EUV photomask and method for manufacturing the same

By employing a multi-layer structure and precise photoresist patterning technology in EUV photomasks, the problems of insufficient reflectivity and contrast in existing EUV photomask manufacturing technologies have been solved, achieving a highly efficient photolithography process.

CN113359383BActive Publication Date: 2024-11-26TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110109572.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-01
Filing Date
2021-01-26
Publication Date
2024-11-26
Estimated Expiration
2041-01-26

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively manufacture high-contrast EUV photomasks, particularly in preventing damage to the back conductive layer and maintaining high reflectivity.

Method used

The multilayer structure includes a substrate, a reflective multilayer, a cap layer, an intermediate layer, an absorber layer, a cover layer, and a hard mask layer. These layers are patterned using a photoresist layer to form openings and remove the hard mask layer. The absorber layer uses materials such as Ir, Pt, and Ru and is precisely patterned using etching techniques.

Benefits of technology

This technology enables the fabrication of high-contrast EUV photomasks, preventing damage to the back conductive layer, maintaining high reflectivity and absorptivity, and improving the precision and effectiveness of the photolithography process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113359383B_ABST
    Figure CN113359383B_ABST
Patent Text Reader

Abstract

The present disclosure relates to an EUV photomask and a method for manufacturing the same. A reflective mask comprises: a substrate, a reflective multilayer disposed on the substrate, a cap layer disposed on the reflective multilayer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, and a covering layer disposed on the absorber layer. The absorber layer comprises one or more layers of Ir-based materials, Pt-based materials, or Ru-based materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to EUV photomasks and methods of manufacturing the same. Background Art

[0002] Photolithography is one of the key operations in the semiconductor manufacturing process. Photolithography technology includes ultraviolet lithography, deep ultraviolet lithography, and extreme ultraviolet lithography (EUVL). Photomask is an important component in photolithography. It is crucial to manufacture EUV photomasks with high contrast, including high reflectivity parts and high absorption parts. Summary of the invention

[0003] According to one embodiment of the present disclosure, a method for manufacturing a reflective mask is provided, comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a reflective multilayer disposed on the substrate, a cap layer disposed on the reflective multilayer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, a covering layer disposed on the absorber layer, and a hard mask layer disposed on the covering layer; patterning the photoresist layer; patterning the hard mask layer by using the patterned photoresist layer; patterning the covering layer and the absorber layer to form an opening by using the patterned hard mask layer; and removing the hard mask layer, wherein the absorber layer comprises A x B y , wherein A and B are respectively one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:1.

[0004] According to another embodiment of the present disclosure, a method for manufacturing a reflective mask is provided, comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a reflective multilayer arranged on the substrate, a barrier layer arranged on the reflective multilayer, a cap layer arranged on the barrier layer, an intermediate layer arranged on the cap layer, an absorber layer arranged on the intermediate layer, a covering layer arranged on the absorber layer, and a hard mask layer arranged on the covering layer; patterning the photoresist layer; patterning the hard mask layer by using the patterned photoresist layer; patterning the covering layer and the absorber layer to form an opening by using the patterned hard mask layer; and removing the hard mask layer, wherein the barrier layer comprises one or more of silicon nitride, BC, BN, CN or graphene.

[0005] According to another embodiment of the present disclosure, a method for manufacturing a reflective mask is provided, comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a first reflective multilayer arranged on the substrate, a first capping layer arranged on the first reflective multilayer, a first etch stop layer arranged on the first capping layer, a second reflective multilayer arranged on the first etch stop layer, a second capping layer arranged on the second reflective multilayer, a second etch stop layer arranged on the second capping layer, and a hard mask layer on the second etch stop layer; patterning the photoresist layer; patterning the hard mask layer by using the patterned photoresist layer; patterning the second etch stop layer, the second capping layer, and the second absorber layer by using the patterned hard mask layer to form a groove; and forming the absorber layer by filling the groove with EUV absorbing material. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] The present disclosure can be best understood from the following specific embodiments when read in conjunction with the accompanying drawings. It is emphasized that, in accordance with standard practice in the industry, various features are not drawn to scale and are only used for illustration purposes. In fact, the dimensions of various features may be arbitrarily increased or reduced for clarity of discussion.

[0007] Figure 1A , Figure 1B , Figure 1C and Figure 1D An EUV photomask blank according to an embodiment of the present disclosure is shown.

[0008] Figure 2A A cross-sectional view of a photomask blank according to an embodiment of the present disclosure is shown, and Figure 2B A cross-sectional view of a photomask according to an embodiment of the present disclosure is shown.

[0009] Figure 3A A cross-sectional view of a photomask blank according to an embodiment of the present disclosure is shown, and Figure 3B A cross-sectional view of a photomask according to an embodiment of the present disclosure is shown.

[0010] Figure 4A A cross-sectional view of a photomask blank according to an embodiment of the present disclosure is shown, and Figure 4B A cross-sectional view of a photomask according to an embodiment of the present disclosure is shown.

[0011] Figure 5A A cross-sectional view of a photomask blank according to an embodiment of the present disclosure is shown, and Figure 5B A cross-sectional view of a photomask according to an embodiment of the present disclosure is shown.

[0012] Fig. 6A , Figure 6B and Figure 6C A cross-sectional view of an absorber layer of a photomask according to an embodiment of the present disclosure is shown.

[0013] Fig. 7A , Figure 7B , Figure 7C , Fig.7D , Fig. 7E and Figure 7F A method for manufacturing an EUV photomask according to an embodiment of the present disclosure is schematically illustrated.

[0014] Fig. 8A , Figure 8B , Figure 8C and Fig.8D A method for manufacturing an EUV photomask according to an embodiment of the present disclosure is schematically illustrated.

[0015] Fig. 9A and Fig. 9B A method for manufacturing an EUV photomask according to an embodiment of the present disclosure is schematically illustrated.

[0016] Fig. 10A , Fig. 10B , Fig. 10C and Fig. 10D A method for manufacturing an EUV photomask according to an embodiment of the present disclosure is schematically illustrated.

[0017] Fig.11A , Fig. 11B , Fig. 11C and Fig.11D A method for manufacturing an EUV photomask according to an embodiment of the present disclosure is schematically illustrated.

[0018] Fig. 12A and Fig. 12B A method for manufacturing an EUV photomask according to an embodiment of the present disclosure is schematically illustrated.

[0019] Fig.13 A flow chart of a method for manufacturing an EUV photomask blank is shown.

[0020] Fig.14A A flowchart showing a method of manufacturing a semiconductor device, and Fig. 14B , Fig. 14C , Fig.14D and Fig.14E Sequential manufacturing operations of a method of manufacturing a semiconductor device according to an embodiment of the present disclosure are shown. Specific embodiments

[0021] It should be understood that the following disclosure provides many different embodiments or examples for realizing different features of the present invention. Specific embodiments or examples of components and arrangements are described below to simplify the present disclosure. Of course, these are only examples and are not intended to be restrictive. For example, the size of the element is not limited to the disclosed range or value, but may depend on the process conditions and / or desired characteristics of the device. In addition, in the following description, forming a first feature above or on a second feature may include an embodiment in which the first feature and the second feature are formed in direct contact, and may also include an additional feature that may be formed between the first feature and the second feature so that the first feature and the second feature may not be in direct contact. For simplicity and clarity, various features may be arbitrarily drawn in different proportions.

[0022] In addition, for ease of description, spatially related terms (e.g., "below," "below," "below," "above," "upper," etc.) may be used herein to describe the relationship of an element or feature shown in the figure to another (one or more) element or (one or more) feature. These spatially related terms are intended to cover different orientations of the device in use or operation except for the orientation shown in the figure. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially related descriptors used herein may also be interpreted accordingly. In addition, the term "made of..." may mean "including" or "consisting of..." In the present disclosure, the phrase "one of A, B and C" refers to "A, B and / or C" (A, B, C, A and B, A and C, B and C, or A, B and C), and unless otherwise specified, it does not mean that one element is from A, one element is from B and one element is from C. The materials, configurations, processes and / or dimensions explained with respect to one embodiment may be used in other embodiments, and their detailed description may be omitted.

