A lithium ion battery positive electrode material and preparation method

By using composite materials of lithium halide and lithium titanate as cathode materials for lithium-ion batteries, the problems of high cost and low energy density of cathode materials are solved, high specific capacity and improvement of the electrochemical reaction platform are achieved, and battery production costs are significantly reduced. .

CN113314699BActive Publication Date: 2024-10-11SHANGHAI MAKESENS ENERGY STORAGE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110381590.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-09
Publication Date
2024-10-11
Estimated Expiration
2041-04-09

AI Technical Summary

Technical Problem

The high cost of cathode materials for lithium-ion batteries limits their industrial application, and the theoretical specific capacity and voltage platform of lithium titanate are low, resulting in a low overall energy density of the battery.

Method used

A composite material of lithium halide and lithium titanate is used as the cathode material of the lithium-ion battery. It is prepared by a high-temperature solid-state reaction method or a sol-gel method. It is combined with polyvinylidene fluoride, conductive carbon black and other ingredients to form a high specific capacity and electric power. Electrode materials for chemical reaction platforms.

Benefits of technology

It significantly improves the specific capacity and electrochemical reaction platform of lithium-ion batteries, reduces production costs, and increases the battery's application range and production profits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113314699B_ABST
    Figure CN113314699B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery materials, and discloses a positive electrode material for a lithium-ion battery, characterized in that it includes an active substance, a binder, a conductive additive, and a binder solvent, wherein the active substance is set as a composite material of a mixture of lithium halide and lithium titanate, and they are mixed in a mass ratio of 1:100 to 1:1. A preparation method of a positive electrode material for a lithium-ion battery is also disclosed. The present invention mixes lithium halide and lithium titanate as active substances to prepare an electrode material, and uses it in the positive electrode of a lithium-ion battery, showing a higher specific capacity and a higher electrochemical reaction platform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a lithium ion battery positive electrode material and a preparation method thereof. Background Art

[0002] From the battery manufacturing process, the key materials of the battery cell are mainly positive electrode (anode), negative electrode (cathode), electrolyte, diaphragm, etc., of which the cost of positive electrode materials accounts for 20-28%. At present, the main positive electrode materials are lithium cobalt oxide, lithium titanate, lithium manganate, lithium vanadate, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide, ternary materials, lithium iron phosphate, etc. Except for lithium vanadate, which is relatively cheap (60,000 / ton), the prices of other positive electrode materials are 150,000-300,000 / ton, which is relatively expensive. Reducing the cost of positive electrode materials has far-reaching significance for the development of lithium-ion batteries.

[0003] Lithium titanate Li4Ti5O with spinel structure 12 The theoretical specific capacity can reach 175mAh·g -1 The reaction voltage is about 1.55V. As a lithium battery electrode material, it can maintain structural stability during the charge and discharge process and its volume change is almost zero. It is widely considered to be an electrode material with good application prospects. However, its medium-level theoretical specific capacity and low voltage platform lead to a low comprehensive energy density of the battery, which has become a factor limiting its industrial application. Summary of the invention

[0004] The invention provides a lithium ion battery positive electrode material and a preparation method thereof, which solves the problem that the positive electrode material of the lithium ion battery is expensive.

[0005] The present invention can be achieved through the following technical solutions:

[0006] A lithium ion battery positive electrode material comprises an active substance, a binder, a conductive additive and a binder solvent, wherein the active substance is a composite material of lithium halide and lithium titanate mixed in a mass ratio of 1:100 to 1:1.

[0007] Furthermore, the lithium halide includes lithium chloride and lithium bromide, wherein the lithium chloride is set to be hydrated lithium chloride or anhydrous lithium chloride, and the lithium bromide is set to be hydrated lithium bromide or anhydrous lithium bromide; the lithium titanate is prepared by a high-temperature solid-phase reaction method or a sol-gel method.

[0008] Further, the binder is configured as an aqueous binder with polyvinylidene fluoride PVDF, styrene butadiene rubber SBR emulsion, carboxymethyl cellulose CMC, polyacrylic acid PAA, polyacrylonitrile PAN or polyacrylate as main components;

[0009] The conductive additive is configured as conductive carbon black Super P, carbon nanotubes CNT or graphene;

[0010] The binder solvent is set to be oily N-methylpyrrolidone NMP or an aqueous binder solvent deionized water.

