Polyethylene with additives for increased environmental stress cracking resistance

By adding polycarbonate-siloxane copolymer, polyethylene glycol and random block copolymer to high-density polyethylene, the environmental stress crack resistance of HDPE is improved, and HDPE is solved in bottle caps and sealing plug applications The problem of insufficient ESCR performance has achieved performance improvement and cost control.

CN113166500BActive Publication Date: 2024-11-08SABIC GLOBAL TECHNOLOGIES BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980081727.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-11-13
Filing Date
2019-11-04
Publication Date
2024-11-08
Estimated Expiration
2039-11-04

AI Technical Summary

Technical Problem

The existing high-density polyethylene (HDPE) has shortcomings in its environmental stress cracking resistance (ESCR) performance, which makes it prone to cracking during long-term use, especially when preparing bottle caps and sealing plugs, which are difficult to meet enhanced performance requirements. In addition, commonly used additives will degrade the flow and mechanical properties of the polymer at high concentrations and increase costs.

Method used

The HDPE is modified at low concentration by blending the mixture at a blend of high density polyethylene (HDPE) and polycarbonate-siloxane copolymers, polyethylene glycol (PEG) and random block copolymers as additives. Improves its ESCR performance while maintaining or improving its processability.

Benefits of technology

Significantly improves the ESCR performance of HDPE, making its melt flow ratio and density at 190°C and 2.16 Kg meet the requirements, and provides at least 40 hours of crack resistance of molded articles in ASTM D1693-15B test, compared with The HDPE performance of the additive-containing additives is improved by 200% to 2000%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003109386850000172
    Figure BDA0003109386850000172
  • Figure BDA0003109386850000251
    Figure BDA0003109386850000251
Patent Text Reader

Abstract

A polyethylene composition with enhanced environmental stress cracking resistance comprises a polymer blend of a multimodal high density polyethylene (HDPE) and at least one additive as follows: a polycarbonate-siloxane copolymer, a polyethylene glycol (PEG) having an average molecular weight (Mw) of at least 2000, and a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks. The additive is present in the polymer blend in an amount of 1 wt% or less based on the weight of the polymer blend.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to high density polyethylene compositions having improved environmental stress cracking resistance. Background Art

[0002] Synthetic polymers, especially thermoplastic resins, are widely used in the production of a variety of end-use products, from medical devices to food containers. Conventional propylene-based polymers have long been used in processes such as thermoforming, blow molding, and coating, where high melt strength is required, which can be achieved by increasing the molecular weight and broadening the molecular weight distribution. In the polymerization process, the molecular weight and molecular weight distribution can be changed by selecting specific process conditions and catalysts.

[0003] Polypropylene (PP) has been widely used in the production of bottle caps and sealing plugs. However, in order to achieve the necessary strength of the bottle cap, a liner (e.g., made of ethylene vinyl acetate (EVA), polyvinyl chloride (PVC), butyl rubber, etc.) is usually required to achieve the necessary sealing and organoleptic properties. Such double-layer bottle caps are expensive. On the other hand, for the preparation of integral seals such as screw-on bottle caps, high-density polyethylene (HDPE) usually has the necessary hardness, flow properties and better organoleptic properties. However, most HDPE lacks the ability to withstand cracking over time (measured by environmental stress cracking resistance (ESCR) test). Therefore, it is necessary to improve the ESCR performance of HDPE compositions.

[0004] There have been many attempts to improve this property. Although there are a variety of methods to increase the ESCR performance of polyethylene, most of them have the disadvantage of being either too costly or only applicable to the process of preparing the starting polyethylene material and not to existing polyethylene materials. These include C4, C6 and / or C8 comonomers added during the polymerization process, which can be carried out in the gas phase or in solution. Fine-tuning of the molecular weight distribution (bimodal or multimodal) has also been applied, as well as blending polyethylene with other polymers. Cross-linking of silane-grafted polyethylene, the use of specific nucleating agents and the use of specific catalyst packages have also been applied.

[0005] Although various additives are used, these are usually used in high concentrations. Such high concentrations of additives deteriorate the flow and mechanical properties of the resulting polymers while increasing the costs associated with their preparation, making their industrial application impractical.

[0006] Considering the growing trend of plastic parts such as bottle caps and closures, bottles and containers, and the application of plastic containers for the storage of corrosive chemicals (bleach bottles), etc., enhanced ESCR performance of plastics even at low thicknesses has become particularly important. For example, reducing the weight of bottle caps from 3g to 1.8-2.0g (as currently required by many brand owners) while maintaining their ESCR performance is a new challenge. Therefore, there is a constant need for improved polyethylene-based compositions with enhanced ESCR, especially those suitable for bottle caps and closures applications. Summary of the invention

[0007] A polyethylene composition having enhanced environmental stress cracking resistance comprises a polymer blend of a multimodal high density polyethylene (HDPE) and an additive comprising at least one of a polycarbonate-siloxane copolymer, a polyethylene glycol (PEG) having an average molecular weight (Mw) of at least 2000, and a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks. The additive is present in the polymer blend in an amount of 1 wt% or less based on the weight of the polymer blend.

[0008] In a specific embodiment, the additive includes at least two of the following: a polycarbonate-siloxane copolymer, polyethylene glycol (PEG), and a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks. In some cases, the additive may be present in an amount of 0.1-1 wt% based on the weight of the polymer blend. In other cases, the additive may be present in an amount of 0.1-0.5 wt% based on the weight of the polymer blend.

[0009] The melt flow rate of HDPE at 190°C and 2.16Kg can be 0.3-6.0; the melt flow rate at 190°C and 21.6Kg is 3-70dg / min; and / or the density is 945-965Kg / m 3 The density can be determined according to ASTM D792 (2013). The melt flow ratio (MFR) can be determined according to ISO 1133-1 (2011). In a specific embodiment, the dispersion index (PDI = Mw / Mn) of HDPE can be 8-30 as determined by gel permeation chromatography. In some cases, HDPE is selected from C3-C 10 A copolymer of a comonomer of an olefin monomer, said comonomer being present in the HDPE copolymer in an amount of 2 wt% or less.

[0010] The polymer blend can provide a molded article having an ESCR of at least 40 hours as measured by ASTM D1693-15B. In some cases, the polymer blend provides a molded article having an ESCR of 30 to 1000 hours.

[0011] In certain embodiments, the additive is a polycarbonate-siloxane copolymer. The average molecular weight (Mw) of the polycarbonate-siloxane copolymer can be 10,000-60,000 and / or the polycarbonate component can include bisphenol-A polycarbonate. The polycarbonate-siloxane copolymer can also be a siloxane copolymer terminated with bisphenol-A and eugenol. In certain embodiments, the siloxane of the polycarbonate-siloxane copolymer can have a chain length of 5-65 siloxane repeating units.

[0012] In some embodiments, the additive is polyethylene glycol (PEG). The average molecular weight (Mw) of the PEG may be 2,000-40,000. In some cases, the average molecular weight (Mw) of the PEG may be 5000-20,000.

[0013] In a specific application, the additive is a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks. At least one of the two different alkane blocks of the random block copolymer can be branched. In some cases, the random block copolymer can be a styrene-(2-methylbutane)-butane-styrene random block copolymer. The average molecular weight of the random block copolymer can be 250,000-450,000 according to polystyrene standards, and the dispersion index (PDI=Mw / Mn) can be 0.9-1.2 determined by gel permeation chromatography. In some cases, the random block copolymer is a hydrogenated styrene-isoprene-butane block polymer.

[0014] The polyethylene composition may further include at least one of the following additional additives: nucleating agents, thermal conductive agents, binders, anti-blocking agents, antistatic agents, antioxidants, neutralizers, acid scavengers, foaming agents, crystallization aids, dyes, flame retardants, fillers, impact modifiers, release agents, oils, other polymers, pigments, processing aids, reinforcing agents, stabilizers, anti-UV agents, clarifying agents, slip agents, flow modifiers, ionic additives and combinations thereof.

[0015] The polymer blend can be formed into a manufactured article. The article can be a film, a molded part, a container, a beverage container lid, a cover, a sheet, a pipe, a fitting, a bottle, a cup, a plate, a tray and / or a toy. The article can be formed by at least one of the following methods: injection molding, blow molding, compression molding, sheet extrusion, film blowing, pipe extrusion, profile extrusion, calendaring and thermoforming.

[0016] In a method of forming a polyethylene composition having enhanced environmental stress cracking resistance, a multimodal high density polyethylene (HDPE) can be modified by combining the multimodal HDPE with at least one of the following additives: a polycarbonate-siloxane copolymer, a polyethylene glycol (PEG) having an average molecular weight (Mw) of at least 2000, and a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks, wherein the additive is present in the polymer blend in an amount of 1 wt% or less based on the weight of the polymer blend. DETAILED DESCRIPTION

[0017] It has been found that the addition of various additives at low concentrations can increase the environmental stress crack resistance (ESCR) of high density polyethylene (HDPE). These additives can be added to multimodal HDPE by melt blending the additives with the multimodal HDPE polymer. The amount and type of additives added to the multimodal HDPE are selected so as to enhance its ESCR properties while leaving the processability of the HDPE relatively unaffected.

