Heads-up display mirror with improved surface and edge quality and method of forming the same
By using curved mirror substrates made of high-precision glass or glass-ceramic materials, the problem of insufficient optical quality of the HUD system is solved and image clarity and safety are improved.
Patent Information
- Application Number
- CN201980086983.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-11-27
- Filing Date
- 2019-11-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-11-25
AI Technical Summary
The optical quality of the HUD system is poor, resulting in blurred projected images, affecting the user's information processing time and reaction speed, and reducing driver safety.
Using a curved mirror substrate made of glass or glass ceramic materials, with concave and convex surfaces, surface roughness less than 30nm, edges not cut, shaped or polished, manufactured by vacuum forming method to ensure high precision and high quality mirrors substrate.
It improves the optical quality of the HUD system, enhances the clarity and aesthetic effect of the projected image, and improves the user's information processing efficiency and the driver's safety.
Smart Images

Figure CN113227881B_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority under 35 USC §119 to U.S. Provisional Application Serial No. 62 / 771,877, filed on November 27, 2018, the contents of which are the basis of the present application and are incorporated herein by reference in their entirety. Background Art
[0002] A head-up display (HUD) system projects visual information onto a transparent surface so that the user can see the information without moving their eyes away from their primary field of view. HUD systems are increasingly being deployed in the transportation sector, including for use in automobiles, aircraft, ships, and other vehicles. For example, a HUD system is used in a vehicle so that the operator or driver of the vehicle can see information related to the operation of the vehicle and maintain a forward line of sight without looking down or toward a display screen. Therefore, HUD systems are believed to improve safety by minimizing the need for the vehicle driver to move away from a safe operating viewpoint.
[0003] Disclosure of the technical problem of the present invention
[0004] However, HUD systems typically have poor optical quality in projected images, which may result in the aesthetic quality of the projected images being less than ideal. Poor optical quality may even reduce the safety of the HUD system, because blurred or unclear projected images make it more difficult for users to read or understand the projected information, resulting in increased processing time for the user to process the information, delayed reaction time based on the information, and easy distraction of the user. HUD systems typically use mirrors to reflect and project images onto transparent surfaces, and imperfections in the reflectors used in HUD systems can lead to reduced optical quality. For example, imperfections in the accuracy of the mirror surface or shape due to poor durability or manufacturing defects can reduce optical performance. These imperfections include inaccuracies in the shape of the curvature of the mirror caused by surface and / or edge imperfections during the forming and / or bending of the mirror or due to cutting, forming and / or polishing the edges of the mirror or mirror substrate.
[0005] Therefore, there remains a need for HUD systems with improved optical quality, and more particularly for improved mirrors for HUD systems.
[0006] Solution to the problem
[0007] In some embodiments of the present disclosure, a head-up display (HUD) mirror substrate is provided. The mirror substrate has a first main surface, a second main surface and a secondary surface, the first main surface has a concave shape, the second main surface is opposite to the first main surface and has a convex shape, and the secondary surface connects the first main surface and the second main surface. The mirror substrate includes a glass or glass ceramic material, and the first main surface has a first surface roughness Ra of 3nm or less and a peak-to-valley (PV) roughness of less than 30nm. In some aspects of the embodiments, when the mirror substrate is in a bent state, the mirror substrate has an edge that is not cut, formed, chamfered or polished. The secondary surface may have a cross-sectional edge profile including a chamfer, and the chamfer includes a C-shaped chamfer or an R-shaped chamfer. The length of the C-shaped chamfer may be 0.1mm or greater, or 0.3mm or greater. The length of the R-shaped chamfer may be 0.5mm or greater. In one aspect of the embodiment, the mirror substrate in a plan view has a rounded corner, and when the mirror substrate is in a bent state, the rounded corner is not formed or polished. According to some embodiments, the concave surface of the mirror substrate has an aspherical shape.
[0008] The HUD mirror substrate of the embodiments herein may have a length of about 200 mm to about 400 mm and a width of about 100 mm to about 250 mm; a length of about 250 mm to about 350 mm and a width of about 100 mm to about 200 mm; a length of about 300 mm to about 350 mm and a width of about 150 mm to about 200 mm; or a length of about 290 mm to about 295 mm and a width of about 130 mm to about 135 mm. As aspects of some embodiments, the profile peak-to-valley (PV) shape accuracy on the concave surface of the mirror substrate is less than 100 μm or less than 50 μm, the arithmetic mean waviness Wa on the concave surface is less than 1 μm per 10 mm, and the surface roughness Ra of the convex surface is less than 30 nm, and the peak-to-valley (PV) roughness is less than 1 μm, or the surface roughness Ra is less than 20 nm, and the peak-to-valley (PV) roughness is less than 300 nm. As an aspect of some embodiments, the thickness of the mirror substrate is defined as the distance between the first major surface and the second major surface, and the thickness is less than or equal to about 3.0 mm, about 0.5 mm to about 3.0 mm, about 0.5 mm to about 1.0 mm, or about 1.0 mm to about 3.0 mm. The glass or glass ceramic material may include soda lime glass, aluminosilicate, boroaluminosilicate or alkali metal aluminosilicate glass, and may be a strengthened or chemically strengthened glass material.
[0009] In some embodiments of the present disclosure, a three-dimensional HUD mirror is provided. The HUD mirror comprises a HUD mirror substrate of the embodiments disclosed herein and a reflective layer disposed on a first major surface of the mirror substrate.
[0010] In other embodiments of the present disclosure, a method for forming a three-dimensional mirror is provided. The method includes providing a mirror preform, the mirror preform having a first main surface, a second main surface opposite to the first main surface, and a secondary surface connecting the first main surface and the second main surface. The mirror preform is a glass or glass ceramic material, and the first main surface and the second main surface are two-dimensional. The method further includes: placing the mirror preform on a molding device having a curved support surface so that the second main surface is facing the curved support surface; and conforming the mirror preform to the curved support surface to form a curved mirror substrate having a convex surface corresponding to the second main surface and a concave surface corresponding to the first main surface, the concave surface having a first radius of curvature. After the conforming step, the concave surface has a roughness Ra of less than 3nm and a peak-to-valley (PV) roughness of less than 30nm. As an aspect of some embodiments, the curved mirror substrate has an edge that is not cut, shaped, chamfered or polished during or after the conforming step. More particularly, according to some embodiments, the cross-sectional edge profile of the secondary surface is the same as the cross-sectional edge profile of the curved mirror substrate.
[0011] In aspects of some embodiments, the method further comprises processing a sub-surface of the two-dimensional mirror preform to achieve a predetermined edge profile of the curved mirror substrate, wherein the processing comprises at least one of cutting, chamfering or polishing.
[0012] In some embodiments of the present disclosure, a method for forming a three-dimensional mirror is provided, which comprises: forming a three-dimensional mirror substrate according to the method disclosed herein and disposing a reflective layer on a first major surface of the substrate.
[0013] Other features and advantages of the claimed object will be set forth in the following detailed description, and some features and advantages will be apparent to those skilled in the art from that description, or may be recognized by practicing the claimed object as described herein (including the following detailed description, claims, and accompanying drawings).
[0014] It should be understood that both the above summary and the following detailed description present embodiments of the present disclosure and are intended to provide an overview or framework for understanding the nature and characteristics of the claimed object. The accompanying drawings are included to provide a further understanding of the present disclosure, and the accompanying drawings are incorporated into and constitute a part of this specification. The drawings illustrate various embodiments and can explain the principles and operation of the claimed object together with the embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] For purposes of illustration, there is shown in the drawings a form that is presently preferred, but it is to be understood that the embodiments disclosed and discussed herein are not limited to the precise arrangements and instrumentalities shown.
[0016] Figure 1 is a schematic diagram of a HUD system in a vehicle according to some embodiments of the present disclosure.
[0017] Figure 2 According to some embodiments, the use Figure 1 Illustration of the car driver's viewpoint when using a HUD system.
[0018] Figure 3 is an illustration of a car driver's viewpoint when using a HUD system with a combiner according to some embodiments.
[0019] Figure 4 is an illustration of an aspheric mirror for a HUD system according to some embodiments.
[0020] Figure 5 The steps of a conventional method of forming a HUD mirror or mirror substrate are illustrated.
[0021] Figure 6 This is a plan view of the sheet material of the HUD mirror substrate being cut.
[0022] Figure 7 is a cross section of a cut HUD mirror substrate having an edge profile with chamfers.
[0023] Figure 8 is a photograph of the edge of a mirror substrate formed according to a conventional method.
[0024] Fig.9A and Fig. 9B They are Figure 8 Magnified view of the convex and concave surfaces of the mirror substrate.
[0025] FIG. 10A to FIG. 10D is a microscope image of a rough edge of a mirror substrate formed according to a conventional method.
[0026] Fig.11 The steps of a method of forming a HUD mirror or mirror substrate according to an embodiment of the present disclosure are illustrated.
[0027] Fig. 12A and Fig. 12B is a plan view of a HUD mirror preform according to an embodiment of the present disclosure.
[0028] Fig.13 yes Fig. 12B A cross-sectional view of the edge of the mirror preform at line segment 13'-13'.
[0029] Fig.14 is a microscope image of an edge of a HUD mirror substrate formed by a method according to an embodiment of the present disclosure.
[0030] FIG. 15A to FIG. 15C is a microscope image of the edge of a HUD mirror substrate formed according to the method of the present disclosure.
[0031] Fig.16 is a plan view of a vacuum forming surface for forming a two-dimensional substrate into a three-dimensional substrate according to some embodiments of the present disclosure. DETAILED DESCRIPTION
[0032] HUD systems can be used to provide a variety of information to improve the safety and convenience of HUD users. For example, in transportation, information related to vehicle operation (e.g., vehicle metering or navigation) can be projected to the area in front of the driver. This can include real-time information about vehicle speed, fuel level, climate control settings, entertainment settings, turn-by-turn navigation indicators, estimated arrival time, and alerts related to speed, traffic, or dangerous conditions. The information can be represented as text, symbols, pictures, videos, animations, and one or more colors. It is also desirable to have a HUD system including an augmented reality (AR) function to present information related to the current external environment of the vehicle, and from the user's perspective, such information can overlap or otherwise interact with those related external environment elements. For example, when a user approaches a point of interest, an AR HUD image can highlight the point of interest. Since AR HUD can display information that overlaps or interacts with the information seen by the user, a larger projected image is more advantageous. However, since it is difficult to produce a mirror or optical component of the right size for projecting a larger AR HUD image, a larger image may be more difficult to produce. It is believed that as vehicles become more interconnected and intelligent, the use and application frequency of these HUD systems will increase. Therefore, the above are merely examples of HUD system usage, and implementations of the present disclosure are not intended to be limited to these examples.