[0011] A preparation method of a positive electrode material for a lithium ion battery based on the above-mentioned method comprises first adding a binder and a conductive additive into a binder solvent and mixing them thoroughly to prepare a mixed solution, then mixing lithium halide and lithium titanate in a mass ratio of 1:100 to 1:1, adding the mixture into the mixed solution to prepare a suspension, and then coating the suspension on an electrode current collector. After being fully dried, the suspension can be used as a positive electrode material for a lithium ion battery.

[0012] Furthermore, the mixed lithium halide powder and lithium titanate powder were placed in a tubular furnace, argon gas was introduced to isolate the air, and the temperature was continuously raised from room temperature to 600°C at a uniform rate, kept constant for 1 hour, then heated to 700°C, kept constant for 2 hours, and then naturally cooled to room temperature, ground into powder with an agate mortar, and finally added to the mixed solution.

[0013] Furthermore, the binder and the conductive additive are first added to the binder solvent, stirred and fully mixed using a magnetic stirrer to prepare a mixed solution;

[0014] Then, lithium halide and lithium titanate are mixed in a mass ratio of 1:100 to 1:1, and then added into the mixed solution, and then stirred and fully mixed using a magnetic stirrer to prepare a suspension;

[0015] Finally, the suspension is coated on the electrode current collector. The prepared electrode sheet is first placed in a forced air drying oven for drying at a temperature of 50 to 100°C for 2 to 5 hours, and then moved into a vacuum drying oven for drying at a temperature of 60 to 120°C for 12 to 24 hours. It can then be used as a positive electrode material for a lithium-ion battery.

[0016] Further, the following steps are included:

[0017] (1) 10 ml of N-methyl-2-pyrrolidone (NMP) solution was measured, and then 0.2 g of polyvinylidene fluoride (PVDF) powder and 0.2 g of conductive carbon black super P powder were weighed respectively, and the weighed powders were added to the N-methyl-2-pyrrolidone (NMP) solution, and then stirred for 2 hours using a magnetic stirrer to dissolve the powders in the N-methyl-2-pyrrolidone (NMP) solution to prepare a mixed solution;

[0018] (2) Weigh 1.42g of finished product lithium titanate Li4Ti5O 12and 0.18 g of lithium chloride LiCl powder, adding the powder to the mixed solution, stirring on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0019] (3) coating the suspension on a copper foil current collector using a coating machine to form an electrode sheet with a coating thickness of 0.4 mm;

[0020] (4) The electrode sheet is first placed in a forced air drying oven for 2 hours, the temperature of which is set at 80° C., and then placed in a vacuum drying oven for 12 hours, the temperature of which is set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate.

[0021] Further, the following steps are included:

[0022] (1) 10 ml of N-methyl-2-pyrrolidone (NMP) solution was measured, and then 0.2 g of polyvinylidene fluoride (PVDF) powder and 0.2 g of conductive carbon black super P powder were weighed respectively, and the weighed powders were added to the N-methyl-2-pyrrolidone (NMP) solution, and stirred for 2 hours using a magnetic stirrer to fully dissolve the powders in the N-methyl-2-pyrrolidone (NMP) solution to prepare a mixed solution;

[0023] (2) Weigh 1.58 g lithium titanate Li4Ti5O 12 and 0.02g lithium chloride LiCl powder, put the weighed powder into a tube furnace for heating, introduce argon gas to isolate the air, first heat from room temperature to 600°C at a uniform rate of 5°C / min, keep the temperature constant for 1 hour, then heat to 700°C, keep the temperature constant for 2 hours, and then naturally cool to room temperature, then grind into powder with an agate mortar, add the powder to the mixed solution, and stir on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0024] (3) coating the suspension on a copper foil current collector using a coating machine to form an electrode sheet with a coating thickness of 0.4 mm;

[0025] (4) The electrode sheet is first placed in a forced air drying oven for 2 hours, the temperature of which is set at 80° C., and then placed in a vacuum drying oven for 12 hours, the temperature of which is set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate.

