aryl group may have, for example, 6, 12, 15, 18, 20, 24, or 25 carbon atoms. The C6-C25 substituted or unsubstituted heteroaryl group may have, for example, 6, 12, 15, 18, or 24 carbon atoms. 1 and Ar 2 Specific examples of the substituents in include, but are not limited to, deuterium, fluorine, -CN, methyl, ethyl, n-propyl, isopropyl, tert-butyl, trimethylsilyl, cyclohexyl, adamantyl, triphenylsilyl.
[0105] Optionally, Ar 1 ,Ar 2 Independently selected from the following structures:
[0106]
[0107] According to an exemplary embodiment, Ar 1 ,Ar 2 Independently selected from the group consisting of:
[0108]
[0109] Optionally, the fused ring compound may be selected from the group consisting of the following compounds:
[0110]
[0111]
[0112]
[0113]
[0114]
[0115]
[0116] In a second aspect, the present invention provides a method for preparing the condensed ring compound, comprising the following steps:
[0117] (1) under nitrogen protection, raw material Ia, xylene, raw material Ib, potassium carbonate, cuprous bromide and 18-crown ether-6 are added, and then the temperature is raised to reflux state for reaction, and after the liquid phase monitoring reaction is complete, the reaction liquid is cooled, and then the inorganic salt in the reaction is washed with water, and the liquid is separated, and the obtained organic phase is dried over anhydrous sodium sulfate, filtered, and the filtrate is concentrated to dryness and recrystallized from toluene to obtain intermediate Id;
[0118] (2) Under nitrogen protection, add intermediate Id, bipyraclostrobin, potassium acetate and 1,4-dioxane, add [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride at 30-80°C, continue heating to reflux state to react for 3-9 hours, cool the reaction solution, pour water and toluene into the solution under stirring, extract the solution after standing, separate the solution, extract the aqueous phase with toluene once more, separate the solution, combine the organic phases, add anhydrous sodium sulfate into the organic phases, stir and dry, and obtain intermediate Ie;
[0119] (3) Under nitrogen protection, toluene, raw material Ic, intermediate Ie, potassium carbonate, tetrabutylammonium bromide, ethanol and water are added, tetrakistriphenylphosphine palladium is added at 30-100° C., and the mixture is heated to reflux state for reaction until the reaction is complete as monitored by liquid phase. The reaction solution is cooled, poured into water with stirring, and allowed to stand for separation. The aqueous phase is extracted with toluene, the organic phases are combined, dried with anhydrous sodium sulfate and filtered, the filtrate is concentrated until no solvent is distilled off, and then recrystallized with toluene to obtain the condensed ring compound.
[0120] In step (1), the molar ratio of raw material Ia to raw material Ib can be 1:(1-1.3); the molar ratio of raw material Ia to potassium carbonate, cuprous bromide, and 18-crown ether-6 can be 1:(4-5):(0.2-0.4):(0.1-0.3).
[0121] In step (2), the molar ratio of the intermediate Id, pinacol diboron, potassium acetate and [1,1'-bis[(diphenylphosphino)ferrocene]palladium dichloride can be 1:(1.2-1.5):(5-8):(0.01-0.05).
[0122] In step (3), the molar ratio of the raw material Ic, the intermediate Ie, potassium carbonate, tetrabutylammonium bromide and tetrakistriphenylphosphine palladium can be 0.4:(0.4-0.6):(4-8):(0.05-0.1):(0.25-0.4).
[0123] In each step, heating to reflux means that the heating temperature of the heating device (e.g., heating jacket) used in the reaction is greater than the boiling point of the solvent, for example, the heating temperature can be 5-10° C. higher than the boiling point. The raw materials of the present invention can be obtained commercially or synthesized by methods well known in the art.
[0124] According to a specific embodiment, the method for preparing the condensed ring compound comprises:
[0125] (1) Under nitrogen protection, raw material Ia and xylene are added to a three-necked flask in sequence, and then raw material Ib, potassium carbonate, cuprous bromide, and 18-crown ether-6 are added. After the addition is completed, the reaction mixture is heated to reflux by an electric heating mantle. After the reaction is complete, the reaction solution is cooled to room temperature (15-30° C.), and then the inorganic salt in the reaction is washed with water. The organic phase is separated and dried over anhydrous sodium sulfate, filtered, and the filtrate is concentrated to dryness and recrystallized from toluene to obtain intermediate Id.
[0126]
[0127] (2) Nitrogen was passed into a three-necked glass bottle equipped with a mechanical stirrer, a thermometer, and a condenser, and intermediate Id, bipyraclostrobin, potassium acetate, and 1,4-dioxane were added in sequence. Stirring was started, the temperature was raised to 30-80°C, and [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride was quickly added, and the mixture was heated to reflux for 3-9 hours. The reaction solution was quickly cooled to room temperature, and water and toluene were poured into the mixture for extraction under stirring. The mixture was allowed to stand for 30 minutes, and the liquid phase was separated. The aqueous phase was extracted with toluene again, and the liquid phase was separated and the organic phase was combined. Anhydrous sodium sulfate was added to the organic phase and stirred for 5 minutes, dried for 0.5 hours, filtered, and concentrated until no solvent was distilled off to obtain intermediate Ie.
