A ferrovanadium continuous nitriding device and process thereof

By designing a continuous nitriding device for ferrous vanadium, continuous preparation and automated control of ferrous vanadium is achieved, and the problems of independent and inefficient existing process steps are solved, and production efficiency and process continuity are improved.

CN113122796BActive Publication Date: 2024-11-22CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110528562.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-14
Publication Date
2024-11-22
Estimated Expiration
2041-05-14

AI Technical Summary

Technical Problem

The existing nitriding process cannot achieve continuous preparation of ferrous vanadium, resulting in a long process manufacturing cycle and low efficiency.

Method used

A continuous nitriding device of ferrovana vanadium is designed, including a gas tank, feed table, material support table and discharge table, to realize automatic feeding and preheating, and control temperature through multiple temperature zones to achieve continuous and automation of reactions. control.

Benefits of technology

It shortens the preheating time, improves production efficiency, realizes the continuity of process steps, liberates labor, and reduces time and labor costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113122796B_ABST
    Figure CN113122796B_ABST
Patent Text Reader

Abstract

The present invention discloses a ferrovanadium continuous nitriding device and a process thereof, the device comprises a gas tank, a feed table, a material room support table and a discharge table which are horizontally arranged in sequence; a first cylinder is horizontally arranged on the feed table, one end of the first cylinder is connected to the gas tank through a connecting channel, a vertically arranged push plate is installed at the end of the push rod at the other end of the first cylinder, a plurality of feed plates are arranged in parallel in sequence at the end of the push plate away from the first cylinder, and the feed plates are used to place material blocks; a material room with openings at both ends is fixedly arranged on the material room support table, and a nitriding zone is arranged in the material room. The ferrovanadium continuous nitriding process based on the above device of the present invention can automatically add materials and preheat, can be prepared continuously, shortens the preheating time, and realizes the automatic control of the entire nitriding device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nitriding, and in particular to a ferrovanadium continuous nitriding device and a process thereof. Background Art

[0002] Due to the rapid development of my country's equipment manufacturing industry, the requirements for nitriding of some parts have become more precise, especially the requirements for high-precision transmission parts, which leads to expensive equipment, difficult maintenance services, high processing costs and maintenance costs. Therefore, nitriding equipment has a large market in China.

[0003] Nitriding technology refers to a chemical heat treatment process that allows nitrogen atoms to penetrate into the surface of a workpiece in a certain medium at a certain temperature. Common methods include liquid nitriding, gas nitriding, and ion nitriding. Traditional gas nitriding is to place the workpiece in a sealed container, pass flowing ammonia gas through it and heat it. After keeping it warm for a long time, the ammonia gas will thermally decompose to produce active nitrogen atoms, which will continuously adsorb to the surface of the workpiece and diffuse into the surface of the workpiece, thereby changing the chemical composition and organization of the surface layer and obtaining excellent surface properties. The principle is that the nitrogen that penetrates into the steel will form iron nitride with different nitrogen contents from the surface to the inside with iron, and will combine with the alloy elements in the steel to form various alloy nitrides, especially aluminum nitride and chromium nitride. These nitrides have high hardness, thermal stability and high dispersivity, so that the nitrided steel parts can obtain high surface hardness, wear resistance, fatigue strength, seizure resistance, atmospheric and superheated steam corrosion resistance, tempering softening resistance, and reduce notch sensitivity, with little effect on the size of the parts.

[0004] Ferrovanadium nitride is a new type of vanadium-nitrogen alloy additive with better performance than ferrovanadium and vanadium nitride. It can be widely used in high-strength screw-rebar, high-strength pipeline steel, high-strength steel (H-shaped steel, I-shaped steel, channel steel, angle steel), thin slab continuous casting and rolling high-strength steel strip, non-quenched and tempered steel, high-speed tool steel and other products. However, when preparing ferrovanadium nitride, the process steps are carried out independently, and continuous preparation cannot be achieved, which makes the process manufacturing cycle long and inefficient. Summary of the invention

[0005] The purpose of the present invention is to provide a vanadium-ferronitriding device and a process thereof to solve the problems existing in the above-mentioned prior art, which can automatically feed and preheat, can be prepared continuously, shorten the preheating time, and realize the automatic control of the entire nitriding device.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] The present invention provides a vanadium-iron continuous nitriding device, comprising a gas tank, a feed table, a material room support table and a discharge table which are horizontally arranged in sequence; a first cylinder is horizontally arranged on the feed table, one end of the first cylinder is connected to the gas tank through a connecting channel, a switch valve is provided on the connecting channel, and the switch and flow rate can be controlled; a vertically arranged push plate is installed at the end of a push rod at the other end of the first cylinder, a plurality of feed plates are sequentially arranged in parallel at one end of the push plate away from the first cylinder, and the feed plates are used for placing material blocks; a material room with openings at both ends is fixedly arranged on the material room support table, and a nitriding zone is arranged in the material room.

