A water-cooled wall tube row, a boiler including the same, and a method for preventing high-temperature corrosion
By using the S-type first fin of alloy material and the second fin of carbon steel material in the water-cooled wall pipe row, the water-cooled wall pipe is protected by the primary battery effect, and the high-temperature corrosion problem in the prior art is solved. It achieves the effect of effectively reducing corrosion and extending service life.
Patent Information
- Application Number
- CN202110551086.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-19
- Publication Date
- 2025-02-21
- Estimated Expiration
- 2041-05-19
AI Technical Summary
The prior art has problems such as short maintenance time, high cost and serious environmental pollution in preventing high temperature corrosion, and it is difficult to effectively reduce the corrosion of water-cooled walls and extend the service life.
The water-cooled wall pipe row is adopted, including a water-cooled wall pipe arranged side by side, an S-shaped first fin and a rectangular second fin arranged alternately. The first fin material is an alloy, and the second fin and baffle material are carbon steel. , protect the water-cooled wall tube through the primary battery effect, and the baffle relieves the airflow erosion.
It effectively reduces the corrosion of water-cooled walls, extends service life, simplifies processes, improves economic benefits, and reduces environmental pollution.
Smart Images

Figure CN113237088B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of pulverized coal boilers and relates to a water-cooled wall resistant to high-temperature corrosion, and in particular to a water-cooled wall tube row and a pulverized coal boiler comprising the same, and a method for resistant to high-temperature corrosion. Background Art
[0002] In recent years, as boilers develop towards larger capacity and higher parameters, the temperature of the boiler water-cooled wall has increased accordingly, resulting in a more serious problem of high-temperature corrosion of the water-cooled wall. In order to reduce the amount of NOx generated, most power plants currently use staged air supply or low-oxygen combustion, which makes it easy for the area near the water-cooled wall to form a reducing atmosphere, which in turn leads to high-temperature corrosion of the water-cooled wall. If the water-cooled wall is thinned to a certain extent, it will cause a boiler tube burst accident, posing a serious threat to the safe and economical operation of the boiler unit.
[0003] The water-cooled wall heating surface of the pulverized coal boiler thermal power unit is located in a harsh environment. The corrosion of the water-cooled wall in the deposited coal ash is molten salt corrosion under the combined action of reducing and corrosive gases under anoxic conditions, and the largest proportion is sulfide-type corrosion. The outer wall of the heating surface is subjected to the erosion of flames containing a large amount of unburned coal powder for a long time, causing high-temperature corrosion on the heating surface, resulting in a reduction in the effective thickness of the wall, a decrease in the effective load-bearing capacity, and the matrix no longer having the required various good high-temperature mechanical properties.
[0004] CN103712234A discloses a seal between T-shaped water-cooled walls, which is composed of sealing fin A, sealing fin B, sealing fin C and a semicircular arc seal, wherein one end of sealing fin A and sealing fin B are respectively connected to the two ends of the semicircular arc seal, and one end of sealing fin C is connected to the top of the middle part of the semicircular arc seal. The angle between sealing fin A and sealing fin C, and the angle between sealing fin B and sealing fin C are both 90°. The diameter of the semicircular arc seal is equal to the diameter of the water-cooled wall tube. All connections between the semicircular arc seal, sealing fin A, sealing fin B, sealing fin C, water-cooled wall tube, and water-cooled wall tube fins are welded.
[0005] CN110030545A discloses an anti-corrosion and wear-resistant membrane water-cooled wall structure, comprising a membrane water-cooled wall body, which is formed by welding a plurality of water-cooled wall tubes and fins in parallel. The outer surface of the membrane water-cooled wall body facing the fire side is coated with a weldable metal coating, an anti-corrosion and wear-resistant metal coating and an inorganic sealing agent coating in sequence from the inside to the outside; the outer surface of the water-cooled wall tube facing the fire side is spot-welded with a plurality of welding spots to tightly bond the weldable metal coating to the outer surface of the water-cooled wall tube and the fin facing the fire side, and to tightly bond the anti-corrosion and wear-resistant metal coating to the outer surface of the weldable metal coating.