[0033] like Figure 1 As shown, the HUD system 100 may be disposed in a vehicle V, which may be, for example, a car operated by a driver D. For example, the HUD system 100 may be built into the vehicle itself, wherein Figure 1 As shown, all or some portion is incorporated into a dashboard 110 of a vehicle V. The HUD system 100 includes a picture generation unit (PGU) 102 connected to a display 103, which is configured to generate an image based on a signal from the PGU 102. The image is then directed from the display 103 to an area viewable by a user (e.g., an area of a windshield 108 or other surface) in one or other manner. Figure 1, the image is reflected by the flat mirror 104 to the curved mirror 106. The image is projected from the curved mirror 106 toward the windshield 108 and onto a projection area 112 of the windshield 108. The HUD system 100 may be configured such that the projection area 112 is within the normal line of sight of the driver D when driving the vehicle V, or within a predetermined area suitable for viewing when driving the vehicle V. For example, the projection area 112 may be positioned such that the projected image is overlaid on the road from the driver's perspective. Figure 2 The icon of shows an example of this, where the dashed line defines the invisible projection area 112 and the image is projected into the invisible projection area 112 on the windshield 108 .
[0034] The display may include a cathode ray tube (CRT) display, a light emitting diode (LED) display, a liquid crystal display (LCD) assembly, a laser projection system, a waveguide display, or other types of displays known to those skilled in the art. The PGU may include a computer or processor for generating or processing images produced by the display. For example, the optical components may include some combination of lenses, beam splitters, mirrors, and combiners, and these components are not limited to the HUD system design. Figure 1 Example shown. The combination of components of the HUD system can be configured to produce collimated light. The collimated light is projected onto a surface or combiner in the user's field of view so that the user can see the projected image and the general field of view simultaneously. For example, in a vehicle application, the combiner can be a windshield. Alternatively, the combiner can be a separate component built into the vehicle, or can be a portable component that can be installed in the vehicle at a location where the driver or passenger can see the projected image on a transparent surface of the combiner.
[0035] although Figure 1 and Figure 2 The projection area 112 is located on the windshield 108, but Figure 3 An alternative embodiment is illustrated in which a combiner 208 for projection area 212 is separate from the windshield and positioned between the windshield and the driver. The combiner 208 can be built into the dashboard 210 of the vehicle, or can be a portable or detachable component positioned on top of the dashboard 210. Those skilled in the art will understand the basic arrangement of components in a HUD system, and thus embodiments of the present disclosure are not limited to any one or more HUD systems or a particular arrangement of optical components of a HUD system. The present disclosure is primarily directed to curved or three-dimensional mirrors for HUD systems or mirror substrates for forming three-dimensional HUD mirrors and methods of forming and shaping the same. A three-dimensional (3D) mirror in a HUD system (e.g., Figure 1The curved mirror 106 in the figure is composed of some type of mirror substrate, which is usually made of plastic material. The embodiments of the present disclosure are mainly directed to mirror substrates made of glass or glass ceramic materials, although aspects of some embodiments are relevant to mirror substrates of various other materials. The 3D mirror can have a reflective coating on the concave surface of the substrate. The curved substrate can be spherical, aspherical, Fresnel-shaped and / or diffractive. In a preferred embodiment, the reflective surface or coating is disposed on the concave aspherical surface. The aspherical surface has multiple radii of curvature. For example, in the case of a four-sided aspherical mirror, the aspherical surface can have a different radius of curvature along each of the four edges. Therefore, as Figure 4 As shown, the mirror 300 has a reflective surface 308, which is shaped as an aspherical surface with a radius of curvature R1 along a first edge, a radius of curvature R2 along a second edge, a radius of curvature R3 along a third edge, and a radius of curvature R4 along a fourth edge. Because the surface 308 is an aspherical surface, R1≠R2≠R3≠R4. Figure 4 Also illustrated is how different points on the curved surface 308 are displaced by varying amounts a to e relative to a two-dimensional plane connecting the four corners of the reflector 300. This plane may be a reference plane representing the two-dimensional mirror substrate prior to being formed into the three-dimensional shape shown. In some embodiments, a HUD mirror is provided where a≠b≠c≠d.
[0036] However, the curved mirrors for HUD systems and the methods of forming these mirrors can be improved in terms of the resulting shape accuracy and the surface and edge quality of the mirror. For example, in order to prevent a decrease in image quality when an image is reflected by a curved mirror, the mirror should have a high level of shape accuracy and surface roughness. In an embodiment of the present disclosure, a shape accuracy of less than 50 μm and a surface roughness (Ra) of less than 3 nm are achieved. A special type of optical distortion that occurs in the mirrors of a HUD system is referred to as edge distortion, i.e., optical distortion of light reflected at or near the edge of the mirror. In existing HUD systems, optically influential imperfections may be introduced into the mirror during the manufacture or forming of the mirror. This includes the most common methods of forming 3D-shaped mirrors or mirror substrates, which can be divided into two categories: press forming methods and vacuum forming methods. However, both press and vacuum forming methods may have disadvantages.
[0037] In the pressing forming method, an upper mold and a lower mold are used to press a substrate (e.g., a glass substrate) by physical force. For example, the upper mold can be pressed into the lower mold, wherein the 2D glass preform is arranged between the two molds, and the glass preform is formed according to the shape of the surface on one or both molds. Therefore, the mold imprint may remain on the concave and convex surfaces of the formed glass substrate, which then needs to be polished. In addition, due to the deviation in the profile of the upper mold and the lower mold, it may be difficult to accurately match the profile of the upper mold and the lower mold, so it is difficult for the formed glass substrate to obtain an accurate shape. For example, the specification of the spherical mirror profile can be less than ±25μm, while the mold profile deviation after processing is typically 30 to 50μm.
[0038] In the vacuum forming method, a single mold (e.g., a lower mold) can be used, wherein vacuum holes are formed on the surface of the mold. A flat or two-dimensional (2D) glass plate is placed on the surface of the mold, and vacuum pressure is supplied via the vacuum holes to conform the glass to the curved or three-dimensional (3D) surface of the mold. The vacuum surface is usually formed of a ceramic material, and holes are present on the entire forming surface. However, it is difficult to avoid forming vacuum hole marks on the surface of the formed glass substrate. These vacuum hole marks or manufacturing errors can damage the optical properties of the substrate or the final mirror. In addition, compared to the pressing method, a typical vacuum forming method may require a higher forming temperature. A higher forming temperature may affect the surface quality and form defects (e.g., dents, pits, and embossing).
[0039] Reference Figure 5 and Figure 6 , conventional methods use the oversized two-dimensional substrate 350 provided in step S1 in a 3D forming process (press forming or vacuum forming bending process). As used herein, "oversized" means that the length and / or width of the 2D substrate material is greater than the size required for the final 3D HUD mirror. As described below, using an oversized substrate means that the oversized substrate must then be cut into a smaller size to form the final 3D mirror. In step S2, the oversized 2D substrate 350 is formed into a three-dimensional shape. Then, in step S3, the resulting oversized and curved substrate material is cut along the defined path 352 to obtain a 3D mirror substrate 354 of the desired size, and the external waste glass 356 can be discarded. In addition, after cutting, additional surface and edge processing including shaping, chamfering and / or polishing can be performed in step S4. Edge processing after cutting may be necessary to repair or minimize defects caused by the cutting itself or to shape the cut edge into the desired contour shape. Figure 7An example of a typical chamfer at the edge of a 3D HUD mirror 360 is illustrated, wherein a chamfer 362 is provided on a first major surface 363 of the 3D HUD mirror 360 , and a chamfer 364 is provided on a second major surface 364 of the 3D HUD mirror 360 .
[0040] However, since the oversized substrate has been formed into a 3D shape when cutting, it is very difficult to cut the oversized substrate into the size of a 3D mirror. Therefore, due to the difficulty in cutting the 3D surface, it may be difficult to cut into the exact shape and size desired by the final product. This move results in a relatively large change in the product size of the final product. In addition, due to the 3D shape of the aspherical mirror, the edge cannot be easily polished or chamfered using a standard wheel polishing method, but must rely on complex, slow and expensive computer numerical control (CNC) chamfering. Due to chamfering along the 3D curved edge, it is difficult to maintain a constant chamfering quality. For the same reason, it is difficult to finish the corners of the mirror. For example, due to aesthetic purposes or improved durability and handling, it may be necessary to form the corner 358 of the 3D mirror (when viewed in a plan view) into a rounded shape. However, due to the difficulty in finishing the corners of the 3D substrate, straight line cutting corners or chamfering are usually applied.
[0041] Figure 8 is a micrograph of a glass sheet 400 viewed from a side view. The glass sheet 400 has been formed into a 3D shape having a convex side 402, a concave side 404, and an edge surface 406. Fig.9A and Fig. 9B As shown, the thickness t1 of the glass sheet is 1.71 mm, and after edge polishing, both the convex side and the concave side have chamfers C x and C v . Chamfer C x and C y Created by grinding a rough edge. In this example, chamfer C x and C v The thicknesses of the C-shaped chamfers are t2 and t3, respectively, and are both 0.06 mm in the samples shown. Since the rough edge grinding is performed on the 3D formed substrate, the quality of the chamfer is obviously rough and inconsistent, and causes the glass at the edge to break. In addition, it is very difficult to achieve a C-shaped chamfer of 0.1 mm or more according to conventional methods. Defects may impair performance and reduce the structural integrity of the glass sheet 400.
[0042] exist FIG. 10A to FIG. 10D The rough quality of the edge of this conventional formation method can be more clearly seen in the micrograph image of FIG. More specifically, Fig. 10A Shown is a side view of a glass sheet 410 having a rough edge 412 as a result of being cut from an oversized 3D sheet. Fig. 10BAnother portion of the edge of the glass sheet is shown with a chip 414 visible in the edge. Fig. 10C In FIG. 4 , a plan view of the surface of the glass sheet near the edge shows non-uniform edge quality as evidenced by the variation in dark and light areas at edge 416. Fig. 10D As shown, because it is difficult to create controlled rounded corners on a 3D glass substrate, a linear corner cut 418 is used to cut the corners of the glass sheet 410.