[0128]
[0129] (3) A three-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and toluene, raw material Ic, intermediate Ie, potassium carbonate, tetrabutylammonium bromide, ethanol, and water were added in sequence. Stirring was started, the temperature was raised to 30-100°C, tetrakistriphenylphosphine palladium was quickly added, and the reaction was continued to be heated to reflux state until the reaction was complete as monitored by the liquid phase. The reaction solution was quickly cooled to room temperature, poured into water under stirring, and allowed to stand for 30 minutes. The liquids were separated, the aqueous phase was extracted with toluene again, the organic phases were combined, dried with anhydrous sodium sulfate for 0.5 hours, filtered, and the filtrate was concentrated (65-70°C; -0.08--0.09MPa, about 8 hours), concentrated until no solvent was distilled off, and recrystallized from toluene to obtain compound I.
[0130]
[0131] The above specific implementation method obtains the condensed ring compound shown in Formula 1. The synthetic routes of the condensed ring compounds shown in Formula 2 and Formula 3 are the same as Formula 1, except that the raw material Ia and the corresponding intermediates Id and Ie are shown in Table 1.
[0132] Table 1
[0133]
[0134]
[0135] In a third aspect, the present invention provides an organic electroluminescent device, comprising an anode, a cathode, and an organic layer deposited between the anode and the cathode, wherein the organic layer comprises a hole transport layer, an electron blocking layer, a light-emitting layer and an electron transport layer, wherein the electron transport layer or the light-emitting layer contains the condensed ring compound.
[0136] According to one embodiment, the host material of the light-emitting layer includes the condensed ring compound.
[0137] According to another embodiment, the electron transport layer comprises the condensed ring compound.
[0138] like Figure 1 As shown, the organic electroluminescent device includes an anode 100 and a cathode 200 disposed opposite to each other, and a functional layer 300 (ie, an organic layer) disposed between the anode 100 and the cathode 200 .
[0139] Specifically, the organic electroluminescent device includes an anode 100, a hole transport layer 320, an organic electroluminescent layer 330 (ie, a light-emitting layer), an electron transport layer 350, and a cathode 200, which are sequentially stacked. The hole transport layer 320 may include one or two layers.
[0140] Optionally, an electron injection layer 360 is further disposed between the cathode 200 and the electron transport layer 350 .
[0141] Optionally, a hole blocking layer 340 is further disposed between the organic electroluminescent layer 330 and the electron transport layer 350 .
[0142] Optionally, an electron blocking layer 370 may be further provided between the organic electroluminescent layer 330 and the hole transport layer 320 .
[0143] Optionally, the hole transport layer 320 may be composed of a first hole transport layer 321 and a second hole transport layer 322 , and the first hole transport layer 321 is relatively close to the anode.
[0144] According to one embodiment, the electron transport layer 350 comprises a condensed ring compound provided by the present invention. The material forming the electron transport layer 350 may be composed of the condensed ring compound or may be composed of the condensed ring compound and other materials. Thus, the condensed ring compound is applied to the electron transport layer 350 of the organic electroluminescent device, which can effectively improve the electronic properties of the organic electroluminescent device.
[0145] According to another embodiment, the light-emitting layer comprises the condensed ring compound provided by the present invention. The light-emitting layer can be composed of the condensed ring compound provided by the present invention, or can be composed of the condensed ring compound provided by the present invention and other materials. Thus, the condensed ring compound provided by the present invention is applied to the light-emitting layer of the organic electroluminescent device, which can effectively improve the light-emitting properties of the organic electroluminescent device.
[0146] In the present invention, the anode 100 includes an anode material, which can be selected with reference to the prior art, and is preferably selected from a material with a large work function that facilitates hole injection into the functional layer. Specific examples of the anode material include, but are not limited to: metals such as nickel, platinum, vanadium, chromium, copper, zinc and gold or their alloys; metal oxides such as zinc oxide, indium oxide, indium tin oxide (ITO) and indium zinc oxide (IZO); combined metals and oxides such as ZnO:Al or SnO 2 : Sb; or a conductive polymer such as poly (3-methylthiophene), poly [3,4- (ethylene-1,2-dioxy) thiophene] (PEDT), polypyrrole and polyaniline. More preferably, a transparent electrode comprising indium tin oxide (indium tin oxide, indium tin oxide) (ITO) as an anode.
[0147] In the present invention, the cathode 200 includes a cathode material, which can be selected with reference to the prior art, and is a material with a small work function that facilitates electron injection into the functional layer. Specific examples of cathode materials include, but are not limited to, metals such as magnesium, calcium, sodium, potassium, titanium, indium, yttrium, lithium, gadolinium, aluminum, silver, tin and lead or alloys thereof; or multilayer materials such as LiF / Al, Liq / Al, LiO 2 / Al, LiF / Ca, LiF / Al and BaF 2 / Ca.
[0148] In a fourth aspect, the present invention provides an electronic device, comprising the organic electroluminescent device according to the third aspect. The electronic device may be any electronic device comprising the organic electroluminescent device, such as a mobile phone (e.g. Figure 2 As shown), computers, etc. The organic electroluminescent device can be applied to the screen of the electronic device.
[0149] The present invention will be further described below in conjunction with the embodiments.
[0150] The following examples are used to illustrate the fused ring compounds and the preparation methods thereof of the present invention.
