A boiler steam-water system corrosion simulation experimental device and experimental method

By designing a boiler steam and water system corrosion simulation experimental device with heating furnace, reactor, cooling tube and sample hanger, the problem of metal corrosion in traditional devices cannot simulate high temperature and high pressure environments is solved, and corrosion experiments and water are realized for different parts of the boiler The evaluation of the corrosion-resistant effect of the treatment agent improves the experimental efficiency and ease of operation.

CN113237824BActive Publication Date: 2024-11-05CHINA SPECIAL EQUIP INSPECTION & RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110630065.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-07
Publication Date
2024-11-05
Estimated Expiration
2041-06-07

AI Technical Summary

Technical Problem

The traditional boiler steam and water system simulation experimental device cannot simulate metal corrosion of boiler water supply system, superheater and reheater in high temperature and high pressure environments, and cannot effectively study the corrosion conditions of different components under high temperature and high pressure.

Method used

A corrosion simulation experimental device for boiler steam system including heating furnace, reactor, cooling tube, sample hanger and high-pressure gas cylinder was designed. By rotating the sample hanger for 72 hours, the corrosion experiment was carried out at a constant temperature and pressure. And use cooling tubes and suction tubes to achieve rapid cooling and sample sampling.

Benefits of technology

Metal corrosion simulation experiments on different parts of the boiler under high temperature and high pressure environment can be achieved, and the corrosion inhibition effect and high temperature stability of boiler water treatment agents can be evaluated, improving experimental efficiency and simplicity of operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113237824B_ABST
    Figure CN113237824B_ABST
Patent Text Reader

Abstract

The present invention discloses a boiler steam-water system corrosion simulation experimental device and an experimental method thereof, comprising a heating furnace, a reactor, a cooling pipe, a reactor cover and a sample hanger, wherein the heating furnace is provided with a reactor, the reactor is provided with a cooling pipe, the cooling pipe realizes cooling in the reactor through cooling water circulation of an external water tank, and a rotatable sample hanger device is provided on the reactor cover of the reactor. The present invention can realize metal corrosion experiments in a steam-water environment with a relatively high temperature and pressure, the cooling pipe in the reactor can realize accelerated cooling, the suction pipe can realize fast and simple sampling, and can be used to simulate metal corrosion of boiler feed water systems, superheaters, reheaters and other systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of boiler experimental equipment, and in particular to a boiler steam-water system corrosion simulation experimental device and an experimental method thereof. Background Art

[0002] When metals in boiler steam-water system come into contact with water and steam at higher temperature, chemical and electrochemical reactions will occur, which will damage the metals and cause metal corrosion. This is a common phenomenon in boiler steam-water system, which is easy to cause accidents such as failure of heating surface, and has a significant impact on the operation of the entire boiler system. The temperature, pressure and medium environment of different parts of the boiler are different, resulting in different corrosion laws and corrosion mechanisms of different parts. When the boiler does not have a deoxygenation system or the deoxygenation is not thorough, the oxygen content in the water is high, forming a primary battery with the metal, electrochemical reaction and a series of chemical reactions, which lead to metal corrosion. Generally, dissolved oxygen corrosion is prone to occur in the feed water pipe and economizer inlet; because the boiler feed water contains free carbon dioxide and carbonates in the water decompose to produce carbon dioxide and other gases, which are dissolved in water to form carbonic acid, the water quality pH is significantly reduced, resulting in acid corrosion of metals. The boiler feed water system and condensate system are prone to carbon dioxide corrosion due to the high concentration of carbon dioxide; and superheated steam with a temperature higher than 450°C can react chemically with metals to form metal oxides, leading to metal corrosion. Generally, superheaters and reheaters are prone to water vapor corrosion.

[0003] However, in the conventional technology, a rotating coupon corrosion test device is usually used to simulate the corrosion of metals in the boiler circulating water system. The device includes a base and a constant temperature water tank fixed on the base. A plurality of experimental beakers are placed in the constant temperature water tank. A rotatable sample hanger corresponding to the experimental beakers is provided on the upper side of the constant temperature water tank. A coupon can be detachably connected to the fixing rod of the stirring paddle to perform the coupon corrosion test. The rotating coupon corrosion test device can only simulate metal corrosion experiments under normal pressure, and the temperature is usually below 100°C. Therefore, the corrosion coupon test can only simulate the metal corrosion of the boiler feed water system under normal pressure, and cannot realize the metal corrosion simulation experiment of the boiler condensate system, superheater and reheater. Therefore, in order to study the corrosion of metal materials of different parts of the boiler under high temperature and high pressure, a boiler steam-water system corrosion simulation test device is needed. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcoming that the existing metal corrosion simulation experiment cannot be carried out in the high temperature and high pressure steam-water environment of the boiler feed water system, superheater and reheater system, and propose a boiler steam-water system corrosion simulation experiment device and its experimental method.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] The invention comprises a heating furnace, a reactor, a cooling pipe, a reactor cover and a sample rack. The reactor is arranged in the heating furnace, and the reactor is provided with a cooling pipe. The cooling pipe realizes cooling of the reactor through the cooling water circulation of an external water tank, and a rotatable sample rack device is arranged on the reactor cover.

