Test apparatus and test methods for measuring the hoop tensile properties of composite pipes used in structural engineering

By designing a test device for composite pipes, the bending and friction problems in the measurement of the circumferential tensile performance of composite pipes are solved by using tensile arc steel blocks and needle roller structures, and high-precision and versatility measurements are achieved As a result, it is suitable for composite pipes of different sizes.

CN113252453BActive Publication Date: 2024-11-15SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202110662927.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-15
Publication Date
2024-11-15
Estimated Expiration
2041-06-15

AI Technical Summary

Technical Problem

The existing test methods for measuring the circumferential tensile properties of composite pipes have problems of bending and friction, resulting in large measurement errors and poor adaptability to pipe diameter deviations, making it impossible to accurately measure the circumferential elastic mode of composite pipes. quantity, Poisson's ratio and circumferential ultimate tensile strain.

Method used

A test device including tensile arc steel blocks, fixed arc steel blocks, screws, connecting nodes, support rods and traction mechanisms was designed. The spacing between steel blocks is adjusted by cross-shaped screws, and the arc is kept unchanged using a roller needle to reduce the Friction force ensures that the test section of the annular sample maintains its original arc during the stretching process, and combines lubricating oil to reduce the impact of friction.

Benefits of technology

Achieve high-precision and versatile measurements, suitable for composite pipes of different diameters and thicknesses, accurately determine the circumferential tensile properties of composite pipes, including circumferential tensile stress, elastic modulus, Poisson's ratio and ring Extreme tensile strain.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113252453B_ABST
    Figure CN113252453B_ABST
Patent Text Reader

Abstract

The present invention relates to a test device for measuring the circumferential tensile properties of composite pipes for structural engineering, comprising two tensioned arc steel blocks, two fixed arc steel blocks, four screws, a connection node, two connectors, two support rods, a traction mechanism, an axial strain gauge, and an annular strain gauge; the four screws are all fixed to the connection node; the connector is threadedly connected to the fixed arc steel block, the connector is threadedly connected to the screw, and the two connectors are arranged in a straight line; the support rod is threadedly connected to the screw, the support rod is against the inner side of the tensioned arc steel block, and the two support rods are arranged in a straight line; the traction mechanism is detachably connected to the two tensioned arc steel blocks; the axial strain gauge and the annular strain gauge are arranged on the outer surface of the annular sample. The present invention also relates to a test method for measuring the circumferential tensile properties of composite pipes for structural engineering. The present invention has high measurement proficiency and strong versatility, and belongs to the technical field of structural material performance detection in civil engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a structural material performance detection technology in civil engineering, and in particular to a test device and a test method for measuring the circumferential tensile performance of a composite material pipe used in structural engineering. Background Art

[0002] As a new type of material, fiber reinforced polymer (FRP) has excellent properties such as high strength and good corrosion resistance. In recent years, it has been widely used in the field of civil engineering. The most typical application is fiber reinforced composite tube (hereinafter referred to as composite tube) confined concrete. Composite tubes can be made by hand by wet laying method, or directly by pultrusion or fiber winding. Under the action of axial pressure, the lateral expansion of concrete can be effectively constrained by the fibers arranged close to the annular direction, thereby greatly improving the strength and ductility of the component. For composite tube confined concrete, the annular tensile properties of the composite tube (including annular ultimate tensile strain, annular elastic modulus and Poisson's ratio), especially the annular elastic modulus and annular ultimate tensile strain, have a crucial influence on its mechanical properties. Among the test methods for measuring the tensile properties of composite materials, in addition to the straight strip sheet tensile test and the traditional split disk test, scholars from all over the world have also proposed various test methods, but these existing methods have certain limitations in practical applications, and there is still no accurate and convenient solution.

[0003] The use of straight sheet tensile test method to measure the tensile properties of fiber reinforced composites is clearly described in the test specifications of many countries and regions, such as "Standard Test Method for Tensile Properties of Polymer Matrix Composites" [ASTM D3039 / D3039M-14 (2014)], "Standard Test Method for Tensile Properties of Fiber Reinforced Composites for Civil Engineering Reinforcement" [ASTM D7565 / D7565 M-10 (2017)], "Test Method for Tensile Properties of Directed Fiber Reinforced Polymer Matrix Composites" [GB / T 3354 (2014), "Test Method for Elastic Constants of Fiber Reinforced Composites" [GB / T 32376 (2015)], etc. However, the straight sheet tensile test method is mainly applicable to continuous unidirectional fiber reinforced composite flat plates. For composite pultruded or wound tubes, only arc-shaped specimens can be cut out along the circumferential direction, and the straight sheet tensile test method cannot be used; for composite tubes made by manual wet laying, although straight sheet specimens with the same material and the same layup as the tube can be made and tensile tested, due to the difference in curvature between the two and the different production methods, the results of the straight sheet tensile test method are difficult to accurately calibrate the actual performance of the composite tube.

[0004] Compared with the straight sheet test method, the traditional split disk test method uses an annular specimen, which relatively completely maintains the original shape of the pipe and is widely used to measure the circumferential properties of composite pipes, such as "Standard Test Method for Apparent Circumferential Tensile Strength of Plastic or Reinforced Plastic Pipe" [ASTM D2290-16 (2016)] and "Plastic Piping System - Test Method for Apparent Initial Circumferential Tensile Strength of Glass Fiber Reinforced Thermosetting Plastic Pipe" [ISO 8521 (2009)] both use this method. However, in the traditional split disk test method, in order to reduce the adverse effect of the friction between the annular specimen and the split disk on the test results, the test section of the annular specimen should be as close as possible to the gap between the two semicircular split disks. However, as the test proceeds, the two split disks gradually separate under the action of tension, which will inevitably cause bending on the test section of the annular specimen, resulting in the inability to obtain accurate circumferential tensile elastic modulus of the composite pipe in the test. In response to this problem, people have proposed many measures to improve the split disk test, such as keeping the test section of the annular specimen away from the gap of the split disk to eliminate the influence of the bending of the annular specimen on the test results. However, this treatment brings another problem: the friction between the annular specimen and the split disk causes a tensile stress gradient in the circumferential direction on the annular specimen, resulting in the inability to obtain the accurate tensile stress of the test section, and thus the inability to obtain accurate circumferential tensile material properties of the composite tube. In addition, whether it is an industrially produced composite winding tube or a composite tube made by manual wet laying, its tube diameter and wall thickness have a certain degree of discreteness, and the split disk of fixed size has poor adaptability to the discreteness of the composite tube diameter. The greater the difference in diameter between the split disk and the composite tube, the greater the measurement error caused by the bending of the test section.