[0008] Optionally, the nitriding zone in the material room includes a preheating zone, a transition zone, a high temperature zone, a high temperature slow cooling zone, a low temperature slow cooling zone and a water cooling zone which are arranged in sequence; the temperature of the preheating zone is 400°C to 900°C, the temperature of the transition zone is from 1100°C to 1250°C, the temperature of the high temperature zone is always 1550-1600°C, and the temperature of the high temperature slow cooling zone is reduced from 1250°C to 1100°C.

[0009] Optionally, a first heating component is wrapped around the preheating zone, a heat insulation board is wrapped around the transition zone, a second heating component is wrapped around the high temperature zone, a cooling water jacket is wrapped around the water cooling zone, a water inlet is opened at the top of the cooling water jacket, and a water outlet is opened at the bottom of the cooling water jacket.

[0010] Optionally, a plurality of nitrogen inlet channels are evenly arranged on one side of the material room, and a plurality of waste gas collecting pipes are evenly arranged on the other side of the material room.

[0011] Optionally, the discharge platform is a stepped structure, the height of one end of the discharge platform away from the material room is less than the height of one end of the discharge platform close to the material room, and the end of the discharge platform is lower and can be used to stack the feed plates.

[0012] Optionally, a mechanical claw is provided above the discharging platform, and a sensor is installed at the bottom of the discharging platform, and the sensor is electrically connected to the control end of the mechanical claw. When the workpiece is pushed onto the sensor, the mechanical claw starts to work and grabs the workpiece, thereby completing the separation of the workpiece from the material holding platform.

[0013] Optionally, the feed plate is a mesh structure, and 19 material blocks can be placed on one feed plate.

[0014] Optionally, furnace doors are provided at the openings at both ends of the material room, and vertically arranged second cylinders are installed on both sides of the bottom of the furnace door. The second cylinder is connected to the gas tank through an air charging channel, and a switch valve is provided on the air charging channel to adjust the gas flow. The top of the support push rod of the second cylinder is connected to the bottom of the furnace door, and a pressure sensor is provided in the rod cabin of the second cylinder; a crossbeam is fixedly provided above the openings at both ends of the material room, and a bearing is installed on the crossbeam, and a chain is wound in the bearing, and the end of the chain is fixedly connected to the bottom of the furnace door. During operation, as the air pressure in the second cylinder increases, the support push rod of the second cylinder is pushed out, and the support push rod of the second cylinder supports the furnace door to open. When the support push rod of the second cylinder is pushed to the top, the pressure sensor in the rod cabin of the second cylinder senses a certain concentration, the ventilation valve of the second cylinder opens, the pressure of the second cylinder decreases, the support push rod falls back, and the furnace door falls.

[0015] The present invention also provides a vanadium-ferronitriding process, comprising the following steps:

[0016] Step 1, pressing a powder mixed with vanadium oxide, iron oxide and carbon into a block and placing it on a feed plate;

[0017] Step 2: Push the material into the material room through the first cylinder. As the subsequent materials continue to advance, the first material enters through the preheating zone, transition zone, high temperature zone, high temperature slow cooling zone, low temperature slow cooling zone, and water cooling zone in sequence. At the same time, open the vent to let in nitrogen, open the exhaust port to remove the waste gas in the reaction process, and the reaction begins;

[0018] Step three, after the above steps are completed, the furnace door at the end of the material room is opened. Since the first cylinder continuously delivers the material plate and the material to the material room, the material plate that completes the process first is pushed by the material plate behind to the position of the discharge table, and then the continuous nitriding product vanadium ferronitride is taken out, and the feed plate is recycled and used again.