[0043] However, according to an embodiment of the present disclosure, chamfering, polishing and / or edge forming are performed on a 2D mirror preform. As used herein, "preform" refers to a basic two-dimensional mirror substrate before 3D forming (e.g., vacuum forming), and the size of the preform is pre-cut or formed to be the desired size of a 3D mirror after 3D forming. Therefore, when the preform is in a 2D state, the edges of the preform can be easily and effectively chamfered, polished, or formed. After these edge finishing steps, vacuum forming can be performed on the mirror preform. Therefore, once the mirror substrate is in a 3D state, edge finishing (chamfering, polishing, or forming) is not required. In addition, the length and width of the 2D preform can be sized to take into account some losses of the substrate when it is formed into a 3D substrate.
[0044] Therefore, using an oversized glass substrate for forming requires an additional step of cutting the glass after forming; glass utilization is low due to trimmed glass or waste glass after forming; difficult and relatively ineffective edge polishing and / or chamfering is required after cutting; and larger equipment is required even though the size of the final end product may be the same as that of preform-type forming. On the other hand, in 3D forming of a mirror preform using an embodiment of the present disclosure, there is no need to cut the mirror substrate after vacuum forming, and the generation of waste glass or broken glass is reduced. In addition, preform-type forming can be a simpler process, more cost-effective, and can produce 3D mirrors of excellent quality (more specifically, surface edge quality, roughness, and dimensional stability).
[0045] Fig.11Describe the steps in the above method according to one or more embodiments of the present disclosure. In step S11, a substrate material (e.g., a glass sheet) is provided. The 2D substrate material is cut or resized to approximately the size of the final 3D mirror to solve the problem of slightly reduced lateral dimensions of the preform after 3D formation, and a 2D mirror preform is formed. In step S12, any surface or edge processing (e.g., edge forming, chamfering and / or polishing) is performed on the 2D mirror preform before forming (e.g., vacuum forming) in the 3D mirror substrate. In step S13, after completing the surface and / or edge processing, the 2D mirror preform is formed into a 3D mirror substrate. After step S13, no additional edge processing (e.g., edge forming, chamfering, cornering or polishing) is performed. A reflective coating may be deposited on the recessed surface before or after 3D formation.
[0046] As described above, by using a 2D preform to build a 3D mirror substrate, the size of the resulting 3D mirror can be achieved with very high accuracy and very little variation. In one or more embodiments, a dimensional tolerance of ±0.1 mm is possible, regardless of the curvature complexity or product size of the 3D mirror. For example, the variation in the length and width dimensions of the large mirror substrate produced is less than 0.05 mm, wherein the length of the substrate is about 291 mm and the width is about 130.5 mm. In one or more embodiments, the shape accuracy measured by the profile PV or profile deviation is less than or equal to 50 μm for a HUD mirror substrate having a horizontal dimension of less than about 250 mm, and less than or equal to about 100 μm for a HUD mirror substrate having a horizontal dimension of less than about 350 mm. Therefore, even for larger HUD mirrors, dimensional consistency can be maintained while maintaining the edge quality of the 2D preform. For example, the length of the HUD mirror substrate included in the embodiments of the present disclosure is about 200 mm or more, about 250 mm or more, about 300 mm or more, or about 350 mm or more. The width of the HUD mirror substrate may be about 100 mm or more, about 150 mm or more, or about 200 mm or more. In some specific embodiments, the HUD mirror substrate may have a length of about 350 mm or more and a width of about 200 mm or more.
[0047] Fig. 12A and Fig. 12B FIG. 2 is a plan view of a 2D mirror preform according to some embodiments of the present disclosure. Fig. 12A As shown, the mirror preform 500 has rounded corners 501, which, as mentioned above, are easier to achieve on a 2D preform than on a 3D mirror substrate. Fig. 12BA similar mirror preform 502 is shown, but with a pair of opposing rounded rather than straight edges 503. These rounded edges 503 may be advantageous in a method of vacuum forming a 2D mirror preform, where the rounded edges 503 correspond to the curvature of the vacuum mold so that vacuum pressure does not leak between the rounded edges 503 and the vacuum mold surface.
[0048] Fig.13 It is along Fig. 12A A partial cross-sectional view of the mirror preform 500 taken along line 13'-13' in FIG. Fig.13 As shown, the HUD mirror preform 500 has a first major surface 504 as the mirror side of the preform, a second major surface 506 opposite to the first major surface 504, and a minor surface 508 between the first major surface 504 and the second major surface 506. The thickness t of the mirror preform 500 is defined as the distance between the first major surface 504 and the second major surface 506. The edges of the first major surface 504 and the second major surface 506 have a first chamfer 510 and a second chamfer 512, respectively. According to various embodiments of the present disclosure, the first chamfer 510 and the second chamfer 512 may be symmetrical, meaning having equal lengths, or may be asymmetrical in the case where one chamfer is longer than the other.
[0049] The geometry of the first chamfer 510 and the second chamfer 512 can be described by the x and y components of the chamfered surface. The x component used herein refers to the distance measured in the direction parallel to the first main surface or the second main surface of the two-dimensional preform. The y component refers to the distance measured in the direction perpendicular to the first main surface or the second main surface of the two-dimensional preform or parallel to the secondary surface of the two-dimensional preform. For example, the first chamfer 510 can have an x component x1 and a y component y1, and the second chamfer 512 can have an x component x2 and a y component y2. The size range of x1, y1, x2 and y2 can be from about 0.2 to about 0.3mm, for example, wherein x1 is the same as x2, and y1 is the same as y2, resulting in a symmetrical chamfer. However, the chamfer can also be asymmetrical. For example, one of the chamfers 510 and 512 can be a larger chamfer with a larger x or y component.
[0050] According to some embodiments, the asymmetric chamfer of the edge of the substrate can lead to improved formability and reduce the visibility of the distorted image reflected by the edge of the mirror. In the case of edge distortion, the reflection angle of the displayed image changes due to the inclination of the chamfered surface, and the user can be prevented from seeing the distorted image. This can produce a projected image with no perceived edge distortion. Since the chamfer is large, it is believed that the formability of the edge can be improved by reducing the thickness of the edge area, so that the formability of the edge area is higher. For example, when the same vacuum pressure is used, the edge profile deviation relative to the computer-aided design (CAD) model is reduced compared to the symmetrical edge, and the profile accuracy of the asymmetric edge is increased. This improvement in profile accuracy reduces image distortion. In addition, the asymmetric chamfer can help prevent unwanted or dangerous light from entering the edge of the glass and guide the eyes of the user toward the HUD system. Such unwanted light may include, for example, sunlight, which may distract the driver's attention or interfere with vision. However, in some embodiments, symmetrical chamfers may be preferred.
[0051] Fig.14 A microscope image of a side view of a 3D mirror substrate 600 according to an embodiment of the present disclosure is shown. The 3D mirror substrate 600 has a first major surface 602 having a concave surface and a C-shaped chamfer C1 at the edge of the surface, a second major surface 604 having a convex surface and a C-shaped chamfer C2 at the edge of the surface, and a minor surface 603 separating the first major surface 602 and the second major surface 604. Fig.14 In the 2D mirror preform, edge shaping, profiling and chamfering are performed before 3D forming, compared to Fig. 10A , edge quality is more consistent and relatively defect-free. Fig.14 The sample in the figure is made of a glass sheet with a thickness of t T is 2.0 mm and has a thickness of t C1 and t C2 The symmetrical C-chamfers are 0.424 mm each. Therefore, using the mirror preform method of the present disclosure, it is possible to have a larger C-chamfer. Because edge polishing is performed on the 2D preform, very fine polishing can be achieved on the chamfers C1 and C2 on the concave and convex sides, and fine polishing is also performed on the sub-surface 603 of the edge.
[0052] Fig.15A The 3D mirror substrate 600 is shown near one of the four corners. Fig.14 The side view of the 3D mirror substrate 600 is shown in FIG. Fig. 10B , with little chipping at the edges. Fig. 15B The edge consistency is higher than Fig. 10C The consistency shown. Fig. 15C The rounded corners are formed on 2D preforms. It is easier to form rounded corners on 2D preforms and can avoid Fig. 10D The straight angle of .
[0053] By comparison Figures 14 to 15C As seen in the above examples using conventional methods based on cutting oversized 3D substrates, the edge quality produced by the mirror substrate and method of the present disclosure is unattainable by conventional methods. Thus, a 3D mirror substrate or HUD mirror with very fine surface roughness and edge profile can be achieved due to the finest roughness and precise edge shaping possible through fine grinding, shaping and polishing of the 2D preform.
[0054] As described above, embodiments of the present disclosure include using a vacuum forming method to form a curved or 3D mirror substrate. In one aspect, as Fig.16 As shown, the vacuum forming method uses a mold 700. The mold 700 has a forming surface 702, which is formed into the desired shape of a 3D mirror or a mirror substrate. The mold 700 may optionally include a housing 706, which surrounds the periphery of the forming surface 702 and at least partially surrounds and defines a space for placing a mirror preform for forming. In order to make the mirror substrate (not shown) conform to the forming surface 702, vacuum pressure is supplied through one or more vacuum holes. However, as described above, the vacuum holes may leave manufacturing errors in the form of imperfections, where the vacuum holes shorten the substrate. Therefore, the mold 700 does not include vacuum holes in the area that will contact the effective area of the mirror substrate. Instead, the mold 700 has a groove-type vacuum hole 704 at the periphery of the forming surface 702. Due to the location of the groove-type vacuum hole 704 relative to the larger chamfer, the imperfection will not be located in the effective area of the mirror, so any imperfection or error caused by the groove-type vacuum hole 704 will not be presented to the user of the HUD system. According to some embodiments, the trench-type vacuum holes 704 will be positioned about 2.0 mm or less inside the edge of the 2D mirror preform when the preform is placed on the forming surface 702. As used herein, the active area is the portion of the mirror or mirror substrate that will reflect the image to be projected and viewed by the user, and is located within the chamfered edge region of the mirror or mirror substrate.
[0055] At least a portion of the first main surface of the 3D HUD mirror is a reflective surface. For example, the reflective surface includes a coating or other layer applied to the first main surface, and may include one or more metal oxides, ceramic oxides, or metal ceramic alloys. In a specific embodiment, the reflective coating is made of aluminum or silver. The reflective surface can be formed via sputtering, evaporation (e.g., CVD, PVD), electroplating, or other methods known to those skilled in the art for coating or supplying a reflective surface. After the substrate is formed into a curved or aspherical shape, a reflective surface is established on the 3D forming substrate. However, the embodiment is not limited to this order, and it is conceivable that a 2D preform with a reflective surface can be used to form a 3D mirror. More particularly, the vacuum 3D forming method disclosed herein allows a 3D mirror to be established from a 2D mirror preform with a reflective surface without degrading the reflective surface on the first main surface. In addition, embodiments of the present invention also allow low-temperature 3D formation, which can help maintain the reflective surface during bending of the glass preform.