[0023] Embodiments of the present disclosure provide a method for manufacturing an EUV photomask. More specifically, the present disclosure provides a technique for preventing or suppressing damage to a back conductive layer of an EUV photomask.

[0024] EUV lithography (EUVL) uses scanners that use light in the extreme ultraviolet (EUV) region, with a wavelength of about 1 nm to about 100 nm, for example, 13.5 nm. The mask is a key component of the EUVL system. Since optical materials are not transparent to EUV radiation, the EUV photomask is a reflective mask. The circuit pattern is formed in an absorber layer disposed above the reflective structure. The absorber layer has a low EUV reflectivity, for example, less than 3-5%. The present disclosure provides an EUV reflective photomask having a low reflective (high absorption) absorber structure.

[0025] Figure 1A and Figure 1B An EUV reflective photomask blank according to an embodiment of the present disclosure is shown. Figure 1D A patterned EUV reflective photomask is shown ready for EUV lithography. Figure 1A is a plan view (seen from the top), and Figure 1B is a cross-sectional view along the X direction. Some layers described in the following embodiments are not shown in FIG. Figure 1A-Figure 1D Shown in.

[0026] In some embodiments, an EUV photomask having a circuit pattern is formed from an EUV photomask blank 5. The EUV photomask blank 5 includes a substrate 10, a multilayer Mo / Si stack 15 of a plurality of alternating layers of silicon and molybdenum, a cap layer 20, an absorber layer 25, a capping (or anti-reflection) layer 27, and a hard mask layer 30. Figure 1B As shown, a back conductive layer 45 is formed on the back side of the substrate 10 .

[0027] In some embodiments, the substrate 10 is formed of a low thermal expansion material. In some embodiments, the substrate is a low thermal expansion glass or quartz, for example, fused silica glass or fused quartz. In some embodiments, the low thermal expansion glass substrate transmits light of a visible wavelength, a portion of infrared wavelengths (near infrared) near the visible spectrum, and a portion of ultraviolet wavelengths. In some embodiments, the low thermal expansion glass substrate absorbs extreme ultraviolet wavelengths and deep ultraviolet wavelengths close to extreme ultraviolet wavelengths. In some embodiments, the size of the substrate 10 is about 152 mm×about 152 mm, and the thickness is about 20 mm. In other embodiments, the size of the substrate 10 is less than 152 mm×152 mm, and is equal to or greater than 148 mm×148 mm. In some embodiments, the shape of the substrate 10 is square or rectangular.

[0028] In some embodiments, the width of the functional layers (multilayer Mo / Si stack 15, cap layer 20, absorber layer 25, cap layer 27, and hard mask layer 30) above the substrate is less than the width of the substrate 10. In some embodiments, the size of the functional layer is in the range of from about 138 mm×138 mm to 142 mm×142 mm. In some embodiments, the shape of the functional layer is square or rectangular.

[0029] In other embodiments, the absorber layer 25, the cap layer 27, and the hard mask layer 30 have smaller dimensions than the substrate 10, the multilayer Mo / Si stack 15, and the cap layer 20, ranging from about 138 mm×138 mm to about 142 mm×142 mm, as shown in FIG. Figure 1CWhen forming each functional layer by, for example, sputtering, a smaller size of one or more functional layers can be formed by using a frame-shaped cover having an opening ranging from about 138 mm×138 mm to about 142 mm×142 mm. In other embodiments, all layers above substrate 10 have the same size as substrate 10.

[0030] In some embodiments, the Mo / Si multilayer stack 15 includes about 30 pairs of alternating silicon and molybdenum layers to about 60 pairs of alternating silicon and molybdenum layers. In certain embodiments, about 40 to about 50 pairs of alternating silicon and molybdenum layers are formed. In some embodiments, for a wavelength of interest, such as 13.5nm, the reflectivity is higher than about 70%. In some embodiments, the silicon layer and the molybdenum layer are formed by chemical vapor deposition (CVD), plasma enhanced CVD (PECVD), atomic layer deposition (ALD), physical vapor deposition (PVD) (sputtering), or any other suitable method for forming a film. Each layer of silicon and molybdenum is about 2nm to about 10nm thick. In some embodiments, the silicon layer and the molybdenum layer have about the same thickness. In other embodiments, the silicon layer and the molybdenum layer have different thicknesses. In some embodiments, the thickness of each silicon layer is about 4nm, and the thickness of each molybdenum layer is about 3nm. In some embodiments, the bottom layer of the multilayer stack 15 is a Si layer or a Mo layer.

[0031] In other embodiments, the multilayer stack 15 includes alternating layers of molybdenum and beryllium. In some embodiments, the number of layers in the multilayer stack 15 ranges from about 20 to about 100, but any number of layers is allowed as long as sufficient reflectivity is maintained for imaging the target substrate. In some embodiments, the reflectivity is higher than about 70% for wavelengths of interest, such as 13.5 nm. In some embodiments, the multilayer stack 15 includes about 30 to about 60 layers of alternating layers of Mo and Be. In other embodiments of the present disclosure, the multilayer stack 15 includes about 40 to about 50 layers of alternating layers of Mo and Be.

[0032] In some embodiments, the capping layer 20 is disposed on the Mo / Si multilayer stack 15 to prevent oxidation of the multilayer stack 15. In some embodiments, the capping layer 20 is composed of elemental ruthenium (greater than 99% Ru, non-Ru compounds), ruthenium alloys (e.g., RuNb, RuZr, RuZrN, RuRh, RuNbN, RuRhN, RuV, RuVN, RuIr, RuTi, RuB, RuP, RuOs, RuPd, RuPt, or RuRe), or ruthenium-based oxides (e.g., RuO 2 , RuNbO, RiVO or RuON) with a thickness of about 2 nm to about 10 nm. In some embodiments, the cap layer 20 is a ruthenium compound Ru x M1-x , wherein M is one or more of Nb, Ir, Rh, Zr, Ti, B, P, V, Os, Pd, Pt, or Re, and x is greater than zero and equal to or less than about 0.5

[0033] In some embodiments, the thickness of the capping layer 20 is from about 2 nm to about 5 nm. In some embodiments, the thickness of the capping layer 20 is 3.5 nm ± 10%. In some embodiments, the capping layer 20 is formed by chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition (e.g., sputtering), or any other suitable method of forming a film. In other embodiments, a Si layer is used as the capping layer 20. As described below in some embodiments, one or more layers are provided between the capping layer and the multilayer 15.

[0034] In some embodiments, the capping layer 20 includes two or more layers of different materials. In some embodiments, the capping layer 20 includes two or more layers of different Ru-based materials. In some embodiments, the capping layer 20 includes two layers including a lower layer and an upper layer, and the lower layer has a higher carbon absorption resistance than the upper layer, and the lower layer has a higher etching resistance during absorber etching. In certain embodiments, the capping layer 20 includes a RuNb-based layer (RuNb or RuNbN) disposed on a RuRh-based layer (RuRh or RuRhN).

[0035] The absorber layer 25 is disposed on the cap layer 20. The absorber layer includes a high EUV absorbing material having a k value greater than about 0.03 or greater than about 0.045. In some embodiments, the absorber layer 25 is a Ta-based material. In some embodiments, the absorber layer 25 is made of TaN, TaO, TaB, TaBO, or TaBN. In other embodiments, the absorber layer 25 includes a Cr-based material, for example, CrN, CrBN, CrO, and / or CrON. In some embodiments, the absorber layer 25 has a multilayer structure of Cr, CrO, or CrON. In some embodiments, the absorber layer is Ir or an Ir-based material, for example, IrRu, IrPt, IrN, IrAl, IrSi, or IrTi. In some embodiments, the absorber layer is a Ru-based material, for example, IrRu, RuPt, RuN, RuAl, RuSi, or RuTi, or a Pt-based material, for example, PtIr, RuPt, PtN, PtAl, PtSi, or PtTi. In other embodiments, the absorber layer includes an Os-based material, a Pd-based material, or a Re-based material. In some embodiments of the present disclosure, the X-based material refers to an amount of X equal to or greater than 50 atomic %.