[0005] If you want to eliminate the influence of adverse factors such as bending and friction on the determination of the circumferential performance of composite pipes, the new split disc test method is the best choice. First of all, the annular specimen of the new split disc test method ensures the integrity of the composite pipe. In addition, the new split disc test method uses a cross-shaped four-way screw to adjust the spacing between the two test section fixed arc steel blocks, which can well adapt to the discreteness of the diameter of the composite pipe. At the same time, considering the difference in curvature between the actual composite pipe and the test section fixed arc steel block, a roller with a gradually changing diameter is inserted in the gap between the two to ensure that the test section of the annular specimen can always maintain its original curvature during the test and be in a tensile state without local bending. In addition, the gap between the tension arc steel block and the fixed arc steel block is very close to the test section of the annular specimen. In addition, the friction between the test section of the annular specimen and the fixed arc steel block is eliminated as much as possible by applying lubricating oil, so the influence of friction on the test results during the test can be ignored. Based on the above points, the circumferential elastic modulus and circumferential tensile limit strain of the composite pipe measured by the new split disc test method are very reliable.

[0006] In summary, based on the analysis of the prior art, it can be seen that the traditional test methods for measuring the mechanical properties of composite materials have the following two main defects, which make them unsuitable for measuring the hoop tensile elastic modulus, Poisson's ratio, hoop ultimate tensile strain and hoop tensile strength of composite pipes for structural engineering:

[0007] Defect 1: The straight sheet tensile test method is only applicable to the determination of the relevant properties of the composite flat plate, and cannot solve the problem that the composite tube has an arc along the circumferential direction;

[0008] Defect 2: The unavoidable bending or friction problems of the traditional split disk test method lead to large errors in the measured circumferential elastic modulus of the composite tube, and the split disk of fixed size has poor adaptability to the diameter deviation of the composite tube;

[0009] In addition, according to the characteristics of composite pipes used in structural engineering, some scholars have proposed internal pressure test methods and arc specimen tensile test methods to test the circumferential performance of composite pipes. However, the former is difficult to seal the ends of the composite pipe under high pressure during the test, and the latter requires the arc specimen to be straightened, so both test methods cannot measure the circumferential tensile strength and circumferential ultimate tensile strain of the specimen; in addition, these two test methods are not applicable to composite pipes with smaller diameters and thicker walls.

[0010] In order to solve the limitations of the existing test methods, based on the existing technical conditions, the present invention proposes a test method for measuring the annular elastic modulus, Poisson's ratio, annular ultimate tensile strain and annular tensile strength of composite pipes for structural engineering, which is simple, feasible, reliable and widely applicable. Summary of the invention

[0011] In view of the technical problems existing in the prior art, the purpose of the present invention is to provide a test device and a test method for measuring the circumferential tensile properties of composite material pipes for structural engineering with high measurement accuracy and strong versatility.

[0012] In order to achieve the above object, the present invention adopts the following technical solution:

[0013] The test device for measuring the circumferential tensile properties of composite material pipes for structural engineering comprises two tensioning arc steel blocks, two fixed arc steel blocks, four screws, connection nodes, two connectors, two support rods, a traction mechanism, an axial strain gauge, and an annular strain gauge; the four screws are all fixed to the connection nodes, and the four screws are distributed in a cross shape; one end of the connector is a screw, and the other end of the connector is a nut; threaded holes are provided on the inner sides of the two fixed arc steel blocks, the screw ends of the connectors are threadedly connected to the threaded holes of the fixed arc steel blocks, the nut ends of the connectors are threadedly connected to the screws, and the two connectors are arranged Arranged in a straight line; one end of the support rod is a nut, and the other end of the support rod is a steel rod. The nut end of the support rod is threadedly connected to the screw rod, and the steel rod end of the support rod is against the inner side of the tension arc steel block. The two support rods are arranged in a straight line; the traction mechanism that stretches the two tension arc steel blocks outward is detachably connected to the two tension arc steel blocks; the outer side surfaces of the two tension arc steel blocks that fit the inner wall of the annular specimen are both convex arc surfaces; the outer side surfaces of the two fixed arc steel blocks that fit the inner wall of the annular specimen are both convex arc surfaces; the axial strain gauge and the annular strain gauge are arranged on the outer surface of the annular specimen. After adopting this structure, the measurement accuracy is high and the versatility is strong, which solves the problem that the split disk with fixed size has poor adaptability to the diameter deviation of the composite pipe.

[0014] As a preferred embodiment, it also includes a sliding baffle and multiple sets of roller needles; the tensioned arc steel block is provided with a slide groove, and the number of the slide grooves is two, and the two slide grooves are respectively located on the two sides of the tensioned arc steel block inclined from the inside to the outside; the number of sliding baffles is four, and in one tensioned arc steel block, the two slide grooves cooperate with the two sliding baffles; the slide groove is provided with a retracted position and an extended position, and when the sliding baffle is in the retracted position, the end of the sliding baffle is aligned with the end of the outer side surface of the tensioned arc steel block, and when the sliding baffle slides outward from the retracted position to the extended position, the end of the sliding baffle is against the inner wall of the annular specimen; a roller needle mounting portion is formed between the inner wall of the annular specimen, the outer side surface of the tensioned arc steel block and the sliding baffle, and a set of roller needles is arranged at each roller needle mounting portion, and each set of roller needles includes multiple roller needles, and the multiple roller needles are arranged in descending order according to diameter. After adopting this structure, a needle roller of appropriate diameter is selected and inserted into the needle roller installation part surrounded by the annular specimen, the tensioning arc steel block and the steel baffle to ensure that the curvature of the annular specimen can remain unchanged during the tensioning process of the annular specimen, solving the problem of large error in the measured annular elastic modulus of the composite tube caused by the bending or friction problems that cannot be avoided in the traditional split disk test method.