[0056] According to one or more embodiments of the present disclosure, a head-up display (HUD) mirror substrate is provided, and has a first main surface, a second main surface and a secondary surface, the first main surface having a concave shape, the second main surface opposite to the first main surface and having a convex shape, and the secondary surface connecting the first main surface and the second main surface. The mirror substrate includes a glass or glass ceramic material, and the first main surface presents a first surface roughness Ra of 3nm or less and a peak-to-valley (PV) roughness of less than 30nm. As described above, when the mirror substrate is in a bent state, the HUD mirror substrate has an edge that is not cut, formed, chamfered or polished. Specifically, before the preform is formed into the 3D shape of the HUD mirror substrate, any cutting, forming, chamfering or polishing is applied to the 2D mirror preform, and after the 3D formation of the HUD mirror substrate, no further cutting, forming, chamfering or polishing is performed on the edge.
[0057] As an aspect of one or more embodiments, for example, the secondary surface has a cross-sectional edge profile including a chamfer, and can be formed as a C-shaped chamfer or an R-shaped chamfer. However, the cross-sectional edge profile can be formed in other ways not discussed herein, because it is easy to form and polish the 2D mirror preform and allow various finishing steps to be easily performed. In the case of a C-shaped chamfer, the length of the chamfer can be 0.1 mm or greater, or 0.3 mm or greater. In the case of an R-shaped chamfer, the length of the chamfer can be 0.5 mm or greater. In addition, the mirror substrate can have rounded corners. Specifically, when the mirror substrate is viewed in a plan view, the corners of the first and / or second main surface are rounded. In addition, when the mirror substrate is in a bent or 3D state, the rounded corners of the mirror substrate are not formed or polished.
[0058] In one or more specific embodiments, the concave surface of the HUD mirror substrate has an aspherical shape. Regardless of the specific shape or complexity of the curvature, the convex surface and the concave surface can have symmetrical chamfers. In addition, the mirror substrate can be large enough for so-called AR HUD applications. For example, the mirror substrate can have a length of about 200mm to about 400mm and a width of about 100mm to about 250mm; a length of about 250mm to about 350mm and a width of about 100mm to about 200mm; a length of about 300mm to about 350mm and a width of about 150mm to about 200mm; or a length of about 290mm to about 295mm and a width of about 130mm to about 135mm.
[0059] Although large sizes can be achieved, shape accuracy and surface and / or edge quality or roughness can be maintained at desired levels. As an aspect of one or more embodiments, the profile peak-to-valley (PV) shape accuracy on the recessed surface of the mirror substrate is less than 100 μm or less than 50 μm. The arithmetic mean waviness Wa on the recessed surface of the mirror substrate is less than 1 μm per 10 mm. As a further aspect of the embodiment, the raised surface has a surface roughness Ra of less than 30 nm, and a peak-to-valley (PV) roughness of less than 1 μm. The raised surface may have a surface roughness Ra of less than 20 nm and a peak-to-valley (PV) roughness of less than 300 nm. The raised surface may further include a groove-type vacuum hole imprint within 2 mm from the edge of the raised surface. According to some embodiments, the groove-type vacuum hole imprint may have a depth of less than 1 μm. In addition, the raised surface does not have any other vacuum hole imprints except the groove-type vacuum hole imprints. As a further aspect of one or more embodiments, the recessed surface has a roughness Ra of less than 2 nm or less than 1 nm and a peak-to-valley (PV) roughness of less than 20 nm, less than 15 nm, or less than 12 nm.
[0060] In one or more embodiments, the thickness of the mirror substrate is defined as the distance between the first major surface and the second major surface, and the thickness is less than or equal to about 3.0 mm, about 0.5 mm to about 3.0 mm, about 0.5 mm to about 1.0 mm, or about 1.0 mm to about 3.0 mm. The glass or glass ceramic material for the mirror substrate may include soda lime glass, aluminosilicate, boroaluminosilicate, or alkali metal aluminosilicate glass. In addition, the glass or glass ceramic material may be a strengthened glass material (e.g., chemically strengthened).
[0061] According to one or more embodiments, a three-dimensional HUD mirror is provided, and includes the above-mentioned HUD mirror substrate and a reflective layer disposed on a first major surface of the mirror substrate.
[0062] In a further embodiment, a method for forming a three-dimensional mirror is provided. The method includes providing a mirror preform, the mirror preform having a first major surface, a second major surface opposite to the first major surface, and a secondary surface connecting the first major surface and the second major surface. The mirror preform includes a glass or glass ceramic material, and the first major surface and the second major surface of the preform are two-dimensional. The method further includes: placing the mirror preform on a molding device having a curved support surface so that the second major surface faces the curved support surface; and conforming the mirror preform to the curved support surface to form a curved mirror substrate having a convex surface corresponding to the second major surface and a concave surface corresponding to the first major surface, wherein the concave surface includes a first radius of curvature. After the conforming step, the concave surface has a roughness Ra of less than 3nm and a peak-to-valley (PV) roughness of less than 30nm.
[0063] As an aspect of one or more embodiments of the above method, the curved mirror substrate has an edge that has not been cut, shaped, chamfered or polished during or after the conforming step. The cross-sectional edge profile of the secondary surface is the same as the cross-sectional edge profile of the curved mirror substrate. The edge profile of the mirror preform may include a chamfer on at least one of the first major surface side of the secondary edge and the second major surface side of the secondary edge, and the chamfer may be a C-shaped chamfer or an R-shaped chamfer. In the case of a C-shaped chamfer, the length of the C-shaped chamfer is 0.1 mm or greater, or 0.3 mm or greater. In the case of an R-shaped chamfer, the length of the R-shaped chamfer is 0.5 mm or greater.
[0064] In further aspects of some embodiments, the surface roughness of the subsurface after the conforming step is within 2% of the surface roughness of the subsurface before the conforming step. The surface roughness of the subsurface after the conforming step may be the same as the surface roughness of the subsurface before the conforming step. The mirror preform has rounded corners when viewed in a plan view. During or after the conforming step, the rounded corners may be the same as the rounded corners of the mirror preform and are not formed or polished. In one or more embodiments, the method includes processing the subsurface of the two-dimensional mirror preform to achieve a predetermined edge profile of the curved mirror substrate, the processing including at least one of cutting, chamfering or polishing.
[0065] As aspects of some embodiments, the curved mirror substrate has a length of about 200 mm to about 400 mm and a width of about 100 mm to about 250 mm; a length of about 250 mm to about 350 mm and a width of about 100 mm to about 200 mm; a length of about 300 mm to about 350 mm and a width of about 150 mm to about 200 mm; or a length of about 290 mm to about 295 mm and a width of about 130 mm to about 135 mm. The profile peak-to-valley (PV) shape accuracy on the concave surface of the curved mirror substrate is less than 100 μm or less than 50 μm. The arithmetic mean waviness Wa on the concave surface of the curved mirror substrate may be further less than 1 μm per 10 mm. In addition, the maximum roughness R on the concave surface of the curved mirror substrate max The convex surface has a surface roughness Ra of less than 30 nm and a peak-to-valley (PV) roughness of less than 1 μm, or has a surface roughness Ra of less than 20 nm and a peak-to-valley (PV) roughness of less than 300 nm.
[0066] In some aspects of the embodiments, the curved support surface includes a groove type vacuum hole. More particularly, when the mirror preform is set on the molding device, the groove type vacuum hole is within 2mm of the edge of the second main surface. After the conforming step, the convex surface has a groove type vacuum hole imprint within 2mm of the edge of the convex surface along the entire edge. The groove type vacuum hole imprint can have a depth of less than 1μm. In addition to the groove type vacuum hole imprint, the convex surface does not have any other vacuum hole imprint. As a further aspect of one or more embodiments, the concave surface has a roughness Ra of less than 2nm or less than 1nm and a peak-to-valley (PV) roughness of less than 20nm, less than 15nm or less than 12nm. In one or more embodiments, the mirror preform has a thickness defined as the distance between the first main surface and the second main surface, wherein the thickness is less than or equal to about 3.0mm, about 0.5mm to about 3.0mm, about 0.5mm to about 1.0mm, or about 1.0mm to about 3.0mm.
[0067] As a further aspect of one or more embodiments of the method, the conforming step is performed at a temperature less than the glass transition temperature of the mirror preform. During or after the conforming step, the temperature of the mirror preform or the bent mirror substrate is not raised above the glass transition temperature of the mirror preform. The glass or glass ceramic material may include soda lime glass, aluminosilicate, boroaluminosilicate or alkali aluminosilicate glass. The glass or glass ceramic material may be a strengthened glass material and may be strengthened via chemical strengthening.
[0068] In one or more embodiments, a method of forming a three-dimensional mirror is provided, the method comprising: forming a three-dimensional mirror substrate according to the embodiments described herein; and disposing a reflective layer on a first major surface.
[0069] According to one or more embodiments of the present disclosure, a mirror for a HUD system is provided, and a 3D mirror substrate is formed using the glass-based preform described herein. The mirror includes a reflective layer on a first major surface of the 3D mirror substrate. The 3D mirror substrate has a first radius of curvature such that the first major surface has a concave shape and the second major surface has a convex shape, wherein the first radius of curvature is measured relative to a first axis of curvature. The 3D mirror substrate has a second radius of curvature, the second radius of curvature is measured relative to a second axis of curvature, the second axis of curvature is different from the first axis of curvature, wherein the first axis of curvature is perpendicular to the second axis of curvature. In some embodiments, the first major surface has an aspherical shape.
[0070] In another embodiment, a method of forming a three-dimensional (3D) mirror is provided, the method comprising: providing a two-dimensional (2D) mirror preform, the two-dimensional (2D) mirror preform comprising a first major surface, a second major surface, and a secondary surface, the first major surface having an edge with a chamfer, the second major surface opposite the first major surface and having an edge with a second chamfer, the secondary surface connecting the first major surface and the second major surface, placing the 2D mirror preform on a molding device having a curved support surface, wherein the second major surface faces the curved support surface, and conforming the 2D mirror preform to the curved support surface to form a curved or 3D mirror substrate having a first radius of curvature.
[0071] In one or more embodiments, conforming of the 2D mirror preform to the curved support surface is performed at a temperature below the glass transition temperature of the preform. During or after conforming, the temperature of the mirror substrate may not rise above the glass transition temperature of the glass-based substrate material.
[0072] In aspects of embodiments of the HUD system, the display unit includes an LCD, LED, OLED, or μLED display panel, and may include a projector.
[0073] The glass-based substrate has a thickness of less than or equal to 3.0 mm; about 0.5 mm to about 3.0 mm; about 0.5 mm to about 1.0 mm; about 1.0 mm to about 3.0 mm; or about 2.0 mm.