[0036] In other embodiments, the absorbent layer material is composed of A x B y, wherein A and B are one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al, or Re, respectively, and x:y is from about 0.25:1 to about 4:1. In some embodiments, x is different from y (less than or greater than). In some embodiments, the absorber layer further includes one or more of Si, B, or N in an amount greater than zero to about 10 atomic %.

[0037] In some embodiments, the thickness of the absorber layer 25 is in the range of about 25 nm to about 100 nm, and in other embodiments, in the range of about 50 nm to about 75 nm. In some embodiments, the absorber layer 25 is formed by chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, or any other suitable method of forming a film. As described below in some embodiments, one or more layers are disposed between the cap layer 20 and the absorber layer 25.

[0038] In some embodiments, a capping layer or anti-reflection layer 27 is disposed on the absorber layer 25. In some embodiments, the capping layer 27 comprises a Ta-based material, such as TaB, TaO, or TaBO, silicon, a silicon-based compound (e.g., silicon oxide, SiN, SiON, or MoSi), ruthenium, or a ruthenium-based compound (Ru or RuB). In some embodiments, the capping layer 27 is made of tantalum oxide (Ta 2 O 5 or non-stoichiometric (e.g., oxygen-deficient) tantalum oxide) and has a thickness of about 2 nm to about 20 nm. In other embodiments, a TaBO layer having a thickness ranging from about 2 nm to about 20 nm is used as a capping layer. In some embodiments, the thickness of capping layer 27 is about 2 nm to 5 nm. In some embodiments, capping layer 27 is formed by chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, or any other suitable film-forming method.

[0039] Furthermore, in some embodiments, a protective layer 28 is formed on the cover layer 27 (see FIGS. 2A and 2B ). Figure 2B ). Protective layer 28 includes a silicon compound, such as silicon oxide, silicon nitride, SiON, SiOCN, or MoSiN. In other embodiments, protective layer 28 includes BN or BC. In some embodiments, protective layer 28 has a thickness of about 0.5 nm to about 5 nm, and in other embodiments, about 1 nm to about 3 nm.

[0040] In some embodiments, the hard mask layer 30 is disposed on the protective layer 28. In some embodiments, when the absorber layer 25 is made of a Ta-based material, the hard mask layer 30 is made of a Cr-based material, for example, CrO, CrON, or CrCON. In other embodiments, when the absorber layer 25 is made of a Cr-based material, the hard mask layer 30 is made of a Ta-based material, for example, TaB, TaO, TaBO, or TaBN. In other embodiments, the hard mask layer 30 is made of silicon, a silicon-based compound (for example, SiN or SiON), ruthenium, or a ruthenium-based compound (Ru or RuB). In some embodiments, the hard mask layer 30 has a thickness of about 4 nm to about 20 nm. In some embodiments, the hard mask layer 30 includes two or more different material layers. In some embodiments, the hard mask layer 30 is formed by chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, or any other suitable method of forming a film.

[0041] In some embodiments, the back conductive layer 45 is disposed on the second main surface of the substrate 10, which is opposite to the first main surface of the substrate 10 on which the Mo / Si multilayer stack 15 is formed. In some embodiments, the back conductive layer 45 is made of TaB (tantalum boride) or other Ta-based conductive materials. In some embodiments, the tantalum boride is crystalline. Crystalline tantalum boride includes TaB, Ta 5 B 6 、 3 B 4 and TaB 2. In other embodiments, the tantalum boride is polycrystalline or amorphous. In other embodiments, the back conductive layer 45 is made of a Cr-based conductive material (CrN or CrON). In some embodiments, the sheet resistance of the back conductive layer 45 is equal to or less than 20Ω / □. In certain embodiments, the sheet resistance of the back conductive layer 45 is equal to or greater than 0.1Ω / □. In some embodiments, the surface roughness Ra of the back conductive layer 45 is equal to or less than 0.25nm. In certain embodiments, the surface roughness Ra of the back conductive layer 45 is equal to or greater than 0.05nm. In addition, in some embodiments, the flatness of the back conductive layer 45 is equal to or less than 50nm. In some embodiments, the flatness of the back conductive layer 45 is greater than 1nm. In some embodiments, the thickness of the back conductive layer 45 is in the range from about 50nm to about 400nm. In other embodiments, the back conductive layer 45 has a thickness of about 50nm to about 100nm. In certain embodiments, the thickness is in the range from about 65nm to about 75nm. In some embodiments, the back conductive layer 45 is formed by atmospheric chemical vapor deposition (CVD), low pressure CVD, plasma enhanced CVD, laser enhanced CVD, atomic layer deposition (ALD), molecular beam epitaxy (MBE), physical vapor deposition (including thermal deposition, pulsed laser deposition, electron beam evaporation, ion beam assisted evaporation and sputtering), or any other suitable film forming method. In some embodiments, in the case of CVD, the source gas includes TaCl 5 and BCl 3 .

[0042] Figure 2A and Figures 2B to 5A and Figure 5B Various structures of a mask blank ("A" panel) and a patterned photomask ("B" panel) are shown.

[0043] In some embodiments, Figure 2A and Figure 2B As shown, an intermediate layer 22 is formed between the cap layer 20 and the absorber layer 25. In some embodiments, the intermediate layer 22 is used as an etch stop layer during the patterning operation of the absorber layer and is used to protect the cap layer 20. In some embodiments, the intermediate layer 22 includes a Ta-based compound, such as TaB, TaO, TaBO, or TaBN; a Cr-based compound, such as CrO, CrON, or CrN; silicon; a silicon-based compound (e.g., silicon oxide, SiN (Si:N is about 1:1 to about 3:4), SiON, or MoSi); molybdenum; niobium; niobium oxide; ruthenium; a ruthenium-based compound (RuO 2or RuB); BC (the atomic ratio of B and C is about 1:1 to about 4:1); BN; CN (the atomic ratio of C and N is about 1:1 to about 3:4) or a two-dimensional material, for example, graphene. In some embodiments, the intermediate layer is composed of A x B y Representing, wherein A is Ta and / or Cr, and B is one or more of Si, O, N, Al, or Ti, in some embodiments, x:y is about 0.2:1 to about 5:1.

[0044] In other embodiments, the intermediate layer 22 includes a metal oxide, such as niobium oxide, tantalum oxide, ruthenium oxide, and / or molybdenum oxide. In other embodiments, the intermediate layer 22 includes an elemental metal (not a compound), such as Mo, Ta, Cr, Ni, Co, and / or Ir. In some embodiments, the intermediate layer 22 is composed of tantalum oxide (Ta 2 O 5 In some embodiments, the intermediate layer 22 is made of the same or similar material as the cap layer 27. In some embodiments, the intermediate layer 22 has a lower hydrogen diffusion rate than Ru (a hydrogen barrier), and / or a lower carbon solubility or reactivity than Ru (a protective layer against carbon or hydrocarbon contamination).

[0045] In some embodiments, the intermediate layer 22 has a thickness of about 0.5 nm to about 5 nm, and in other embodiments, the thickness is in the range of about 1 nm to about 3 nm. In some embodiments, the intermediate layer 22 is formed by chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, or any other suitable film forming method.