[0006] CN212430931U provides a biomass boiler membrane water-cooled wall sprayed with a high-temperature wear-resistant and anti-corrosion coating, including a body of the biomass boiler membrane water-cooled wall, a sandblasting coating and a ceramic coating. The body of the biomass boiler membrane water-cooled wall is welded by a water-cooled wall tube and a fin; the surface of the body of the biomass boiler membrane water-cooled wall is a sandblasting coating with a thickness of 0.6 to 0.7 mm; the outer side of the sandblasting coating is a ceramic coating, and the ceramic coating material is Si3N4 with a thickness of 3 to 4 mm. The water-cooled wall tube uses 20 / GB3087 round seamless steel pipe. The steel pipe wall thickness of the water-cooled wall tube is 4 to 5 mm, and the outer diameter is 60 to 70 mm. The material selected for the fin is Q235B membrane wall steel plate. The body of the biomass boiler membrane water-cooled wall with a sandblasting coating and a ceramic coating is a body that has been ground and polished.
[0007] The above-reported patents mainly use corrosion-resistant coating technologies such as spraying to form a protective layer on the surface of the tube wall. The disadvantages are that the maintenance time is short, the spraying cost is high, and the gas generated by the spraying is toxic and easily causes environmental pollution. Therefore, how to effectively reduce the corrosion of the water-cooled wall, extend the service life, simplify the process, improve the economic effect, and reduce environmental pollution has become an urgent problem to be solved. Summary of the invention
[0008] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a water-cooled wall tube row and a boiler including the same, as well as a method for preventing high-temperature corrosion, which can effectively reduce the corrosion of the water-cooled wall, extend the service life, and have higher economic benefits.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a water-cooled wall tube row, the water-cooled wall tube row comprising at least three water-cooled wall tubes arranged side by side, two adjacent water-cooled wall tubes being connected by fins, the fins being divided into S-shaped first fins and rectangular second fins, the first fins and the second fins being arranged alternately, the outer wall of the second fin being provided with a baffle, the baffle being arranged perpendicular to the second fin, the material of the first fin comprising an alloy, and the material of the water-cooled wall tube comprising carbon steel.
[0011] The first fin in the water-cooled wall tube row provided by the present invention adopts an "S"-shaped structure, which is conducive to absorbing thermal expansion, reducing the tension of the weld between the fin and the water-cooled wall tube, and increasing the heat exchange area. The setting of the baffle on the outer wall of the second fin can alleviate the scouring of the water-cooled wall by the airflow, reducing the risk of high-temperature fatigue cracks and overheating of the tube wall.
[0012] As a preferred technical solution of the present invention, the alloy material of the first fin includes any one of aluminum alloy, zinc alloy, indium alloy, titanium alloy or cadmium alloy, or a combination of at least two of them.
[0013] As a preferred technical solution of the present invention, the thickness of the first fin is 5 to 10 mm, for example, it can be 5 mm, 5.5 mm, 5.8 mm, 6 mm, 6.2 mm, 6.5 mm, 6.8 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 8.8 mm, 9 mm, 9.2 mm, 9.5 mm or 10 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] Preferably, the first fin is an integrally formed structure.
[0015] It should be noted that the material of the first fin provided in the present invention can be an alloy of different metals according to specific working conditions. For example, all the first fins are made of the same metal alloy, or part of the first fin is made of an alloy of one metal and the other part is made of an alloy of another metal.
[0016] As a preferred technical solution of the present invention, the material of the second fin includes carbon steel.
[0017] Preferably, the thickness of the second fin is 5 to 10 mm, for example, it can be 5 mm, 5.5 mm, 5.8 mm, 6 mm, 6.2 mm, 6.5 mm, 6.8 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, 8.8 mm, 9 mm, 9.2 mm, 9.5 mm or 10 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] As a preferred technical solution of the present invention, the material of the baffle includes carbon steel.
[0019] Preferably, the thickness of the baffle is 3 to 6 mm, for example, it can be 3 mm, 3.2 mm, 3.5 mm, 3.8 mm, 4 mm, 4.2 mm, 4.5 mm, 4.8 mm, 5 mm, 5.3 mm, 5.5 mm, 5.7 mm or 6 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] As a preferred technical solution of the present invention, the distance between two adjacent water-cooled wall tubes is 10-15 mm, for example, it can be 10 mm, 10.5 mm, 10.8 mm, 11 mm, 11.2 mm, 11.5 mm, 11.8 mm, 12 mm, 12.5 mm, 13 mm, 13.5 mm, 13.8 mm, 14 mm, 14.2 mm, 14.5 mm or 15 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] In a second aspect, the present invention provides a boiler comprising the water-cooled wall tube row as described in the first aspect, wherein the boiler comprises a furnace body, at least part of the surface of the furnace body is provided with the water-cooled wall tube row, a baffle is provided on the outer wall of the heating surface side of the second fin, and coal ash is deposited on the surface of the water-cooled wall tube row.