[0074] As an aspect of some embodiments, the chamfer of the first major surface is configured to reduce edge distortion of the projected image. The chamfer of the first major surface can be configured to reduce the amount of unwanted light reflected toward the user. The projection surface can be a windshield of a vehicle, or can be a combiner configured to be mounted inside a vehicle.
[0075] The mirror has a first radius of curvature such that the first major surface has a concave shape and the second major surface has a convex shape, the first radius of curvature being relative to a first axis of curvature. The mirror may also have a second radius of curvature, the second radius of curvature being relative to a second axis of curvature, the second axis of curvature being different from the first axis of curvature, wherein the first axis of curvature is perpendicular to the second axis of curvature. In some preferred embodiments, the first major surface has an aspherical shape.
[0076] The reflective first major surface includes a reflective coating on a glass-based substrate, wherein the reflective coating includes a metal, a metal oxide, a ceramic oxide, or a metal-ceramic alloy, and may include aluminum or silver. The display unit may include an LCD, LED, OLED, or μLED display panel and / or a projector. The HUD system may further include a projection surface for a projected image viewed by a user of the HUD system, wherein the display unit is configured to generate an image, and the mirror is configured to reflect the image to form a projected image on the projection surface. The shape of the projection surface is substantially the same as the shape of the mirror, wherein the projection surface is a windshield or a combiner, and the projection surface may have an aspherical shape.
[0077] The glass-based substrate has a thickness of less than or equal to 3.0 mm; about 0.5 mm to about 3.0 mm; about 0.5 mm to about 1.0 mm; about 1.0 mm to about 3.0 mm; or about 2.0 mm.
[0078] Substrate material
[0079] Suitable glass substrates for mirrors in HUD systems can be non-strengthened glass sheets or strengthened glass sheets. The glass sheets (whether strengthened or not) can include soda-lime glass, aluminosilicate, boroaluminosilicate or alkali aluminosilicate glass. Optionally, the glass sheets can be heat strengthened.
[0080] Suitable glass substrates can be chemically strengthened by an ion exchange process. In this process, ions at or near the surface of the glass sheet are exchanged with larger metal ions from the salt bath, typically by immersing the glass sheet in a molten salt bath for a predetermined period of time. In one embodiment, the temperature of the molten salt bath is about 430° C. and the predetermined period of time is about eight hours. The sheet can be strengthened by incorporating larger ions into the glass by creating compressive stresses in the near-surface region. Corresponding tensile stresses are induced in the central region of the glass to balance the compressive stresses.
[0081] Exemplary ion exchange glasses suitable for forming the glass substrate are soda lime glass, alkali aluminosilicate glass, or alkali aluminoborosilicate glass, and other glass compositions are also contemplated. As used herein, "ion exchangeable" means that the glass is capable of exchanging cations at or near the surface of the glass with cations of the same valence of larger or smaller size. An exemplary glass composition includes: SiO2, B2O3, and Na2O, wherein (SiO2+B2O3)≥66 mol%, and Na2O≥9 mol%. In an embodiment, the glass sheet includes at least 6 wt% alumina. In a further embodiment, the glass sheet includes one or more alkaline earth oxides such that the content of the alkaline earth oxides is at least 5 wt%. In some embodiments, suitable glass compositions further include at least one of K2O, MgO, and CaO. In a particular embodiment, the glass can include 61 to 75 mol % SiO2; 7 to 15 mol % Al2O3; 0 to 12 mol % B2O3; 9 to 21 mol % Na2O; 0 to 4 mol % K2O; 0 to 7 mol % MgO; and 0 to 3 mol % CaO.
[0082] Further exemplary glass compositions suitable for forming a glass substrate include: 60 to 70 mol% SiO2; 6 to 14 mol% Al2O3; 0 to 15 mol% B2O3; 0 to 15 mol% Li2O; 0 to 20 mol% Na2O; 0 to 10 mol% K2O; 0 to 8 mol% MgO; 0 to 10 mol% CaO; 0 to 5 mol% ZrO2; 0 to 1 mol% SnO2; 0 to 1 mol% CeO2; less than 50 ppm As2O3; and less than 50 ppm Sb2O3; wherein 12 mol% ≤ (Li2O + Na2O + K2O) ≤ 20 mol%, and 0 mol% ≤ (MgO + CaO) ≤ 10 mol%.
[0083] Another further exemplary glass composition includes: 63.5 to 66.5 mol % SiO2; 8 to 12 mol % Al2O3; 0 to 3 mol % B2O3; 0 to 5 mol % Li2O; 8 to 18 mol % Na2O; 0 to 5 mol % K2O; 1 to 7 mol % MgO; 0 to 2.5 mol % CaO; 0 to 3 mol % ZrO2; 0.05 to 0.25 mol % SnO2; 0.05 to 0.5 mol % CeO2; less than 50 ppm As2O3; and less than 50 ppm Sb2O3; wherein 14 mol % ≤ (Li2O + Na2O + K2O) ≤ 18 mol %, and 2 mol % ≤ (MgO + CaO) ≤ 7 mol %.
[0084] In certain embodiments, the alkali-aluminosilicate glass comprises aluminum oxide, at least one alkali metal, greater than 50 mol % SiO2 in some embodiments, at least 58 mol % SiO2 in other embodiments, and at least 60 mol % SiO2 in other embodiments, wherein the ratio Where the ratios of the components are expressed in mole %, the modifier is an alkali metal oxide. In a specific embodiment, the glass comprises, consists essentially of, or consists of: 58 to 72 mole % SiO2; 9 to 17 mole % Al2O3; 2 to 12 mole % B2O3; 8 to 16 mole % Na2O; and 0 to 4 mole % K2O, wherein the ratios are
[0085] In another embodiment, the alkali aluminosilicate glass comprises, consists essentially of, or consists of: 61 to 75 mol% SiO2; 7 to 15 mol% Al2O3; 0 to 12 mol% B2O3; 9 to 21 mol% Na2O; 0 to 4 mol% K2O; 0 to 7 mol% MgO; and 0 to 3 mol% CaO.
[0086] In yet another embodiment, the alkali aluminosilicate glass substrate comprises, consists essentially of, or consists of: 60 to 70 mol% SiO2; 6 to 14 mol% Al2O3; 0 to 15 mol% B2O3; 0 to 15 mol% Li2O; 0 to 20 mol% Na2O; 0 to 10 mol% K2O; 0 to 8 mol% MgO; 0 to 10 mol% CaO; 0 to 5 mol% ZrO2; 0 to 1 mol% SnO2; 0 to 1 mol% CeO2; less than 50 ppm As2O3; and less than 50 ppm Sb2O3; wherein 12 mol% ≤ Li2O+Na2O+K2O ≤ 20 mol%, and 0 mol% ≤ MgO+CaO ≤ 10 mol%.
[0087] In yet another embodiment, the alkali aluminosilicate glass comprises, consists essentially of, or consists of: 64 to 68 mol% SiO2; 12 to 16 mol% Na2O; 8 to 12 mol% Al2O3; 0 to 3 mol% B2O3; 2 to 5 mol% K2O; 4 to 6 mol% MgO; and 0 to 5 mol% CaO, wherein: 66 mol%≤SiO2+B2O3+CaO≤69 mol%; Na2O+K2O+B2O3+MgO+CaO+SrO>10 mol%; 5 mol%≤MgO+CaO+SrO≤8 mol%; (Na2O+B2O3)-Al2O3≤2 mol%; 2 mol%≤Na2O-Al2O3≤6 mol%; and 4 mol%≤(Na2O+K2O)-Al2O3≤10 mol%.
[0088] In some embodiments, the chemically strengthened and non-chemically strengthened glasses may have 0 to 2 mol % of at least one fining agent selected from the group consisting of Na2SO4, NaCl, NaF, NaBr, K2SO4, KCl, KF, KBr, and SnO2.
[0089] In one exemplary embodiment, the sodium ions in the chemically strengthened glass are replaced by potassium ions from the molten bath, while other alkali metal ions with larger atomic radius (e.g., rubidium or cesium) can also replace smaller alkali metal ions in the glass. According to a specific embodiment, the smaller alkali metal ions in the glass can be replaced by Ag. + Ion Exchange. Similarly, in the ion exchange process, other alkali metal salts such as, but not limited to, sulfates, halides, etc. may be used.
[0090] The stress profile is caused by the replacement of smaller ions with larger ions at a temperature lower than the temperature at which the glass network can relax, resulting in an ion distribution throughout the glass surface. The larger volume of introduced ions can produce compressive stress (CS) on the surface and tension (center tension or CT) in the center of the glass. The relationship between compressive stress and center tension is as follows:
[0091]
[0092] Where t is the total thickness of the glass sheet and DOL is the depth of exchange (also referred to as depth of layer).
[0093] According to various embodiments, glass substrates comprising ion-exchanged glass can have a range of desirable properties including low weight, high impact resistance, and improved sound attenuation. In one embodiment, the chemically strengthened glass sheet can have a surface compressive stress of at least 300 MPa (e.g., at least 400, 450, 500, 550, 600, 650, 700, 750, or 800 MPa), a depth of layer of at least about 20 μm (e.g., at least about 20, 25, 30, 35, 40, 45, or 50 μm), and / or a central tension greater than 40 MPa (e.g., greater than 40, 45, or 50 MPa) but less than 100 MPa (e.g., less than 100, 95, 90, 85, 80, 75, 70, 65, 60, or 55 MPa).
[0094] Suitable glass substrates can be heat strengthened by heat tempering or annealing.The thickness of the heat strengthened glass sheet can be less than about 2 mm or less than about 1 mm.
[0095] Exemplary glass sheet forming methods include fusion stretching and slot stretching processes, each of which is an example of a downward stretching process and a floating process. These methods can be used to form strengthened and non-strengthened glass sheets. The fusion stretching process uses a stretching cylinder having a channel for receiving molten glass raw materials. The weirs of the channel are open at the top along the length of the channel on both sides of the channel. When the channel is filled with molten material, the molten glass overflows the weir. Due to gravity, the molten glass flows down the outer surface of the stretching cylinder. These outer surfaces extend downward and inward and are connected at the edge below the stretching cylinder. The two flowing glass surfaces are connected together at this edge to fuse and form a single flowing sheet. The advantage of the fusion stretching method is that since the two glass films flowing on the channel are fused together, the outer surface of the resulting glass sheet will not contact any part of the equipment. Therefore, the surface properties of the fusion stretched glass sheet are not affected by such contact.