[0018] The HDPE polymers used in the polymer blends can include those prepared by any polymerization process used in the industry (such as "high pressure" process, slurry process, solution process and / or gas phase process) and using any known catalyst (for example, multi-site catalysts such as Ziegler-Natta catalysts and / or single-site catalysts such as chromium or Phillips catalysts, metallocene catalysts, etc.).

[0019] HDPE is a multimodal HDPE with or without a certain amount of unimodal or bimodal HDPE. As used herein, when the phrase or term "high density polyethylene" or "HDPE" is used and is not characterized as unimodal, bimodal or multimodal HDPE, the phrase or term should be understood to refer to multimodal HDPE, which may or may not contain a certain amount of unimodal and / or bimodal HDPE. Bimodal / multimodal HDPE can be produced by using two or more reactors in series using transition metal catalysts. Such a multimodal HDPE composition comprises 35-65wt% of a density>960Kg / m produced in one or more reactors. 3 A reactive blend of ethylene homopolymer and 65-35 wt% of ethylene copolymer. HDPE is available from commercial suppliers. The Mw / Mn of unimodal / multimodal HDPE is 6-30 and the comonomer content is 0.4-2.0 wt%.

[0020] HDPE can be characterized by various properties, such as melt flow rate (MFR) at 190°C and 2.16Kg / or 21.6Kg, density, ESCR, tensile strength at yield tensile modulus, yield tensile elongation, Charpy notched impact strength (-30°C), hardness or a combination thereof. The density of unimodal, bimodal or multimodal HDPE can be 945-965Kg / m 3 , or at least, equal to and / or between any two of the following: 945Kg / m 3 , 950Kg / m 3 , 955Kg / m 3 , 960Kg / m 3 and 965Kg / m 3 .

[0021] It should be noted that in this specification, if a value, concentration or range is given, each value should be modified by the term "about" when it is first read (unless it has been explicitly modified), and it is not necessary to be so modified when it is read again (unless it is explicitly indicated in the text). Similarly, in the specification, it should be understood that the range of amounts listed or described as useful, suitable or similar is considered to have been described by any and all values ​​(including endpoints) within the range. For example, the range "1-10" should be interpreted as referring to each and all possible values ​​in a row between about 1 and about 10. Therefore, even if a specific point within the range is explicitly pointed out or mentioned, or a point within the range is not pointed out or mentioned, it should be understood that the inventor is aware of and understands that any and all points within the range have been specified, and the inventor owns the entire range and all points within the range.

[0022] All or a major part of the HDPE component is multimodal HDPE. The multimodal HDPE may be 50 wt% or greater than 50-100 wt% of the HDPE component. In a particular embodiment, the multimodal HDPE content of the HDPE component may be at least, equal to and / or between any two of the following: 50 wt%, 51 wt%, 52 wt%, 53 wt%, 54 wt%, 55 wt%, 56 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 61 wt%, 62 wt%, 63 wt%, 64 wt%, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 71 wt% %, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 78wt%, 79wt%, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%, 96wt%, 97wt%, 98wt%, 99wt% and 100wt%. In a specific embodiment, the HDPE component may contain 80-100wt% of multimodal HDPE. If the HDPE component uses less than 100wt% of multimodal HDPE, the remainder may be composed of unimodal and / or bimodal HDPE, and / or non-HDPE polyethylene (such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE) and medium density polyethylene (MDPE)). In some embodiments, the polymer blend is free of linear low density polyethylene (LLDPE).In certain aspects, the polymer blends of the present invention are free of polypropylene.

[0023] The MFR of the multimodal HDPE at 190°C and 2.16 Kg may be from 0.2 to 1.0 dg / min, or at least, equal to and / or between any two of: 0.2 to 1.0 dg / min, or at least, equal to and / or between any two of: 0.2 dg / min, 0.3 dg / min, 0.4 dg / min, 0.5 dg / min, 0.6 dg / min, 0.7 dg / min, 0.8 dg / min, 0.9 dg / min and 1.0 dg / min. In a specific embodiment, the MFR of the multimodal HDPE at 190°C and 2.16 Kg may be from 0.3 to 0.6 dg / min. The MFR of the multimodal HDPE at 190°C and 21.6 kg may also be 2-40 dg / min, or at least, equal to and / or between any two of the following: 2 dg / min, 3 dg / min, 4 dg / min, 5 dg / min, 6 dg / min, 7 dg / min, 8 dg / min, 9 dg / min, 10 dg / min, 11 dg / min, 12 dg / min, 13 dg / min, 14 dg / min, 15 dg / min, 16 dg / min, 17 dg / min, 18 dg / min In a specific embodiment, the MFR at 190°C and 21.6 Kg is 3 to 35 dg / min.

[0024] The dispersion index (PDI = Mw / Mn) of the multimodal HDPE of the HDPE component may be 8-30 as determined by gel permeation chromatography.

[0025] If bimodal HDPE is used, it can be used in an amount greater than 0 to 50 wt% or less than 50 wt%, based on the total weight of the polymer blend. In a particular embodiment, the bimodal HDPE content of the HDPE component can be at least, equal to, and / or between any two of the following: 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, based on the total weight of the polymer blend. %, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% and 50wt%.

[0026] The MFR of the bimodal HDPE at 190°C and 2.16 Kg and / or 21 Kg may be 0.2-20 dg / min, or at least, equal to and / or between any two of the following: 0.2-20 dg / min, or at least, equal to and / or between any two of the following: 0.2 dg / min, 0.3 dg / min, 0.4 dg / min, 0.5 dg / min, 0.75 dg / min, 1 dg / min, 1.25 dg / min, 1.5 dg / min, 1.75 dg / min, 2 dg / min, 3 dg / min, 4 dg / min and 5 dg / min, 6 dg / min, 7 dg / min, 8 dg / min, 9 dg / min, 10 dg / min, 11 dg / min, 12 dg / min, 13 dg / min, 14 dg / min, 15 dg / min, 16 dg / min dg / min, 17dg / min, 18dg / min, 19dg / min and 20dg / min, 21dg / min, 22dg / min, 23dg / min, 24dg / min , 25dg / min, 26dg / min, 27dg / min, 28dg / min, 29dg / min, 30dg / min, 31dg / min, 32dg / min, 33dg / min, 34dg / min, 35dg / min, 36dg / min, 37dg / min, 38dg / min, 39dg / min, 40dg / min.41dg / min, 42 dg / min, 43dg / min, 44dg / min, 45dg / min, 46dg / min, 47dg / min, 48dg / min, 49dg / min and 50dg / min. In a specific embodiment, the MFR is 0.5-5 dg / min at 190°C and 2.16 Kg load.

[0027] The tensile modulus of the bimodal or multimodal HDPE may be 850-1300 MPa, or at least, equal to and / or between any two of 850 MPa, 900 MPa, 950 MPa, 1000 MPa, 1050 MPa, 1100 MPa, 1150 MPa, 1200 MPa, 1250 MPa and 1300 MPa, as measured by ASTM D638. The tensile strength at yield of the bimodal and multimodal HDPE may be 20 MPa-40 MPa, or at least, equal to and / or between any two of 20 MPa, 25 MPa, 30 MPa, 35 MPa and 40 MPa, as measured by ASTM D638.

[0028] The Charpy notched impact strength of bimodal or multimodal HDPE components at -30°C can be 3-6 kJ / m2 , or at least, equal to and / or between any two of the following: 3 kJ / m 2 , 4kJ / m 2 , 5kJ / m 2 and 6 kJ / m 2 The Charpy notched impact strength of bimodal or multimodal HDPE components at 23°C can be 14-22 kJ / m 2 , or at least, equal to and / or between any two of the following: 14 kJ / m 2 、15kJ / m 2 、16kJ / m 2 、17kJ / m 2 、18kJ / m 2 、19kJ / m 2 、20kJ / m 2 、21kJ / m 2 and 22 kJ / m 2 The izod notched impact strength of the HDPE component at 23°C can be 5-20 kJ / m 2 , or at least, equal to and / or between any two of the following: 5 kJ / m 2 , 6kJ / m 2 , 7kJ / m 2 , 8kJ / m 2 , 9kJ / m 2 、10kJ / m 2 、11kJ / m 2 、12kJ / m 2 、13kJ / m 2 、14kJ / m 2 、15kJ / m 2 、16kJ / m 2 、17kJ / m 2 、18kJ / m 2 、19kJ / m 2 and 20 kJ / m 2 .

[0029] In some embodiments, a portion of the HDPE component may be unimodal. If unimodal HDPE is used, it may be greater than 0 to 50 wt% or less than 50 wt% of the total weight of the polymer blend. In specific embodiments, the unimodal HDPE content of the HDPE component may be at least, equal to, and / or between any two of the following based on the total weight of the polymer blend: 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt% %, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% and 50wt%.