[0151] In order to facilitate the understanding of the present invention, the numbers of the following raw materials, intermediates and prepared compounds correspond, for example, "raw material 1a", "raw material 1b", "raw material 1c" refer to the raw material Ia, raw material Ib, and raw material Ic specifically selected when preparing compound 1; "raw material 5a", "raw material 5b", "intermediate 5d", "raw material 5c", and "intermediate 5d" refer to the raw material Ia, raw material Ib, intermediate Id, raw material Ic, and intermediate Id specifically selected when preparing compound 5. In addition, the present invention also describes the preparation method of some raw materials Ib, wherein the compounds involved in the preparation of raw material Ib are represented in the form of Ib-number number, for example, 5b-1 and 5b-2 refer to two compounds used in the preparation of raw material 5b.
[0152] Preparation Example
[0153] The preparation examples are used to illustrate the synthesis of starting material Ib.
[0154] 1. Synthesis of raw material 5b (1)
[0156]
[0157] Under nitrogen protection, compound 5b-1 (50 mmol) and compound 5b-2 (55 mmol) and 460.0 ml of acetic acid were added to a three-necked reaction bottle equipped with a mechanical stirrer, a thermometer, and a condenser. The temperature was raised to 80-90°C, and concentrated sulfuric acid (1 mmol) was added dropwise. The reaction was kept warm for 4 hours. 600.0 ml of water was added, the temperature was lowered to 25°C, and a large amount of solid was precipitated by stirring. The solid was filtered and the filter cake was rinsed with ethanol to obtain compound 5b-3 (25 mmol) with a yield of 50%. (2)
[0159]
[0160] A three-necked flask equipped with a mechanical stirrer, a thermometer, and a constant pressure adding funnel was passed with nitrogen (0.100 L / min) for 15 min, compound 5b-3 (25 mmol) and 100 ml of tetrahydrofuran were added, stirring was started, the liquid nitrogen was cooled to -80°C to -90°C, 2 mol / L n-butyllithium (26 mmol) was added dropwise, and the mixture was kept warm for 1 h. Tributyl borate (29 mmol) was added dropwise, and the mixture was kept warm for 1 h. 200.0 ml of water, 40.0 ml of petroleum ether, and 5 ml of concentrated hydrochloric acid were added to the reaction solution. The mixture was stirred thoroughly and then separated. The organic phase was washed with water 4 times, the crude product was filtered, and then slurried with 50.0 mL of toluene for 0.5 h, filtered, and washed with toluene to obtain compound 5b-4 (20 mmol) with a yield of 80%. (3)
[0162]
[0163] A three-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser was purged with nitrogen, and 100.0 mL of toluene, compound 5b-4 (20 mmol), raw material 3-chloro-5-bromoiodobenzene (i.e., compound 5b-5, 21 mmol), potassium carbonate (40 mmol), 20 mL of ethanol, and 20 mL of water were added in sequence. Stirring was started, the temperature was raised to 55°C, tetrakistriphenylphosphine palladium (0.2 mmol) was quickly added, and the mixture was heated to reflux for 6 h. The mixture was poured into 100 mL of water under stirring, allowed to stand, and separated. The aqueous phase was extracted with 50 mL of toluene, the organic phases were combined, dried with 10 g of anhydrous sodium sulfate, filtered, and the filtrate was concentrated (70°C, -0.09 MPa), concentrated until no solvent was distilled off, 50 mL of n-heptane was added, and filtered to obtain compound 5b-6 (17.4 mmol), with a yield of 87%. (4)
[0165]
[0166] A three-necked flask equipped with a mechanical stirrer, a thermometer, and a constant pressure dropping funnel was replaced with nitrogen (0.100 L / min) for 15 min, compound 5b-6 (15 mmol) and 80.5 ml of tetrahydrofuran were added, stirring was started, the liquid nitrogen was cooled to -80°C to -90°C, 2 mol / L n-butyllithium (17 mmol) was added dropwise, and the mixture was kept warm for 1 h. Tributyl borate (19 mmol) was added dropwise, and the mixture was kept warm for 1 h. 100.0 mL of water, 20.0 ml of petroleum ether, and 3 mL of concentrated hydrochloric acid were added to the reaction solution. After sufficient stirring, the liquids were separated, and the organic phase was washed with water 4 times. The crude product was filtered, and then slurried with 25.0 mL of toluene for 0.5 h, filtered, and washed with toluene to obtain intermediate 5b-7 (12.75 mmol) with a yield of 85%. (5)
[0168]
[0169] A three-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser was purged with nitrogen, and 70.0 mL of toluene, compound 5b-7 (12 mmol), compound 5b-8 (14 mmol), potassium carbonate (25 mmol), 15 mL of ethanol, and 15 mL of water were added in sequence. Stirring was started, the temperature was raised to 50°C, tetrakistriphenylphosphine palladium (0.1 mmol) was quickly added, and the mixture was heated to reflux for 8 h. The mixture was poured into 90 mL of water under stirring, and allowed to stand for 30 min. The aqueous phase was then separated, and the aqueous phase was extracted with 35 mL of toluene. The organic phases were combined, dried with 5 g of anhydrous sodium sulfate for 0.5 h, filtered, and the filtrate was concentrated (70°C, -0.09 MPa, about 8 h), concentrated until no solvent was distilled off, 50 ml of ethanol was added, and filtered to obtain raw material 5b (8.64 mmol) with a yield of 72%.