[0096] The slot stretch process is different from the fusion stretch process. Here, molten raw glass is provided to a stretching cylinder. The bottom of the stretching cylinder has an open slot with a nozzle extending the length of the slot. The molten glass flows through the slot / nozzle and is drawn down as a continuous sheet into the annealing area. Compared to the fusion stretch process, the slot stretch process can provide thinner sheets because only a single sheet is stretched through the slot instead of fusing two sheets together.
[0097] The down-draw process produces a glass sheet of uniform thickness with a relatively pristine surface. Since the strength of the glass surface is controlled by the number and size of surface defects, the pristine surface with minimal contact has a higher initial strength. When this high-strength glass is subsequently chemically strengthened, the resulting strength can be higher than a ground and polished surface. The down-drawn glass can be drawn to a thickness of less than about 2 mm. In addition, the down-drawn glass has a very flat and smooth surface and can be used in the final application without the need for expensive grinding and polishing processes.
[0098] In the float glass process, a glass sheet characterized by a smooth surface and uniform thickness can be made by floating molten glass on a bed of molten metal, typically tin. In an exemplary process, molten glass fed onto the surface of a molten tin bed forms a floating ribbon. As the glass ribbon flows along the tin bath, the temperature gradually decreases until a solid glass sheet can be lifted from the tin onto rollers. Once out of the bath, the glass sheet can be further cooled and annealed to reduce internal stresses.
[0099] As described in the previous paragraphs, exemplary glass substrates may include glass sheets of chemically strengthened glass (e.g., Glass). The glass sheet may be heat processed, ion exchanged and / or annealed. In the laminated structure, the strengthened glass sheet may be the inner layer, while the outer layer may be a non-chemically strengthened glass sheet (e.g., conventional soda-lime glass, annealed glass, or the like). The laminated structure may also include a polymer interlayer sandwiched between the outer and inner glass layers. The strengthened glass sheet may have a thickness of less than or equal to 1.0 mm, and have a residual surface CS level of between about 250 MPa and about 350 MPa, and have a DOL greater than 60 microns. In another embodiment, the CS level of the strengthened glass sheet is preferably about 300 MPa. Exemplary thicknesses of the glass sheets may range from about 0.3 mm to about 1.5 mm, from 0.5 mm to 1.5 mm, to 2.0 mm or more.
[0100] In a preferred embodiment, the surface stress of the thin chemically strengthened glass sheet can be between about 250 MPa and 900 MPa, and the thickness can range from about 0.3 mm to about 1.0 mm. In embodiments where the laminate structure includes this strengthened glass sheet, the outer layer can be annealed (non-chemically strengthened) glass and have a thickness of about 1.5 mm to about 3.0 mm, or greater. Of course, in the corresponding laminate structure, the thickness of the outer layer and the inner layer can be different. Another preferred embodiment of the exemplary laminate structure can include an inner layer of 0.7 mm chemically strengthened glass, a polyvinyl butyral layer having a thickness of about 0.76 mm, and an outer layer of 2.1 mm annealed glass.
[0101] In some embodiments, the exemplary glass substrates of the embodiments described herein can be used in vehicles (cars, airplanes, etc.) with head-up display (HUD) systems. The clarity of the fusion formed according to some embodiments may be better than that of the glass formed by the float process because the information can be easier to read and less distracting, thereby providing a better driving experience and improving safety. A non-limiting HUD system may include a projector unit, a combiner, and a video generating computer. The projection unit in the exemplary HUD may be (but not limited to) an optical collimator having a convex lens or a concave mirror and a display at the focus (e.g., an optical waveguide, a scanning laser, an LED, a CRT, a video image, or the like). The projection unit can be used to produce the desired image. In some embodiments, the HUD system may also include a combiner or a beam splitter to redirect the projected image from the projection unit to change or alter the field of view and the projected image. Some combiners may include special coatings to reflect the monochromatic light projected thereon while allowing light of other wavelengths to pass through. In additional embodiments, the combiner may also be bent to refocus the image from the projection unit. Any exemplary HUD system may also include a processing system to provide an interface between the projection unit and applicable vehicle systems from which data may be received, manipulated, monitored and / or displayed. Some processing systems may also be used to generate images and symbols displayed by the projection unit.
[0102] Using such an exemplary HUD system, a display of information (e.g., numbers, images, directions, text, etc.) may be created by projecting an image from the HUD system onto the interior-facing surface of a glass-based mirror substrate. The mirror may then redirect the image so that it is within the driver's field of view.
[0103] Thus, an exemplary glass substrate according to some embodiments can provide a thin, pristine surface for a mirror. In some embodiments, fusion-stretched Gorilla Glass can be used as a glass substrate. Such glass does not include any typical float lines of conventional glass (e.g., soda-lime glass) manufactured using a float process.
[0104] HUDs according to embodiments of the present disclosure may be used in automotive vehicles, aircraft, synthetic vision systems, and / or visor displays (e.g., head mounted displays (e.g., goggles, visors, helmets, etc.) using the exemplary glass substrates described herein. Such HUD systems may project critical information (speed, fuel, temperature, turn signals, navigation, warning information, etc.) in front of the driver through the glass laminate structure.
[0105] According to some embodiments, the HUD system described herein can use nominal HUD system parameters (radius of curvature, refractive index, and angle of incidence (e.g., radius of curvature Rc =8301mm, distance from source: R i =1000mm, refractive index n=1.52 and incident angle θ=62.08°)).
[0106] Applicants have demonstrated that the glass substrates and laminate structures disclosed herein have excellent durability, impact resistance, toughness, and scratch resistance. As is known to those skilled in the art, the strength and mechanical impact performance of a glass sheet or laminate is limited by defects in the glass, both surface and internal. When a glass sheet or laminate is impacted, the point of impact is compressed, and a ring or "hoop" around the point of impact (and the opposing face of the impacted sheet) is tensioned. Typically, the source of breakage is a flaw, often at or near the point of highest tension on the surface of the glass. This may occur on the opposing face, but may occur within the ring. If a flaw in the glass is tensioned during an impact event, the flaw may propagate and the glass will typically break. Therefore, higher magnitude and depth of compressive stress (depth of layer) are preferred.
[0107] As a result of strengthening, one or both surfaces of the strengthened glass sheets disclosed herein are placed in compression. Introducing compressive stress in the near-surface region of the glass can inhibit crack propagation and breakage of the glass sheet. In order for a flaw to propagate and break, the tensile stress from the impact must exceed the surface compressive stress at the tip of the flaw. In embodiments, the high compressive stress and high depth of the layers of the strengthened glass sheet enable the use of thinner glass than would be the case with non-chemically strengthened glass.
[0108] The foregoing description of the present disclosure is provided as a teaching and the best currently known embodiment. It will be appreciated by those skilled in the art that many changes may be made to the embodiments described herein while still achieving the beneficial results of the present disclosure. It should be appreciated that some desired benefits of the present disclosure may be achieved by selecting some features of the present disclosure without using other features. Therefore, it will be appreciated by those skilled in the art that many modifications and adaptations of the present disclosure are possible, and in some cases even desirable, and are a part of the present disclosure. Therefore, the foregoing description is provided as an illustration of the principles of the present disclosure rather than a limitation.
[0109] Those skilled in the art will appreciate that many modifications may be made to the exemplary embodiments described herein without departing from the spirit and scope of the present disclosure. Therefore, the description is not intended and should not be interpreted as being limited to the examples given, but rather should be given the full protection provided by the claims and their equivalents. In addition, some features of the present disclosure may be used without corresponding use of other features. Therefore, the foregoing description of exemplary or illustrative embodiments is provided for the purpose of illustrating the principles of the present disclosure rather than for limiting purposes, and the foregoing description may include modifications and substitutions therein.
[0110] In the foregoing description, like component symbols represent like or corresponding parts in the several views shown in the drawings. It should also be understood that terms such as "top", "bottom", "outward", "inward", etc. are words of convenience and should not be interpreted as limiting terms unless otherwise specified. In addition, whenever a group is described as including at least one of a set of elements and combinations thereof, it should be understood that the group can include, consist essentially of, or consist of any number of those elements, either individually or in combination with each other.
[0111] Similarly, whenever a group is described as consisting of at least one of a set of elements or combinations thereof, it is understood that the group may consist of any number of those elements, alone or in combination with each other. Unless otherwise specified, when stated, the range of values includes the upper and lower limits of the range. The indefinite articles "a" and "an" and the corresponding definite articles "the" used herein mean "at least one" or "one or more", unless otherwise specified.
[0112] Although this description may include many details, these descriptions should not be interpreted as limitations on the scope of this description, but rather as descriptions of features that would be specific to a particular embodiment. Certain features that have been described heretofore in the context of separate embodiments may also be implemented in combination in a single embodiment. Conversely, various features described in the context of a single embodiment may also be implemented individually in multiple embodiments or using any suitable sub-combination. In addition, although features may be described above as working in certain combinations and such features may even be requested in the first place, one or more features from the claimed combination may be removed from the combination in some cases, and the claimed combination may be directed to sub-combinations or variations of sub-combinations.
[0113] Similarly, while operations are depicted in a particular order in the accompanying drawings or diagrams, this should not be understood as requiring that such operations be performed in the particular order shown or in sequential order, or that all illustrated operations be performed, to achieve desirable results. In certain circumstances, multitasking and parallel processing may be advantageous.
[0114] Ranges expressed herein may be from "about" one particular value and / or to "about" another particular value. When such a range is expressed, examples include from a particular value and / or to another particular value. Similarly, when an approximation of a value is expressed by use of the preposition "about," it will be understood that the particular value will form another aspect. It will be further understood that each endpoint of a range is expressly related to, and independent of, the other endpoint.
[0115] It should also be noted that statements herein refer to components of the present disclosure being "configured" or "adapted" to function in a particular manner. In this case, such components are "configured" or "adapted" to embody particular properties or to function in a particular manner, wherein such statements are structural statements, rather than statements of intended use. More specifically, references herein to the manner in which components are "configured" or "adapted" refer to the existing physical condition of the components and, therefore, should be considered as explicit statements of the structural features of the components.
[0116] As shown in the various configurations and implementations illustrated in the figures, various glass-based structures for heads-up displays have been described.
[0117] According to aspect (1) of the present disclosure, there is provided a head-up display (HUD) mirror substrate, comprising a first main surface having a concave shape, a second main surface opposite to the first main surface and having a convex shape, and a secondary surface connecting the first main surface and the second main surface, wherein the first main surface comprises a first surface roughness Ra of 3 nm or less and a peak-to-valley (PV) roughness of less than 30 nm, and wherein the mirror substrate comprises glass or glass ceramic material.