[0030] The MFR of the unimodal HDPE at 190°C and 2.16 Kg and / or 21.6 Kg may be from 0.2 to 50 dg / min, or at least, equal to and / or between any two of the following: 0.2 dg / min, 0.3 dg / min, 0.4 dg / min, 0.5 dg / min, 0.75 dg / min, 1 dg / min, 1.25 dg / min, 1.5 dg / min, 1.75 dg / min, 2 dg / min, 3 dg / min, 4 dg / min and 5 dg / min, 6 dg / min, 7 dg / min, 8 dg / min, 9 dg / min, 10 dg / min, 11 dg / min, 12 dg / min, 13 dg / min, 14 dg / min, 15 dg / min, 16 dg / min, 17 dg / min, 18dg / min, 19dg / min and 20dg / min, 21dg / min, 22dg / min, 23dg / min, 24dg / min, 25dg / min, 26 dg / min, 27dg / min, 28dg / min, 29dg / min, 30dg / min, 31dg / min, 32dg / min, 33dg / min, 34dg / min, 35dg / min, 36dg / min, 37dg / min, 38dg / min, 39dg / min, 40dg / min. 41dg / min, 42dg / min, 43dg / min, 44dg / min, 45dg / min, 46dg / min, 47dg / min, 48dg / min, 49dg / min and 50dg / min. In a specific embodiment, the MFR is 0.5-5 dg / min at 190°C and 2.16 Kg load.

[0031] The unimodal HDPE may have a tensile modulus and / or a flexural modulus of 850-1300 MPa, or at least, equal to, and / or between any two of 850 MPa, 900 MPa, 950 MPa, 1000 MPa, 1050 MPa, 1100 MPa, 1150 MPa, 1200 MPa, 1250 MPa, and 1300 MPa, as measured according to ISO 527-2. The unimodal HDPE may have a tensile strength at yield and / or a flexural strength of 20-40 MPa, or at least, equal to, and / or between any two of 20 MPa, 25 MPa, 30 MPa, 35 MPa, and 40 MPa, as measured according to ISO 527-2.

[0032] The Charpy notched impact strength of the unimodal HDPE component at -30°C can be 3-6 kJ / m 2, or at least, equal to and / or between any two of the following: 3 kJ / m 2 , 4kJ / m 2 , 5kJ / m 2 and 6 kJ / m 2 The izod notched impact strength of the HDPE component at 23°C can be 5-20 kJ / m 2 , or at least, equal to and / or between any two of the following: 5 kJ / m 2 , 6kJ / m 2 , 7kJ / m 2 , 8kJ / m 2 , 9kJ / m 2 、10kJ / m 2 、11kJ / m 2 、12kJ / m 2 、13kJ / m 2 、14kJ / m 2 、15kJ / m 2 、16kJ / m 2 、17kJ / m 2 、18kJ / m 2 、19kJ / m 2 and 20 kJ / m 2 .

[0033] In certain embodiments, the HDPE component of the polymer blend consists of ethylene homopolymers. These may include homopolymers of pure HDPE. However, in other embodiments, the HDPE component may include a polymer blend containing non-HDPE polyethylenes. These may include low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and medium density polyethylene (MDPE). When such non-HDPE polyethylenes are used, they may be present in the HDPE polymer component in an amount of 2 wt%, 1.5 wt%, 1 wt%, 0.5 wt%, 0.1 wt% or less.

[0034] In other embodiments, the HDPE component may include ethylene and at least one C3-C 10 The HDPE copolymer is a copolymer of α-olefins. Typically, it is at least one α-olefin of butene, hexene and / or octene. In some embodiments, the HDPE is a copolymer containing 1-butene (polyethylene-1-butene) or a copolymer containing 1-hexene (polyethylene-1-hexene). When such a copolymer is used, the non-ethylene comonomer may be present in the HDPE copolymer in an amount of 2 wt%, 1.5 wt%, 1 wt%, 0.5 wt%, 0.1 wt% or less. In a specific embodiment, there is no butene or no C3-C 10α-Olefin Comonomers. Those percentages given previously for the HDPE component for multimodal HDPE, bimodal HDPE and / or unimodal HDPE may be used for the HDPE incorporating such copolymers.

[0035] In certain embodiments, the HDPE may be unfunctionalized pure HDPE having no functional groups along the polymer chain. In particular embodiments, the HDPE polyethylene does not include any anhydride modified HDPE.

[0036] As described above, the HDPE component is used as a polymer blend in combination with one or more different primary additives used to provide enhanced environmental stress cracking resistance. These primary additives may include one or more of the following: polycarbonate-siloxane copolymers, polyethylene glycol (PEG) having an average molecular weight (Mw) of at least 2000, and a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks. The total amount of such primary additives present in the polymer blend may be 1 wt% or less based on the total weight of the polymer blend. In certain embodiments, the total amount of the primary additive can be at least, equal to, and / or between any two of the following based on the total weight of the polymer blend: 0.10 wt%, 0.11 wt%, 0.12 wt%, 0.13 wt%, 0.14 wt%, 0.15 wt%, 0.16 wt%, 0.17 wt%, 0.18 wt%, 0.19 wt%, 0.20 wt%, 0.21 wt%, 0.22 wt%, 0.23 wt%, 0.24 wt%, 0.25 wt%, 0.26 wt%, 0.27 wt%, 0.28 wt%, 0.29 wt%, 0.30 wt%, 0.31 wt%, 0.32 %, 0.33 wt%, 0.34 wt%, 0.35 wt%, 0.36 wt%, 0.37 wt%, 0.38 wt%, 0.39 wt%, 0.40 wt%, 0.41 wt%, 0.42 wt%, 0.43 wt%, 0.44 wt%, 0.45 wt%, 0.46 wt%, 0.47 wt%, 0.48 wt%, 0.49 wt%, 0.50 wt%, 0.55 wt%, 0.60 wt%, 0.65 wt%, 0.70 wt%, 0.75 wt%, 0.80 wt%, 0.85 wt%, 0.90 wt%, 0.95 wt% and 1.00 wt%. In a specific embodiment, the total amount of the above additives in the polymer blend is 0.10-0.60 wt% based on the total weight of the polymer blend. These additives are typically mixed with the HDPE component by polymer melt blending.

[0037] In certain embodiments, as described above, the HDPE component can be used as a polymer blend in combination with a polycarbonate-siloxane copolymer. The polycarbonate-siloxane copolymer can be used as a primary additive alone as the sole primary additive, or in combination with one or more other primary additives. In other embodiments, when the polycarbonate-siloxane copolymer is not used, one or more other primary additives are applied. The polycarbonate-siloxane copolymer and its combination with the HDPE component as a polymer blend can be the same or similar to that described in U.S. Patent Application No. 62 / 677,319 filed on May 28, 2018, which is incorporated herein by reference for all purposes.

[0038] In order to impart the desired ESCR characteristics to the final product, the amount of polycarbonate-siloxane copolymer used can be 1 wt% or less based on the total weight of the polymer blend, or at least, equal to and / or between any two of the following based on the total weight of the polymer blend: 0.01 wt%, 0.02 wt%, 0.03 wt%, 0.04 wt%, 0.05 wt%, 0.06 wt%, 0.07 wt%, 0.08 wt%, 0.09 wt%, 0.10 wt%, 0.11 wt%, 0.12 wt%, 0.13 wt%, 0.14 wt%, 0.15 wt%, 0.16 wt%, 0.17 wt%, 0.18 wt%, 0.19 wt%, 0.20 wt%, 0.21 wt%, 0.22 wt%, 0.23 wt%, 0.24 wt%, 0.25 wt%, 0.26wt%, 0.27wt%, 0.28wt%, 0.29wt%, 0.30wt%, 0.31wt%, 0.32wt%, 0.33wt%, 0. 34wt%, 0.35wt%, 0.36wt%, 0.37wt%, 0.38wt%, 0.39wt%, 0.40wt%, 0.41wt%, 0.42wt%, 0 %, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt%, 0.50wt%, 0.55wt%, 0.60wt%, 0.65wt%, 0.70wt%, 0.75wt%, 0.80wt%, 0.85wt%, 0.90wt%, 0.95wt% and 1.0wt%. In a specific embodiment, the polycarbonate-siloxane copolymer additive can be present in the polymer blend in an amount of 0.01-0.5wt% based on the total weight of the polymer blend.