[0007] Furthermore, the rotatable sample rack comprises a motor, a belt and a sample rack, the output end of the motor is connected to the rotating shaft of the sample rack through the pulley, and the sample rack is vertically arranged in the reactor.

[0008] Furthermore, the sample rack is multi-layered.

[0009] Furthermore, a gas phase valve is provided at the outlet end of the reactor, an external high-pressure gas cylinder is connected to the gas phase valve of the reactor, and gas is introduced into the reactor through an air inlet pipe.

[0010] Furthermore, a safety component is provided at the outlet end of the reactor.

[0011] Furthermore, a temperature measuring tube is provided in the reactor to measure the reaction temperature in the reactor.

[0012] A boiler steam-water system corrosion simulation experimental method comprises the following steps:

[0013] A. Add the experimental medium into the reactor, place the metal sample on the sample rack, and place it in the reactor;

[0014] B. Make the sample be located in the liquid phase, gas-liquid interface and gas phase corresponding to the sample rack;

[0015] C. Cover the reactor lid to make the reactor seal intact, introduce nitrogen into the reactor through the air inlet pipe, and then heat it to the experimental temperature through the heating furnace. Start the experiment after the temperature and pressure are stable;

[0016] D drives the sample rack to rotate slowly through the rotating shaft, reacts at a constant temperature and pressure for 72 hours, turns off the heating furnace, cools down, and takes out the sample to collect its corrosion data after it cools to room temperature.

[0017] Furthermore, the experimental medium is deionized water.

[0018] Furthermore, in a metal corrosion experiment simulating a boiler condensate system, the sample was placed in the gas phase in the kettle, and the medium in the reactor was heated to steam. After reacting for 72 hours, the cooling pipe in the reactor was opened to cool it to 80°C to form condensate on the surface of the metal sample. The reaction was continued for 72 hours, and the sample was taken out.

[0019] Furthermore, the method for evaluating the corrosion inhibition performance of the boiler water treatment agent comprises adding an experimental medium and a water treatment agent into a reactor, hanging a metal sample on a sample hanger, placing the metal sample in the reactor, covering the reactor cover, introducing nitrogen into the reactor through an air inlet pipe, and then heating the reactor to an experimental temperature through a heating furnace, reacting at a constant temperature and pressure for 72 hours, cooling the sample naturally, taking out the sample, and evaluating the corrosion inhibition effect of the boiler water treatment agent by comparing the corrosion conditions of the sample with and without the water treatment agent;

[0020] Furthermore, after the experiment, the medium in the reactor was taken out through a suction pipe, and the high-temperature stability of the boiler water treatment agent was analyzed by the changes in the medium composition before and after the experiment.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention can realize metal corrosion experiments in a relatively high temperature and pressure steam-water environment. The cooling pipe in the kettle can realize accelerated cooling, and the suction pipe can realize fast and simple sampling. It can be used to simulate the metal corrosion of boiler feed water systems, superheaters, reheaters, condensate water and other systems, and can also be used to evaluate the corrosion inhibition effect of boiler water treatment agents and their high-temperature stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the main structure of a boiler steam-water system corrosion simulation experimental device proposed by the present invention;

[0024] In the figure: 1-heating furnace, 2-reactor, 3-cooling pipe, 4-temperature measuring tube, 5-safety component, 6-motor, 7-rotating shaft, 8-pulley, 9-belt, 10-gas phase valve, 11-liquid phase valve, 12-hanging rack, 13-suction pipe, a-burst valve port, b1 / b2-cooling water inlet and outlet. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0026] Reference Figure 1 As shown, the present invention includes a heating furnace, a reactor, a cooling pipe, a reactor cover and a sample rack. The heating furnace is provided with a reactor, and the reactor is provided with a cooling pipe. The cooling pipe realizes cooling of the reactor through the cooling water circulation of an external water tank, and a rotatable sample rack device is provided on the reactor cover.