[0019] Compared with the prior art, the present invention has achieved the following technical effects:

[0020] The present invention can realize the continuity of the steps of the preparation process, can realize the continuity of the reaction, liberate the labor force, and improve the production efficiency. The temperature zone design of the ferrovanadium continuous nitriding device of the present invention can meet the requirements for temperature control, shorten the preheating and reaction time, and save time cost. The automatic feeding design of the ferrovanadium continuous nitriding device of the present invention can complete the continuous addition of materials and realize automatic control. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a schematic diagram of the structure of the ferrovanadium continuous nitriding device of the present invention;

[0023] Figure 2 The material temperature zone structure of the vanadium-ferronitriding device of the present invention;

[0024] Figure 3 This is a schematic diagram of material placement in the present invention;

[0025] Figure 4 This is a schematic diagram of the furnace door structure of the present invention;

[0026] In the figure: vanadium iron continuous nitriding device 100, 1 gas tank, 2 first cylinder, 3 feed table, 4 push rod, 5 material room support table, 6 nitrogen gas inlet channel, 7 exhaust gas collection channel, 8 water outlet, 9 cooling water jacket, 10 discharge table, 11 furnace door, 12 first heating component, 13 insulation board, 14 second heating component, 15 insulation component, 16 water inlet, 17 mechanical claw, 18 material room, 19 feed plate, 20 support push rod, 21 chain, 22 furnace door, 23 crossbeam, 24 bearing, 25 second cylinder, 26 charging channel, 27 preheating zone, 28 transition zone, 29 high temperature zone, 30 high temperature slow cooling zone, 31 low temperature slow cooling zone, 32 water cooling zone, 33 material block. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The purpose of the present invention is to provide a vanadium-ferronitriding device and a process thereof to solve the problems existing in the above-mentioned prior art, which can automatically feed and preheat, can be prepared continuously, shorten the preheating time, and realize the automatic control of the entire nitriding device.

[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] The powder mixed with vanadium oxide, iron oxide and carbon is pressed into blocks and nitrogen is introduced, and it is reacted at a certain temperature. During the reaction, intermediate products such as CO2, CO, VC, VN, etc. are produced. These intermediate products continue to participate in the reaction as reactants, and finally vanadium ferronitride is generated. The production process is completed in the continuous nitriding device designed by the present invention.

[0031] Reference Figure 1 -Attached Figure 4 As shown, the present invention provides a vanadium-iron continuous nitriding device 100, the main structure of which includes: a gas tank 1, a first cylinder 2, a feed table 3, a push rod 4, a material room support platform 5, a nitrogen inlet channel 6, an exhaust gas collection channel 7, a water outlet 8, a cooling water jacket 9, a discharge table 10, a furnace door 11, a first heating component 12, an insulation board 13, a second heating component 14, an insulation component 15, a water inlet 16, a mechanical claw 17, a material room 18, and a feed plate 19.

[0032] Specifically, the first cylinder 2 is connected to the gas tank 1 through a connecting channel, and a switch valve is provided on the connecting channel to control the switch and the flow rate. A push plate perpendicular to the ground is installed at the end of the push rod 4 of the first cylinder 2, and the push plate can push the feed plate 19 to move slowly. The first cylinder 2 and the feed plate 19 are both placed on the feed table 3, and the feed plates 19 are placed side by side on the feed table 3.

[0033] The material room 18 is divided into six temperature zones, namely, a preheating zone 27, a transition zone 28, a high temperature zone 29, a high temperature slow cooling zone 30, a low temperature slow cooling zone 31, and a water cooling zone 32. The temperature of the preheating zone 27 is 400°C to 900°C, the temperature of the transition zone 28 is 1100°C to 1250°C, the temperature of the high temperature zone 29 is always 1550-1600°C, and the temperature of the high temperature slow cooling zone 30 is reduced from 1250°C to 1100°C. The first heating component 12 is wrapped around the preheating zone 27, the heat insulation board 13 is wrapped around the transition zone 28, the second heating component 14 is wrapped around the high temperature zone 29, the cooling water jacket 9 is wrapped around the water cooling zone 32, the cooling water jacket 9 is provided with a water inlet 16 at the top, and a water outlet 8 at the bottom. A number of nitrogen inlet channels 6 are provided on one side of the material room 18, and a number of waste gas collection pipes 7 are provided on the other side of the material room 18. When the workpiece is processed, the nitrogen gas bottle is connected to the nitrogen inlet channel 6, and the waste gas collection pipe 7 is opened at the same time to connect the waste gas bottle. A sensor is installed at the bottom of the discharge table 10. When the workpiece is pushed onto the sensor, the mechanical claw 17 starts to work and grabs the workpiece, so that the workpiece and the feed plate 19 can be separated. The discharge table 10 is stepped, with a lower end, and can be used to stack the feed plate 19. When the workpiece is grabbed by the mechanical claw 17, only the feed plate 19 is left on the discharge table 10. With the subsequent discharge, the feed plate 19 is pushed down to the step.