[0039] The polycarbonate-siloxane copolymer component of the polymer blend can have an average molecular weight (Mw) of 10,000-60,000, or at least, equal to, and / or between any two of 10,000, 15,000, 20,000, 25,000, 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, and 60,000. The polycarbonate component of the polycarbonate-siloxane copolymer can be present in an amount of 75-98 mol%, or at least, equal to and / or between any two of the following: 75 mol%, 76 mol%, 77 mol%, 78 mol%, 79 mol%, 80 mol%, 81 mol%, 82 mol%, 83 mol%, 84 mol%, 85 mol%, 86 mol%, 87 mol%, 88 mol%, 89 mol%, 90 mol%, 91 mol%, 92 mol%, 93 mol%, 94 mol%, 95 mol%, 96 mol%, 97 mol% and 98 mol%. Carbonate monomers for forming polycarbonate can include phosgene, dimethyl carbonate and / or diphenyl carbonate. In a specific embodiment, an aromatic dihydroxy comonomer for preparing polycarbonate-siloxane copolymer is bisphenol-A. Comonomers that can be used include those described in U.S. Pat. No. 7,365,124, which are incorporated herein by reference for this purpose. They include, but are not limited to: 2,4′-dihydroxydiphenylmethane; bis(2-hydroxyphenyl)methane; bis(4-hydroxyphenyl)methane; bis(4-hydroxy-5-nitrophenyl)methane; bis(4-hydroxy-2,6-dimethyl-3-methoxyphenyl)methane; 1,1-bis(4-hydroxyphenyl)ethane; 1,1-bis(4-hydroxy-2-chlorophenyl)ethane; 2,2-bis(4-hydroxyphenyl)propane (bisphenol A); 2,2-bis(3-chloro-4-hydroxyphenyl)propane; 2,2-bis(3-bromo-4-hydroxyphenyl)propane; 2,2-bis(4-hydroxy-3-methylphenyl)propane; 2,2-bis(4-hydroxy-3-isopropylphenyl)propane; 2,2-bis(3-tert-butyl-4-hydroxyphenyl)propane ) propane; 2,2-bis(3-phenyl-4-hydroxyphenyl)propane; 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane; 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane; 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane; 2,2-bis(3-chloro-4-hydroxy-5-methylphenyl)propane; 2,2-bis(3-bromo-4-hydroxy-5-methylphenyl)propane; 2,2-bis(3-chloro-4-hydroxy-5-isopropylphenyl)propane; 2,2-bis(3-bromo-4-hydroxy-5-isopropylphenyl)propane; 2,2-bis(3-tert-butyl-5-chloro-4-hydroxyphenyl)propane; 2,2-bis(3-bromo-5-tert-butyl-4-hydroxyphenyl)propane;2,2-bis(3-chloro-5-phenyl-4-hydroxyphenyl)propane; 2,2-bis(3-bromo-5-phenyl-4-hydroxyphenyl)propane; 2,2-bis(3,5-diisopropyl-4-hydroxyphenyl)propane; 2,2-bis(3,5-di-tert-butyl-4-hydroxyphenyl)propane; 2,2-bis(3,5-diphenyl-4-hydroxyphenyl)propane; 2,2-bis(4-hydroxy-2,3,5,6-tetrachlorophenyl)propane; 2,2-bis(4-hydroxy-2,3,5,6-tetrabromophenyl)propane; 2,2-bis(4-hydroxy-2,3,5,6-tetramethylphenyl)propane; 2,2-bis(2,6-dichloro-3,5-dimethyl-4-hydroxyphenyl)propane; 2,2-bis( 2,6-dibromo-3,5-dimethyl-4-hydroxyphenyl)propane; 2,2-bis(4-hydroxy-3-ethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(3,5,3′,5′-tetrachloro-4,4′-dihydroxyphenyl)propane, bis(4-hydroxyphenyl)cyclohexylmethane, 2,2-bis(4-hydroxyphenyl)-1-phenylpropane, 1,1-bis(4-hydroxyphenyl)cyclohexane; 1,1-bis(3-chloro-4-hydroxyphenyl)cyclohexane; 1,1-bis(3-bromo-4-hydroxyphenyl)cyclohexane; 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane; 1,1-bis(4-hydroxy-3-isopropylphenyl)cyclohexane; 1, 1-bis(3-tert-butyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(3-phenyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(3,5-dichloro-4-hydroxyphenyl)cyclohexane; 1,1-bis(3,5-dibromo-4-hydroxyphenyl)cyclohexane; 1,1-bis(4′-hydroxy-3′-methylphenyl)cyclohexane (DMBPC), 1,1-bis(3,5-dimethyl-4-hydroxyphenyl)cyclohexane; 4,4′-[1-methyl-4-(1-methyl-ethyl)-1,3-cyclohexanediol]bisphenol (1,3BHPM), 4-[1-[3-(4-hydroxyphenyl)-4-methylcyclohexyl]-1-methyl-ethyl]-phenol (2,8BHPM), 3,8-dihydroxyphenyl 1,1-bis(3-chloro-4-hydroxy-5-methylphenyl)cyclohexane; 1,1-bis(3-bromo-4-hydroxy-5-methylphenyl)cyclohexane; 1,1-bis(3-chloro-4-hydroxy-5-isopropylphenyl)cyclohexane; 1,1-bis(3-bromo-4-hydroxy-5-isopropylphenyl)cyclohexane; 1,1-bis(3-tert-butyl-5-chloro-4-hydroxyphenyl)cyclohexane; 1,1-bis(3-bromo-5-tert-butyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(3-chloro-5-phenyl-4-hydroxyphenyl)cyclohexane;1,1-bis(3-bromo-5-phenyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(3,5-diisopropyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(3,5-di-tert-butyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(3,5-diphenyl-4-hydroxyphenyl)cyclohexane; 1,1-bis(4-hydroxy-2,3,5,6-tetrachlorophenyl)cyclohexane; 1,1-bis(4-hydroxy-2,3,5,6-tetrabromophenyl)cyclohexane; 1,1-bis(4-hydroxy-2,3,5,6-tetramethylphenyl)cyclohexane; 1,1-bis(2,6-dichloro-3,5-dimethyl-4-hydroxyphenyl)cyclohexane; Hydroxyphenylcyclohexane; 1,1-bis(2,6-dibromo- 3,5-Dimethyl-4-1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-chloro-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-bromo-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(4-hydroxy-3-methylphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(4-hydroxy-3-isopropylphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-tert-butyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-phenyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3,5-dichloro-4 -hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3,5-dibromo-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3,5-dimethyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-chloro-4-hydroxy-5-methylphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-bromo-4-hydroxy-5-methylphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-chloro-4-hydroxy-5-isopropylphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-bromo-4-hydroxy-5-isopropylphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3 -tert-butyl-5-chloro-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-bromo-5-tert-butyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; bis(3-chloro-5-phenyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3-bromo-5-phenyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3,5-diisopropyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3,5-di-tert-butyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(3,5-diphenyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane;1,1-Bis(4-hydroxy-2,3,5,6-tetrachlorophenyl)-3,3,5-trimethylcyclohexane; 1,1-Bis(4-hydroxy-2,3,5,6-tetrabromophenyl)-3,3,5-trimethylcyclohexane; 1,1-Bis(4-hydroxy-2,3,5,6-tetramethylphenyl)-3,3,5-trimethylcyclohexane; 1,1-Bis(2,6-dichloro-3,5-dimethyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 1,1-bis(2,6-dibromo-3,5-dimethyl-4-hydroxyphenyl)-3,3,5-trimethylcyclohexane; 4,4-bis(4-hydroxyphenyl)heptane, 4,4′-dihydroxy-1,1-biphenyl; 4,4′-dihydroxy-3,3′-dimethyl-1,1-biphenyl; 4,4′-dihydroxy-3,3′-dioctyl-1,1-biphenyl; 4,4′-(3,3,5-trimethylcyclohexylene)diphenol, 4,4′-bis(3,5- 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene; 1,3-bis(2-(4-hydroxy-3-methylphenyl)-2-propyl)benzene; 1,4-bis(2-(4-hydroxyphenyl)-2-propyl)benzene, 1,4-bis(2-(4-hydroxy-3-methylphenyl)-2-propyl)benzene dihydroxydiphenyl sulfone (BPS), 2,4'-dihydroxyphenyl ether; 4,4'-dihydroxydiphenyl sulfide; ...4-bis(2-(4-hydroxy-3-methylphenyl)-2-propyl)benzene Hydroxyphenyl sulfone, 4,4′-bis(4-hydroxyphenyl)methane, 2,6-dihydroxynaphthalene; hydroquinone; resorcinol, C1-C3 alkyl-substituted resorcinol, 3-(4-hydroxyphenyl)-1,1,3-trimethylindan-5-ol, 1-(4-hydroxyphenyl)-1,3,3-trimethylindan-5-ol and 2,2,2′,2′-tetrahydro-3,3,3′,3′-tetramethyl-1,1′-spirobi[1H-indene]-6,6′-diol. The most typical aromatic dihydroxy compound is bisphenol A (BPA). ;

[0040] In some embodiments, an isosorbide comonomer or a 2-hydrocarbyl-3,3-bis(4-hydroxyaryl)phthalimide comonomer may be used with BPA to produce a polycarbonate copolymer.

[0041] The copolycarbonates have an average molecular weight (Mw) of 3000 to about 150,000.