[0118] According to aspect (2) of the present disclosure, there is provided the HUD mirror substrate of aspect (1), wherein when the mirror substrate is in a bent state, the mirror substrate has an edge that is not cut, shaped, chamfered or polished.
[0119] According to aspect (3) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (2), wherein the sub-surface includes a cross-sectional edge profile having a chamfer.
[0120] According to aspect (4) of the present disclosure, there is provided the HUD mirror substrate of aspect (3), wherein the chamfer is a C-shaped chamfer or an R-shaped chamfer.
[0121] According to aspect (5) of the present disclosure, there is provided the HUD mirror substrate of aspect (4), wherein the C-shaped chamfer is 0.1 mm or more or 0.3 mm or more.
[0122] According to aspect (6) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (4) to (5), wherein the R-shaped chamfer is 0.5 mm or more.
[0123] According to aspect (7) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (6), wherein the mirror substrate in a plan view includes rounded corners.
[0124] According to aspect (8) of the present disclosure, there is provided the HUD mirror substrate of aspect (7), wherein the rounded corners of the mirror substrate are not formed or polished when the mirror substrate is in a bent state.
[0125] According to aspect (9) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (8), wherein the concave surface has an aspherical shape.
[0126] According to aspect (10) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (9), wherein the convex surface and the concave surface include symmetrical chamfers.
[0127] According to aspect (11) of the present disclosure, a HUD mirror substrate of any one of aspects (1) to (10) is provided, wherein the mirror substrate has a length of about 200 mm to about 400 mm and a width of about 100 mm to about 250 mm; a length of about 250 mm to about 350 mm and a width of about 100 mm to about 200 mm; a length of about 300 mm to about 350 mm and a width of about 150 mm to about 200 mm; or a length of about 290 mm to about 295 mm and a width of about 130 mm to about 135 mm.
[0128] According to aspect (12) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (11), wherein the profile peak-to-valley (PV) shape accuracy on the concave surface of the mirror substrate is less than 100 μm or less than 50 μm.
[0129] According to aspect (13) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (12), wherein an arithmetic mean waviness Wa on the concave surface of the mirror substrate is less than 1 μm per 10 mm.
[0130] According to aspect (14) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (13), wherein the surface roughness Ra of the convex surface is less than 30 nm, and the peak-to-valley (PV) roughness is less than 1 μm.
[0131] According to aspect (15) of the present disclosure, there is provided the HUD mirror substrate of aspect (14), wherein the surface roughness Ra of the convex surface is less than 20 nm, and the peak-to-valley (PV) roughness is less than 300 nm.
[0132] According to aspect (16) of the present disclosure, there is provided a HUD mirror substrate according to any one of aspects (1) to (15), wherein the convex surface includes a groove-type vacuum hole imprint within 2 mm from an edge of the convex surface.
[0133] According to aspect (17) of the present disclosure, there is provided the HUD mirror substrate of aspect (16), wherein the depth of the groove-type vacuum hole embossing is less than 1 μm.
[0134] According to aspect (18) of the present disclosure, there is provided the HUD mirror substrate of aspect (16), wherein the convex surface does not have any other vacuum hole imprinting except the groove type vacuum hole imprinting.
[0135] According to aspect (19) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (15).
[0136] 19. The HUD mirror substrate of any one of claims 1 to 18, wherein the concave surface has a roughness Ra of less than 2 nm or less than 1 nm and a peak-to-valley (PV) roughness of less than 20 nm, less than 15 nm or less than 12 nm.
[0137] According to aspect (20) of the present disclosure, a HUD mirror substrate of any one of aspects (1) to (19) is provided, wherein the mirror substrate includes a thickness defined as the distance between the first major surface and the second major surface, wherein the thickness is less than or equal to about 3.0 mm, about 0.5 mm to about 3.0 mm, about 0.5 mm to about 1.0 mm, or about 1.0 mm to about 3.0 mm.
[0138] According to aspect (21) of the present disclosure, there is provided a HUD mirror substrate according to any one of aspects (1) to (20), wherein the glass or glass ceramic material comprises soda lime glass, aluminosilicate, boroaluminosilicate or alkali metal aluminosilicate glass.
[0139] According to aspect (22) of the present disclosure, there is provided the HUD mirror substrate of any one of aspects (1) to (21), wherein the glass or glass ceramic material is a strengthened glass material.
[0140] According to aspect (23) of the present disclosure, there is provided the HUD mirror substrate of aspect (22), wherein the glass or glass ceramic material is chemically strengthened.
[0141] According to aspect (24) of the present disclosure, there is provided a three-dimensional HUD mirror comprising the HUD mirror substrate of any one of aspects (1) to (23) and a reflective layer provided on a first major surface of the mirror substrate.
[0142] According to aspect (25) of the present disclosure, a method for forming a three-dimensional mirror is provided. The method comprises: providing a mirror preform, the mirror preform comprising a first main surface, a second main surface opposite to the first main surface, and a secondary surface connecting the first main surface and the second main surface, the mirror preform comprising a glass or glass ceramic material, and the first main surface and the second main surface are two-dimensional; placing the mirror preform on a molding device having a curved support surface so that the second main surface faces the curved support surface; conforming the mirror preform to the curved support surface to form a curved mirror substrate having a convex surface corresponding to the second main surface and a concave surface corresponding to the first main surface, the concave surface having a first radius of curvature, wherein after the conforming step, the concave surface has a roughness Ra of less than 3 nm and a peak-to-valley (PV) roughness of less than 30 nm.
[0143] According to aspect (26) of the present disclosure, there is provided the method of aspect (25), wherein during or after the conforming step, the curved mirror substrate has edges that are not cut, shaped, chamfered or polished.
[0144] According to aspect (27) of the present disclosure, there is provided the method of any one of aspects (25) to (26), wherein the cross-sectional edge profile of the subsurface is the same as the cross-sectional edge profile of the curved mirror substrate.
[0145] According to aspect (28) of the present disclosure, a method according to any one of aspects (25) to (27) is provided, wherein an edge profile of the mirror preform includes a chamfer on at least one of a first major surface side of the secondary edge and a second major surface side of the secondary edge.
[0146] According to aspect (29) of the present disclosure, there is provided the method of aspect (28), wherein the chamfer is a C-shaped chamfer or an R-shaped chamfer.
[0147] According to aspect (30) of the present disclosure, there is provided the method of aspect (29), wherein the C-shaped chamfer is 0.1 mm or greater or 0.3 mm or greater.
[0148] According to aspect (31) of the present disclosure, there is provided the method of any one of aspects (25) to (30), wherein the R-shaped chamfer is 0.5 mm or more.
[0149] According to aspect (32) of the present disclosure, there is provided the method of any one of aspects (25) to (31), wherein the surface roughness of the subsurface after the conforming step is within 2% of the surface roughness of the subsurface before the conforming step.
[0150] According to aspect (33) of the present disclosure, there is provided the method of aspect (32), wherein the surface roughness of the subsurface after the conforming step is the same as the surface roughness of the subsurface before the conforming step.
[0151] According to aspect (34) of the present disclosure, there is provided the method of any one of aspects (25) to (33), wherein the mirror preform comprises rounded corners when viewed in a plan view.
[0152] According to aspect (35) of the present disclosure, there is provided the method of aspect (34), wherein the rounded corners of the bent mirror substrate are the same as the rounded corners of the mirror preform.
[0153] According to aspect (36) of the present disclosure, there is provided the method of aspect (35), wherein the rounded corners of the curved mirror substrate are not shaped or polished during or after the conforming step.
[0154] According to aspect (37) of the present disclosure, a method according to any one of aspects (25) to (36) is provided, further comprising: processing a sub-surface of the two-dimensional mirror preform to achieve a predetermined edge profile of the curved mirror substrate, the processing comprising at least one of cutting, chamfering or polishing.
[0155] According to aspect (38) of the present disclosure, there is provided the method of any one of aspects (25) to (37), wherein the concave surface has an aspherical shape.
[0156] According to aspect (39) of the present disclosure, there is provided the method of any one of aspects (25) to (38), wherein the convex surface and the concave surface include symmetrical chamfers.
[0157] According to aspect (40) of the present disclosure, a method of any one of aspects (25) to (39) is provided, wherein the curved mirror substrate has a length of about 200 mm to about 400 mm and a width of about 100 mm to about 250 mm; a length of about 250 mm to about 350 mm and a width of about 100 mm to about 200 mm; a length of about 300 mm to about 350 mm and a width of about 150 mm to about 200 mm; or a length of about 290 mm to about 295 mm and a width of about 130 mm to about 135 mm.
[0158] According to aspect (41) of the present disclosure, there is provided the method of any one of aspects (25) to (40), wherein the profile peak-to-valley (PV) shape accuracy on the concave surface of the curved mirror substrate is less than 100 μm or less than 50 μm.
[0159] According to aspect (42) of the present disclosure, there is provided the method of any one of aspects (25) to (41), wherein an arithmetic mean waviness Wa on the concave surface of the curved mirror substrate is less than 1 μm per 10 mm.
[0160] According to aspect (43) of the present disclosure, there is provided a method according to any one of aspects (25) to (42), wherein the maximum roughness depth Rmax Less than 30nm.
[0161] According to aspect (44) of the present disclosure, there is provided the method of any one of aspects (25) to (43), wherein the surface roughness Ra of the protruding surface is less than 30 nm, and the peak-to-valley (PV) roughness is less than 1 μm.
[0162] According to aspect (45) of the present disclosure, there is provided the method of aspect (44), wherein the surface roughness Ra of the protruding surface is less than 20 nm, and the peak-to-valley (PV) roughness is less than 300 nm.
[0163] According to aspect (46) of the present disclosure, there is provided the method of any one of aspects (25) to (45), wherein the curved support surface comprises groove-type vacuum holes.
[0164] According to aspect (47) of the present disclosure, there is provided the method of aspect (46), wherein when the mirror preform is set on the molding apparatus, the groove-shaped vacuum holes are within 2 mm of the edge of the second major surface.
[0165] According to aspect (48) of the present disclosure, a method according to any one of aspects (25) to (47) is provided, wherein after the conforming step, the raised surface includes groove-type vacuum hole embossing within 2 mm of the edge of the raised surface along the entire edge.
[0166] According to aspect (49) of the present disclosure, there is provided the method of aspect (48), wherein the depth of the trench-type vacuum hole embossing is less than 1 μm.
[0167] According to aspect (50) of the present disclosure, there is provided the method of any one of aspects (48) to (49), wherein the raised surface does not have any other vacuum hole imprints other than the trench type vacuum hole imprints.