[0026] Further, the following steps are included:

[0027] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0028] (2) Lithium acetate, tetrabutyl titanate, citric acid monohydrate, and ethanol solution are mixed by a stoichiometric method, and then placed in a magnetic stirrer for thorough mixing. The mixture is dried in a vacuum drying oven to form a white solid. The white solid is ground into powder using an agate mortar. The mixture is then placed in a tube furnace and heated to 800°C at a constant speed of 5°C / min. The mixture is kept at a constant temperature for 12 hours, and then ground into powder to obtain lithium titanate Li4Ti5O 12 ;

[0029] (3) Weigh 0.96 g lithium titanate Li4Ti5O 12 and 0.64 g of lithium chloride LiCl powder, adding the powder to the mixture, stirring on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0030] (4) using a coating machine to apply the suspension onto a copper foil current collector to form an electrode sheet to be tested with a coating thickness of 0.4 mm;

[0031] (5) The electrode sheet is first placed in a forced air drying oven for 2 hours with the temperature of the forced air drying oven set at 80° C., and then placed in a vacuum drying oven for 12 hours with the temperature of the drying oven set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate.

[0032] Further, the following steps are included:

[0033] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder respectively, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and then stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0034] (2) Lithium acetate, tetrabutyl titanate, citric acid monohydrate, and ethanol solution are mixed by a stoichiometric method, and then placed in a magnetic stirrer for thorough mixing. The mixture is dried in a vacuum drying oven to form a white solid. The white solid is ground into powder using an agate mortar. The mixture is then placed in a tube furnace and heated to 800°C at a constant speed of 5°C / min. The mixture is kept at a constant temperature for 12 hours, and then ground into powder to obtain lithium titanate Li4Ti5O 12 ;

[0035] (2) Weigh 1.44 g lithium titanate Li4Ti5O 12 and 0.16 g of lithium bromide LiBr powder, adding the powder to the mixed solution, stirring on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0036] (3) coating the suspension on a copper foil current collector using a coating machine to form an electrode sheet with a coating thickness of 0.4 mm;

[0037] (4) The electrode sheet is first placed in a forced air drying oven for 2 hours, the temperature of which is set at 80° C., and then placed in a vacuum drying oven for 12 hours, the temperature of which is set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate.

[0038] The beneficial technical effects of the present invention are:

[0039] The present invention proposes to mix lithium halide and lithium titanate as active material to prepare electrode material, and use it for the positive electrode of lithium ion battery, which shows higher specific capacity and higher electrochemical reaction platform, and its specific capacity can reach 500mAh·g -1 The voltage platform is between 1.5-2.7V, which is much higher than the specific capacity of pure lithium titanate batteries; and the composite material is cheap, industrial grade, the price is less than 5000 yuan / ton, and the price of lithium chloride is less than 1 / 30 of that of lithium titanate, which can significantly reduce the production cost of lithium-ion batteries and increase production profits. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is the overall flow chart of the present invention;

[0041] Figure 2 It is a comparison chart of the test results of Examples 1-5 of the present invention. DETAILED DESCRIPTION

[0042] The specific implementation of the present invention is described in detail below with reference to the accompanying drawings and preferred embodiments.

[0043] The present invention provides a positive electrode material for a lithium ion battery, comprising an active substance, a binder, a conductive additive and a binder solvent, wherein the active substance is set as a composite material of a mixture of lithium halide and lithium titanate, which are mixed in a mass ratio of 1:100 to 1:1, preferably 1:80 to 4:6, the lithium halide can be set as lithium chloride, lithium bromide, lithium fluoride and lithium iodide, preferably lithium chloride and lithium bromide, the lithium chloride can be set as hydrated lithium chloride or anhydrous lithium chloride, and the lithium bromide can also be set as hydrated lithium bromide or anhydrous lithium bromide; the lithium titanate can be prepared by a high-temperature solid phase reaction method or a sol-gel method, as described in Examples 4 and 5, or the finished product can be directly used; the solvent can be an organic solvent or water. In this way, the lithium halide and lithium titanate mixed in a certain mass ratio are used as the active substance for preparing the positive electrode of the lithium ion battery, and the prepared battery has a higher specific capacity and a higher electrochemical reaction platform, thereby significantly improving the performance of the battery and increasing the application range of the battery.