[0027] In this embodiment, the rotatable sample rack includes a motor, a belt and a sample rack. The output end of the motor is connected to the rotating shaft of the sample rack through the pulley, and the sample rack is vertically arranged in the reactor.

[0028] In this embodiment, the sample rack is multi-layered and is used to collect data of different phases in the reactor.

[0029] In this embodiment, an electric heating furnace is used to facilitate rapid heating.

[0030] In this embodiment, a gas phase valve is provided at the outlet end of the reactor, and an external high-pressure gas cylinder is connected to the gas phase valve of the reactor. Gas is introduced into the reactor through an air inlet pipe to remove dissolved oxygen in the experimental medium. At the same time, the reactor can be pressurized to different pressures to simulate different corrosion environments.

[0031] In this embodiment, a safety component is provided at the outlet of the reactor, which can quickly release the pressure when the pressure in the reactor is too high.

[0032] In this embodiment, the reactor is provided with a temperature measuring tube for measuring the reaction temperature in the reactor, and one or more temperature measuring tubes may be provided.

[0033] A boiler steam-water system corrosion simulation experimental method comprises the following steps:

[0034] A. Add the experimental medium into the reactor, place the metal sample to be tested on the sample rack, and place it in the reactor;

[0035] B. placing the sample in the liquid phase, gas-liquid interface and gas phase positions corresponding to the sample rack;

[0036] C. Cover the reactor lid to make the reactor seal intact, introduce nitrogen into the reactor through the air inlet pipe, and then heat it to the experimental temperature through the heating furnace. Start the experiment after the temperature and pressure are stable;

[0037] D drives the sample hanger to rotate slowly through the rotating shaft. After reacting for 72 hours at constant temperature and pressure, the heating furnace is turned off and cooled. After it cools to room temperature, the sample is taken out for metal corrosion data collection and corrosion inhibition evaluation of boiler water treatment agents.

[0038] The boiler steam-water system corrosion simulation experimental device includes a reactor, a cooling pipe, a reactor cover, a sample hanger and a high-pressure gas cylinder. The electric heating furnace heats the temperature in the reactor to the experimental temperature. There is a temperature measuring tube in the reactor to monitor the temperature in the reactor in real time; the cooling pipe mainly includes the cooling pipe in the reactor and an external water tank, and the cooling of the reactor is achieved through the cooling water circulation of the external water tank; the sample hanger is divided into three layers, connected to the reactor cover through a rotating shaft, and placed in the reactor. The metal sample can be hung on different layers of the sample hanger to place it at different heights in the reactor; the high-pressure gas cylinder is connected to the gas phase valve of the reactor, and gas is introduced into the reactor through the air inlet pipe.

[0039] In this embodiment, the experimental medium is deionized water.

[0040] In this embodiment, when simulating the metal corrosion experiment of the boiler condensate system, the medium in the reactor is heated to the form of water vapor. After reacting for 72 hours, the cooling pipe in the reactor is opened to cool it to 80°C to form condensate on the surface of the metal sample. The reaction is continued for 72 hours and the sample is taken out.

[0041] The method for evaluating the corrosion inhibition performance of the boiler water treatment agent in this embodiment includes adding an experimental medium and a water treatment agent into a reactor, hanging a metal sample on a sample hanger, placing the metal sample in the reactor, covering the reactor cover, introducing nitrogen into the reactor through an air inlet pipe, and then heating the reactor to an experimental temperature through a heating furnace. After reacting for 72 hours at a constant temperature and pressure, the sample is naturally cooled, and the corrosion inhibition effect of the boiler water treatment agent is evaluated according to the corrosion condition of the sample.

[0042] In this embodiment, the medium in the reactor is taken out through a suction pipe before and after the reaction, and the high-temperature stability of the boiler water treatment agent is analyzed by the changes in the medium composition before and after the experiment.

[0043] Boiler steam-water system corrosion test method: add the experimental medium (pure water) to the reactor, hang the metal sample on the sample rack, place it in the reactor, make the sample in the liquid, gas-liquid interface and gas phase respectively, cover the reactor cover, introduce nitrogen into the reactor through the air inlet pipe, control the pressure in the reactor at 101-400kPa, and then heat it to the experimental temperature through the heating furnace; drive the sample rack to rotate slowly through the rotating shaft, react at constant temperature and pressure for 72 hours, turn off the heating furnace, cool it, and take out the sample after it drops to room temperature. In addition, when simulating the metal corrosion experiment of the boiler condensate system, adjust the pressure and temperature in the reactor to a certain value so that the medium in the reactor is in the form of water vapor. After 72 hours of reaction, open the cooling pipe in the reactor to cool it to 80°C, so that condensed water forms on the surface of the metal sample, continue to react for 72 hours, and take out the sample.