[0015] As a preferred embodiment, in each set of needle rollers, the diameter of the needle rollers is 0.5mm-5mm; and the difference in diameter between two adjacent needle rollers is 0.5mm.

[0016] As a preferred embodiment, the traction mechanism includes two steel chucks and two pins; the two tensioned arc steel blocks are provided with through holes in the thickness direction, the steel chucks are provided with fixing holes corresponding to the through holes, the tensioned arc steel blocks are connected to the steel chucks through the pins, the pins pass through the through holes, and the two ends of the pins cooperate with the fixing holes; the steel chucks are provided with end rods connected to the tensile testing machine.

[0017] As a preferred embodiment, the connection node is a cubic structure, and the screw rod and the connection node are an integrally formed structure.

[0018] As a preferred embodiment, the inner side surface of the tensioned arc steel block is flat, the steel rod end of the support rod is flat, the steel rod end of the support rod is against the inner side surface of the tensioned arc steel block, and the tail of the steel rod end of the support rod is provided with a threaded section, which is threadedly connected to the nut end of the support rod.

[0019] As a preferred embodiment, the annular specimen is an annular strip structure, comprising two connecting sections with a larger width and two testing sections with a smaller width, wherein the connecting sections and the testing sections are alternately distributed; the two testing sections are respectively centered with the outer sides of the two tensioned arc steel blocks; and the axial strain gauge and the annular strain gauge are located in the middle of the testing section.

[0020] The test method for measuring the hoop tensile properties of composite material pipes for structural engineering uses a test device for measuring the hoop tensile properties of composite material pipes for structural engineering, and comprises the following steps:

[0021] (1) Preparation of ring specimens: The ring specimens are taken from the same batch of composite pipes used for testing or actual engineering use, and the total number of ring specimens is not less than 5;

[0022] (2) Ring specimen installation:

[0023] a. A strain gauge is attached along the annular direction at the center of the two test sections of the annular specimen. The strain gauge attached in the annular direction is an annular strain gauge. Two strain gauges are attached along the axial direction of the annular specimen at both ends of the annular strain gauge. The two axially attached strain gauges are axial strain gauges.

[0024] b. Apply lubricating oil to the inner wall of the annular specimen;

[0025] c. Place two tensioned arc steel blocks and two fixed arc steel blocks in the annular specimen, ensuring that the arc tops of the two tensioned arc steel blocks and the two fixed arc steel blocks contact the inner wall of the annular specimen, wherein the tensioned arc steel block is aligned with the test section of the annular specimen;

[0026] d. Connect two connectors and two support rods to four screws respectively and place them in the annular specimen. Adjust the total length of the connector and the screw by rotating the nut end of the connector, and adjust the total length of the support rod and the screw by rotating the nut end of the support rod. The screw ends of the two connectors are screwed into the threaded holes of the fixed arc steel block to ensure that the position of the fixed arc steel block remains unchanged. The steel rod ends of the two support rods are against the inner side of the tensioned arc steel block to temporarily fix the position of the tensioned arc steel block.

[0027] e. The sliding baffle of the sliding tensioned arc steel block is pressed against the inner wall of the annular specimen, and the annular specimen, the outer side surface of the tensioned arc steel block and the sliding baffle form a needle roller installation part;

[0028] f. Select a needle roller corresponding to the size of the needle roller mounting portion from multiple sets of needle rollers and insert it into the needle roller mounting portion;

[0029] g. Install the pins and steel clamps on the tension arc steel block;

[0030] h. The end rod on the steel chuck is connected to the tensile testing machine;

[0031] (3) Loading: The tensile test was carried out at a constant rate of 3-5 mm / min until the annular specimen was broken;

[0032] (4) Data selection and calculation: record the maximum load value borne by the annular specimen during the test; select the test data of the annular strain of the annular specimen during the test, and calculate the annular tensile elastic modulus and Poisson's ratio of each test section of the annular specimen; the failure mode required by the test method is: the fracture surface appears in the middle of the test section of the annular specimen, only record the test data when the fracture surface appears in the middle of the test section of the annular specimen, and calculate the annular tensile strength and annular ultimate tensile strain of the annular specimen.

[0033] As a preferred embodiment, in step d, the test data of the hoop strain of the annular specimen during the test is selected to calculate the hoop tensile elastic modulus and Poisson's ratio of the test section of the annular specimen;

[0034] The hoop tensile stress of the ring specimen test section is calculated by the following formula:

[0035]

[0036] Where:

[0037] σ θ ——Annular tensile stress of the test section of the annular specimen, in MPa;

[0038] F t ——Tensile load of the ring specimen, in N;

[0039] t——average thickness of the test section of the annular specimen, in mm;

[0040] h——average width of the test section of the annular specimen, in mm;

[0041] The hoop tensile elastic modulus of the ring specimen test section is calculated by the following formula:

[0042]

[0043] Where:

[0044] E θ ——The hoop tensile elastic modulus of the test section of the annular specimen, in MPa;

[0045] ε θ ——The hoop strain of the test section of the annular specimen is the reading of the hoop strain gauge on the test section;

[0046] Δε θ ——The hoop strain increment of the ring specimen test section within the elastic range should be at least 0.2%. It is recommended to select the hoop strain range of 0.1% to 0.3% of the test section;

[0047] Δσ θ ——and the circumferential strain increment Δε of the test section θ The corresponding circumferential tensile stress increment of the test section, in N;

[0048] The annular Poisson's ratio of the annular specimen test section is calculated by the following formula:

[0049]

[0050] Where:

[0051] v θx ——Annular Poisson’s ratio of the test section of the annular specimen;

[0052] ε x ——The average axial strain of the test section of the annular specimen is the average value of the readings of the two axial strain gauges on the test section;

[0053] Δε x ——and the circumferential strain increment Δε of the test section θ The corresponding increment of the average axial strain of the test section.