[0168] According to aspect (51) of the present disclosure, a method according to any one of aspects (25) to (50) is provided, wherein the recessed surface has a roughness Ra of less than 2 nm or less than 1 nm and a peak-to-valley (PV) roughness of less than 20 nm, less than 15 nm or less than 12 nm.
[0169] According to aspect (52) of the present disclosure, a method of any one of aspects (25) to (51) is provided, wherein the mirror preform comprises a thickness defined as the distance between the first major surface and the second major surface, wherein the thickness is less than or equal to about 3.0 mm, about 0.5 mm to about 3.0 mm, about 0.5 mm to about 1.0 mm, or about 1.0 mm to about 3.0 mm.
[0170] According to aspect (53) of the present disclosure, there is provided the method of any one of aspects (25) to (52), wherein the conforming step is performed at a temperature less than a glass transition temperature of the mirror preform.
[0171] According to aspect (54) of the present disclosure, a method according to any one of aspects (25) to (53) is provided, wherein during or after the conforming step, the temperature of the mirror preform or the bent mirror substrate is not raised above the glass transition temperature of the mirror preform.
[0172] According to aspect (55) of the present disclosure, a method according to any one of aspects (25) to (54) is provided, wherein the glass or glass ceramic material comprises soda lime glass, aluminosilicate, boroaluminosilicate or alkali aluminosilicate glass.
[0173] According to aspect (56) of the present disclosure, there is provided the method of any one of aspects (25) to (55), wherein the glass or glass-ceramic material is a strengthened glass material.
[0174] According to aspect (57) of the present disclosure, there is provided the method of aspect (56), wherein the glass or glass ceramic material is chemically strengthened.
[0175] According to aspect (58) of the present disclosure, there is provided a method of forming a three-dimensional mirror, the method comprising: forming a three-dimensional mirror substrate according to the method of any one of aspects (25) to (57); and disposing a reflective layer on a first major surface.
[0176] Although preferred embodiments of the present disclosure have been described, it should be understood that the described embodiments are only illustrative and the scope of the present disclosure is defined solely by the claims covering the full range of equivalents, numerous variations and modifications that would naturally occur to those skilled in the art upon reading this document.
Claims
1. A method for forming a three-dimensional mirror, the method include: Providing a two-dimensional mirror preform, the mirror preform comprising a first major surface, a second major surface opposite to the first major surface, and a minor surface connecting the first major surface and the second major surface, the mirror preform comprising glass or glass ceramic material, and the first major surface and the second major surface are two-dimensional, wherein the size of the two-dimensional mirror preform is pre-cut or shaped to a desired size that can be used as a three-dimensional mirror after three-dimensional formation; forming a chamfer on the two-dimensional mirror preform, wherein the chamfer is a C-shaped chamfer or an R-shaped chamfer, wherein when the chamfer is a C-shaped chamfer, the length of the chamfer is 0.1 mm or more, wherein when the chamfer is an R-shaped chamfer, the length of the chamfer is 0.5 mm or more; After forming the chamfer, placing the two-dimensional mirror preform on a molding device having a curved support surface so that the second major surface faces the curved support surface; and conforming the two-dimensional mirror preform to the curved support surface to form a curved mirror substrate having a convex surface corresponding to the second major surface and a concave surface corresponding to the first major surface, the concave surface having a first radius of curvature, wherein after the conforming step, the concave surface has a roughness Ra of less than 3 nm and a peak-to-valley (PV) roughness of less than 30 nm, Wherein the curved mirror substrate does not include edges that are cut, shaped, chamfered or polished during or after the conforming step.
2. The method of claim 1, wherein a cross-sectional edge profile of the secondary surface is the same as a cross-sectional edge profile of the curved mirror substrate. 3 . The method of claim 1 , wherein an edge of the first major surface includes a first chamfer and an edge of the second major surface includes a second chamfer, wherein the first chamfer and the second chamfer have different lengths.
4. The method of any one of claims 1 to 3, wherein the surface roughness of the subsurface after the conforming step is within 2% of the surface roughness of the subsurface before the conforming step.
5. The method of claim 4, wherein the surface roughness of the subsurface after the conforming step is the same as the surface roughness of the subsurface before the conforming step.
6. The method of any one of claims 1 to 3, wherein the concave surface has an aspherical shape.
7. The method of any one of claims 1 to 3, wherein the curved mirror substrate has a length of 200 mm to 400 mm and a width of 100 mm to 250 mm; a length of 250 mm to 350 mm and a width of 100 mm to 200 mm; a length of 300 mm to 350 mm and a width of 150 mm to 200 mm; or a length of 290 mm to 295 mm and a width of 130 mm to 135 mm.
8. The method of any one of claims 1 to 3, wherein a profile peak-to-valley (PV) shape accuracy on the concave surface of the curved mirror substrate is less than 100 μm or less than 50 μm.
9. The method of any one of claims 1 to 3, wherein the curved mirror substrate has at least one of the following: The arithmetic mean waviness Wa on the concave surface is less than 1 μm per 10 mm; The maximum roughness depth R on the concave surface max is less than 30 nm; and The surface roughness Ra is less than 30 nm, and the peak-to-valley (PV) roughness is less than 1 μm.
10. The method of any one of claims 1 to 3, wherein the curved support surface comprises trench-type vacuum holes.
11. The method of claim 10, wherein the trench-type vacuum holes are within 2 mm of an edge of the second major surface when the mirror preform is disposed on the molding apparatus.
12. The method of any one of claims 1 to 3, wherein after the conforming step, the raised surface includes a groove-type vacuum hole embossing within 2 mm of the edge of the raised surface along the entire edge.
13. The method of claim 12, wherein the trench-type vacuum hole embossing has a depth of less than 1 μm.
14. The method of claim 12, wherein the raised surface is free of any other vacuum hole imprints other than the trench type vacuum hole imprints.
15. The method of any one of claims 1 to 3, wherein the recessed surface has a roughness Ra of less than 2 nm and a peak-to-valley (PV) roughness of less than 20 nm.
16. The method of any one of claims 1 to 3, wherein the mirror preform comprises a thickness defined as the distance between the first major surface and the second major surface, wherein the thickness is 0.5 mm to 3.0 mm.
17. The method of any one of claims 1 to 3, wherein the conforming step is performed at a temperature less than the glass transition temperature of the mirror preform.
18. The method of any one of claims 1 to 3, wherein during or after the conforming step, the temperature of the mirror preform or the curved mirror substrate is not raised above the glass transition temperature of the mirror preform.
19. The method of any one of claims 1 to 3, wherein the glass or glass ceramic material comprises soda lime glass, aluminosilicate, boroaluminosilicate or alkali aluminosilicate glass.
20. A method of forming a three-dimensional mirror, the method include: Forming a three-dimensional mirror substrate according to the method of any one of claims 1 to 3; and A reflective layer is disposed on the first major surface.
21. A HUD mirror substrate formed by the method according to any one of claims 1 to 19, the HUD mirror substrate comprising a first main surface having a concave shape, a second main surface opposite to the first main surface and having a convex shape, and a secondary surface connecting the first main surface and the second main surface, wherein the first major surface comprises a first surface roughness Ra of 3 nm or less and a peak-to-valley (PV) roughness of less than 30 nm, wherein the mirror substrate comprises glass or glass ceramic material, wherein the subsurface comprises a cross-sectional edge profile having a chamfer, wherein the chamfer is a C-shaped chamfer or an R-shaped chamfer, wherein when the chamfer is a C-shaped chamfer, the length of the chamfer is 0.1 mm or greater, When the chamfer is an R-shaped chamfer, the length of the chamfer is 0.5 mm or greater.
22. The HUD mirror substrate of claim 21, wherein the mirror substrate has an edge that is not cut, shaped, chamfered or polished when the mirror substrate is in a bent state.
23. The HUD mirror substrate of claim 21, wherein an edge of the first major surface comprises a first chamfer, and an edge of the second major surface comprises a second chamfer, wherein the first chamfer and the second chamfer have different lengths.
24. The HUD mirror substrate of claim 21, wherein the mirror substrate comprises rounded corners in a plan view.
25. The HUD mirror substrate of claim 24, wherein the rounded corners of the mirror substrate are not shaped or polished when the mirror substrate is in a bent state.
26. The HUD mirror substrate of claim 24, wherein the concave surface has an aspherical shape.
27. The HUD mirror substrate of any one of claims 21 to 26, wherein the convex surface and the concave surface comprise symmetrical chamfers.
28. The HUD mirror substrate of any one of claims 21 to 26, wherein the mirror substrate has a length of 200 mm to 400 mm and a width of 100 mm to 250 mm; a length of 250 mm to 350 mm and a width of 100 mm to 200 mm; a length of 300 mm to 350 mm and a width of 150 mm to 200 mm; or a length of 290 mm to 295 mm and a width of 130 mm to 135 mm.
29. The HUD mirror substrate of any one of claims 21 to 26, wherein a profile peak-to-valley (PV) shape accuracy on the concave surface of the mirror substrate is less than 100 μm or less than 50 μm.
30. The HUD mirror substrate according to any one of claims 21 to 26, wherein an arithmetic mean waviness Wa on the concave surface of the mirror substrate is less than 1 μm per 10 mm.
31. The HUD mirror substrate according to any one of claims 21 to 26, wherein the surface roughness Ra of the convex surface is less than 30 nm, and the peak-to-valley (PV) roughness is less than 1 μm.
32. The HUD mirror substrate of any one of claims 21 to 26, wherein the raised surface comprises a groove-type vacuum hole imprint within 2 mm from the edge of the raised surface.
33. The HUD mirror substrate according to claim 32, wherein the depth of the groove type vacuum hole embossing is less than 1 μm.
34. The HUD mirror substrate of claim 32, wherein the raised surface is free of any other vacuum hole imprinting other than the trench type vacuum hole imprinting.
35. The HUD mirror substrate of any one of claims 21 to 26, wherein the recessed surface has a roughness Ra of less than 2 nm or less than 1 nm and a peak-to-valley (PV) roughness of less than 20 nm, less than 15 nm or less than 12 nm.
36. The HUD mirror substrate of any one of claims 21 to 26, wherein the mirror substrate comprises a thickness defined as a distance between the first major surface and the second major surface, wherein the thickness is 0.5 mm to 3.0 mm.
37. The HUD mirror substrate of any one of claims 21 to 26, wherein the glass or glass ceramic material comprises soda lime glass, aluminosilicate, boroaluminosilicate or alkali aluminosilicate glass.
38. A three-dimensional HUD mirror, include: The HUD mirror substrate according to any one of claims 21 to 26; and A reflective layer is disposed on the first major surface of the mirror substrate.