[0022] The boiler provided by the present invention has a water-cooled wall tube row arranged on at least part of its surface, wherein the water-cooled wall tube and the fin are seamlessly connected, thereby increasing the heat exchange area; the baffle on the second fin can alleviate the scouring of the water-cooled wall by the airflow, withstand the stress caused by the high temperature of the furnace and the negative pressure fluctuation of the furnace, and reduce the probability of tube burst accidents.
[0023] It should be noted that the baffle in the boiler provided in the present invention is vertically arranged on the heating surface side of the second fin, wherein the heating surface refers to the metal surface for heat exchange of the boiler on the side in contact with the flame or smoke, that is, the baffle provided in the present invention is arranged on the side close to the boiler surface. The arrangement of the baffle can alleviate the scouring of the water-cooled wall by the airflow, and reduce the risk of high-temperature fatigue cracks and overheating of the tube wall.
[0024] As a preferred technical solution of the present invention, the coal ash includes molten salt.
[0025] As a preferred technical solution of the present invention, the molten salt includes any one of sulfate, silicate or sodium salt, or a combination of at least two of them.
[0026] It should be noted that in the boiler provided by the present invention, water-cooled wall tube rows can be arranged on the surface of key corrosion-prone areas, or cold wall tube rows can be arranged throughout the furnace, both of which can play a protective role. When coal powder is burned in the boiler, the melted or semi-melted coal powder particles entrained in the flue gas collide, condense and settle, and the coal ash includes salts with low melting points such as sulfates, silicates or sodium salts.
[0027] In a third aspect, the present invention provides a method for preventing high temperature corrosion of the boiler according to the second aspect, the method comprising:
[0028] A galvanic cell effect is formed between the first fin and the adjacent water-cooled wall tube, wherein the first fin corrodes as an anode, the water-cooled wall tube is protected as a cathode, and the molten salt deposited on the surface of the water-cooled wall tube row serves as an electrolyte for the galvanic cell reaction.
[0029] The method for preventing high temperature corrosion of the boiler provided by the present invention is that the activity of the alloy material used for the first fin is higher than that of the water-cooled wall pipe made of carbon steel, and the first fin is seamlessly and tightly welded to the water-cooled wall pipe, and the molten salt deposited on the pipe wall is used as an electrolyte, which is equivalent to forming a large number of galvanic cell effects. The water-cooled wall pipe is protected as a cathode, and the first fin is corroded and gradually thinned as an anode.
[0030] It should be noted that the order of activity of the alloy materials in the present invention is determined based on the standard electrode potential of the metal reaction in a neutral solution. The smaller the standard electrode potential, the stronger the activity and the easier it is to react with other substances. The alloy material used in the first fin provided by the present invention is more active than the carbon steel material of the water-cooled wall tube, and is therefore more likely to react.
[0031] It should also be noted that the first fins and the second fins on the water-cooled wall tube row provided by the present invention are arranged alternately, wherein a galvanic effect is formed between the first fin and two adjacent water-cooled wall tubes, which plays a role in protecting the water-cooled wall tubes. The second fins and the water-cooled wall tubes are made of the same material, so they do not react, ensuring that the first fins react only with the water-cooled wall tubes at both ends.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention provides a water-cooled wall tube row, a boiler including the same, and a method for preventing high-temperature corrosion. Since the first fin of the alloy material is seamlessly and tightly welded to the water-cooled wall tube, and the activity of the alloy material is higher than that of carbon steel, a large amount of galvanic effect will be generated under the condition of molten salt deposition on the tube wall, and the water-cooled wall tube as the cathode is protected from corrosion. The fins are conducive to absorbing thermal expansion and increasing the heat exchange area. The setting of the baffle can alleviate the scouring of the water-cooled wall by the airflow, reducing the risk of high-temperature fatigue cracks and overheating of the tube wall. After a certain period of reaction, the fins become thinner and their service life ends. At this time, only the damaged fins need to be replaced, and there is no need to replace the water-cooled wall tubes that are subjected to high pressure, which simplifies maintenance work. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A top view of the structure of a water-cooled wall tube row provided in a specific embodiment of the present invention.