[0170] 2. Synthesis of raw materials 1b, 4b, 6b, 12b, 15b, 18b, 21b, 30b, 44b, 48b, 56b, 58b, 70b, 90b and 93b
[0171] The above raw materials were synthesized according to steps (2) to (5) of raw material 5b, except that compound Ib-3 and part of compound Ib-5 were replaced. The main raw materials used and the corresponding prepared compounds are shown in the following table:
[0172]
[0173]
[0174]
[0175] 2. Synthesis of raw materials 7b and 85b
[0176] Raw materials 7b and 85b were synthesized respectively by referring to the method of raw material 5b, except that compound Ib-2 was replaced. The main raw materials used and the corresponding prepared compounds are shown in the following table:
[0177]
[0178] 3. Synthesis of raw materials 38b and 81b
[0179] Referring to step (4) and step (5) of the method for raw material 5b, raw materials 38b and 81b were synthesized respectively, except that compounds 5b-6 and 5b-8 were replaced. The main raw materials used and the corresponding prepared compounds are shown in the following table:
[0180]
[0181] Example 1: Compound 1 and its synthesis method
[0182] The steps include:
[0183] (1) Under nitrogen protection, 1 mmol of raw material 1a, 40 mL of xylene, 1.3 mmol of raw material 1b, 4 mmol of potassium carbonate, 0.2 mmol of cuprous bromide, and 0.1 mmol of 18-crown ether-6 were added to a three-necked flask in sequence with stirring. After the addition was completed, the electric heating mantle was heated to reflux state for reaction until the liquid phase monitoring showed that the reaction was complete. The reaction liquid was cooled to room temperature, and then the inorganic salt in the reaction was washed with water, and the liquid was separated. The obtained organic phase was dried over anhydrous sodium sulfate and filtered. The filtrate was concentrated to dryness and recrystallized from toluene to obtain intermediate 1d.
[0184]
[0185] (2) A three-necked glass bottle equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and 1 mmol of intermediate 1d, 1.5 mmol of pinacol diboron, 5 mmol of potassium acetate, and 40 mL of 1,4-dioxane were added in sequence. Stirring was started, the temperature was raised to 40°C, and 0.01 mmol of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride was quickly added. The mixture was heated to reflux and kept warm for 3 hours. The reaction solution was quickly cooled to 20°C, and 50 mL of water and 50 mL of toluene were poured into the mixture for extraction while stirring. The mixture was allowed to stand for 30 minutes, and the liquid phase was separated. The aqueous phase was extracted once with 50 mL of toluene, and the liquid phase was separated and the organic phase was combined. 10 g of anhydrous sodium sulfate was added to the organic phase and stirred for 5 minutes. The mixture was dried for 0.5 hours, filtered, and concentrated until no solvent was evaporated to obtain intermediate 1e.
[0186]
[0187] (3) A three-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and 50 mL of toluene, 0.4 mmol of raw material 1c, 0.5 mmol of intermediate 1e, 5 mmol of potassium carbonate, 0.05 mmol of tetrabutylammonium bromide, 10 mL of ethanol, and 5 mL of water were added in sequence. Stirring was started, the temperature was raised to 50°C, 0.25 mmol of tetrakistriphenylphosphine palladium was added, and the mixture was heated to reflux and kept warm for reaction until the reaction was complete after liquid phase monitoring. The reaction solution was cooled to 20°C, poured into 100 mL of water with stirring, and allowed to stand for 30 min. The liquid was separated, and the aqueous phase was extracted with 50 mL of toluene. The organic phases were combined, dried with 10 g of anhydrous sodium sulfate for 0.5 h, filtered, and the filtrate was concentrated (70°C; -0.08 MPa, about 8 h) until no solvent was distilled off. Recrystallization was performed with 20 mL of toluene to obtain 0.23 g of compound 1 (0.3 mmol, yield 75%), m / z = 769.3 [M+H] + .
[0188]
[0189] Calculated value of element content (%) of compound 1 C 55 H 36 N 4 O, C: 85.91; H: 4.72; N: 7.29; O: 2.08; Found C 55 H 36 N 4 O: C: 85.88; H: 4.74; N: 7.31; O: 2.07. NMR data of compound 1: 1 H NMR (CDCl 3, 300MHz): δ (ppm) = 8.75-8.70 (d, 2H), δ (ppm) = 8.31-8.28 (s, 3H), δ (ppm) = 8.19-8.15 (d, 2H), δ (ppm) = 8.09-8.01 (m, 6H), δ(ppm)=7.82-7.25(m,17H), δ(ppm)=7.20-7.17(d,1H), δ(ppm)=7.13-7.09(m,3H), δ(ppm)=7.05-7.01(s,2H).
[0190] Example 2: Compound 15 and its synthesis method
[0191] The steps include:
[0192] (1) Under nitrogen protection, 1 mmol of raw material 15a, 50 mL of xylene, 1.2 mmol of raw material 15b, 4 mmol of potassium carbonate, 0.3 mmol of cuprous bromide, and 0.2 mmol of 18-crown ether-6 were added to a three-necked flask in sequence. After the addition was completed, the reaction system was heated to reflux for reaction until the reaction was complete as monitored by liquid phase. The reaction solution was then cooled to room temperature, and then the inorganic salts in the reaction were washed with water, and the liquid was separated. The obtained organic phase was dried over anhydrous sodium sulfate and filtered. The filtrate was concentrated to dryness and recrystallized from toluene to obtain intermediate 15d.