[0054] As a preferred embodiment, in step d, test data of a test section that meets the failure mode requirements are selected to calculate the hoop tensile strength and hoop ultimate tensile strain value of the annular specimen;

[0055] The hoop tensile strength of the ring specimen is calculated by the following formula:

[0056]

[0057] Where:

[0058] P t ——Annular tensile strength of the test section that meets the failure mode requirements, in MPa;

[0059] F t,max ——The maximum tensile load of the ring specimen, in N;

[0060] t——average thickness of the test section of the annular specimen that meets the failure mode requirements, in mm;

[0061] h is the average width of the test section of the annular specimen that meets the failure mode requirements, in mm;

[0062] The ultimate tensile strain of the ring specimen, ε h,max , is the maximum strain value measured by the annular strain gauge on the test section that meets the failure mode requirements at the moment of fracture of the annular specimen.

[0063] In general, the present invention has the following advantages:

[0064] (1) The present invention can accurately measure the hoop tensile properties of the composite material pipe, including hoop tensile stress, hoop tensile elastic modulus, Poisson's ratio, hoop tensile strength and hoop ultimate tensile strain.

[0065] (2) The screw designed in the present invention can be used to adjust the spacing between the arc-shaped steel blocks, and the needle roller can ensure that the tensioned arc-shaped steel blocks can well adapt to the discrete diameter of the composite pipe.

[0066] (3) The present invention has wide applicability in the following aspects: a. In addition to typical composite pultruded winding tubes, the present invention is also applicable to composite tubes manually made by wet laying; b. It has a high degree of acceptance of the discrete level of the measured composite tube geometric dimensions (diameter and thickness); c. It is applicable to composite tubes with any fiber winding or laying angle; d. It is applicable to composite tubes of any diameter and thickness. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1a It is a top view of the ring specimen;

[0068] Figure 1b is a side view of the annular specimen;

[0069] Figure 2 It is a schematic diagram of the strain gauge pasted on the outer side of the annular specimen;

[0070] Figure 3a It is a three-dimensional image of a tensioned curved steel block;

[0071] Figure 3b It is a top view of the tensioned arc steel block;

[0072] Figure 4a It is a three-dimensional picture of the fixed curved steel block;

[0073] Figure 4b It is a top view of the fixed arc steel block;

[0074] Figure 5a It is an exploded view of the connection nodes, screws, connectors and support rods;

[0075] Figure 5b It is a schematic diagram of the connection of the connection nodes, screw rods, connectors and support rods;

[0076] Figure 6 It is a stereogram of a set of rolling pins;

[0077] Figure 7 It is a schematic diagram of the tensioned arc steel block and the fixed arc steel block installed on the inner side of the annular specimen;

[0078] Figure 8 It is a schematic diagram of the connection nodes, screw rods, connectors, support rods, tension arc steel blocks and fixed arc steel blocks installed on the inner side of the annular specimen;

[0079] Fig. 9 is an enlarged view of the sliding baffle;

[0080] Fig.10a Schematic diagram of the needle roller being installed in the needle roller installation part;

[0081] Fig.10b This is a partial enlarged view of the needle roller installed in the needle roller installation part;

[0082] Fig.11 This is a schematic diagram of the steel chuck installation;

[0083] Fig.12 is a perspective view of a test apparatus for measuring the hoop tensile properties of composite pipes used in structural engineering;

[0084] Fig.13a It is a schematic diagram of a ring specimen that meets the failure mode requirements;

[0085] Fig.13b It is a schematic diagram of a ring specimen that does not meet the failure mode requirements;

[0086] Fig.14 It is the hoop stress-strain curve of the test.

[0087] Among them, 1 is the tensioning arc steel block, 2 is the fixed arc steel block, 3 is the roller needle, 4 is the connecting piece, 5 is the pin, 6 is the steel chuck, 7 is the sliding baffle, 8 is the annular specimen, 9 is the annular strain gauge, 10 is the axial strain gauge, 11 is the support rod, 12 is the connecting node, 13 is the screw, and A is the maximum load point. DETAILED DESCRIPTION

[0088] The present invention will be further described in detail below in conjunction with specific implementation methods.

[0089] The test device for measuring the circumferential tensile properties of composite material pipes for structural engineering comprises two tensioning arc steel blocks, two fixed arc steel blocks, four screws, connection nodes, two connectors, two support rods, a traction mechanism, an axial strain gauge, and an annular strain gauge; the four screws are all fixed to the connection nodes, and the four screws are distributed in a cross shape; one end of the connector is a screw, and the other end of the connector is a nut; threaded holes are provided on the inner sides of the two fixed arc steel blocks, the screw ends of the connectors are threadedly connected to the threaded holes of the fixed arc steel blocks, the nut ends of the connectors are threadedly connected to the screws, and the two connectors are arranged Arranged in a straight line; one end of the support rod is a nut, and the other end of the support rod is a steel rod. The nut end of the support rod is threadedly connected to the screw rod, and the steel rod end of the support rod is against the inner side of the tension arc steel block. The two support rods are arranged in a straight line; the traction mechanism that stretches the two tension arc steel blocks outward is detachably connected to the two tension arc steel blocks; the outer side surfaces of the two tension arc steel blocks that fit the inner wall of the annular specimen are both convex arc surfaces; the outer side surfaces of the two fixed arc steel blocks that fit the inner wall of the annular specimen are both convex arc surfaces; the axial strain gauge and the annular strain gauge are arranged on the outer surface of the annular specimen. The connecting piece cooperates with the screw rod to adjust the distance between the two fixed arc steel blocks, and the support rod cooperates with the screw rod to adjust the distance between the two tension arc steel blocks, thereby ensuring that the outer side surfaces of the two fixed arc steel blocks and the two tension arc steel blocks are both attached to the inner wall of the annular specimen.