[0034] like Figure 2The figure shows the temperature zone structure between materials of the vanadium-iron continuous nitriding device, including the preheating zone 27, transition zone 28, high temperature zone 29, high temperature slow cooling zone 30, low temperature slow cooling zone 31, and water cooling zone 32. The length ratios of the six temperature zones are 4:2:4:2:4:2.5 respectively; the four temperature intervals of the preheating zone 27 are 400℃, 650℃, 650℃, and 900℃ respectively; the temperature interval of the transition zone 28 is 1100℃ and 1250℃; the temperature of the high temperature zone 29 is constant at 1550℃; the temperature of the high temperature buffer zone 30 is 1250℃ and 1100℃. The heating material of the preheating zone 27 is a resistance wire; the temperature of the first temperature interval of the transition zone 28 and the second temperature interval of the high temperature slow cooling zone 30 are both 1100℃.

[0035] like Figure 3 The figure shows the schematic diagram of the placement structure of the feed plate 19 and the material block 33. The feed plate 19 is a mesh structure, which can ensure that the bottom of the material block 33 is also fully reacted. The placement of the material block 33 can complete as many material processing as possible in a limited space, while ensuring that the material and the gas are fully contacted, making the reaction more thorough. One feed plate 19 can hold 19 material blocks 33, 12 blocks are placed on the first layer, divided into three piles, 4 blocks are stacked in each pile, and the interval between each pile is about one-quarter of the length of the feed plate 19, and 7 material blocks 33 are placed side by side on the second layer.

[0036] like Figure 4 The figure shows a schematic diagram of the structure of the furnace door 22. The second cylinder 25 is arranged on both sides of the bottom of the furnace door 22. The second cylinder 25 is connected to the gas tank 1 through an air charging channel 26. The air charging channel 26 is provided with a switch valve to adjust the gas flow rate. When the second cylinder 25 is connected to the gas tank 1, as the air pressure in the second cylinder 25 increases, the support push rod 20 is pushed out to support the furnace door 22 to open. When the support push rod 22 is pushed to the top, the pressure sensor in the rod cabin of the second cylinder 25 senses a certain concentration, the air charging channel 26 starts to deflate, the pressure in the second cylinder 25 decreases, the support push rod 20 falls back, and the furnace door 22 falls.

[0037] The general working process of the ferrovanadium continuous nitriding process of the present invention is as follows: a powder mixed with vanadium oxide (V2O5 and V2O3), iron oxide and carbon is pressed into a block and placed on a feed plate 19. The material is pushed into the material room 18 by the push rod 4 through the first cylinder 2. As the subsequent materials continue to be pushed, the first entering material passes through the preheating zone 27, the transition zone 28, the high temperature zone 29, the high temperature slow cooling zone 30, the low temperature slow cooling zone 31, and the water cooling zone 32 in sequence. The temperature is increased from 400°C to 1550°C, and then the heat preservation and cooling treatment is carried out from 1550°C. At the same time, the nitrogen inlet channel 6 is opened to pass nitrogen, and the exhaust gas collection pipeline 7 is opened to remove the exhaust gas in the reaction process, and the reaction begins. The material first enters the preheating temperature zone, and the temperature rises from 400°C to 900°C. During this process, the material is dried; as the temperature rises, vanadium oxide reacts with carbon powder to form gold vanadium, and iron oxide reacts with carbon powder to form metallic iron. In this process, carbon monoxide, vanadium nitride, vanadium carbide and other intermediate products are generated. The generated vanadium nitride fuses with iron at high temperature to form vanadium nitride iron. After high-temperature fusion, the material is buffered by the high-temperature slow cooling zone and the low-temperature slow cooling zone to react more thoroughly. Finally, the final cooling treatment is carried out in the water cooling zone. After the above steps are completed, the discharge door at the end of the material room 18 is opened. Since the push rod 4 continuously delivers the feed plate 19 and the material to the material room 18, the feed plate 19 that completes the process first is pushed by the feed plate 19 behind to reach the position of the discharge table 10, and then the continuous nitridation product vanadium nitride iron is taken out, and the feed plate 19 is recycled and used again.