[0193]
[0194] (2) A three-necked glass bottle equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and 1 mmol of intermediate 15d, 1.2 mmol of biphenylphosphinoyl ferrocene, 5 mmol of potassium acetate, and 40 mL of 1,4-dioxane were added in sequence. Stirring was started, the temperature was raised to 80°C, 0.02 mmol of 1,1'-[bis(diphenylphosphino)ferrocene]palladium dichloride was added, and the temperature was continued to be raised to reflux state for reaction for 6 hours. The reaction solution was quickly cooled to 20°C, and 50 mL of water and 50 mL of toluene were poured into it for extraction while stirring. The mixture was allowed to stand for 30 minutes, and the liquid phase was separated. The aqueous phase was extracted once with 50 mL of toluene, and the liquid phase was separated and the organic phase was combined. 10 g of anhydrous sodium sulfate was added to the organic phase, and the mixture was stirred for 5 minutes, dried for 0.5 hours, filtered, and concentrated until no solvent was distilled off to obtain intermediate 15e.
[0195]
[0196] (3) A three-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and 50 mL of toluene, 0.4 mmol of the raw material 4c, 0.5 mmol of the intermediate 15e, 5 mmol of potassium carbonate, 0.05 mmol of tetrabutylammonium bromide, 10 mL of ethanol, and 5 mL of water were added in sequence. Stirring was started, the temperature was raised to 100°C, 0.25 mmol of tetrakistriphenylphosphine palladium was added, and the temperature was continued to be raised to reflux state for reaction until the reaction was complete after liquid phase monitoring. After the reaction was complete, the reaction liquid was cooled to 20°C, poured into 100 mL of water with stirring, and allowed to stand for 30 min. The liquid was separated, and the aqueous phase was extracted with 50 mL of toluene again. The organic phases were combined, dried with 10 g of anhydrous sodium sulfate for 0.5 h, filtered, and the filtrate was concentrated (65°C; -0.082 MPa, about 8 h) until no solvent was evaporated. Recrystallization with 20 mL of toluene gave 0.31 g of compound 15 (0.34 mmol, yield 68%), m / z = 909.3 [M+H] + .
[0197]
[0198] Calculated value of element content (%) of compound 15 C 65 H 40 N 4 S: C: 85.88; H: 4.44; N: 6.16; S: 3.53; Measured value: C 65 H 40 N 4 S: C: 85.3; H: 4.42; N: 6.17; S: 4.11.
[0199] Example 3: Compound 30 and its synthesis method
[0200] The steps include:
[0201] (1) Under nitrogen protection, 1 mmol of raw material 30a, 50 mL of xylene, 1.1 mmol of raw material 30b, 4 mmol of potassium carbonate, 0.3 mmol of cuprous bromide, and 0.1 mmol of 18-crown ether-6 were added to a three-necked flask in sequence with stirring. After the addition was completed, the reaction system was heated to reflux for reaction until the reaction was complete as monitored by liquid phase. The reaction solution was cooled to room temperature, and then the inorganic salt in the reaction was washed with water. The organic phase was separated and dried over anhydrous sodium sulfate and filtered. The filtrate was concentrated to dryness and recrystallized from toluene to obtain intermediate 30d.
[0202]
[0203] (2) A three-necked glass bottle equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and 1 mmol of intermediate 30d, 1.4 mmol of biphenylphosphinoyl ferrocene, 6 mmol of potassium acetate, and 40 mL of 1,4-dioxane were added in sequence. Stirring was started, the temperature was raised to 80°C, 0.01 mmol of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride was added, and the mixture was heated to reflux for 6 hours. The reaction solution was cooled to 20°C, 50 mL of water and 50 mL of toluene were poured into the mixture for extraction while stirring, and the mixture was allowed to stand for 30 minutes. The mixture was separated, and the aqueous phase was extracted once with 50 mL of toluene. The mixture was separated, and the organic phases were combined. 10 g of anhydrous sodium sulfate was added to the organic phase, and the mixture was stirred for 5 minutes. The mixture was dried for 0.5 hours, filtered, and concentrated until no solvent was distilled off to obtain intermediate 30e.
[0204]
[0205] (3) A three-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser was passed with nitrogen, and 50 mL of toluene, 0.4 mmol of the raw material 30c, 0.5 mmol of the intermediate 30e, 5 mmol of potassium carbonate, 0.05 mmol of tetrabutylammonium bromide, 10 mL of ethanol, and 5 mL of water were added in sequence. Stirring was started, the temperature was raised to 100°C, 0.25 mmol of tetrakistriphenylphosphine palladium was added, and the reaction was continued to be heated to reflux state until the reaction was complete after liquid phase monitoring. The reaction liquid was quickly cooled to 20°C, poured into 100 mL of water under stirring, and allowed to stand for 30 min. The liquid was separated, and the aqueous phase was extracted with 50 mL of toluene again. The organic phases were combined, dried with 10 g of anhydrous sodium sulfate for 0.5 h, filtered, and the filtrate was concentrated (67°C; -0.084 MPa, about 8 h) until no solvent was evaporated. Recrystallization with 20 mL of toluene gave 0.4 g of compound 30 (0.33 mmol, yield 66%), m / z = 1198.5 [M+H] + .