[0042] The amount of siloxane present in the polycarbonate-siloxane copolymer additive is 2-25 mol%, or is at least, equal to and / or between any two of the following: 2 mol%, 3 mol%, 4 mol%, 5 mol%, 6 mol%, 7 mol%, 8 mol%, 9 mol%, 10 mol%, 11 mol%, 12 mol%, 13 mol%, 14 mol%, 15 mol%, 16 mol%, 17 mol%, 18 mol%, 19 mol%, 20 mol%, 21 mol%, 22 mol%, 23 mol%, 24 mol% and 25 mol%. In a specific embodiment, the siloxane of the polycarbonate-siloxane copolymer can be a eugenol-terminated siloxane. In other embodiments, the siloxane of the polycarbonate-siloxane copolymer can be composed of a chain of siloxane units composed of siloxane D-units having the general formula (R) 2SiO units, wherein R is a C1-C4 alkane. The chain length of the siloxane repeating D units may be 5-65 units, or at least, equal to, and / or between any two of 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, and 65 units.

[0043] In certain embodiments, the polymer blend of HDPE to which the polycarbonate-siloxane copolymer additive is added may also include a polycarbonate homopolymer. The polycarbonate homopolymer may be present in an amount of 0.1-40 wt% based on the total weight of the polymer blend, or at least, equal to, and / or between any two of the following based on the total weight of the polymer blend: 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1 wt%, 1.5 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, 50 wt%, 51 wt%, 52 wt%, 53 wt%, 54 wt%, 55 wt%, 56 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt %, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% and 40wt%.

[0044] As previously mentioned, the carbonate monomers used to form the polycarbonate homopolymer can be the same as the polycarbonate components used for the polycarbonate-siloxane copolymer. They can include phosgene, dimethyl carbonate and / or diphenyl carbonate. In a particular embodiment, the polycarbonate segments of the polycarbonate-siloxane copolymer are based on bisphenol-A polycarbonate.

[0045] As described above, the HDPE component can also be used as a polymer blend in combination with PEG as a primary additive. PEG can be used alone as a primary additive, or in combination with one or more other primary additives. In other embodiments, one or more other primary additives are applied without the application of PEG. PEG and its combination with the HDPE component as a polymer blend can be the same or similar as described in U.S. Patent Application No. 62 / 681,362 filed on June 6, 2018, which is incorporated herein by reference for all purposes.

[0046] %, 0.14 wt%, 0.15 wt%, 0.16 wt%, 0.17 wt%, 0.18 wt%, 0.19 wt%, 0.20 wt%, 0.21 wt%, 0.22 wt%, 0.23 wt%, 0.24 wt%, 0.25 wt%, 0.26 wt%, 0.27 wt%, 0.28 wt%, 0.29 wt%, 0.30 wt%, 0.31 wt%, 0.32 wt%, 0.33 wt%, 0.34 wt%, 0.35 wt%, 0.36 wt%, 0.37 wt%, 0.38 wt%, 0.39 wt%, 0.40 wt%, 0.41 wt%, 0.42 wt%, 0.43 wt%, 0.44 wt%, 0.45 wt%, 0.46 wt%, 0.47 wt%, 0.48 wt%, 0.49 wt%, 0.50 wt%, 0.51 wt%, 0.52 wt%, 0.53 wt%, 0.54 wt%, 0.55 wt%, 0.56 wt%, 0.57 wt%, 0.58 wt%, 0.59 wt%, % , 0.26wt%, 0.27wt%, 0.28wt%, 0.29wt%, 0.30wt%, 0.31wt%, 0.32wt%, 0.33wt%, 0.34wt%, 0.35wt%, 0.36wt%, 0.37wt%, 0.38wt%, 0.39wt%, 0.40wt%, 0.41wt%, 0.42wt%, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt%, 0.50wt%, 0.55wt%, 0.60wt%, 0.65wt%, 0.70wt%, 0.75wt%, 0.80wt%, 0.85wt%, 0.90wt%, 0.95wt% and 1.0wt%. In certain embodiments, the PEG additive may be present in the polymer blend in an amount of 0.01 to 0.6 wt % based on the total weight of the polymer blend.

[0047] The PEG component additive used in the polymer blend is a high molecular weight PEG. The average molecular weight (Mw) of the PEG can be 2000-40,000, or at least, equal to and / or between any two of the following average molecular weights (Mw): 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 31,000, 32,000, 33,000, 34,000, 35,000, 36,000, 37,000, 38,000, 39,000, 40,000, 41,000, 42,000, 43,000, 44,000, 45,000, 46,000, 47,000, 48,000, 49,000, 50,000, 51,000, 52,000 In some embodiments, the average Mw of PEG is 4,000-20,000, 30,000 or 40,000.

[0048] As described above, the HDPE component can also be used as a polymer blend only in combination with a random block copolymer primary additive comprising two different saturated alkane blocks between two aromatic blocks or in combination with one or more other primary additives. In other embodiments, one or more other primary additives are applied without using a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks. The random block copolymer and its combination with the HDPE component as a polymer blend can be the same or similar to that described in U.S. Patent Application No. 62 / 662,396 filed on April 25, 2018, which is incorporated herein by reference for all purposes.

[0049] In order to impart the desired ESCR characteristics to the final product, the amount of random block copolymer used can be 1 wt% or less, based on the total weight of the polymer blend, or at least, equal to and / or between any two of the following: 0.01 wt%, 0.02 wt%, 0.03 wt%, 0.04 wt%, 0.05 wt%, 0.06 wt%, 0.07 wt%, 0.08 wt%, 0.09 wt%, 0.10 wt%, 0.11 wt%, 0.12 wt%, 0.13 wt%, 0.14 wt%, 0.15 wt%, 0.16 wt%, 0.17 wt%, 0.18 wt%, 0.19 wt%, 0.20 wt%, 0.21 wt%, 0.22 wt%, 0.23 wt%, 0.24 wt%, 0.25 wt%, based on the total weight of the polymer blend. %, 0.26wt%, 0.27wt%, 0.28wt%, 0.29wt%, 0.30wt%, 0.31wt%, 0.32wt%, 0.33wt%, 0.34 wt%, 0.35wt%, 0.36wt%, 0.37wt%, 0.38wt%, 0.39wt%, 0.40wt%, 0.41wt%, 0.42wt%, 0. %, 0.43wt%, 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt%, 0.48wt%, 0.49wt%, 0.50wt%, 0.55wt%, 0.60wt%, 0.65wt%, 0.70wt%, 0.75wt%, 0.80wt%, 0.85wt%, 0.90wt%, 0.95wt% and 1.0wt%. In a specific embodiment, the random block copolymer additive can be present in the polymer blend in an amount of 0.01-0.5wt% based on the total weight of the polymer blend.

[0050] The random block copolymer can be any random block copolymer having two different saturated alkyl blocks between the aromatic blocks (such as two aromatic blocks). The random block copolymer can be a random ternary block copolymer. The general formula of the random block copolymer can be ABCA, wherein A is an aromatic repeating unit, block B is a saturated branched alkane repeating unit, and block C is a saturated straight chain alkane repeating unit. Non-limiting examples of block A aromatic groups include styrene or substituted styrene units. Block B can have a branched saturated alkane unit of 4-8 carbon atoms. The side chain can include 1-2 alkyl groups. Non-limiting examples of block B saturated alkane repeating units include 1-methylpropane, 2-methylbutane, 2-propylbutane, 2-methylpentane, 3-methylpentane, 2,3-dimethylpentane, 2-propylpentane, 2-methylhexane, 2-propylhexane, 2-methylheptane, etc. Block C may be a linear saturated alkane repeating unit having 3 to 8 carbon atoms. Non-limiting examples of the linear saturated alkane repeating unit of block C include alkanes such as propane, butane, pentane, hexane, heptane and octane.

[0051] The random block copolymer may have an average molecular weight of 250,000-450,000 (e.g., 250,000; 275,000; 300,000; 325,000; 375,000; 400,000; 425,000; 450,000, or any range or value therebetween) as determined by polystyrene standards, and a polydispersity index (PDI=Mw / Mn) of 0.9-1.2 as determined by gel permeation chromatography. Polystyrene standards include monodisperse polystyrene standards having a specified molecular weight for calibration when determining the molecular weight of a new sample.

[0052] Random block copolymers are available from commercial sources. For example, suitable random block copolymers are available from Kuraray (Japan) under the trademark The random block copolymers are sold as 4033, 4044, 4055, 4077 and 4099. The non-limiting structure of the random block copolymer is represented by the following formula (1):

[0053]

[0054] The polyethylene composition can also include at least one additional optional or auxiliary additive to distinguish it from the main additive discussed above. This optional or auxiliary additive can be an additive that does not necessarily affect or increase the ESCR of the final product. The non-limiting examples of the additional optional or auxiliary additive include nucleating agents, thermal conductive agents, bonding agents, anti-caking agents, antistatic agents, antioxidants, neutralizing agents, acid scavengers, foaming agents, crystallization aids, dyes, flame retardants, fillers (hard fillers or soft fillers), impact modifiers, release agents, oils, other polymers, pigments, processing aids, reinforcing agents, stabilizers (including light stabilizers), UV inhibitors, clarifying agents, slip agents, flow modifiers and combinations thereof. In certain embodiments, there is no carbon black in the HDPE composition.