[0044] In addition, the binder is set to be an aqueous binder with polyvinylidene fluoride PVDF, styrene-butadiene rubber SBR emulsion, carboxymethyl cellulose CMC, polyacrylic acid PAA, polyacrylonitrile PAN or polyacrylate as the main components; the conductive additive is set to be conductive carbon black Super P, carbon nanotube CNT or graphene; the binder solvent is set to be oily N-methylpyrrolidone NMP or aqueous binder solvent deionized water.

[0045] The present invention also provides a method for preparing the positive electrode material of a lithium-ion battery based on the above-mentioned method, firstly adding a binder and a conductive additive into a binder solvent and mixing them thoroughly to prepare a mixed solution, then mixing lithium halide and lithium titanate in a mass ratio of 1:100 to 1:1, preferably 1:80 to 4:6, and adding them into the mixed solution prepared above to prepare a suspension, and then coating the suspension on the electrode collector, and after being fully dried, it can be used as a positive electrode material for a lithium-ion battery. The mixing method of lithium halide and lithium titanate can be a mixing method in a solvent, dry ball milling, or a high-temperature solution mixing method, depending on the actual situation. The high-temperature solution mixing method is as follows:

[0046] The mixed lithium halide powder and lithium titanate powder are placed in a tubular furnace, argon gas is introduced to isolate the air, and the temperature is continuously raised from room temperature to 600°C at a uniform rate. The uniform heating rate can be set to 5°C / min, and the temperature is kept constant for 1 hour. The temperature is then continuously raised to 700°C at a uniform rate and kept constant for 2 hours. After naturally cooling to room temperature, it is ground into powder with an agate mortar and finally added to the mixed solution.

[0047] The specific preparation method is as follows:

[0048] First, the binder and the conductive additive are added to the binder solvent, and stirred and fully mixed by a magnetic stirrer to prepare a mixed liquid;

[0049] Then, lithium halide and lithium titanate are mixed in a mass ratio of 1:100 to 1:1, preferably 1:80 to 4:6, and added to the mixed solution, and then stirred and fully mixed using a magnetic stirrer to prepare a suspension;

[0050] Finally, the suspension is coated on the electrode current collector. The prepared electrode sheet is first placed in a forced air drying oven for drying at a temperature of 50 to 100°C for 2 to 5 hours, and then moved into a vacuum drying oven for drying at a temperature of 60 to 120°C for 12 to 24 hours. It can then be used as a positive electrode material for a lithium-ion battery.

[0051] Example 1

[0052] A pure lithium titanate electrode material, wherein pure lithium titanate is used as an active material, and is mixed with a conductive additive (conductive carbon black super P) and a binder (polyvinylidene fluoride PVDF) in a binder solvent N-methyl-2-pyrrolidone (NMP) solution, as follows:

[0053] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder respectively, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0054] (2) Weigh 1.6 g of finished product lithium titanate Li4Ti5O 12 , add it to the prepared mixed solution, and stir it on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0055] (3) using a coating machine to apply the above suspension onto a copper foil current collector to form an electrode sheet with a coating thickness of 0.4 mm;

[0056] (4) The prepared electrode sheet is first placed in a blast drying oven for 2 hours, the temperature of the blast drying oven is set to 80°C, and then placed in a vacuum drying oven for 12 hours, the temperature of the drying oven is set to 60°C, to obtain a composite electrode sheet of lithium chloride and lithium titanate;

[0057] (5) The electrode sheets were sliced ​​into Φ14 mm electrode discs and assembled into button batteries in a glove box. The button battery structure included: a positive electrode shell, a circular electrode sheet, a diaphragm, an electrolyte (LiPF6), a lithium sheet, a gasket, a circular spring, and a negative electrode shell.

[0058] (6) Finally, the assembled button battery is subjected to performance testing.