[0046] In other embodiments, the intermediate layer 22 is a photocatalytic layer that can catalyze hydrocarbon residues formed on the photomask into CO when exposed to EUV radiation. 2 and / or H 2 O. Thus, in-situ self-cleaning of the mask surface is performed. In some embodiments, in an EUV scanner system, oxygen and hydrogen are injected into the EUV chamber to maintain the chamber pressure (e.g., about 2 Pa). The chamber background gas can be a source of oxygen for the cleaning operation. In addition to the photocatalytic function, the photocatalytic layer is also designed to have sufficient durability and resistance to various chemicals and various chemical processes (e.g., cleaning and etching). In some examples, ozonated water used in subsequent processes to manufacture EUV reflective masks can damage the cap layer 20 made of Ru and cause a significant decrease in EUV reflectivity. In addition, after Ru oxidation, Ru oxide is easily oxidized by substances such as Cl 2 or CF 4In some embodiments, the photocatalytic layer includes titanium oxide (TiO 2 ), tin oxide (SnO), zinc oxide (ZnO), and cadmium sulfide (CdS). In some embodiments, the thickness of the photocatalytic layer 22 is in a range from about 2 nm to about 10 nm, and in other embodiments, in a range from about 3 nm to about 7 nm. When the thickness is too thin, the photocatalytic layer may not be sufficient to serve as an etch stop layer. When the thickness is too large, the photocatalytic layer may absorb EUV radiation.

[0047] Furthermore, in some embodiments, a barrier layer 18 is formed between the multilayer 15 and the cap layer 20, and the uppermost layer of the multilayer 15 is a Si layer that is not in contact with the cap layer 20. In some embodiments, the barrier layer 18 comprises a silicon compound, such as silicon oxide, silicon nitride, SiON, SiOCN, or MoSiN. In other embodiments, the barrier layer 18 comprises a metal oxide, such as niobium oxide, tantalum oxide, ruthenium oxide, and / or molybdenum oxide. In other embodiments, the barrier layer 18 comprises an elemental metal (not a compound), such as Be, Mo, Ta, Cr, Ni, Co, and / or Ir. In some embodiments, the barrier layer comprises BN or BC.

[0048] In some embodiments, the thickness of barrier layer 18 is in the range of about 0.5 nm to about 5 nm, and in other embodiments, the thickness is in the range of about 1 nm to about 3 nm. In some embodiments, barrier layer 18 is formed by chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, thermal oxidation or chemical oxidation, or any other suitable film-forming method.

[0049] When the capping layer 20 made of Ru or Ru alloy layer is in direct contact with the Si layer of the multilayer stack 15, the adhesion of the Ru-based layer to the Si layer may be weak due to hydrogen diffusion and hydrogen accumulation at the interface between the Ru-based layer and the Si layer. Figure 2A and Figure 2B In the illustrated embodiment, with the barrier layer 18 interposed between the multilayer stack 15 and the capping layer 20 , sufficient bonding or adhesion strength may be maintained between the capping layer and the multilayer stack 15 .

[0050] like Figure 2B As shown, after forming the circuit pattern 42 , the hard mask layer 30 is removed, and thus the EUV photomask does not include the hard mask layer.

[0051] In some embodiments, Figure 3A and Figure 3B As shown, the uppermost layer of the multilayer stack 15 is a Mo layer. The remaining layer structure is the same as that of Figure 2A and Figure 2BThe illustrated layer structures are the same and their detailed description is omitted. In other words, the uppermost Si layer of the multilayer 15 does not contact the barrier layer 20. As shown in FIG. 3B, after forming the circuit pattern 42, the hard mask layer 30 is removed, so the EUV photomask does not include the hard mask layer.

[0052] In some embodiments, Figure 4A and Figure 4B As shown, barrier layer 18 is not formed. The uppermost layer of multilayer stack 15 is a Si layer. In some embodiments, cap layer 20A is continuously formed on multilayer stack 15 in the same film deposition apparatus. In some embodiments, an ion beam deposition process is used to form multilayer stack 15 and cap layer 20A by changing a target material. Compared with the case where the cap layer is formed by a different deposition apparatus or the multilayer stack 15 is exposed to the atmosphere before forming the cap layer 20A, the continuously formed cap layer 20A has a higher adhesion strength to the multilayer stack 15. The remaining layer structures are the same as those described above. Figure 2A and Figure 2B The layer structures described are the same, and their detailed descriptions are omitted.

[0053] In some embodiments, Figure 5A and Figure 5B As shown, barrier layer 18 is not formed, and the uppermost layer of multilayer stack 15 is a Mo layer. In some embodiments, cap layer 20A is continuously formed on multilayer stack 15 in the same film deposition apparatus, as described above. When a cap layer made of Ru or a Ru alloy layer is in direct contact with a Si layer of multilayer stack 15, the Ru-based layer may have weak adhesion to the Si layer due to hydrogen diffusion and hydrogen accumulation at the interface between the Ru-based layer and the Si layer. Figure 5A and Figure 5B In some of the embodiments shown, where the multilayer stack 15 is terminated by a Mo layer, sufficient bonding or adhesion strength is maintained between the cap layer and the multilayer stack 15 .

[0054] Fig. 6A , Figure 6B and Figure 6C A cross-sectional view of an absorber layer of a photomask according to an embodiment of the present disclosure is shown.

[0055] The configuration of the absorber layer 25 is not limited to the aforementioned embodiment. Fig. 6A In some embodiments, the absorber layer 25 is a single layer. In some embodiments, the absorber layer is a double layer of a lower layer 25A and an upper layer 25B, such as Figure 6BAs shown. Any combination of the two materials described above can be used for the lower layer 25A and the upper layer 25B. In some embodiments, one of the lower layer and the upper layer is a Ru-based material as listed above, and the other is an Ir-based material as listed above. The thickness of the lower layer 25A can be the same as or different (smaller or larger) than the thickness of the upper layer 25B.

[0056] In other embodiments, Figure 6C As shown, the absorber layer 25M has a multi-layer structure (more than two layers and equal to or less than 10 layers). In some embodiments, two materials are alternately stacked in the absorber layer 25M, and in other embodiments, three or more materials are used. In the case of using two materials, the two materials have the same Figure 6B Double layers of the same or similar configuration.

[0057] Figure 7A-7F and Figure 8A-8D The method for manufacturing an EUV photomask for extreme ultraviolet lithography (EUVL) is schematically shown. It should be understood that the method can be Figures 7A-8D Additional operations are provided before, during, and after the processes shown, and some of the operations described below may be replaced or eliminated for additional embodiments of the method. The order of these operations / processes may be interchangeable. Figure 7A-7F and Figure 8A-8D In the figure, for simplicity, the optional protective layer 28 and the barrier layer 18 are omitted. In addition, the uppermost layer of the multilayer stack may be a Mo layer.

[0058] In the manufacture of the EUV photomask, a first photoresist layer 35 is formed on the hard mask layer 30 of the EUV photomask blank. Fig. 7A As shown, the photoresist layer 35 is selectively exposed to actinic radiation EB, as shown Figure 7B In some embodiments, before forming the first photoresist layer 35, the EUV photomask blank is inspected. The selectively exposed first photoresist layer 35 is developed to form a pattern 40 in the first photoresist layer 35, as shown in FIG. Figure 7C In some embodiments, the actinic radiation EB is an electron beam or an ion beam. In some embodiments, pattern 40 corresponds to the pattern of semiconductor device features that an EUV photomask will be used to form in a subsequent operation.

[0059] Next, the pattern 40 in the first photoresist layer 35 is extended into the hard mask layer 30, thereby forming a pattern 41 in the hard mask layer 30, exposing portions of the capping layer 27, such as Fig.7DIn some embodiments, a pattern 41 extending into the hard mask layer 30 is formed by etching using a suitable wet or dry etchant that is selective to the cap layer 27. After the pattern 41 in the hard mask layer 30 is formed, the first photoresist layer 35 is removed using a photoresist stripper to expose the upper surface of the hard mask layer 30, as shown in FIG. Fig. 7E shown.