[0055] Non-limiting examples of nucleating agents include calcium carbonate (CaCO3), barium sulfate (BaSO4), silicon dioxide (SiO2), kaolin, talc, mica, titanium dioxide (TiO2), aluminum oxide (Al2O3), zeolite, mono- or polyaromatic carboxylic acid, dye, pigment, carboxylic acid metal salt, aromatic carboxylic acid metal salt, hexahydrophthalic acid metal salt, stearate, organic phosphate, bisamide, sorbitol or a combination thereof. Non-limiting examples of aromatic carboxylic acid metal salts include sodium benzoate.

[0056] In some cases, the thermally conductive additive is present in the polymer blend in an amount of at least, equal to, and / or between any two of the following: 0.01 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, and 1.0 wt%, based on the total weight of the polymer blend. Non-limiting examples of thermally conductive additives include aluminum oxide, titanium dioxide, graphite compounds, graphene, boron nitride, aluminum nitride, and zinc oxide.

[0057] In certain aspects, the amount of binding molecule present in the polymer blend is at least, equal to and / or between any two of the following based on the total weight of the polymer blend: 0.01wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% and 1.0wt%. Non-limiting examples of binding molecules include linear low density polyethylene, low density polyethylene, medium density polyethylene.

[0058] In some embodiments, the amount of filler present in the polymer blend is at least, equal to and / or between any two of the following based on the total weight of the polymer blend: 0.01wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 2.0wt%, 3.0wt%, 4.0wt%, 5.0wt%, 6.0wt%, 7.0wt%, 8.0wt%, 9.0wt%, 10.0wt%, 20.0wt%, 30.0wt%. The filler can be a hard filler. Non-limiting examples of hard fillers include inorganic particulate fillers (such as silica, calcium carbonate), inorganic layered fillers (such as clay, mica). The filler can also be a soft filler. Non-limiting examples of soft fillers include immiscible granular elastomers / polymer resins. The filler can also be a hollow filler. Non-limiting examples of hollow fillers include glass microspheres, plastic microspheres, ceramic microspheres, such as hollow microspheres composed of aluminosilicate microspheres, metal microspheres composed of aluminum and copper / silver microspheres, and phenolic microspheres.

[0059] In certain aspects, the amount of light stabilizer present in the polymer blend is at least, equal to and / or between any two of the following based on the total weight of the polymer blend: 0.01wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% and 1.0wt%. The light stabilizer can be a hindered amine light stabilizer. The term "hindered amine light stabilizer" refers to a class of amine compounds with a certain light stability. Non-limiting examples of hindered amine light stabilizers (HALS) include: 1-cyclohexyloxy-2,2,6,6-tetramethyl-4-octadecylaminopiperidine; bis(2,2,6,6-tetramethylpiperidin-4-yl) sebacate; bis(1-acetoxy-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; bis(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate; bis(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; bis(1-octyloxy-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; bis (1-Acyl-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; bis(1,2,2,6,6-pentamethyl-4-piperidinyl) n-butyl-3,5-di-tert-butyl-4-hydroxybenzylmalonate; 2,4-bis[(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-6-(2-hydroxyethylamino-s-triazine; bis(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)adipate; 2,4-bis[(1-cyclohexyloxy-2,2,6,6-piperidin-4-yl)butylamino]-6- Chloro-s-triazine; 1-(2-hydroxy-2-methylpropoxy)-4-hydroxy-2,2,6,6-tetramethylpiperidine; 1-(2-hydroxy-2-methylpropoxy)-4-oxy-2,2,6,6-tetramethylpiperidine; 1-(2-hydroxy-2-methylpropoxy)-4-octadecanoyloxy-2,2,6,6-tetramethylpiperidine; bis(1-(2-hydroxy-2-methylpropoxy)-2,2,6,6-tetramethylpiperidin-4-yl) sebacate; bis(1-(2-hydroxy-2-methylpropoxy)-2,2,6,6-tetramethylpiperidin-4-yl) adipate ; 2,4-bis{N-[1-(2-hydroxy-2-methylpropoxy)-2,2,6,6-tetramethylpiperidin-4-yl]-N-butylamino}-6-(2-hydroxyethylamino)-s-triazine; 4-benzoyl-2,2,6,6-tetramethylpiperidin; di-(1,2,2,6,6-pentamethylpiperidin-4-yl) p-methoxybenzylidene malonate; 2,2,6,6-tetramethylpiperidin-4-yl octadecanoate; bis(1-octyloxy-2,2,6,6-tetramethylpiperidinyl) succinate; 1,2,2,6,6-pentamethyl-4-aminopiperidin;2-Undecyl-7,7,9,9-tetramethyl-1-oxa-3,8-diaza-4-oxa-spiro[4,5]decane; tris(2,2,6,6-tetramethyl-4-piperidinyl)nitrilotriacetate; tris(2-hydroxy-3-(amino-(2,2,6,6-tetramethylpiperidin-4-yl)propyl)nitrilotriacetate; tetrakis(2,2,6,6-tetramethyl-4-piperidinyl)-1,2,3,4-butane-tetracarboxylate; tetrakis(1,2,2,6,6-pentamethyl-4-piperidinyl)-1,2,3,4-butane-tetracarboxylate; 1,1′-(1,2-ethanediyl)-bis(3,3,5,5-tetramethylpiperazinone); 3-n-octyl-7,7,9,9- Tetramethyl-1,3,8-triazaspiro[4.5]decane-2,4-dione; 8-acetyl-3-dodecyl-7,7,9,9-tetramethyl-1,3,8-triazaspiro[4.5]decane-2,4-dione; 3-dodecyl-1-(2,2,6,6-tetramethyl-4-piperidinyl)pyrrolidinyl-2,5-dione; 3-dodecyl-1-(1,2,2,6,6-pentamethyl-4-piperidinyl)pyrrolidinyl-2,5-dione; N,N′-bis-formyl-N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)hexanediamine; 2,4-bis[(1-cyclohexyloxy-2,2,6,6-piperidin-4-yl)butylamino]-6-chloro-s- Triazine, reaction products with N,N′-bis(3-aminopropyl)ethylenediamine); 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-hydroxypiperidine, condensed with succinic acid; N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-hexanediamine, condensed with 4-tert-octylamino-2,6-dichloro-1,3,5-triazine; N,N′-bis(2,2,6,6-tetramethyl-4-piperidinyl)-hexanediamine, condensed with 4-cyclohexylamino-2,6-dichloro-1,3,5-triazine; N,N′-bis-(2,2,6,6-tetramethyl-4-piperidinyl)-hexanediamine, condensed with 4-morpholinyl-2,6-dichloro-1,3,5-triazine; N,N′- Condensate of bis-(1,2,2,6,6-pentamethyl-4-piperidinyl)hexanediamine and 4-morpholinyl-2,6-dichloro-1,3,5-triazine; Condensate of 2-chloro-4,6-bis(4-n-butylamino-2,2,6,6-tetramethylpiperidinyl)-1,3,5-triazine and 1,2-bis(3-aminopropylamino)ethane; Condensate of 2-chloro-4,6-di-(4-n-butylamino-1,2,2,6,6-pentamethylpiperidinyl)-1,3,5-triazine and 1,2-bis-(3-aminopropylamino)ethane; Reaction products of 7,7,9,9-tetramethyl-2-cycloundecyl-1-oxa-3,8-diaza-4-oxaspiro[4,5]decane and epichlorohydrin;Poly[methyl(3-oxy-(2,2,6,6-tetramethylpiperidin-4-yl)propyl)]siloxane, CAS#182635-99-0; reaction products of maleic anhydride-C18-C22-alpha-olefin-copolymer and 2,2,6,6-tetramethyl-4-aminopiperidine; 4,4′-hexamethylenebis(amino-2,2,6,6-tetramethylpiperidine) and 2-chloro-4,6-bis(dibutylamino)-s-triazine end-capped Oligomeric condensates of 2,4-dichloro-6-[(2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-s-triazine; oligomeric condensates of 4,4′-hexamethylenebis(amino-1,2,2,6,6-pentamethylpiperidine) and 2,4-dichloro-6-[(1,2,2,6,6-pentamethylpiperidin-4-yl)butylamino]-s-triazine end-capped with 2-chloro-4,6-bis(dibutylamino)-s-triazine; 4,4 Oligomeric condensation product of '-hexamethylenebis(amino-1-propoxy-2,2,6,6-tetramethylpiperidine) and 2,4-dichloro-6-[(1-propoxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-s-triazine terminated with 2-chloro-4,6-bis(dibutylamino)-s-triazine; oligomeric condensation product of 4,4'-hexamethylenebis(amino-1-acyloxy-2,2,6,6-tetramethylpiperidine) and 2-chloro-4,6-bis(dibutylamino) ...; oligomeric condensation product of 4,4'-hexamethylenebis(amino-1-acyloxy-2,2,6,6-tetramethylpiperidine) and 2-chloro-4,6-bis(dibutylamino)-s-triazine; oligomeric condensation product of 4,4'-hexamethylenebis(amino-1-acyloxy-2,2,6,6-tetramethylpiperidine Oligomeric condensates of 2,4-dichloro-6-[(1-acyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino]-s-triazine terminated with bis(dibutylamino)-s-triazine; and products obtained by reacting (a) with (b), wherein (a) is the product obtained by reacting 1,2-bis(3-aminopropylamino)ethane with cyanuric chloride, and (b) is (2,2,6,6-tetramethylpiperidin-4-yl)butylamine. Also included are sterically hindered NH, N-methyl, N-methoxy, N-hydroxy, N-propoxy, N-octyloxy, N-cyclohexyloxy, N-acyloxy and N-(2-hydroxy-2-methylpropoxy) analogs of any of the above mentioned compounds. Non-limiting examples of industrial light stabilizers are manufactured by BASF under the trademark; 4050H, 4077H, 4092H, 5062H, 5050H, 4092H, 4077H, 3026, 3027, 3028, 3029, 3033P and 3034 or 622 substances obtained.