[0059] Example 2

[0060] A lithium chloride and lithium titanate composite electrode material, wherein lithium chloride and lithium titanate are mixed in a mass ratio of 1:8 as active materials, and the active materials are mixed with a conductive additive (super P) and a binder (PVDF) in a binder solvent N-methyl-2-pyrrolidone (NMP) solution, as follows:

[0061] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder respectively, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and then stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0062] (2) Weigh 1.42g of finished product lithium titanate Li4Ti5O 12 and 0.18 g of lithium chloride LiCl powder, adding the powder to the mixed solution, stirring on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0063] (3) coating the suspension on a copper foil current collector using a coating machine to form an electrode sheet with a coating thickness of 0.4 mm;

[0064] (4) placing the electrode sheet in a blast drying oven for 2 hours, the temperature of which is set at 80° C., and then placing it in a vacuum drying oven for 12 hours, the temperature of which is set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate;

[0065] (5) The electrode sheets were sliced ​​into Φ14 mm electrode discs and assembled into button batteries in a glove box. The button battery structure included: a positive electrode shell, a circular electrode sheet, a diaphragm, an electrolyte (LiPF6), a lithium sheet, a gasket, a circular spring, and a negative electrode shell.

[0066] (6) Finally, the assembled button battery is subjected to performance testing.

[0067] Example 3

[0068] A composite electrode material of lithium chloride and lithium titanate, wherein the lithium chloride and lithium titanate are mixed as active materials in a mass ratio of 1:80, and they are mixed by a high temperature solution method, and mixed with a conductive additive (super P) and a binder (PVDF) in a binder solvent N-methyl-2-pyrrolidone (NMP) solution, as follows:

[0069] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder respectively, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and stir with a magnetic stirrer for 2 hours to fully dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0070] (2) Weigh 1.58 g lithium titanate Li4Ti5O 12 and 0.02g lithium chloride LiCl powder, put the weighed powder into a tube furnace for heating, introduce argon gas to isolate the air, first heat from room temperature to 600°C at a constant speed of 5°C / min, keep the temperature constant for 1 hour, then heat to 700°C, keep the temperature constant for 2 hours, and then naturally cool to room temperature, then grind into powder with an agate mortar, add the powder to the mixed solution, and stir on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0071] (3) coating the suspension on a copper foil current collector using a coating machine to form an electrode sheet with a coating thickness of 0.4 mm;

[0072] (4) placing the electrode sheet in a blast drying oven for 2 hours, the temperature of which is set at 80° C., and then placing it in a vacuum drying oven for 12 hours, the temperature of which is set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate;

[0073] (5) Slice the electrode sheet into Φ14 mm electrode discs and assemble them into button batteries in a glove box. The button battery structure includes: a positive electrode shell, a circular electrode sheet, a diaphragm, an electrolyte (LiPF6), a lithium sheet, a gasket, a circular spring, and a negative electrode shell;

[0074] (6) Finally, the assembled button battery is subjected to performance testing.

[0075] Example 4

[0076] A composite electrode material of lithium chloride and lithium titanate is mixed, wherein the lithium titanate is prepared by a sol-gel method, and is mixed with lithium chloride in a mass ratio of 4:6 as an active material, and is mixed with a conductive additive (super P) and a binder (PVDF) in a binder solvent N-methyl-2-pyrrolidone (NMP) solution, as follows:

[0077] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0078] (2) Lithium acetate, tetrabutyl titanate, citric acid monohydrate, and ethanol solution are mixed by a stoichiometric method, and then placed in a magnetic stirrer for thorough mixing. The mixture is dried in a vacuum drying oven to form a white solid. The white solid is ground into powder using an agate mortar. The mixture is then placed in a tube furnace and heated to 800°C at a constant speed of 5°C / min. The mixture is kept at a constant temperature for 12 hours, and then ground into powder to obtain lithium titanate Li4Ti5O 12 ;

[0079] (3) Weigh 0.96 g lithium titanate Li4Ti5O 12 and 0.64 g of lithium chloride LiCl powder, adding the powder to the mixture, stirring on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0080] (4) using a coating machine to apply the suspension onto a copper foil current collector to form an electrode sheet to be tested with a coating thickness of 0.4 mm;

[0081] (5) placing the electrode sheet in a blast drying oven for 2 hours, the temperature of which is set at 80° C., and then placing it in a vacuum drying oven for 12 hours, the temperature of which is set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate;

[0082] (6) The electrode sheet is sliced ​​into Φ14 mm electrode discs and assembled into a button battery in a glove box. The button battery structure includes: a positive electrode shell, a circular electrode sheet, a diaphragm, an electrolyte (LiPF6), a lithium sheet, a gasket, a circular spring, and a negative electrode shell.