[0035] Among them, 1-water-cooled wall tube; 2-first fin; 3-second fin; 4-baffle. DETAILED DESCRIPTION
[0036] It should be understood that, in the description of the present invention, the terms "longitudinal", "lateral", "upper", "lower", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0037] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0038] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementations:
[0039] In a specific embodiment, the present invention provides a water-cooled wall tube row, such as Figure 1 As shown, the water-cooled wall tube row includes at least three water-cooled wall tubes 1 arranged side by side, and two adjacent water-cooled wall tubes 1 are connected by fins. The fins are divided into S-shaped first fins 2 and rectangular second fins 3, and the first fins 2 and the second fins 3 are arranged alternately. The material of the water-cooled wall tubes 1 includes carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 10 to 15 mm. The first fin 2 is an integrally formed structure, and the material includes any one of aluminum, zinc, indium, titanium or cadmium or a combination of at least two of them. The thickness of the first fin 2 is 5 to 10 mm. The material of the second fin 3 includes carbon steel, and the thickness is 5 to 10 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel, and the thickness is 3 to 6 mm.
[0040] In a specific embodiment, the present invention provides a boiler including a water-cooled wall tube row provided in a specific embodiment, wherein the boiler includes a furnace body, wherein the water-cooled wall tube row is arranged on at least a part of the surface of the furnace body. A first fin 2 and a second fin 3 are alternately arranged between two adjacent water-cooled wall tubes 1 of the water-cooled wall tube row, and a baffle 4 is vertically arranged on the outer wall of the heating surface side of the second fin 3. Coal ash is deposited on the surface of the water-cooled wall tube row, and the coal ash component includes a molten salt of any one of sulfate, silicate or sodium salt or a combination of at least two of them.
[0041] In another specific embodiment, the present invention provides a method for preventing high temperature corrosion of a boiler provided in a specific embodiment, specifically comprising:
[0042] By using first fins 2 and water-cooled wall tubes 1 made of different materials, a closed-loop galvanic cell is formed between the first fins 2 and adjacent water-cooled wall tubes 1, wherein the first fins 2 corrode as an anode, the water-cooled wall tubes 1 are protected as cathodes, and the molten salt deposited on the surface of the water-cooled wall tube row serves as an electrolyte for the galvanic cell reaction.
[0043] Example 1
[0044] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 15 mm. The first fins 2 are all made of aluminum alloy with a thickness of 5 mm. The second fins 3 are made of carbon steel with a thickness of 5 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 6 mm.
[0045] Example 2
[0046] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 14 mm. The first fins 2 are all made of zinc alloy with a thickness of 6 mm. The second fins 3 are made of carbon steel with a thickness of 6 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 5 mm.
[0047] Example 3
[0048] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 13 mm. The first fins 2 are all made of indium alloy with a thickness of 7 mm. The second fins 3 are made of carbon steel with a thickness of 7 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 4 mm.
[0049] Example 4
[0050] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 12 mm. The first fins 2 are all made of titanium alloy with a thickness of 8 mm. The second fins 3 are made of carbon steel with a thickness of 8 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 4 mm.
[0051] Example 5
[0052] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 10 mm. The first fins 2 are all made of cadmium alloy with a thickness of 10 mm. The second fins 3 are made of carbon steel with a thickness of 10 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 3 mm.
[0053] Example 6
[0054] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 15 mm. The first fins 2 are all made of aluminum-titanium alloy with a thickness of 5 mm. The second fins 3 are made of carbon steel with a thickness of 5 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 6 mm.
[0055] Example 7
[0056] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 14 mm. The first fins 2 are all made of aluminum-zinc alloy with a thickness of 6 mm. The second fins 3 are made of carbon steel with a thickness of 6 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 5 mm.
[0057] Example 8
[0058] In the present embodiment, a water-cooled wall tube row is provided, including nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 15 mm. Two of the first fins 2 are made of aluminum alloy, and the rest are made of zinc alloy, and the thickness is 5 mm. The second fin 3 is made of carbon steel with a thickness of 5 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 6 mm.