[0206]
[0207] Embodiment 4-11
[0208] Compound 4, Compound 5, Compound 6, Compound 7, Compound 12, Compound 38, Compound 58, and Compound 81 were synthesized according to the method of Example 1, except that Raw Material 1a, Raw Material 1b, and Raw Material 1c in Example 1 were replaced by corresponding raw materials, respectively. The raw materials used, the corresponding prepared compounds, and mass spectrometry data are specifically shown in Table 2.
[0209] Examples 12-17
[0210] Compound 18, Compound 21, Compound 56, Compound 70, Compound 90, and Compound 93 were synthesized according to the method of Example 2, except that Raw Material 1a, Raw Material 1b, and Raw Material 1c in Example 1 were replaced by corresponding raw materials, respectively. The raw materials used, the corresponding prepared compounds, and mass spectrometry data are specifically shown in Table 2.
[0211] Examples 18-20
[0212] Compound 44, Compound 48 and Compound 85 were synthesized according to the method of Example 3, except that Raw Material 1a, Raw Material 1b and Raw Material 1c in Example 1 were replaced by corresponding raw materials, respectively. The raw materials used, the corresponding prepared compounds and mass spectrum data are specifically shown in Table 2.
[0213] Table 2
[0214]
[0215]
[0216]
[0217] NMR data of compound 48, 1 H NMR (CDCl 3 , 300MHz): δ (ppm) = 8.69-8.64 (m, 4H), δ (ppm) = 8.59-8.56 (s, 1H), δ (ppm) = 8.53-8.48 (m, 4H), δ (ppm) = 8.39-8.34 (m, 4H), δ (ppm) = 8.25-8.19 (m) , 6H), δ (ppm) = 8.13-8.07 (m, 8H), δ (ppm) = 8.02-7.96 (m, 9H), δ (ppm) = 7.90-7.86 (m, 3H), δ (ppm) = 7.82-7.78 (m, 5H), δ (ppm) = 7.71-7.66 (m, 3H).
[0218] The following application examples 1 to 10 are used to illustrate the application of the condensed ring compound of the present invention in the electron transport layer of an organic electroluminescent device.
[0219] Application Example 1
[0220] A method for manufacturing an organic light-emitting device comprises the following steps:
[0221] (1) First, ultrasonically clean the Glass substrate with indium tin oxide (ITO) electrode, dry;
[0222] (2) Cleaning with oxygen plasma for 5 minutes, and then loading the cleaned anode bottom plate into the vacuum deposition equipment;
[0223] (3) Vacuum depositing the compound 2-TNATA (structure as shown in formula A) onto the ITO electrode to form A hole injection layer HIL having a thickness of 100 mm is formed, and NPB (N,N'-diphenyl-N,N'-di(1-naphthyl)-1,1'-biphenyl-4,4'-diamine) is vacuum deposited on the hole injection layer to form a A hole transport layer HTL having a thickness of 1000 mm is formed by evaporating TCTA (the structure of which is shown in Formula B) on the hole transport layer to form a Then, the main luminescent material BPO (structure shown in formula C) and the dopant EM (structure shown in formula D) are co-deposited onto the hole transport region at a mass ratio of 96:4 to form an electron blocking layer EBL. Thickness of the light emitting layer EML;
[0224] (4) DPVBi (structure as shown in Formula E) is vacuum deposited on the light-emitting layer to form Thickness of hole blocking layer;
[0225] (5) Compound 1 is vacuum deposited on the hole blocking layer to form The electron transport layer is formed by evaporating LiQ (8-hydroxyquinoline-lithium) on the electron transport layer. Then, magnesium (Mg) and silver (Ag) are mixed at a deposition rate of 1:9 and vacuum-deposited on the electron injection layer to form an electron injection layer EIL. Thickness of cathode.
[0226] In addition, a layer with a thickness of CP-1 (structure as shown in Formula F) is prepared to form a covering layer (CPL), thereby completing the manufacture of the organic light-emitting device. The prepared organic light-emitting device is recorded as A1.
[0227]
[0228] Comparative Example 1
[0229] The organic electroluminescent device was manufactured by the same method as in Application Example 1, except that the compound 1 as the electron transport layer was replaced by the compound A (Alq 3 ) is substituted to obtain an organic electroluminescent device D1. 3 The structure is as follows:
[0230]
[0231] Comparative Example 2
[0232] The organic electroluminescent device D2 was prepared by the same method as in Application Example 1, except that the compound 1 used as the electron transport layer was replaced by the compound B. The structural formula of the compound B is shown below:
[0233]
[0234] Application Example 2-Application Example 10
[0235] Organic electroluminescent devices were manufactured by the same method as in Application Example 1, except that in Application Examples 2-10, compound 1 as an electron transport layer was replaced by the compounds listed in Table 3, thereby preparing organic electroluminescent devices A2 to A10.
[0236] For the organic electroluminescent devices A1 to A10 and D1 and D2 prepared as above, the data voltage, efficiency and color coordinates are obtained at a constant current density of 10 mA / cm 2 The device life of T95 is tested at a constant current density of 15mA / cm 2 The electronic luminescence characteristics were tested and analyzed, and the results are shown in Table 3.