[0090] The invention also includes a sliding baffle and multiple sets of needle rollers; the tensioned arc steel block is provided with a sliding groove, and the number of the sliding grooves is two, and the two sliding grooves are respectively located on the two side surfaces of the tensioned arc steel block inclined from the inside to the outside; the two side surfaces here are the connecting surfaces between the two ends of the outer side surface (arc surface) of the tensioned arc steel block and the two ends of the inner surface (plane), and the number of sliding baffles is four. In one tensioned arc steel block, the two sliding grooves cooperate with the two sliding baffles; the sliding groove is provided with a retracted position and an extended position, and when the sliding baffle is in the retracted position, the end of the sliding baffle is aligned with the end of the outer side surface of the tensioned arc steel block, and when the sliding baffle slides outward from the retracted position to the extended position, the end of the sliding baffle is against the inner wall of the annular specimen; a needle roller mounting portion is formed between the inner wall of the annular specimen, the outer side surface of the tensioned arc steel block and the sliding baffle, and a set of needle rollers is arranged at each needle roller mounting portion, and each set of needle rollers includes multiple needle rollers, and the multiple needle rollers are arranged in descending order according to diameter. In each set of needle rollers, the diameter of the needle rollers is 0.5mm-5mm; the difference in diameter between two adjacent needle rollers is 0.5mm. The needle roller mounting parts are formed at both ends of the outer side of the tension arc steel block. The needle rollers installed on the needle roller mounting parts are arranged in a row from the end of the outer side of the tension arc steel block to the top of the arc. The length direction of the needle rollers is consistent with the thickness direction of the tension arc steel block. When the sliding baffle slides outward from the contraction position to the extension position, the end of the sliding baffle abuts against the inner wall of the annular specimen, limiting the needle rollers from sliding off the outer side of the tension arc steel block.

[0091] The traction mechanism includes two steel chucks and two latches; through holes are provided in the thickness direction of the two tension arc steel blocks, and the steel chucks are provided with fixing holes corresponding to the through holes. The tension arc steel blocks are connected to the steel chucks through the latches, and the latches pass through the through holes, and the two ends of the latches match the fixing holes; the steel chucks are provided with end rods connected to the tensile testing machine. The steel chucks include a horizontal plate, two vertical plates, and end rods; the two vertical plates are arranged in parallel at both ends of the horizontal plate, the vertical plates are perpendicular to the horizontal plate, and the vertical plates and the horizontal plate are an integrated structure, the vertical plates are provided with fixing holes corresponding to the through holes, and the size of the fixing holes corresponds to the latches, the end rods are perpendicular to the horizontal plate, the end rods are located in the middle of the horizontal plate, and the direction of the end rods is opposite to that of the vertical plates.

[0092] The connection node is a cubic structure, and the screw rod and the connection node are an integrally formed structure. The inner side of the tension arc steel block is a plane, and the steel rod end of the support rod is a plane. The steel rod end of the support rod is against the inner side of the tension arc steel block, and the tail of the steel rod end of the support rod is provided with a threaded section, which is threadedly connected with the nut end of the support rod.

[0093] The annular specimen is an annular strip structure. The annular specimen includes two connecting sections with a larger width and two testing sections with a smaller width. The connecting sections and the testing sections are distributed alternately. The two testing sections are centered on the outer sides of the two tensioning arc steel blocks respectively. The axial strain gauge and the annular strain gauge are located in the middle of the testing section. The axial strain gauge and the annular strain gauge are used to measure the annular and axial strains of the annular specimen during the annular tensile process. The annular tensile elastic modulus, Poisson's ratio, annular tensile strength and annular ultimate tensile strain of the annular specimen are calculated based on the tensile force data and strain data measured in the test.

[0094] 1 Ring specimen

[0095] 1.1 Ring specimen type

[0096] The ring specimens shall be taken from the same batch of composite pipes used for testing or actual engineering, and the total number of ring specimens shall not be less than 5. Figure 1a and Figure 1b The smaller width of the annular specimen is the test section of the annular specimen. D is the inner diameter of the annular specimen; t is the thickness of the annular specimen; H is the width of the connecting section of the annular specimen; h is the width of the test section of the annular specimen; l is the arc length of the test section of the annular specimen.

[0097] 1.2 Ring specimen size

[0098] The width of the test section (h) should not exceed 35mm. In order to facilitate the pasting of strain gauges, the width of the test section should not be less than 20mm. The width of the annular specimen connection section H = 20mm + the width of the test section h. The arc length of the test section (l) should not be less than 20mm. In order to reduce the friction of the test section, it should not be greater than 50mm. Figure 1a and Figure 1b shown.

[0099] 1.3 Requirements for the inner wall of the annular specimen

[0100] In order to ensure that the inner wall of the annular specimen fits tightly with the outer side surfaces of the fixed arc steel block and the tensioned arc steel block, the inner wall of the annular specimen should be smooth, without delamination or tearing, and the other surfaces should be free of damage.

[0101] 1.4 Pasting of ring specimen strain gauge

[0102] like Figure 2 As shown, a unidirectional strain gauge is pasted in the annular direction at the center of the test section of the annular specimen. The strain gauge pasted in the annular direction is an annular strain gauge. A unidirectional strain gauge is pasted in the axial direction of the annular specimen on both sides of the annular strain gauge. The two axially pasted ones are axial strain gauges. It is advisable to use a strain gauge with a gauge length of 5mm to 20mm.

[0103] 1.5 Number of ring specimens

[0104] Each group of mechanical properties ring specimens shall not be less than 5, and 5 valid ring specimens shall be guaranteed in the same batch. The physical properties ring specimens shall comply with the provisions of the corresponding standards.

[0105] 2 Test conditions

[0106] 2.1 Test environment conditions

[0107] 2.1.1 Laboratory standard environmental conditions

[0108] Temperature: (23±2)℃; Relative humidity: (50±10)%.

[0109] 2.1.2 Non-standard laboratory environmental conditions

[0110] If the laboratory standard environmental conditions are not available, select laboratory environmental conditions that are close to the laboratory standard environmental conditions.

[0111] 2.2 Test status adjustment

[0112] If conditions permit, place the device in an environment with a temperature of (23±2)℃ and a relative humidity of (50±10)% for at least 24 hours and conduct the test in the same environment. If conditions do not permit, conduct the test at the laboratory ambient temperature.