[0060] Then, the pattern 41 in the hard mask layer 30 is extended into the cap layer 27 and the absorber layer 25, thereby forming a pattern 42 in the cap layer 27 and the absorber layer 25 (see Fig. 8A ), exposing multiple portions of the intermediate layer 22, such as Figure 7F As shown, the hard mask layer 30 is then removed, as shown in FIG. Fig. 8A As shown. In some embodiments, a pattern 42 extending into the capping layer 27 and the absorber layer 25 is formed by etching using a suitable wet or dry etchant that is selective to the intermediate layer 22. In some embodiments, plasma dry etching is used. In some embodiments, when the intermediate layer 22 is made of the same material or a similar material as the hard mask layer 30, or when the intermediate layer 22 and the hard mask layer 30 have similar etching resistance to the etching of the absorber layer 25, the etching is substantially stopped at the intermediate layer 22. In some embodiments, the capping layer 27 is patterned by using the patterned hard mask layer 30, and then the absorber layer 25 is patterned by using the patterned capping layer 27 as an etching mask with or without the hard mask layer 30 (i.e., the capping layer is used as a hard mask).

[0061] like Figure 8B As shown, a second photoresist layer 50 is formed on the absorber layer 25, filling the cap layer 27 and the pattern 42 in the absorber layer 25. The second photoresist layer 50 is selectively exposed to actinic radiation, such as an electron beam, an ion beam, or UV radiation. The selectively exposed second photoresist layer 50 is developed to form a pattern 55 in the second photoresist layer 50, as shown in FIG. Figure 8B As shown. Pattern 55 corresponds to a black edge surrounding the circuit pattern. The black edge is a frame-shaped area created by removing all the multiple layers on the EUV photomask in the area around the circuit pattern area. The frame-shaped area is created to prevent exposure of adjacent fields when the EUV photomask is printed on the wafer. In some embodiments, the width of the black edge ranges from about 1 mm to about 5 mm.

[0062] Next, the pattern 55 in the second photoresist layer 50 is extended into the capping layer 27, the absorber layer 25, the capping layer 20 and the Mo / Si multilayer 15 to form the pattern 57 in the absorber layer 25, the capping layer 20 and the Mo / Si multilayer 15 (see Fig.8D ), exposing multiple portions of substrate 10, as shown in FIG8C. In some embodiments, pattern 57 is formed by etching using one or more suitable wet or dry etchants that are selective to each layer being etched. In some embodiments, plasma dry etching is used.

[0063] Then, the second photoresist layer 50 is removed using a suitable photoresist stripper to expose the upper surface of the absorber layer 25, such as Fig.8D In some embodiments of the present disclosure, the black edge pattern 57 in the capping layer 27, the absorber layer 25, the capping layer 20, and the Mo / Si multilayer 15 defines a black edge of the photomask.

[0064] Fig. 9A and Fig. 9B A cross-sectional view of an EUV reflective photomask according to an embodiment of the present disclosure is shown. The materials, configurations, processes and / or dimensions described with respect to the previous embodiments may be adopted in the following embodiments, and a detailed description thereof may be omitted.

[0065] exist Fig. 9A and Fig. 9B In an embodiment, the absorber layer is embedded in the multi-layer reflective layer.

[0066] like Fig. 9A As shown, an additional upper multilayer reflective layer 56 is formed on the intermediate layer 22. The structure of the upper multilayer reflective layer 56 is the same as that of the multilayer structure 15 described above. In some embodiments, the number of pairs of Si layers and Mo layers (or the number of pairs of Mo layers and Be layers) of the upper multilayer reflective layer 56 is equal to or less than that of the multilayer structure 15, and is in the range of about 20 to about 40. An upper barrier layer 48 is formed on the upper multilayer reflective layer 56. The material of the upper barrier layer 48 has the same or similar configuration as the barrier layer 18, and includes one or more materials as described above with respect to the barrier layer 18. In some embodiments, at least one of the barrier layer 18 or the upper barrier layer 48 is not formed.

[0067] In addition, in some embodiments, an upper capping layer 51 is formed on the upper barrier layer. The material of the upper capping layer 51 has the same or similar configuration as the capping layer 20, and includes one or more materials as described above with respect to the capping layer 20. In some embodiments, an upper etch stop layer 52 is formed on the upper capping layer. The material of the upper etch stop layer 52 has the same or similar configuration as the intermediate (etch stop) layer 22, and includes one or more materials as described above with respect to the intermediate layer 22.

[0068] In some embodiments, the absorber layer 80 is formed in a groove corresponding to the circuit pattern formed in the upper etch stop layer 52, the upper cap layer 51, and the upper multi-layer reflective layer 56, as shown in FIG. Fig. 9A The material of the absorber layer 80 has the same or similar configuration as that of the absorber layer 25 (see Figure 2A-Figure 6C ), and includes one or more materials as described above with respect to the absorber layer 25. In some embodiments, an anti-reflection layer 82 is formed on the absorber layer 25. The material of the anti-reflection layer 82 has the same or similar configuration as the anti-reflection layer 27 (see Figure 2A-Figure 6C ), and includes one or more materials as described above with respect to the anti-reflective layer 27. In some embodiments, the anti-reflective layer is not formed. In addition, in some embodiments, a protective layer 85 is formed over the upper etch stop layer 52 and the anti-reflective layer 82 (if present). The material of the protective layer 85 has the same or similar configuration as the protective layer 28 (see Figure 2A-Figure 6C ), and includes one or more materials as described above with respect to protection layer 28. In some embodiments, one or more layers of upper barrier layer 48, upper capping layer 51, and upper etch stop layer 52 are not formed.

[0069] exist Fig. 9B In the embodiment, the absorber layer 80 is at least partially embedded in the multilayer structure 15. In some embodiments, the bottom of the absorber layer 80 is spaced apart from the substrate 10, and in other embodiments, the bottom of the absorber layer 80 is in contact with the substrate 10. Fig. 9B As shown, in some embodiments, a protective layer 85 is formed over the intermediate layer 22 and the anti-reflective layer 82 (if present).

[0070] Figures 10A-10D , Figures 11A-11D and Figure 12A-12B The schematic diagram shows the manufacturing process of Fig. 9A It should be understood that the EUV photomask method shown in FIG. Figures 10A-12BAdditional operations are provided before, during and after the processes shown, and for other embodiments of the method, some operations described below may be replaced or eliminated. The order of operations / processes may be interchangeable. In the following embodiments, materials, configurations, processes and / or dimensions explained relative to the aforementioned embodiments may be adopted, and their detailed description may be omitted.

[0071] Fig. 10A The mask set structure is shown. The hard mask layer 30 is formed on the upper etch stop layer 52. The first photoresist layer 65 is formed on the hard mask layer 30 of the EUV photomask blank, as shown in FIG. Fig. 10B The first photoresist layer 65 is selectively exposed to actinic radiation (eg, electron beam), and the selectively exposed first photoresist layer 65 is developed to form a pattern 70 in the photoresist layer 65, as shown. Fig. 10C shown.

[0072] Next, the pattern 70 in the photoresist layer 65 is extended into the hard mask layer 30, thereby forming a pattern 71 in the hard mask layer 30, exposing portions of the upper etch stop layer 52, as shown in FIG. 10D. In some embodiments, the pattern 71 extending into the hard mask layer 30 is formed by etching using a suitable wet or dry etchant that is selective to the upper etch stop layer 52. After forming the pattern 71 in the hard mask layer 30, the photoresist layer 65 is removed by a photoresist stripper to expose the upper surface of the hard mask layer 30, as shown in FIG. Fig. 10D shown.

[0073] Then, the pattern 71 in the hard mask layer 30 is extended into the upper etch stop layer 52, the upper cap layer 51, the upper barrier layer 48 and the upper multi-layer reflective layer 56, thereby forming a groove pattern 72, as shown in FIG. Fig.11A In some embodiments, the trench etching stops at the intermediate (etch stop) layer 22. Then, the hard mask layer 30 is removed, as shown in FIG. Fig. 11B shown.

[0074] Next, if Fig. 11C As shown, one or more layers 80L for the absorber layer 80 are formed in the groove pattern 72 and on the upper etch stop layer 52. Then, a planarization operation, such as a chemical mechanical polishing (CMP) operation, is performed to remove excess material on the upper etch stop layer 52 to form the absorber layer (pattern) 80, as shown in FIG. Fig.11D In some embodiments, the hard mask layer is not removed prior to forming layer 80L, and is removed after or during the CMP operation.