[0059] Example 9
[0060] In the present embodiment, a water-cooled wall tube row is provided, comprising nine water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 15 mm. Two of the first fins 2 are made of zinc alloy, and the rest are made of titanium alloy, and the thickness is 5 mm. The second fin 3 is made of carbon steel with a thickness of 5 mm. The outer wall of the second fin 3 is vertically provided with a baffle 4 made of carbon steel with a thickness of 6 mm.
[0061] Example 10
[0062] In the present embodiment, a boiler is provided, in which water-cooled wall tube rows are arranged in key corrosion-prone areas of the furnace body. The water-cooled wall tube row includes thirteen water-cooled wall tubes 1 arranged side by side, and S-shaped first fins 2 and rectangular second fins 3 are alternately arranged between two adjacent water-cooled wall tubes 1. Sulfate is deposited on the surface of the water-cooled wall tube row. The water-cooled wall tubes 1 are made of carbon steel, and the distance between two adjacent water-cooled wall tubes 1 is 15 mm. The first fin 2 is made of aluminum alloy with a thickness of 5 mm. The second fin 3 is made of carbon steel with a thickness of 5 mm. A baffle 4 made of carbon steel with a thickness of 6 mm is vertically arranged on the outer wall of the heating surface side of the second fin 3.
[0063] The water-cooled wall tube row and the boiler including the same and the high-temperature corrosion prevention method provided by the present invention, because the first fins 2 of different materials are seamlessly and tightly welded to the water-cooled wall tube 1, and the activity of the alloy material is higher than that of carbon steel, a large amount of galvanic effect will be generated under the condition of molten salt deposition on the tube wall, and the water-cooled wall tube 1 as the cathode is protected from corrosion. The setting of the baffle 4 can alleviate the scouring of the water-cooled wall tube 1 by the airflow, reducing the risk of high-temperature fatigue cracks and overheating of the tube wall.
[0064] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A water-cooled wall tube bank, characterized in that: The water-cooled wall tube row includes at least three water-cooled wall tubes arranged side by side, and two adjacent water-cooled wall tubes are connected by fins. The fins are divided into S-shaped first fins and rectangular second fins. The first fins and the second fins are arranged alternately. The outer wall of the second fin is provided with a baffle, and the baffle is arranged vertically with the second fin. The material of the first fin includes alloy, and the material of the water-cooled wall tube includes carbon steel.
2. The water-cooled wall tube bank according to claim 1, characterized in that: The material of the first fin includes any one of aluminum alloy, zinc alloy, indium alloy, titanium alloy or cadmium alloy, or a combination of at least two thereof.
3. The water-cooled wall tube bank according to claim 1, characterized in that: The thickness of the first fin is 5-10 mm.
4. The water-cooled wall tube bank according to claim 1, characterized in that: The first fin is an integrally formed structure.
5. The water-cooled wall tube bank according to claim 1, characterized in that: The distance between two adjacent water-cooled wall tubes is 10-15 mm.
6. A boiler comprising the water-cooled wall tube bank according to any one of claims 1 to 5, characterized in that: The boiler comprises a furnace body, at least part of the surface of which is provided with water-cooled wall tube rows, the outer wall of the second fin heating surface side is provided with a baffle, and coal ash is deposited on the surface of the water-cooled wall tube rows.
7. The boiler according to claim 6, characterized in that The coal ash includes molten salt.
8. The boiler according to claim 7, characterized in that: The molten salt includes any one of sulfate, silicate or sodium salt or a combination of at least two of them.
9. A method for preventing boiler from high temperature corrosion according to any one of claims 6 to 8, the method for preventing boiler from high temperature corrosion comprising: A galvanic cell effect is formed between the first fin and the adjacent water-cooled wall tube, wherein the first fin corrodes as an anode, the water-cooled wall tube is protected as a cathode, and the molten salt deposited on the surface of the water-cooled wall tube row serves as an electrolyte for the galvanic cell reaction.
Citation Information
Patent Citations
T-shaped sealing element among water cooling walls
CN103712234A
Anti-corrosion wear-resistant membrane type water-cooled wall structure
CN110030545A
Biomass boiler membrane type water cooling wall sprayed with high-temperature wear-resistant anticorrosive coating
CN212430931U
Water-cooled wall tube bundle and boiler comprising same
CN214949187U