[0113] 3. Devices and Equipment

[0114] 3.1 Test apparatus

[0115] The test device for the circumferential tensile property test method of composite pipes is composed of two tension arc steel blocks, two fixed arc steel blocks, four screws, a connection node, two connecting pieces, two support rods, a traction mechanism, an axial strain gauge, an annular strain gauge, a roller needle and a sliding baffle; Fig.12 As shown. Among them, the diameter of the arc section of the tensioned arc steel block and the fixed arc steel block is d, the radius is r, d = the diameter of the ring specimen D-2mm = 2r, the width is H1 = the width of the ring specimen H + 10mm (the width here refers to the thickness of the tensioned arc steel block and the fixed arc steel block); the arc length of the tensioned arc steel block is l1, l1 = the arc length of the ring specimen test section l + 20mm.

[0116] 3.2 Test equipment

[0117] The tensile equipment for the test can be a tensile system equipped with a tension regulator and a hydraulic reservoir. The test equipment should meet the following requirements:

[0118] 3.2.1 The tension system should be able to stretch the annular specimen evenly and continuously.

[0119] 3.2.2 The tension system needs to be connected to a tension sensor, and its relative error should not be greater than 1% of the full scale.

[0120] 3.2.3 Necessary safety protection measures should be taken during the test and the tension system should be inspected for safety.

[0121] 3.2.4 Test equipment should be calibrated regularly by a qualified metrology department.

[0122] 3.2.5 The test equipment for physical properties should comply with the requirements of relevant standards.

[0123] 3.3 Stretching speed

[0124] The tensile test was carried out at a constant rate of 3-5 mm / min, and the load was applied until the annular specimen was broken.

[0125] 4 Test steps

[0126] 4.1 The preparation of the ring specimen shall be in accordance with the provisions of 1.1, 1.2, 1.3 and 1.4.

[0127] 4.2 Ring specimens must be visually inspected. If there are defects or ring specimens that do not meet the size and preparation requirements, they should be discarded.

[0128] 4.3 Number the qualified annular specimens and measure the inner diameter of the annular specimens and the thickness and width of the annular specimen test section with an accuracy of 0.01mm. On the two end faces of the annular specimen, measure the inner diameter in two directions perpendicular to each other, and take the average value as the average inner diameter. Measure the wall thickness and width at five equally spaced points in the annular specimen test section, discard the maximum and minimum values, and take the average values ​​of the remaining points as the average wall thickness and average width.

[0129] 4.4 Installation of ring specimen:

[0130] 4.4.1 Affix one strain gauge along the annular direction at the center of the two test sections of the annular specimen, and then affix two strain gauges along the axial direction of the annular specimen at both ends of the annular strain gauge, such as Figure 2 As shown;

[0131] 4.4.2 Apply lubricating oil to the inner wall of the annular specimen to reduce the friction between the annular specimen and the arc-shaped steel block during the tensile test;

[0132] 4.4.3 Place two tensioned arc steel blocks and two fixed arc steel blocks in the annular specimen, ensuring that the tops of the two tensioned arc steel blocks and the two fixed arc steel blocks contact the inner wall of the annular specimen, and that the tensioned arc steel blocks are aligned with the test section of the annular specimen, such as Figure 7 As shown;

[0133] 4.4.4 Connect the two connectors and the two support rods to the four screws respectively and place them in the annular specimen. Adjust the total length of the connector and the screw by rotating the nut end of the connector, and adjust the total length of the support rod and the screw by rotating the nut end of the support rod. The screw ends of the two connectors are screwed into the threaded holes of the fixed arc steel block to ensure that the position of the fixed arc steel block remains unchanged. The steel rod ends of the two support rods are against the inner side of the tensioned arc steel block to temporarily fix the position of the tensioned arc steel block. Figure 8 shown.

[0134] 4.4.5 The sliding baffle of the sliding tensioned arc steel block is against the inner wall of the annular specimen, and the annular specimen, the outer side surface of the tensioned arc steel block and the sliding baffle form a roller mounting portion; Fig. 9 As shown;

[0135] 4.4.6 Select a needle roller of the same size as the needle roller mounting portion from the multiple sets of needle rollers and insert it into the needle roller mounting portion; Fig.10a and Fig.10b As shown;

[0136] 4.4.7 Install the pins and steel clamps on the tension arc steel block; Fig.11 As shown;

[0137] 4.4.8 Connect the end rod on the steel clamp to the tensile testing machine; thus the entire test device is installed on the tensile testing machine.

[0138] 4.5 The state of the ring specimen shall be adjusted in accordance with the provisions of 2.2.

[0139] 4.6 The loading speed shall be as specified in 3.3, and the stretching shall be uniform and continuous until the annular specimen fails.

[0140] 4.7 During the test, the data that needs to be collected and stored include: tensile load, strain and tensile time of the annular specimen.

[0141] 5 Failure mode of ring specimen

[0142] The failure mode required by the test method is that the fracture surface appears in the middle of the test section of the annular specimen. Only the test data when the fracture surface appears in the middle of the test section of the annular specimen is recorded, and the hoop tensile strength and hoop ultimate tensile strain of the annular specimen are calculated.

[0143] Finally, the ring specimen was broken. Fig.13a and Fig.13b are two typical failure modes of the ring specimen. Fig.13a The fracture surface shown appears in the middle of the test section. To meet the requirements of the failure mode, the test data of this test section can be used to calculate the hoop tensile strength and hoop ultimate strain of the annular specimen. Fig.13bThe fracture surface appears at the end of the test section, which does not meet the requirements of the failure mode. The test section data where this failure mode appears cannot be used to calculate the annular tensile strength and annular ultimate strain of the annular specimen.

[0144] 6 Calculation

[0145] 6.1 Fig.14 The following is a typical hoop stress-strain curve of the hoop tensile properties test of a composite material pipe for structural engineering. In the above, tension is defined as positive and compression is defined as negative.

[0146] 6.2 Calculate the hoop tensile stress of the test section of the annular specimen according to formula (1):

[0147]

[0148] Where:

[0149] σ θ ——Annular tensile stress of the test section of the annular specimen, in MPa;

[0150] F t ——Tensile load of the ring specimen, in N;

[0151] t——average thickness of the test section of the annular specimen, in mm;

[0152] h is the average width of the test section of the annular specimen, in mm.