[0075] Then, in some embodiments, an anti-reflection layer 82 is formed on the absorber layer 80. When the absorber layer 80 is made of a Ta-based material, the anti-reflection layer 82 is formed by oxidation of the absorber layer 80. Subsequently, a protective layer 85 is formed over the anti-reflection layer 82 and the upper etch stop layer 52, such as Fig. 12B In addition, similar to reference Figure 8B-Figure 8D The operation described above forms a black edge pattern.

[0076] Fig.13 FIG. 1 shows a flow chart of manufacturing one or more mask blanks of the aforementioned embodiments. It can be understood that Fig.13 Additional operations are provided before, during, and after the processes shown, and some of the operations described below may be replaced or eliminated for additional embodiments of the method. The order of operations / processes may be interchangeable.

[0077] At S101, a multilayer stack is formed on a substrate. In some embodiments, before forming the multilayer stack, one or more layers are formed on the substrate. In some embodiments, the multilayer stack is formed by an ion beam deposition method or a sputtering method. In some embodiments, the multilayer stack is terminated with a Si layer, and in other embodiments, the multilayer stack is terminated with a Mo layer. At S102, a barrier layer is formed on the multilayer stack. Then, at S103, a capping layer is formed on the barrier layer.

[0078] In some embodiments, a barrier layer is not formed, and a capping layer is formed directly on the multilayer stack. In some embodiments, the capping layer is continuously formed on the multilayer stack by an ion beam deposition method in the same deposition apparatus as the multilayer stack.

[0079] At S104, an intermediate (barrier) layer is formed on the cap layer. At S105, one or more absorber layers are formed on the intermediate layer. At S106, a capping (anti-reflection) layer is formed on the absorber layer. In some embodiments, the absorber layer is formed by a deposition method, and in other embodiments, the absorber layer is formed by oxidation of a Ta-based absorber layer. At S107, a protective layer is formed on the capping layer, and at S108, a hard mask layer is formed on the capping layer.

[0080] In manufacturing for Fig. 9A In the mask blank of the photomask shown, operations S101-S104 are repeated twice, and operations S105-S107 are skipped.

[0081] Fig.14A A process for manufacturing a semiconductor device is shown, and Fig. 14B , Fig. 14C , Fig.14D and Fig.14ESequential manufacturing operations of a method for manufacturing a semiconductor device according to an embodiment of the present disclosure are shown. A semiconductor substrate or other suitable substrate is provided, which is to be patterned to form an integrated circuit thereon. In some embodiments, the semiconductor substrate includes silicon. Alternatively or additionally, the semiconductor substrate includes germanium, silicon germanium, or other suitable semiconductor material, such as a III-V semiconductor material. Fig.14A In S201, a target layer to be patterned is formed on a semiconductor substrate. In some embodiments, the target layer is a semiconductor substrate. In some embodiments, the target layer includes a conductive layer such as a metallization layer or a polysilicon layer; a dielectric layer such as silicon oxide, silicon nitride, SiON, SiOC, SiOCN, SiCN, hafnium oxide, or aluminum oxide; or a semiconductor layer such as an epitaxially formed semiconductor layer. In some embodiments, the target layer is formed on an underlying structure such as an isolation structure, a transistor, or a wiring. Fig.14A In S202, a photoresist layer is formed on the target layer, such as Fig. 14B As shown. In the subsequent photolithography exposure process, the photoresist layer is sensitive to radiation from the exposure source. In this embodiment, the photoresist layer is sensitive to EUV light used in the photolithography exposure process. The photoresist layer can be formed on the target layer by spin coating or other suitable techniques. The coated photoresist layer can be further baked to drive out the solvent in the photoresist layer. Fig.14A S203, patterning the photoresist layer using the EUV reflective mask as described above, such as Fig. 14B As shown. Patterning the photoresist layer includes performing a photolithography exposure process using an EUV exposure system using an EUV mask. In the exposure process, the integrated circuit (IC) design pattern defined on the EUV mask is imaged to the photoresist layer to form a latent pattern thereon. Patterning the photoresist layer also includes developing the exposed photoresist layer to form a patterned photoresist layer with one or more openings. In an embodiment where the photoresist layer is a positive photoresist layer, the exposed portion of the photoresist layer is removed in the development process. Patterning the photoresist layer may also include other process steps, for example, various baking steps at different stages. For example, a post-exposure baking (PEB) process may be implemented after the photolithography exposure process and before the development process.

[0082] exist Fig.14A S204, using the patterned photoresist layer as an etching mask to pattern the target layer, such as Fig.14DIn some embodiments, patterning the target layer includes applying an etching process to the target layer using the patterned photoresist layer as an etching mask. Portions of the target layer exposed within the openings of the patterned photoresist layer are etched, while the remaining portions are protected from being etched. In addition, the patterned photoresist layer can be removed by wet stripping or plasma ashing, such as Fig.14E shown.

[0083] In the present disclosure, when a high EUV absorption material (e.g., an Ir-based material, a Pt-based material, and / or a Ru-based material) is used as an absorber layer, a high contrast EUV reflective mask can be obtained. In addition, the thickness of the absorber layer can be reduced, which can reduce the three-dimensional effect of the absorber layer. In addition, in some embodiments of the present disclosure, a barrier layer is disposed below the cap layer, which prevents hydrogen diffusion from the EUV mask and the intermediate layer. In addition, in some embodiments of the present disclosure, the multilayer is terminated by a Mo layer, which prevents the cap layer from peeling off from the multilayer.

[0084] It will be understood that not all advantages are necessarily discussed herein, that no particular advantage is necessary for all embodiments or examples, and that other embodiments or examples may provide different advantages.

[0085] According to one aspect of the present application, a reflective mask includes: a substrate, a reflective multilayer disposed on the substrate, a cap layer disposed on the reflective multilayer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, and a covering layer disposed on the absorber layer. The absorber layer includes one or more layers of Ir-based materials, Pt-based materials, or Ru-based materials. In one or more of the foregoing and following embodiments, the absorber layer includes two layers made of materials different from each other. In one or more of the foregoing and following embodiments, the absorber layer includes three or more layers. In one or more of the foregoing and following embodiments, the covering layer is made of the same material as the intermediate layer. In one or more of the foregoing and following embodiments, the intermediate layer and the covering layer include metal oxides. In one or more of the foregoing and following embodiments, the reflective mask also includes an opening pattern formed in the covering layer and the absorber layer, and the intermediate layer is exposed at the bottom of the opening pattern. In one or more of the foregoing and following embodiments, the reflective multilayer includes Si layers and Mo layers stacked alternately, and the Si layer of the reflective multilayer is in contact with the cap layer. In one or more of the foregoing and following embodiments, the reflective multilayer includes Si layers and Mo layers stacked alternately, and the Mo layer of the reflective multilayer is in contact with the cap layer.

[0086] According to another aspect of the present disclosure, a reflective mask includes: a substrate, a reflective multilayer disposed on the substrate, a barrier layer disposed on the reflective multilayer, a cap layer disposed on the barrier layer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, and a covering layer disposed on the absorber layer. The barrier layer includes one or more of silicon nitride, BC, BN, CN, or graphene. In one or more of the foregoing and following embodiments, the absorber layer includes one or more layers of Ir-based materials, Pt-based materials, or Ru-based materials. In one or more of the foregoing and following embodiments, the one or more layers of Ir-based materials, Pt-based materials, or Ru-based materials also include one or more of Si, B, or N. In one or more of the foregoing and following embodiments, the absorber layer includes A x B y , wherein A and B are one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:1. In one or more of the foregoing and following embodiments, the absorber layer further comprises: one or more of Si, B or N, with a content greater than zero to 10 atomic %. In one or more of the foregoing and following embodiments, the intermediate layer comprises a material having a lower hydrogen diffusion rate than the material of the cap layer. In one or more of the foregoing and following embodiments, the intermediate layer comprises one or more of BC, BN, CN or graphene. In one or more of the foregoing and following embodiments, the cap layer comprises Ru x M 1-x , wherein M is one or more of Nb, Ir, Rh, Zr, Ti, B, P, V, Os, Pd, Pt or Re, and x is greater than zero and equal to or less than about 0.5.