[0060] Antistatic agents can be applied to suppress the accumulation of dust on plastic products. Antistatic agents can improve the conductivity of plastic compositions and thus eliminate any surface charge generated during production and use. Therefore, dust particles are less attracted to the surface of plastic products and thus reduce the accumulation of dust. In certain aspects of the present invention, the antistatic agent can be glyceryl monostearate. The antistatic amount included in the polymer blend can be at least, equal to and / or between any two of the following based on the total weight of the polymer blend: 0.01wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% and 1wt%.

[0061] Lubricants can be added to the polymer blend to improve its molding properties. The lubricant can be a low molecular weight compound selected from the following: fatty acids, fatty acid esters, wax esters, fatty alcohol esters, amide waxes, metal carboxylates, montanic acid, montanic acid esters; or a polymer compound such as paraffin or polyethylene wax. In a certain aspect of the present invention, the lubricant is a metal stearate. Non-limiting examples of metal stearates include zinc stearate, calcium stearate, lithium stearate or a combination thereof, preferably calcium stearate. The amount of lubricant contained in the polymer blend can be at least, equal to and / or between any two of the following based on the total weight of the polymer blend: 0.01wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% and 1wt%.

[0062] Antioxidants can prevent polymer degradation during processing. Phosphites are known thermal oxidative stabilizers for polymers and other organic materials. Antioxidants can be phosphite-based antioxidants. In certain aspects, phosphite antioxidants include but are not limited to triphenyl phosphite, diphenyl alkyl phosphites, phenyl dialkyl phosphites, tris(nonylphenyl)phosphites, trilauryl phosphites, tri(octadecyl) phosphites, distearyl pentaerythritol diphosphites, tris(2,4-di-tert-butylphenyl)phosphites, diisodecyl pentaerythritol diphosphites, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphites, tristearoyl sorbitol triphosphites and tetra(2,4-di-tert-butylphenyl)-4,4′-diphenylene diphosphonates, bis(2,4-dicumylphenyl) pentaerythritol diphosphites. The polymer blend may contain an antioxidant in an amount of at least, equal to, and / or between any two of the following based on the total weight of the polymer blend: 0.01 wt%, 02 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, and 0.1 wt%. Non-limiting examples of commercially available antioxidants include Irganox 1010 available from BASF or Doverphos S9228T available from Dover Chemical Company.

[0063] When forming the composition, the described HDPE and main additive components (which may be in the form of granules, powders, fragments or shredded fleece) and any additional optional additives may be dry blended. These materials are mixed in a conventional mixer, where the HDPE and main additives are mixed with optional additional or auxiliary additives. The optional additional additives may be added at the end of or during the processing step to produce a polymer blend. Suitable machines for such mixing are known to those skilled in the art. Non-limiting examples include mixers, kneaders and extruders. These materials are then fed directly into the feed zone of the extruder. In some cases, the method may be implemented in an extruder and the additives may be introduced during processing. Non-limiting examples of suitable extruders include single screw extruders, counter-rotating and co-rotating twin screw extruders, planetary gear extruders, ring extruders or co-kneaders. The method may be implemented at a temperature of 160-300°C.

[0064] In some embodiments, the HDPE and the primary additive and any optional auxiliary additives used to produce the polymer blends of the present invention can be melt extruded by the following typical procedure: weighing the required amount of HDPE and additives, followed by dry blending, and then feeding the mixture to the main feeder of a twin-screw co-rotating extruder (length / diameter (L / D) ratio of 25:1 or 40:1) to obtain the final composition. The HDPE, additives, or blends thereof can be subjected to high temperatures for a sufficient time during the blending process. The blending temperature can be higher than the softening point of the polymer. In some aspects, the extrusion process can be implemented at a temperature of 160-300°C. The primary additive can be added online with other optional additives during the production process before the HDPE resin is pelletized. The amount of additives combined with the HDPE can be adjusted to provide the weights discussed above.

[0065] The optional auxiliary additives may be premixed or added separately to the polymer blend or its different components. As an example, the auxiliary additives of the present invention may be premixed to form a blend before adding them to the HDPE or the primary additive. During mixing and / or incorporation of the additives, the mixture may be subjected to an elevated temperature for a sufficient period of time. For example, the optional auxiliary additives may be added to the polymer resin by mixing the above components using methods commonly used in process technology. The mixing temperature may be higher than the softening point of the polymer. In some aspects, the method may be implemented at a temperature of 160-300°C. This "melt mixing" or "melt compounding" allows the optional additives of the present invention to be uniformly dispersed in the HDPE and / or primary additive.

[0066] Articles (e.g., end caps) made from blends of HDPE and the primary additive may have a higher ESCR than articles made from HDPE without such additives (i.e., the HDPE used to make the blend). In some embodiments, the ESCR values ​​of the articles of the invention are 200% to 2000% higher than HDPE articles of the same structure made using the same HDPE but without the primary additive. The ESCR values ​​may be at least, equal to, and / or between any two of the following: 200%, 300%, 400%, 500%, 600%, 700%, 800%, 900%, 1000%, and 2000% greater than the ESCR values ​​of HDPE without the primary additive. As exemplified in the Examples section and throughout the specification, the ESCR values ​​of articles containing the polymer blends of the present invention may be from at least 20 hours to 2000 hours (e.g., 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 300, 400, 500, 600, 700, 800, 900, 1000, and 2000 and any ranges or values ​​therebetween, including endpoints). In contrast, the ESCR value of HDPE articles without the primary additive may be less than, but not equal to, 20 hours.

[0067] The polymer blend compositions formed as described are usually collected as particles, which can be stored for a period of time or used immediately during the formation process. The formation method can include injection molding, blow molding, compression molding, sheet extrusion, film blowing, pipe extrusion, profile extrusion, calendaring, thermoforming, rotational molding or a combination thereof. For example, the final formed product can be a molded part, a sheet, a film or a fiber. Examples of molded parts include end caps, bottle caps, containers, lids, sheets, pipes, pipe joints, bottles, cups, plates, trays or toys or a combination thereof. The end caps can be injection molded and / or compression molded. The end caps can be threaded end caps or non-threaded end caps for selectively closing the opening of bottles or other containers. Such end caps can be used for various food and non-food applications. For example, the caps comprising the polymer blends of the present invention can be used together with containers for storing carbonated beverages, pressurized beverages, etc.

[0068] The following examples serve to further describe various embodiments and uses.

[0069] Example 1

[0070] The ESCR performance of multimodal HDPE (HDPE-1 and HDPE-2) was improved by using different main additives. The HPDE had a melt flow rate of 0.6-0.8 dg / min at 190°C and 2.16 kg load measured by ISO 1133 method and a density of 953-955 kg / m3 measured by ASTM D1505 or ISO 1872 method. 3 , tensile modulus measured by ISO 527-2 is 1100-1200MPa, yield tensile strength measured by ISO 527 1&2 is 20-28MPa, izod notched impact strength measured by ISO 180 / A at 23°C is 8-12kJ / m 2 Charpy impact strength measured at 23°C according to ISO 179 is 8-10 kJ / m 2 .

[0071] The HDPE-1 and HDPE-2 used include Experimental grade multimodal HDPE and INEOS CAP 602 multimodal HDPE. The main additives include Septon TM The obtained hydrogenated styrene block copolymer of styrene-ethylene-ethylene-propylene-styrene (SEEPS) was produced by Kraton Polymers as Kraton D TM Styrene-isoprene-styrene (SIS) is obtained from SABIC as Lexan TM Polycarbonate-siloxane copolymer obtained from resin, Clariant as 20000S high molecular weight polyethylene oxide and EI du Pont de Nemours and Company as Ionomerized ethylene copolymers obtained from ionomerized resins. The applied multimodal HDPE is formulated with a total amount of 0.1-0.5 wt% of main additives, which can be used alone or as a mixture of the above main additives, with and without other optional additives. The additives are dry mixed with multimodal HDPE particles in a plastic bag. For comparison, pure multimodal HDPE without any main additives is also tested. The different mixtures are fed into the hopper of a ZSK-25mm 6-barrel twin-screw extruder with a L / D ratio of 25:1. The applied operating parameters are described in Table 1 below:

[0072] Table 1

[0073] Cylinder-1 (connected to hopper) Temperature = 160°C Cylinder-2 Temperature = 185°C Cylinder-3 Temperature = 195°C Cylinder-4 Temperature = 195°C Cylinder-5 Temperature = 200°C Cylinder-6 (die head) Temperature = 210°C Screw speed 250rpm Feed rate 8Kg / hr Batch size 1000g

[0074] The torque measured during melt extrusion of pure HDPE and HDPE formulated with additives was 33-40%, indicating that the addition of ESCR reinforcing main additives did not significantly impair the processing properties of HDPE.