[0153] 6.3 Calculate the hoop tensile elastic modulus of the annular specimen test section according to formula (2):

[0154]

[0155] Where:

[0156] E θ ——The hoop tensile elastic modulus of the test section of the annular specimen, in MPa;

[0157] ε θ ——The hoop strain of the test section of the annular specimen is the reading of the hoop strain gauge on the test section;

[0158] Δε θ ——The hoop strain increment of the ring specimen test section within the elastic range should be at least 0.2%. It is recommended to select the hoop strain range of 0.1% to 0.3% of the test section;

[0159] Δσ θ ——and the circumferential strain increment Δε of the test section θ The corresponding circumferential tensile stress increment of the test section is in MPa;

[0160] 6.4 Calculate the annular Poisson’s ratio of the annular specimen test section according to formula (3):

[0161]

[0162] Where:

[0163] v θx ——Annular Poisson’s ratio of the test section of the annular specimen;

[0164] ε x ——The average axial strain of the test section of the annular specimen is the average value of the readings of the two axial strain gauges on the test section;

[0165] Δε x ——and the circumferential strain increment Δε of the test section θ The corresponding increment of the average axial strain of the test section.

[0166] 6.5 Calculate the hoop tensile strength of the ring specimen according to formula (4):

[0167]

[0168] Where:

[0169] P t ——Annular tensile strength of the test section that meets the failure mode requirements, in MPa;

[0170] F t,max ——The maximum tensile load of the ring specimen, in N;

[0171] t——average thickness of the test section of the annular specimen that meets the failure mode requirements, in mm;

[0172] h is the average width of the test section of the annular specimen that meets the failure mode requirements, in mm.

[0173] The ultimate tensile strain of the ring specimen, ε h,max , is the maximum strain value measured by the annular strain gauge of the test section that meets the failure mode requirements at the moment of fracture of the annular specimen.

[0174] 7 Test results

[0175] The arithmetic mean, standard deviation, dispersion coefficient, etc. of the test results such as the initial hoop elastic modulus and the initial hoop Poisson's ratio should be calculated. For large dispersion coefficients, the specific reasons should be analyzed. If it is due to the quality problems of the annular specimens, a new batch of annular specimens should be made and tested again.

[0176] 7.1 Each annular specimen consists of two test sections. The performance value of each test section (except P t and ε h,maxExternal): X1, X2, X3, …, X n ; Hoop tensile strength P of each ring specimen t and the hoop limit strain ε h,max :X1,X2,X3,…,X n If necessary, the failure of each ring specimen should be stated.

[0177] 7.2 Calculate the arithmetic mean according to formula (5) to three significant figures:

[0178]

[0179] Where:

[0180] ——arithmetic mean;

[0181] X i ——For performance parameter P t and ε h,max For , it is the performance value of each annular specimen that meets the failure mode requirements; for other performance values, it is the performance value of each test section;

[0182] n——For performance parameter P t and ε h,max For , it is the number of ring specimens that meet the failure mode requirements; for other performance values, it is (number of ring specimens × 2).

[0183] 7.3 Calculate the standard deviation S according to formula (6) to two significant figures:

[0184]

[0185] Where:

[0186] S——standard deviation.

[0187] 7.4 Calculate the dispersion coefficient C according to formula (7) v , calculated to two significant figures:

[0188]

[0189] Where:

[0190] C v ——Dispersion coefficient.

[0191] 7.5 Confidence interval for the mean.

[0192] Calculated according to ISO 2602:1980.

[0193] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A test device for measuring the hoop tensile properties of composite pipes for structural engineering, characterized by: It includes two tensioning arc steel blocks, two fixed arc steel blocks, four screws, a connection node, two connecting pieces, two support rods, a traction mechanism, an axial strain gauge, and an annular strain gauge; Four screw rods are all fixed to the connection node, and the four screw rods are distributed in a cross shape; one end of the connecting piece is a screw rod, and the other end of the connecting piece is a nut; the inner sides of the two fixed arc steel blocks are provided with threaded holes, the screw end of the connecting piece is threadedly connected to the threaded hole of the fixed arc steel block, the nut end of the connecting piece is threadedly connected to the screw rod, and the two connecting pieces are arranged in a straight line; one end of the support rod is a nut, and the other end of the support rod is a steel rod, the nut end of the support rod is threadedly connected to the screw rod, and the steel rod end of the support rod is against the inner side of the tensioned arc steel block, and the two support rods are arranged in a straight line; the traction mechanism for stretching the two tensioned arc steel blocks outward is detachably connected to the two tensioned arc steel blocks; the outer sides of the two tensioned arc steel blocks that fit the inner wall of the annular specimen are both convex arc surfaces; the outer sides of the two fixed arc steel blocks that fit the inner wall of the annular specimen are both convex arc surfaces; the axial strain gauge and the annular strain gauge are arranged on the outer surface of the annular specimen; The test device for measuring the circumferential tensile properties of composite material pipes for structural engineering also includes a sliding baffle and multiple sets of needle rollers; the tensioned arc steel block is provided with a slide groove, the number of which is two, and the two slide grooves are respectively located on the two sides of the tensioned arc steel block that are inclined from the inside to the outside; the number of sliding baffles is four, and in one tensioned arc steel block, two slide grooves cooperate with two sliding baffles; the slide groove is provided with a contraction position and an extension position, and when the sliding baffle is in the contraction position, the end of the sliding baffle is aligned with the end of the outer side surface of the tensioned arc steel block, and when the sliding baffle slides outward from the contraction position to the extension position, the end of the sliding baffle abuts against the inner wall of the annular specimen; a needle roller installation portion is formed between the inner wall of the annular specimen, the outer side surface of the tensioned arc steel block and the sliding baffle, and a set of needle rollers is arranged at each needle roller installation portion, and each set of needle rollers includes multiple needle rollers, and the multiple needle rollers are arranged in descending order according to diameter; The traction mechanism includes two steel clamps and two latches; through holes are provided in the thickness direction of the two tension arc steel blocks, and the steel clamps are provided with fixing holes corresponding to the through holes. The tension arc steel blocks are connected to the steel clamps through the latches, and the latches pass through the through holes, and the two ends of the latches match the fixing holes; the steel clamps are provided with end rods connected to the tensile testing machine; The annular specimen is an annular strip structure, including two connecting sections with larger width and two testing sections with smaller width, and the connecting sections and the testing sections are alternately distributed; the two testing sections are centered with the outer sides of the two tensioned arc steel blocks respectively; the axial strain gauge and the annular strain gauge are located in the middle of the testing section.