[0087] According to another aspect of the present disclosure, a reflective mask includes: a substrate, a first reflective multilayer disposed on the substrate, a first cap layer disposed on the first reflective multilayer, a first etch stop layer disposed on the first cap layer, a second reflective multilayer disposed on the first etch stop layer, a second cap layer disposed on the second reflective multilayer, a second etch stop layer disposed on the second cap layer, and an absorber layer disposed in a groove formed in the second etch stop layer, the second cap layer, and the second reflective multilayer. In one or more of the foregoing and following embodiments, the reflective mask further includes a protective layer disposed on the absorber layer and the second etch stop layer. In one or more of the foregoing and following embodiments, the reflective mask further includes an anti-reflection layer between the protective layer and the absorber layer. In one or more of the foregoing and following embodiments, the number of pairs of Si layers and Mo layers in the second multilayer is equal to or less than the number of pairs of Si layers and Mo layers in the first multilayer.

[0088] According to another aspect of the present disclosure, in a method for manufacturing a reflective mask, a photoresist layer is formed on a mask blank. The mask blank includes a substrate, a reflective multilayer disposed on the substrate, a cap layer disposed on the reflective multilayer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, a cover layer disposed on the absorber layer, and a hard mask layer disposed on the cover layer. The photoresist layer is patterned, the hard mask layer is patterned by using the patterned photoresist layer, the cover layer and the absorber layer are patterned by using the patterned hard mask layer to form an opening, and the hard mask layer is removed. The absorber layer includes A x B y , wherein A and B are one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al or Re, respectively, and x:y is 0.25:1 to 4:1. In one or more of the foregoing and following embodiments, the intermediate layer is used as an etch stop layer when patterning the absorber layer. In one or more of the foregoing and following embodiments, the covering layer is made of the same material as the intermediate layer. In one or more of the foregoing and following embodiments, the absorber layer includes two layers made of materials different from each other. In one or more of the foregoing and following embodiments, the absorber layer includes three or more layers. In one or more of the foregoing and following embodiments, the reflective multilayer includes alternately stacked Si layers and Mo layers, and the Si layer of the reflective multilayer is in contact with the cap layer. In one or more of the foregoing and following embodiments, the reflective multilayer includes alternately stacked Si layers and Mo layers, and the Mo layer of the reflective multilayer is in contact with the cap layer. In one or more of the foregoing and following embodiments, the cap layer is continuously formed by an ion beam deposition method in the same deposition device as the reflective multilayer.

[0089] According to another aspect of the present disclosure, in a method for manufacturing a reflective mask, a photoresist layer is formed on a mask blank. The mask blank includes a substrate, a reflective multilayer disposed on the substrate, a barrier layer disposed on the reflective multilayer, a cap layer disposed above the barrier layer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, a cover layer disposed on the absorber layer, and a hard mask layer disposed on the cover layer. The photoresist layer is patterned, the hard mask layer is patterned by using the patterned photoresist layer, the cover layer and the absorber layer are patterned by using the patterned hard mask layer to form an opening, and the hard mask layer is removed. The barrier layer includes one or more of silicon nitride, BC, BN, CN, or graphene. In one or more of the foregoing and following embodiments, the absorber layer includes A x B y, wherein A and B are one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al or Re, respectively, and x:y is 0.25:1 to 4:1. In one or more of the foregoing and following embodiments, the absorber layer includes one or more layers of Ir-based material, Pt-based material or Ru-based material. In one or more of the foregoing and following embodiments, the absorber layer also includes: one or more of Si, B or N, with a content greater than zero to 10 atomic %. In one or more of the foregoing and following embodiments, the intermediate layer includes a material having a lower hydrogen diffusion rate than the material of the cap layer. In one or more of the foregoing and following embodiments, the intermediate layer includes one or more of BC, BN, CN or graphene. In one or more of the foregoing and following embodiments, the thickness of the intermediate layer is in the range of 0.5nm to 3nm.

[0090] According to another aspect of the present disclosure, in a method for manufacturing a reflective mask, a photoresist layer is formed on a mask blank. The mask blank includes a substrate, a first reflective multilayer disposed on the substrate, a first capping layer disposed on the first reflective multilayer, a first etch stop layer disposed on the first capping layer, a second reflective multilayer disposed on the first etch stop layer, a second capping layer disposed on the second reflective multilayer, a second etch stop layer disposed on the second capping layer, and a hard mask layer on the second etch stop layer. The photoresist layer is patterned, the hard mask layer is patterned by using the patterned photoresist layer, the second capping layer and the second absorber layer are patterned by using the patterned hard mask layer to form a groove, and the absorber layer is formed by filling the groove with an EUV absorbing material. In one or more of the foregoing and following embodiments, a protective layer is also formed on the absorber layer and the second etch stop layer. In one or more of the foregoing and following embodiments, when forming the absorber layer, a layer of EUV absorbing material is formed in the groove and on the second etch stop layer, and chemical mechanical polishing is performed to expose the second etch stop layer. In one or more of the foregoing and following embodiments, an anti-reflection layer is formed on the absorber layer. In one or more of the foregoing and following embodiments, the anti-reflection layer is formed by oxidizing a portion of the absorber layer.

[0091] According to another aspect of the present disclosure, in a method for manufacturing a reflective mask blank, a reflective multilayer is formed on a substrate, a cap layer is formed on the reflective multilayer, an intermediate layer is formed on the cap layer, an absorber layer is formed on the intermediate layer, and a hard mask layer is formed on the absorber layer body. The cap layer is continuously formed by ion beam deposition in the same deposition device as the reflective multilayer. In one or more of the foregoing and following embodiments, the absorber layer includes one or more layers of Ir-based materials, Pt-based materials, or Ru-based materials. In one or more of the foregoing and following embodiments, the absorber layer includes two layers made of materials different from each other. In one or more of the foregoing and following embodiments, the absorber layer includes three or more layers. In one or more of the foregoing and following embodiments, the cover layer is made of the same material as the intermediate layer. In one or more of the foregoing and following embodiments, the intermediate layer and the cover layer include metal oxides. In one or more of the foregoing and following embodiments, an anti-reflection layer is formed on the absorber layer. In one or more of the foregoing and following embodiments, the reflective multilayer includes Si layers and Mo layers stacked alternately, and the Si layer of the reflective multilayer is in contact with the cap layer. In one or more of the foregoing and following embodiments, the reflective multilayer includes Si layers and Mo layers stacked alternately, and the Mo layer of the reflective multilayer is in contact with the cap layer.

[0092] The foregoing summarizes the features of several embodiments or examples so that those skilled in the art can better understand the various aspects of the present disclosure. Those skilled in the art will appreciate that they can easily use the present disclosure as a basis for designing or modifying other processes and structures to achieve the same purposes and / or achieve the same advantages as the embodiments or examples introduced herein. Those skilled in the art will also appreciate that these equivalent constructions do not depart from the spirit and scope of the present disclosure, and that they can make various changes, substitutions, and modifications without departing from the spirit and scope of the present disclosure.

[0093] Example 1. A method for manufacturing a reflective mask, comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a reflective multilayer disposed on the substrate, a cap layer disposed on the reflective multilayer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, a cover layer disposed on the absorber layer, and a hard mask layer disposed on the cover layer; patterning the photoresist layer; patterning the hard mask layer by using the patterned photoresist layer; patterning the cover layer and the absorber layer to form an opening by using the patterned hard mask layer; and removing the hard mask layer, wherein the absorber layer comprises A x B y, wherein A and B are respectively one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:1.

[0094] Example 2. The method of Example 1, wherein the intermediate layer is used as an etch stop layer when patterning the absorber layer.