[0075] Example 2

[0076] The pellets obtained after melt extrusion of Example 1 were compression molded into 1.85-1.95 mm thick sheets at a temperature of 195-210° C., with a holding time of 5 min and a cooling time of 5 min. No obvious visual inhomogeneity was seen in the compression molded sheets. The ESCR properties of the compression molded sheets of pure HDPE and formulated HDPE were then evaluated according to ASTM D1693-15B method (Bell test).

[0077] The compression molded sheets were cut into test specimens of 38 mm in length and 13 mm in width. A notch of 0.5 mm in depth was formed at the center of each test specimen before each specimen was stored in a conditioning environment at 23°C and 55% relative humidity. The conditioned specimens were U-bent with the aid of a clamp. For pure HDPE material and formulated HDPE material, 10 bent specimens were placed in an aluminum sample holder and subsequently placed in a test tube filled with an aqueous solution of 10 v / v% Igepol CO-630 (nonylphenoxy poly(ethylene oxide) ethanol, CAS 68412-54-4). The mouth of the test tube was closed with a rubber stopper wrapped in aluminum foil. The specimens placed in the test tube filled with the aqueous solution of Igepol CO-630 were immersed in a silicone oil bath maintained at 50°C. The time for crack formation in the observed specimens was recorded regularly. According to the records, the time taken for 50% of the specimens (i.e., 5 out of 10 specimens) to fail (i.e., crack) can be inferred from the ESCR performance of a given composition.

[0078] Table 2 gives the ESCR properties of pure multimodal HDPE and formulated multimodal HDPE with combined additives:

[0079] Table 2

[0080]

[0081] As can be seen in Table 2, the observed time to 50% sample failure is ~150 and ~470 h for neat HDPE-1 and HDPE-2 respectively. For those multimodal HDPE compositions incorporating ~0.5 wt% of a single primary additive or a mixture of primary additives, the time to 50% sample failure was found to increase by a factor of 2-3.

[0082] The melt flow rate (MFR) of the multimodal HDPE-1 resin (Comparative Sample-1) measured at 190°C with a load of 2.16, 5 and 21.6 Kg according to the ISO 1133-1:2011 method is ~0.8, ~2.8 and ~45 dg / min, respectively. In comparison, the melt flow rate (MFR) of the multimodal HDPE-1 resin (Working Sample-1) incorporating the additive mixture measured at 190°C with a load of 2.16, 5 and 21.6 Kg according to the ISO 1133-1:2011 method is ~0.8, ~2.3 and ~47 dg / min, respectively. These results show that the melt viscosity / flow characteristics of HDPE are hardly affected by the addition of a small amount of the additive mixture. Similarly, the melt flow rate (MFR) of the multimodal HDPE-2 resin (Comparative Sample-2) measured at 190°C with a load of 2.16, 5 and 21.6 Kg according to the ISO 1133-1:2011 method is ~0.7, ~2.6 and ~40 dg / min, respectively. In comparison, the melt flow rate (MFR) of the multimodal HDPE-2 resin (Working Sample-3) incorporating the additive mixture measured at 190°C with a load of 2.16, 5 and 21.6 Kg according to the ISO 1133-1:2011 method is ~0.7, ~2.5 and ~39 dg / min, respectively. These results show that the melt viscosity / flow characteristics of HDPE are hardly affected by the addition of a small amount of a single main additive or a main additive mixture.

[0083] Adding a small amount of a single main additive or a mixture of main additives, the mechanical properties of HDPE-2, such as ~145kJ / m 2 Izod notch impact, ~17kJ / m 2 The Charpy notched impact, tensile modulus of 900 MPa and yield stress of 22 MPa are almost unaffected. Similarly, the strain hardening modulus of pure HDPE-2 of 17 MPa is almost unaffected by adding a small amount of a single main additive or a main additive mixture.

Claims

1. A polyethylene composition with enhanced environmental stress cracking resistance, the composition comprising a polymer melt blend of a multimodal high density polyethylene (HDPE) and a combination of the following additives: a polyethylene glycol (PEG) having an average molecular weight Mw of 2000-40,000 and a random block copolymer having an average molecular weight Mw of 250,000-450,000 comprising two different saturated alkane blocks between two aromatic blocks, wherein the random block copolymer is used as a main additive and is present in the polymer melt blend in an amount of 0.01-0.5 wt% based on the weight of the polymer melt blend, and the additive combination is present in the polymer melt blend in an amount of 0.15-0.6 wt% based on the weight of the polymer melt blend.

2. The composition of claim 1, wherein the additive is present in an amount of 0.15 to 0.5 wt % based on the weight of the polymer melt blend.

3. The composition of claim 1, wherein the HDPE has at least one of the following properties: The melt flow ratio at 190°C and 2.16Kg is 0.3-6.0; A melt flow rate of 3-70 dg / min at 190°C and 21.6 kg; and Density is 945-965Kg / m 3 , Wherein the melt flow ratio is determined according to ISO 1133-1 (2011) and the density is determined according to ASTM D792 (2013).

4. The composition of any one of claims 1 to 3, wherein the HDPE has a dispersion index (PDI), ie, Mw / Mn, of 8 to 30 as measured by high temperature gel permeation chromatography.

5. The composition of any one of claims 1 to 3, wherein the HDPE is selected from C3-C 10 A copolymer of a comonomer of an olefin monomer, said comonomer being present in said HDPE copolymer in an amount of 2 wt% or less.

6. The composition of any of claims 1-3, wherein the polymer melt blend provides a molded article having an ESCR of at least 40 hours as measured by ASTM D1693-15B.

7. The composition of any one of claims 1 to 3, wherein the polymer melt blend provides a molded article having an ESCR of 30 to 1000 hours as measured by ASTM D1693-15B.

8. The composition of any one of claims 1-3, wherein the polyethylene glycol PEG has the following properties: The average molecular weight Mw is 5000-20,000.

9. The composition of any one of claims 1 to 3, wherein the random block copolymer comprising two different saturated alkane blocks between two aromatic hydrocarbon blocks has at least one of the following properties: At least one of the two different saturated alkane blocks is branched; The random block copolymer is a styrene-(2-methylbutane)-butane-styrene random block copolymer; The random block copolymer has an average molecular weight of 275,000 to 425,000 according to polystyrene standards and a dispersion index PDI, i.e., Mw / Mn, of 0.9 to 1.2 as determined by gel permeation chromatography; and The random block copolymer is a hydrogenated styrene-isoprene-butane block polymer.

10. The composition of any one of claims 1-3, further comprising at least one of the following additional additives: nucleating agents, thermal conductive agents, binders, anti-caking agents, antistatic agents, antioxidants, neutralizers, acid scavengers, foaming agents, dyes, flame retardants, pigments, processing aids, reinforcing agents, stabilizers, clarifying agents, slip agents, ionic additives, and combinations thereof.

11. The composition of any one of claims 1 to 3, further comprising at least one additional additive selected from the group consisting of a crystallization aid, a mold release agent, an oil, a flow modifier, a filler, an impact modifier, an anti-UV agent, and combinations thereof.

12. The composition of any one of claims 1-3, wherein the polymer melt blend is formed into an article of manufacture, wherein the article is at least one of a film, a molded part, a container, a lid, a sheet, a pipe, a fitting, a pallet, and a toy.

13. The composition of any one of claims 1-3, wherein the polymer melt blend is formed into an article of manufacture, wherein the article is at least one of: a bottle, a cup, a tray, and a beverage container lid.

14. The composition of claim 12, wherein the article is formed by at least one of the following methods: injection molding, blow molding, compression molding, and profile extrusion.

15. The composition of claim 12, wherein the article is formed by at least one of the following processes: sheet extrusion, film blowing, pipe extrusion, and calendaring.

16. The composition of claim 12, wherein the article is formed by thermoforming.

17. A method of forming a polyethylene composition having enhanced environmental stress cracking resistance, the method comprising: The multimodal high density polyethylene HDPE is modified by melt blending the multimodal HDPE with a combination of polyethylene glycol PEG having an average molecular weight Mw of 2000-40,000 and a random block copolymer comprising two different saturated alkane blocks between two aromatic blocks having an average molecular weight Mw of 250,000-450,000, wherein the random block copolymer is used as a main additive and is present in the polymer melt blend in an amount of 0.01-0.5 wt% based on the weight of the polymer melt blend, and the additive combination is present in the polymer melt blend in an amount of 0.15-0.6 wt% based on the weight of the polymer melt blend.