2. The test device for measuring the hoop tensile properties of composite material pipes for structural engineering according to claim 1, characterized in that: In each set of needle rollers, the diameter of the needle rollers is 0.5mm-5mm; the difference in diameter between two adjacent needle rollers is 0.5mm.

3. The test device for measuring the hoop tensile properties of composite material pipes for structural engineering according to claim 1, characterized in that: The connection node is a cubic structure, and the screw rod and the connection node are an integrally formed structure.

4. The test device for measuring the hoop tensile properties of composite material pipes for structural engineering according to claim 1, characterized in that: The inner side of the tensioned arc steel block is a plane, the steel rod end of the support rod is a plane, the steel rod end of the support rod is against the inner side of the tensioned arc steel block, and the tail of the steel rod end of the support rod is provided with a threaded section, which is threadedly connected with the nut end of the support rod.

5. A test method for measuring the hoop tensile properties of a composite material pipe for structural engineering, using the test device for measuring the hoop tensile properties of a composite material pipe for structural engineering as claimed in any one of claims 1 to 4, characterized in that: The steps include: (1) Preparation of ring specimens: The ring specimens are taken from the same batch of composite pipes used for testing or actual engineering use, and the total number of ring specimens is not less than 5; (2) Ring specimen installation: a. A strain gauge is attached along the annular direction at the center of the two test sections of the annular specimen. The strain gauge attached in the annular direction is the annular strain gauge. Two strain gauges are attached along the axial direction of the annular specimen at both ends of the annular strain gauge. The two axially attached strain gauges are axial strain gauges. b. Apply lubricating oil to the inner wall of the annular specimen; c. Place two tensioned arc steel blocks and two fixed arc steel blocks in the annular specimen, ensuring that the arc tops of the two tensioned arc steel blocks and the two fixed arc steel blocks contact the inner wall of the annular specimen, wherein the tensioned arc steel block is aligned with the test section of the annular specimen; d. Connect two connectors and two support rods to four screws respectively and place them in the annular specimen. Adjust the total length of the connector and the screw by rotating the nut end of the connector, and adjust the total length of the support rod and the screw by rotating the nut end of the support rod. The screw ends of the two connectors are screwed into the threaded holes of the fixed arc steel block to ensure that the position of the fixed arc steel block remains unchanged. The steel rod ends of the two support rods are against the inner side of the tensioned arc steel block to temporarily fix the position of the tensioned arc steel block. e. The sliding baffle of the sliding tensioned arc steel block is pressed against the inner wall of the annular specimen, and the annular specimen, the outer side surface of the tensioned arc steel block and the sliding baffle form a roller mounting portion; f. Select a needle roller corresponding to the size of the needle roller mounting portion from multiple sets of needle rollers and insert it into the needle roller mounting portion; g. Install the pins and steel clamps on the tension arc steel block; h. The end rod on the steel chuck is connected to the tensile testing machine; (3) Loading: The tensile test is carried out at a constant rate of 3-5 mm / min until the annular specimen is broken; (4) Data selection and calculation: record the maximum load value borne by the annular specimen during the test; The test data of the hoop strain of the annular specimen during the test were selected, and the hoop tensile elastic modulus and Poisson's ratio of each test section of the annular specimen were calculated; the failure mode required by the test method was that the fracture surface appeared in the middle of the test section of the annular specimen, and only the test data when the fracture surface appeared in the middle of the test section of the annular specimen was recorded, and the hoop tensile strength and hoop ultimate tensile strain of the annular specimen were calculated.

6. The test method for measuring the hoop tensile properties of composite material pipes for structural engineering according to claim 5, characterized in that: In step d, the test data of the hoop strain of the annular specimen during the test is selected to calculate the hoop tensile elastic modulus and Poisson's ratio of the test section of the annular specimen; The hoop tensile stress of the ring specimen test section is calculated by the following formula: Where: σ θ ——Annular tensile stress of the test section of the annular specimen, in MPa; F t ——Tensile load of the ring specimen, in N; t——average thickness of the test section of the annular specimen, in mm; h——average width of the test section of the annular specimen, in mm; The hoop tensile elastic modulus of the annular specimen test section is calculated by the following formula: Where: E θ ——The hoop tensile elastic modulus of the test section of the annular specimen, in MPa; ε θ ——The hoop strain of the test section of the annular specimen is the reading of the hoop strain gauge on the test section; Δε θ ——The hoop strain increment of the ring specimen test section within the elastic range should be at least 0.2%. It is recommended to select the hoop strain range of 0.1% to 0.3% of the test section; Δσ θ ——and the circumferential strain increment Δε of the test section θ The corresponding circumferential tensile stress increment of the test section, in N; The annular Poisson's ratio of the annular specimen test section is calculated by the following formula: Where: v θx ——Annular Poisson’s ratio of the test section of the annular specimen; ε x ——The average axial strain of the test section of the annular specimen is the average value of the readings of the two axial strain gauges on the test section; Δε x ——and the circumferential strain increment Δε of the test section θ The corresponding increment of the average axial strain of the test section.

7. The test method for measuring the hoop tensile properties of composite material pipes for structural engineering according to claim 5, characterized in that: In step d, the test data of the test section that meets the failure mode requirements are selected to calculate the hoop tensile strength and hoop ultimate tensile strain value of the annular specimen; The hoop tensile strength of the ring specimen is calculated by the following formula: Where: P t ——Annular tensile strength of the test section that meets the failure mode requirements, in MPa; F t,max ——The maximum tensile load of the ring specimen, in N; t——average thickness of the test section of the annular specimen that meets the failure mode requirements, in mm; h is the average width of the test section of the annular specimen that meets the failure mode requirements, in mm; The ultimate tensile strain of the ring specimen, ε h,max , is the maximum strain value measured by the annular strain gauge on the test section that meets the failure mode requirements at the moment of fracture of the annular specimen.

Citation Information

Cited By