[0095] Example 3. The method of Example 2, wherein the cover layer is made of the same material as the intermediate layer.

[0096] Example 4. The method of Example 1, wherein the absorber layer comprises two layers made of different materials from each other.

[0097] Example 5. The method of Example 1, wherein the absorber layer comprises three or more layers.

[0098] Example 6. The method according to Example 1, wherein: the reflective multilayer includes Si layers and Mo layers stacked alternately, and the Si layer of the reflective multilayer is in contact with the cap layer.

[0099] Example 7. The method according to Example 1, wherein: the reflective multilayer includes Si layers and Mo layers stacked alternately, and the Mo layer of the reflective multilayer is in contact with the cap layer.

[0100] Example 8. The method according to Example 1, wherein the capping layer is formed continuously with the reflective multilayer by an ion beam deposition method in the same deposition device.

[0101] Example 9. A method for manufacturing a reflective mask, comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a reflective multilayer arranged on the substrate, a barrier layer arranged on the reflective multilayer, a cap layer arranged on the barrier layer, an intermediate layer arranged on the cap layer, an absorber layer arranged on the intermediate layer, a covering layer arranged on the absorber layer, and a hard mask layer arranged on the covering layer; patterning the photoresist layer; patterning the hard mask layer by using the patterned photoresist layer; patterning the covering layer and the absorber layer to form an opening by using the patterned hard mask layer; and removing the hard mask layer, wherein the barrier layer comprises one or more of silicon nitride, BC, BN, CN or graphene.

[0102] Example 10. The method of Example 9, wherein the absorber layer comprises A x B y, wherein A and B are respectively one or more of Ir, Pt, Ru, Cr, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:1.

[0103] Example 11. The method of Example 9, wherein the absorber layer comprises one or more layers of an Ir-based material, a Pt-based material, or a Ru-based material.

[0104] Example 12. The method of Example 9, wherein the absorber layer further comprises: one or more of Si, B or N, with a content greater than zero to 10 atomic %.

[0105] Example 13. The method of Example 9, wherein the intermediate layer comprises a material having a lower hydrogen diffusion rate than a material of the cap layer.

[0106] Example 14. The method according to Example 9, wherein the intermediate layer includes one or more of BC, BN, CN or graphene.

[0107] Example 15. The method of Example 9, wherein the thickness of the intermediate layer is in the range of 0.5 nm to 3 nm.

[0108] Example 16. A method for manufacturing a reflective mask, comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a first reflective multilayer arranged on the substrate, a first capping layer arranged on the first reflective multilayer, a first etch stop layer arranged on the first capping layer, a second reflective multilayer arranged on the first etch stop layer, a second capping layer arranged on the second reflective multilayer, a second etch stop layer arranged on the second capping layer, and a hard mask layer on the second etch stop layer; patterning the photoresist layer; patterning the hard mask layer by using the patterned photoresist layer; patterning the second etch stop layer, the second capping layer, and the second absorber layer to form a groove by using the patterned hard mask layer; and forming an absorber layer by filling the groove with EUV absorbing material.

[0109] Example 17. The method of Example 16, further comprising: forming a protection layer over the absorber layer and the second etch stop layer.

[0110] Example 18. The method of Example 16, wherein forming the absorber layer comprises: forming a layer of the EUV absorbing material in the trench and over the second etch stop layer; and performing chemical mechanical polishing to expose the second etch stop layer.

[0111] Example 19. The method according to Example 16 also includes: forming an anti-reflection layer on the absorber layer.

[0112] Example 20. The method of Example 19, wherein the anti-reflection layer is formed by oxidizing a portion of the absorber layer.

Claims

1. A method for manufacturing a reflective mask, the method comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a reflective multilayer disposed on the substrate, a cap layer disposed on the reflective multilayer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, a cover layer disposed on the absorber layer, and a hard mask layer disposed on the cover layer; patterning the photoresist layer; patterning the hard mask layer by using a patterned photoresist layer; patterning the capping layer and the absorber layer to form openings by using a patterned hard mask layer; and removing the hard mask layer, Wherein, the absorber layer comprises A x B y , wherein A and B are respectively one or more of Ir, Pt, Ru, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:

1.

2. The method according to claim 1, wherein: The intermediate layer serves as an etch stop layer when patterning the absorber layer.

3. The method according to claim 2, wherein: The cover layer is made of the same material as the intermediate layer.

4. The method according to claim 1, wherein: The absorber layer includes two layers made of materials different from each other.

5. The method according to claim 1, wherein: The absorber layer comprises three or more layers.

6. The method according to claim 1, wherein: The reflective multilayer comprises Si layers and Mo layers stacked alternately, and The Si layer of the reflective multilayer is in contact with the cap layer.

7. The method according to claim 1, wherein: The reflective multilayer comprises Si layers and Mo layers stacked alternately, and The Mo layer of the reflective multilayer is in contact with the cap layer.

8. The method according to claim 1, wherein: The capping layer is continuously formed with the reflective multilayer by an ion beam deposition method in the same deposition apparatus.

9. A method for manufacturing a reflective mask, the method comprising: forming a photoresist layer on a mask blank, the mask blank comprising: a substrate, a reflective multilayer disposed on the substrate, a barrier layer disposed on the reflective multilayer, a cap layer disposed on the barrier layer, an intermediate layer disposed on the cap layer, an absorber layer disposed on the intermediate layer, a cap layer disposed on the absorber layer, and a hard mask layer disposed on the cap layer; patterning the photoresist layer; patterning the hard mask layer by using a patterned photoresist layer; patterning the capping layer and the absorber layer to form openings by using a patterned hard mask layer; and removing the hard mask layer, Wherein, the barrier layer comprises one or more of silicon nitride, BC, BN, CN or graphene, Wherein, the absorber layer comprises A x B y , wherein A and B are respectively one or more of Ir, Pt, Ru, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:

1.

10. The method according to claim 9, wherein: The absorber layer includes one or more layers of Ir-based materials, Pt-based materials or Ru-based materials.

11. The method according to claim 9, wherein: The absorber layer further includes: one or more of Si, B or N, with a content greater than zero to 10 atomic %.

12. The method according to claim 9, wherein: The intermediate layer includes a material having a lower hydrogen diffusion rate than a material of the cap layer.

13. The method according to claim 9, wherein: The intermediate layer includes one or more of BC, BN, CN or graphene.

14. The method according to claim 9, wherein: The thickness of the intermediate layer is in the range of 0.5 nm to 3 nm.

15. A method for manufacturing a reflective mask, the method comprising: forming a photoresist layer over a mask blank, the mask blank comprising: a substrate, a first reflective multilayer disposed over the substrate, a first capping layer disposed over the first reflective multilayer, a first etch stop layer disposed over the first capping layer, a second reflective multilayer disposed over the first etch stop layer, a second capping layer disposed over the second reflective multilayer, a second etch stop layer disposed over the second capping layer, and a hard mask layer on the second etch stop layer; patterning the photoresist layer; patterning the hard mask layer by using a patterned photoresist layer; patterning the second etch stop layer, the second capping layer, and the second absorber layer to form a trench by using the patterned hard mask layer; and forming an absorber layer by filling the trenches with an EUV absorbing material, Wherein, the absorber layer comprises A x B y , wherein A and B are respectively one or more of Ir, Pt, Ru, Ta, Os, Pd, Al or Re, and x:y is 0.25:1 to 4:

1.

16. The method according to claim 15, further comprising: A protection layer is formed over the absorber layer and the second etch stop layer.

17. The method according to claim 15, wherein: Forming the absorber layer comprises: forming a layer of the EUV absorbing material in the trench and over the second etch stop layer; and Chemical mechanical polishing is performed to expose the second etch stop layer.

18. The method according to claim 15, further comprising: An anti-reflection layer is formed on the absorber layer.

19. The method according to claim 18, wherein: The anti-reflection layer is formed by oxidizing a portion of the absorber layer.