[0083] (7) Finally, the assembled button battery is subjected to performance testing.

[0084] Example 5

[0085] A lithium chloride and lithium titanate composite electrode material, wherein lithium bromide and lithium titanate are mixed in a mass ratio of 1:9 as active materials, and then mixed with a conductive additive (super P) and a binder (PVDF) in a binder solvent N-methyl-2-pyrrolidone (NMP) solution, as follows:

[0086] (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder respectively, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and then stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution;

[0087] (2) Lithium acetate, tetrabutyl titanate, citric acid monohydrate, and ethanol solution are mixed by a stoichiometric method, and then placed in a magnetic stirrer for thorough mixing. The mixture is dried in a vacuum drying oven to form a white solid. The white solid is ground into powder using an agate mortar. The mixture is then placed in a tube furnace and heated to 800°C at a constant speed of 5°C / min. The mixture is kept at a constant temperature for 12 hours, and then ground into powder to obtain lithium titanate Li4Ti5O 12 ;

[0088] (3) Weigh 1.44 g lithium titanate Li4Ti5O 12 and 0.16 g of lithium bromide LiBr powder, add the powder to the above mixture, stir on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity;

[0089] (4) coating the suspension on a copper foil current collector using a coating machine to form an electrode sheet with a coating thickness of 0.4 mm;

[0090] (5) The electrode sheet is first placed in a blast drying oven for 2 hours, the temperature of the blast drying oven is set to 80° C., and then placed in a vacuum drying oven for 12 hours, the temperature of the drying oven is set to 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate;

[0091] (6) Slice the electrode sheet into Φ14 mm electrode discs and assemble them into button batteries in a glove box. The button battery structure includes: a positive electrode shell, a circular electrode sheet, a diaphragm, an electrolyte (LiPF6), a lithium sheet, a gasket, a circular spring, and a negative electrode shell;

[0092] (7) Finally, the assembled button battery is subjected to performance testing.

[0093] By testing the performance of button batteries made by the above five methods, we found that with the same coating thickness and the same volume, compared with pure lithium titanate material such as Example 1, the specific capacity of the battery assembled by mixing lithium titanate and lithium chloride in different mass ratios and using different preparation methods as the battery positive electrode is significantly increased. See the attached Figure 2As shown in Table 1 below, the charge and discharge specific capacity of the battery prepared in Example 4 is the highest, followed by Example 2, and Examples 3 and 5 are the lowest, but all of them are higher than the specific capacity of Example 1. At the same time, Implementation Case 1, Implementation Case 2, Implementation Case 3, Implementation Case 4, and Implementation Case 5 all have electrochemical reaction platforms at around 1.55V, but Implementation Case 2 and Implementation Case 4 also have an electrochemical reaction platform at 2.5-3.0V and 2.25-2.5V. Therefore, the battery manufactured using the composite material of the present invention has a higher electrochemical reaction platform.

[0094] Table 1 Charge and discharge specific capacity corresponding to the content of LiCl in the implementation case

[0095] Discharge capacity mAh g Charging capacity mAh g Example 1 157.38 154.12 Example 2 535.27 494.02 Example 3 226.88 203.11 Example 4 557.84 603.80 Example 5 231.58 225.25

[0096] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to these embodiments without departing from the present invention and its essence. Therefore, the scope of protection of the present invention is limited by the appended claims.