[0237] Table 3 List of electronic luminescence characteristics of organic electroluminescent devices
[0238]
[0239] The above results show that the fused ring compound of the present invention as an electron transport material is used in combination with Alq 3 Compared with Comparative Examples 1 and 2 of compound B, the driving voltages of the organic electroluminescent devices A1 to A10 prepared in Application Examples 1 to 10 are between 3.81 and 4.23 V, which are about 10% to 19% and -0.4% to 9% lower than the driving voltages of the organic electroluminescent devices D1 and D2 in Comparative Examples 1 and 2, respectively; the luminous efficiency of the organic electroluminescent devices A1 to A10 is between 5.8 and 6.8 Cd / A, which is about 10% to 19% lower than the driving voltages of the organic electroluminescent devices D1 and D2 in Comparative Examples 1 and 2, respectively; The luminous efficiency of the optical devices D1 and D2 is increased by about 41% to 65% and 20% to 41% respectively; the external quantum efficiency of A1 to A10 is between 11.4% and 13.4%, which is 34% to 57% and 20% to 41% higher than that of D1 and D2 respectively; the T95 life of the organic electroluminescent devices A1 to A10 is between 130 and 160 hours, which is about 27% to 56% and 2% to 26% higher than that of the devices D1 and D2 respectively.
[0240] Therefore, compared with the devices in the comparative examples, the organic electroluminescent devices A1 to A10 prepared in application examples 1 to 10 have lower driving voltage, higher luminous efficiency, higher external quantum efficiency and brightness. That is, compared with the comparative examples, the condensed ring compound of the present invention has better luminous efficiency, better electrical stability and longer life, and can significantly improve the performance of the organic electroluminescent device when used in the electron transport layer of the organic electroluminescent device.
[0241] The following application examples 11 to 20 are used to illustrate the application of the condensed ring compound of the present invention in the light-emitting layer of an organic electroluminescent device.
[0242] Application Example 11
[0243] A method for manufacturing an organic electroluminescent device comprises the following steps:
[0244] (1) First, ultrasonically clean the A glass substrate with an indium tin oxide (ITO) electrode of 1000 mm thick, dried;
[0245] (2) Cleaning with oxygen plasma for 5 minutes, and then loading the cleaned anode bottom plate into the vacuum deposition equipment;
[0246] (3) Compound 2-TNATA is vacuum deposited onto the ITO electrode to form The hole injection layer HIL is formed by vacuum deposition of NPB on the hole injection layer. Thickness of the hole transport layer HTL, TCTA is evaporated on the hole transport layer to form Then, the host light emitting material compound 5 and the dopant EM are co-deposited onto the hole transport region at a mass ratio of 96:4 to form an electron blocking layer EBL. Thickness of the light emitting layer EML;
[0247] (4) DPVBi is vacuum deposited on the light-emitting layer to form Thickness of hole blocking layer;
[0248] (5) Alq3 is vacuum deposited on the hole blocking layer to form The electron transport layer is formed by evaporating LiQ on the electron transport layer. Then, magnesium (Mg) and silver (Ag) are mixed at a deposition rate of 1:9 and vacuum-deposited on the electron injection layer to form an electron injection layer EIL. Thickness of cathode.
[0249] In addition, a layer with a thickness of The CP-1 is formed into a capping layer (CPL), thereby completing the manufacture of an organic light-emitting device. The manufactured organic electroluminescent device is denoted as B1.
[0250] Comparative Example 3
[0251] The organic electroluminescent device was manufactured by the same method as in Application Example 11, except that the compound 5 as the main luminescent material was replaced by the compound C, thereby obtaining the organic electroluminescent device D3. The structural formula of the compound C is shown below:
[0252]
[0253] Application Example 12-Application Example 20
[0254] The organic electroluminescent device was manufactured by the same method as in Application Example 11, except that the compound 5 as the luminescent host material was replaced by the compounds listed in Table 4, thereby preparing organic electroluminescent devices B2 to B10.
[0255] For the electroluminescent devices B1 to B10 prepared as above, the data voltage, efficiency, and color coordinates are obtained at a constant current density of 10 mA / cm 2 The device life of T95 is tested at a constant current density of 15mA / cm 2 The electronic luminescence characteristics were tested and analyzed, and the results are shown in Table 4. In addition, for comparison purposes, Table 4 also shows the electronic luminescence characteristics of the organic light-emitting device of Comparative Example 1 (the difference between Comparative Example 1 and Application Examples 11 to 20 is that the luminescent host material is BPO).
[0256] Table 4
[0257]
[0258]
[0259] According to the above results, the condensed ring compound of the present invention as the light-emitting host material is compared with Comparative Examples 1 and 3 using BPO and Compound C:
[0260] The driving voltage of the organic electroluminescent devices B1 to B10 prepared in Application Examples 11 to 20 is between 3.81 and 4.13 V, which is 13% to 19% lower and 5% to 12% lower than the driving voltage of the organic electroluminescent devices D1 and D3 in Comparative Examples 1 and 3, respectively. The luminous efficiency of the organic electroluminescent devices B1 to B10 is between 5.5 and 6.8 Cd / A, which is 34% to 65% higher and 19% to 47% higher than the luminous efficiency of the devices D1 and D3 in Comparative Examples 1 and 3, respectively. The external quantum efficiency of B1 to B10 is between 11.2% and 12.8%, which is 31% to 50% and 9% to 25% higher than that of devices D1 and D3, respectively; the T95 life of devices B1 to B10 prepared in application examples 11 to 20 is 151 to 188h, which is 48% to 84% and 23% to 54% higher than that of devices D1 and D3, respectively.