[0038] In the description of the present invention, it should be noted that the terms "center", "top", "bottom", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0039] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A ferrovanadium continuous nitriding device, Features: The invention comprises a gas tank, a feed platform, a material room support platform and a discharge platform which are horizontally arranged in sequence; a first cylinder is horizontally arranged on the feed platform, one end of the first cylinder is connected to the gas tank through a connecting channel, a vertically arranged push plate is installed at the end of a push rod at the other end of the first cylinder, a plurality of feed plates are sequentially arranged in parallel at one end of the push plate away from the first cylinder, and the feed plates are used to place material blocks; a material room with openings at both ends is fixedly arranged on the material room support platform, and a nitriding zone is arranged in the material room; a nitriding zone in the material room The chemical zone includes a preheating zone, a transition zone, a high temperature zone, a high temperature slow cooling zone, a low temperature slow cooling zone and a water cooling zone which are arranged in sequence; a first heating component is wrapped around the preheating zone, a heat insulation board is wrapped around the transition zone, a second heating component is wrapped around the high temperature zone, a cooling water jacket is wrapped around the water cooling zone, a water inlet is provided on the top of the cooling water jacket, and a water outlet is provided on the bottom of the cooling water jacket; a plurality of nitrogen inlet channels are evenly provided on one side of the material room, and a plurality of exhaust gas collection pipes are evenly provided on the other side of the material room; the feed plate is a mesh structure.

2. The ferrovanadium continuous nitriding device according to claim 1, Features: The temperature of the preheating zone is 400°C to 900°C, the temperature of the transition zone is from 1100°C to 1250°C, the temperature of the high temperature zone is always 1550-1600°C, and the temperature of the high temperature slow cooling zone is reduced from 1250°C to 1100°C.

3. The ferrovanadium continuous nitriding device according to claim 1, Features: The discharging platform is a stepped structure, and the height of one end of the discharging platform away from the material room is smaller than the height of one end of the discharging platform close to the material room.

4. The ferrovanadium continuous nitriding device according to claim 1, Features: A mechanical claw is arranged above the discharging platform, and a sensor is installed at the bottom of the discharging platform. The sensor is electrically connected to the control end of the mechanical claw.

5. The ferrovanadium continuous nitriding device according to claim 1, Features: 19 material blocks can be placed on one feed plate.

6. The ferrovanadium continuous nitriding device according to claim 1, Features: Furnace doors are provided at the openings at both ends of the material room, and vertically arranged second cylinders are installed on both sides of the bottom of the furnace door. The second cylinder is connected to the gas tank through an inflation channel, and a switch valve is provided on the inflation channel to adjust the gas flow rate. The top of the supporting push rod of the second cylinder is connected to the bottom of the furnace door, and a pressure sensor is provided in the rod cabin of the second cylinder; cross beams are fixedly provided above the openings at both ends of the material room, bearings are installed on the cross beams, chains are wound in the bearings, and the ends of the chains are fixedly connected to the bottom of the furnace door.

7. A ferrovanadium continuous nitriding process based on the ferrovanadium continuous nitriding device according to any one of claims 1 to 6, Features: The steps include: Step 1, pressing a powder mixed with vanadium oxide, iron oxide and carbon into a block and placing it on a feed plate; Step 2: Push the material into the material room through the first cylinder. As the subsequent materials continue to advance, the first material enters through the preheating zone, transition zone, high temperature zone, high temperature slow cooling zone, low temperature slow cooling zone, and water cooling zone in sequence. At the same time, open the vent to let in nitrogen, open the exhaust port to remove the waste gas in the reaction process, and the reaction begins; Step three, after the above steps are completed, the furnace door at the end of the material room is opened. Since the first cylinder continuously delivers the feed plate and the material to the material room, the feed plate that completes the process first is pushed by the feed plate behind to the position of the discharge table, and then the continuous nitriding product vanadium ferronitride is taken out, and the feed plate is recycled and used again.