Claims

1. A positive electrode material for a lithium-ion battery, characterized in that: The invention comprises an active material, a binder, a conductive additive and a binder solvent, wherein the active material is a composite material of lithium halide and lithium titanate mixed in a mass ratio of 4:6; the binder is an aqueous binder with polyvinylidene fluoride (PVDF) as a main component; the conductive additive is conductive carbon black Super P; and the binder solvent is oily N-methylpyrrolidone (NMP); Specifically, 10 ml of N-methyl-2-pyrrolidone NMP solution, 0.2 g of polyvinylidene fluoride PVDF powder, 0.2 g of conductive carbon black super P powder, 0.96 g of lithium titanate Li4Ti5O 12 and 0.64g lithium chloride LiCl powder, The lithium halide includes lithium chloride, wherein the lithium chloride is configured as hydrous lithium chloride or anhydrous lithium chloride; the lithium titanate is prepared by a high-temperature solid phase reaction method or a sol-gel method.

2. A method for preparing a lithium-ion battery positive electrode material according to claim 1, characterized in that: First, the binder and the conductive additive are added to the binder solvent and mixed thoroughly to prepare a mixed solution. Then, lithium chloride and lithium titanate are mixed in a mass ratio of 4:6 and added to the mixed solution to prepare a suspension. The suspension is then coated on the electrode collector. After being fully dried, it can be used as the positive electrode material of the lithium ion battery.

3. The method for preparing a positive electrode material for a lithium ion battery according to claim 2, characterized in that: The mixed lithium chloride powder and lithium titanate powder are placed in a tubular furnace, argon gas is introduced to isolate the air, and the temperature is continuously raised from room temperature to 600°C at a constant speed, kept constant for 1 hour, then heated to 700°C, kept constant for 2 hours, and then naturally cooled to room temperature. It is then ground into powder with an agate mortar and finally added to the mixed liquid.

4. The method for preparing a positive electrode material for a lithium ion battery according to claim 2, characterized in that: First, the binder and the conductive additive are added to the binder solvent, and stirred and fully mixed by a magnetic stirrer to prepare a mixed liquid; Then, lithium chloride and lithium titanate are mixed in a mass ratio of 4:6, added into the mixed solution, and stirred with a magnetic stirrer to be fully mixed to prepare a suspension; Finally, the suspension is coated on the electrode current collector. The prepared electrode sheet is first placed in a blast drying oven for drying at a temperature of 50 to 100°C for 2 to 5 hours, and then moved into a vacuum drying oven for drying at a temperature of 60 to 120°C for 12 to 24 hours. It can be used as a positive electrode material for a lithium-ion battery.

5. The method for preparing a positive electrode material for a lithium ion battery according to claim 4, characterized in that The following steps are involved: (1) first measure 10 ml of N-methyl-2-pyrrolidone NMP solution, then weigh 0.2 g of polyvinylidene fluoride PVDF powder and 0.2 g of conductive carbon black super P powder respectively, add the weighed powders into the N-methyl-2-pyrrolidone NMP solution, and stir with a magnetic stirrer for 2 hours to dissolve the powders into the N-methyl-2-pyrrolidone NMP solution to prepare a mixed solution; (2) Lithium acetate, tetrabutyl titanate, citric acid monohydrate, and ethanol solution are mixed by a stoichiometric method, and then placed in a magnetic stirrer for thorough mixing. The mixture is dried in a vacuum drying oven to form a white solid. The white solid is ground into powder using an agate mortar. The mixture is then placed in a tube furnace and heated to 800°C at a constant speed of 5°C / min. The mixture is kept at a constant temperature for 12 hours, and then ground into powder to obtain lithium titanate Li4Ti5O 12 ; (3) Weigh 0.96 g lithium titanate Li4Ti5O 12 and 0.64 g of lithium chloride LiCl powder, adding the powder to the mixture, stirring on a magnetic stirrer for 3 hours to form a uniform suspension with a certain viscosity; (4) using a coating machine to apply the suspension onto a copper foil current collector to form an electrode sheet to be tested with a coating thickness of 0.4 mm; (5) The electrode sheet is first placed in a forced air drying oven for 2 hours with the temperature of the forced air drying oven set at 80° C., and then placed in a vacuum drying oven for 12 hours with the temperature of the drying oven set at 60° C., thereby preparing a composite electrode sheet of lithium chloride and lithium titanate.