[0261] Therefore, compared with Comparative Example 1 and Comparative Example 3, the organic electroluminescent devices prepared in Application Examples 11 to 20 have lower driving voltage, higher luminous efficiency, higher external quantum efficiency and brightness. That is, compared with Comparative Example 1 and Comparative Example 3, the condensed ring compound provided by the present invention has better luminous efficiency, better electrical stability and longer life, and can significantly improve the performance of the organic electroluminescent device when used in the light-emitting layer of the organic electroluminescent device.
[0262] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the essence and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A condensed ring compound, It is characterized in that The condensed ring compound is represented by the following formula 3: In formula 3, R 1 To R 6 The same or different, each independently selected from hydrogen or C1-C6 alkyl; Y 1 Selected from O, S or N (R 11 ), R 11 Selected from benzene rings; Y 2 is N; A1 is a benzene ring; M is a group represented by formula 4: In formula 4, X 1 , X 2 , X 3 At least 2 of them are N, and the rest are N or CH; L is selected from the group represented by formula 4-1, formula 4-2, formula 4-22, formula 4-23, and formula 4-24: In Formula 4-1, Formula 4-2, Formula 4-22, Formula 4-23, and Formula 4-24, Z 1 To Z 2 Each is independently selected from hydrogen, deuterium; or selected from substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl, wherein the substituent is deuterium, a halogen group, a cyano group, a methyl group, a tert-butyl group, a cyclohexyl group, an adamantyl group; Z 1 To Z 2 In the above, the aryl group is phenyl, biphenyl, naphthyl, fluorenyl, spiro-fluorenyl, 9,9-diphenylfluorenyl; Z 1 To Z 2 In the above, the heteroaryl group is: R-Ar 3 -L 2 -,in, R is phenyl or hydrogen, L 2 Represents a single bond or phenylene, Ar 3 Selected from carbazolyl, triazinyl, dibenzothienyl, dibenzofuranyl; Y 3 Selected from C(R 13 R 14 ), R 13 and R 14 All are methyl; L 1 represents phenylene; a 3 is an integer selected from 1 to 3, a 4 is an integer selected from 1 to 4, and * represents a binding site connected to an adjacent atom; Ar 1 and Ar 2 The same or different, each independently selected from the group consisting of:
2. The fused ring compound according to claim 1, It is characterized in that The condensed ring compound is selected from the group consisting of the following compounds:
3. A method for preparing a condensed ring compound according to any one of claims 1 or 2, It is characterized in that The following steps are involved: (1) under nitrogen protection, raw material Ia, xylene, raw material Ib, potassium carbonate, cuprous bromide and 18-crown ether-6 are added, and then the temperature is raised to reflux state for reaction, and after the liquid phase monitoring reaction is complete, the reaction liquid is cooled, and then the inorganic salt in the reaction is washed with water, and the liquid is separated, and the obtained organic phase is dried over anhydrous sodium sulfate, filtered, and the filtrate is concentrated to dryness and recrystallized from toluene to obtain intermediate Id; (2) Under nitrogen protection, add intermediate Id, bipyraclostrobin, potassium acetate and 1,4-dioxane, add [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride at 30-80°C, continue heating to reflux state to react for 3-9 hours, cool the reaction solution, pour water and toluene into the solution under stirring, extract the solution after standing, separate the solution, extract the aqueous phase with toluene once more, separate the solution, combine the organic phases, add anhydrous sodium sulfate into the organic phases, stir and dry, and obtain intermediate Ie; (3) under nitrogen protection, toluene, raw material Ic, intermediate Ie, potassium carbonate, tetrabutylammonium bromide, ethanol and water are added, tetrakistriphenylphosphine palladium is added at 30-100°C, and the reaction is continued to be heated to reflux state until the reaction is complete after liquid phase monitoring, the reaction solution is cooled, poured into water with stirring, and allowed to stand for separation, the aqueous phase is extracted with toluene, the organic phases are combined, dried with anhydrous sodium sulfate and filtered, the filtrate is concentrated until no solvent is distilled off, and then recrystallized with toluene to obtain the condensed ring compound; The raw material Ib is Br-L-Cl, and the raw material Ic is in, The raw material Ia is And the intermediate ID is Intermediate Ie is The obtained condensed ring compound is shown in Formula 3; In step (1), the molar ratio of raw material Ia to raw material Ib is 1:(1-1.3); the molar ratio of raw material Ia, potassium carbonate, cuprous bromide and 18-crown ether-6 is 1:(4-5):(0.2-0.4):(0.1-0.3); In step (2), the molar ratio of the intermediate Id, pinacol diboron, potassium acetate and [1,1'-bis[(diphenylphosphino)ferrocene]palladium dichloride is 1:(1.2-1.5):(5-8):(0.01-0.05); In step (3), the molar ratio of the raw material Ic, the intermediate Ie, potassium carbonate, tetrabutylammonium bromide and tetrakistriphenylphosphine palladium is 0.4:(0.4-0.6):(4-8):(0.05-0.1):(0.25-0.4).
4. An organic electroluminescent device, It is characterized in that It comprises an anode, a cathode and an organic layer deposited between the anode and the cathode, wherein the organic layer comprises a hole transport layer, an electron blocking layer, a light-emitting layer and an electron transport layer, wherein the electron transport layer or the light-emitting layer comprises the condensed ring compound according to any one of claims 1 or 2.
5. An electronic device, It is characterized in that The invention comprises the electroluminescent device as claimed in claim 4.