[0044] Experimental method for evaluating boiler water treatment agents: add experimental medium (pure water) and a certain concentration of water treatment agent into the reactor, hang the metal sample on the sample rack, place it in the reactor, cover the reactor cover, introduce nitrogen into the reactor through the air inlet pipe, control the pressure in the reactor at 101-400kPa, and then heat it to the experimental temperature through a heating furnace; after reacting at a constant temperature and pressure for 72 hours, cool it naturally, take out the sample, and evaluate the corrosion inhibition effect of the boiler water treatment agent through the corrosion condition of the sample; in addition, take out the medium in the reactor through the suction pipe, and analyze the high-temperature stability of the boiler water treatment agent through the changes in the medium composition before and after the experiment.

[0045] The simulation experimental device of the present invention can withstand a maximum pressure of 20MPa and a maximum operating temperature of 550°C. It can realize corrosion simulation experiments on different components of the boiler steam-water system. There are cooling pipes in the reactor to simulate the corrosion of the boiler condensate system. Therefore, this experimental device is conducive to studying the behavior, law and mechanism of metal corrosion in the entire boiler steam-water system; the cooling pipe in the reactor can speed up the cooling speed, save cooling time, and improve the experimental efficiency; the suction pipe in the reactor makes sampling during or after the experiment convenient and easy to operate. In addition, this experimental device can also be used to evaluate the corrosion inhibition effect and stability of boiler water treatment agents under high temperature and high pressure.

[0046] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A boiler steam-water system corrosion simulation experiment method, the boiler steam-water system corrosion simulation experiment device used in the method includes a reactor, a cooling pipe, a reactor cover, a sample rack and a high-pressure gas cylinder, an electric heating furnace, the temperature in the reactor is heated to the experimental temperature, and a temperature measuring tube is provided in the reactor to monitor the temperature in the reactor in real time; the cooling pipe mainly includes a cooling pipe in the reactor and an external water tank, and the cooling of the reactor is achieved by circulating cooling water in the external water tank; the sample rack is divided into three layers, connected to the reactor cover through a rotating shaft, and placed in the reactor, and the metal sample is hung on different layers of the sample rack so that it is at different heights in the reactor; the high-pressure gas cylinder is connected to the gas phase valve of the reactor, and gas is introduced into the reactor through the air inlet pipe, including the following steps: A. Add the experimental medium into the reactor, place the metal sample on the sample rack, and place it in the reactor; B. Make the sample be located in the liquid phase, gas-liquid interface and gas phase corresponding to the sample rack; C. Cover the reactor lid to make the reactor seal intact, introduce nitrogen into the reactor through the air inlet pipe, and then heat it to the experimental temperature through the heating furnace. After the temperature and pressure are stable, start the experiment; D. The sample rack is driven to rotate slowly by the rotating shaft, and the reaction is carried out at a constant temperature and pressure for 72 hours. The heating furnace is turned off and cooled. After the sample is cooled to room temperature, the sample is taken out to collect its corrosion data; In the metal corrosion experiment simulating the boiler condensate system, the sample is placed in the gas phase in the kettle, and the medium in the reactor is heated to water vapor. After reacting for 72 hours, the cooling pipe in the reactor is opened to cool to 80°C, so that condensed water is formed on the surface of the metal sample. The reaction is continued for 72 hours, and the sample is taken out; When evaluating the corrosion inhibition performance of boiler water treatment agents, add experimental media and water treatment agents into the reactor, hang the metal sample on the sample rack, place it in the reactor, cover the reactor cover, introduce nitrogen into the reactor through the air inlet pipe, and then heat it to the experimental temperature through a heating furnace. After reacting at a constant temperature and pressure for 72 hours, cool it naturally, take out the sample, and evaluate the corrosion inhibition effect of the boiler water treatment agent by comparing the corrosion conditions of the sample with and without the water treatment agent.

2. A boiler steam-water system corrosion simulation experimental method according to claim 1, characterized in that: After the experiment, the medium in the reactor was taken out through the suction tube, and the high-temperature stability of the boiler water treatment agent was analyzed based on the changes in the medium composition before and after the experiment.