A production process for making cement clinker using pebbles

By optimizing specific ingredients and calcining processes for pebbles, clay, coal gangue and iron-aluminum materials, the problems of low yield, easy grinding and poor burnability when pebbles replace limestone are solved, and efficient production and quality of cement clinker are achieved. promote.

CN113372030BInactive Publication Date: 2024-11-26LINXIA CONCH CEMENT CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110634065.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-07
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In cement clinker production, when pebbles replace limestone as raw materials, the yield is low, the raw material is easy to grind and has poor burnability, and the clinker is difficult to calcinate, resulting in difficult quality indicators.

Method used

By mixing pebbles, clay, gangue and iron aluminum materials in specific proportions and crushing, grinding and calcining, calcining conditions such as primary fan pressure, burner inflow opening and third air shutter clearance, improve the calcination conditions, The firepower strength is adopted, and the frequency converter fan and CP cooler are used to optimize process parameters to improve production efficiency and clinker quality.

Benefits of technology

It effectively improves the output and quality of pebbles in cement clinker production, reduces power consumption, improves the firing properties of raw materials and the denseness of clinker, and improves the overall efficiency and economy of the production line.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A production process for making cement clinker using pebbles, the invention relates to the technical field of cement preparation, wherein pebbles, clay, coal gangue and iron materials are crushed and homogenized by a mill, and the particle size of the pebbles entering the pile is controlled to be 60 cm; the raw materials are ground by a raw powder grinding system, and the raw materials out of the mill are controlled to be ≤18.0%, and the moisture content of the raw materials is controlled to be ≤0.5%; a burner is used, and the primary fan pressure is controlled to be about 25000Pa, the internal flow opening of the burner is 25%, and the clearance opening of the tertiary air damper is 50cm to extend the flame length and improve the intensity of the calcination fire in front of the kiln. The invention solves the problems of low output, poor grinding and burning of raw materials, and difficulty in calcining clinker when pebbles are used as raw materials to replace limestone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement preparation, and in particular to a production process for making cement clinker by utilizing pebbles. Background Art

[0002] Limestone is one of the important raw materials in cement clinker production, but the reserves of limestone mines are limited and the grades are uneven. Most companies are looking for and developing new alternative raw materials. The mining waste residue of the sand and gravel plant is pebbles, in which the average CaO content is about 40.0%-49.0%, and the SiO2 content is between 5.0%-15.0%. It has the characteristics of high impurity content and more crystalline silicon. It can be used for batching and producing cement clinker.

[0003] However, due to the high hardness of pebbles and their poor grindability compared to limestone, the output of raw materials during grinding is low, the grindability and burnability of raw materials are poor, the clinker calcination is difficult, and the process quality indicators are not well controlled, which seriously restricts the production of clinker cement. Summary of the invention

[0004] The purpose of the present invention is to provide a production process for making cement clinker using pebbles in view of the defects and shortcomings of the prior art, thereby solving the problems of low yield, easy grinding and poor burnability of raw materials, and difficulty in calcining clinker when pebbles are used as raw materials instead of limestone to burn clinker.

[0005] To achieve the above object, the present invention adopts the following technical scheme: its operation steps are as follows:

[0006] Step 1: crushing and homogenizing the raw materials;

[0007] The pebbles, clay, coal gangue and iron materials are crushed and homogenized by a mill, and the particle size of the pebbles entering the pile is controlled to be 60cm;

[0008] Step 2: Raw material ingredients:

[0009] The raw material is one of a dry-based ingredient or a wet-based ingredient, wherein the wet-based ingredient is composed of the following components in parts by weight: 92-94 parts by weight of pebbles, 4-5 parts by weight of clay, 4-4.5 parts by weight of coal gangue, and 3.5-3.8 parts by weight of iron-aluminum materials, which are mixed and stirred evenly; the dry-based ingredient is composed of the following components in parts by weight: 88-90 parts by weight of pebbles, 3.5-4.0 parts by weight of clay, 3.8-4.2 parts by weight of coal gangue, and 3-3.5 parts by weight of iron-aluminum materials, which are mixed and stirred evenly;

[0010] Step 3: Raw material grinding:

[0011] Grind the raw material obtained in step 2 by using a raw powder grinding system, and control the raw material out of the mill to be ≤18.0% and the moisture content of the raw material to be ≤0.5%;

[0012] Step 4: Calcination of raw materials into clinker:

[0013] The raw material ground in step 3 is calcined: that is, a Yangzhou Shengxu burner is used, and the primary fan pressure is controlled at about 25000Pa, the burner internal flow opening is 25%, and the tertiary air damper clearance opening is 50cm to extend the flame length and improve the calcination fire intensity in front of the kiln.

[0014] Preferably, in the wet-based ingredients described in step 2, pebbles are 93.68 parts by weight, clay is 4.65 parts by weight, coal gangue is 4.18 parts by weight, and the iron-aluminum material is copper waste slag, which is 3.62 parts by weight; in the dry-based ingredients, pebbles are 89.00 parts by weight, clay is 3.70 parts by weight, coal gangue is 4.00 parts by weight, and the iron-aluminum material is copper waste slag, which is 3.30 parts by weight.

[0015] Preferably, during the calcination process of step 4, the control indicators are as follows: coal powder fineness: 4.0±2.0%, moisture ≤3.0%, total sulfur ≤1.0%, ash content adjacent ±2.0%; raw material entering the kiln KH: K±0.02%, SM: K±0.01%, IM: K±0.01%, decomposition rate: 94±3%; clinker out of the kiln KH: K±0.02%, SM: K±0.01%, IM: K±0.01%, f-CaO≤1.20%, liter weight: 1325±75g / l, Mgo≤4.0%, C3A≤8.0% when necessary, strength grade 3-day compressive strength ≥30.0%, 28-day compressive strength ≥54.0%, water-soluble chromium (VI) ≤9.00mg / kg.

[0016] Preferably, the mill specifications used in step 1 are as follows: the mill nozzle ring cover is 2.45m 2 , the grinding pressure is 7.5-8.0MPa, the retaining ring is 90cm, the initial value of the grinding roller skin is 10mm, and the initial value of the grinding disc lining is 10mm.

[0017] Preferably, the inner diameter of the central feed chute used in the mill in step 1 is 470 mm.

[0018] Preferably, the rotary feeder used in the mill in step 1 is a sealed feeder;

[0019] Preferably, the three-fan system configured in the raw material grinding system in step three adopts a variable frequency fan.

[0020] Preferably, the circulating fan motor of the three-fan system of the raw material grinding system in the step three is 2500KW with a rated current of 171.7A and a maximum current of 145A in normal operation; the kiln tail exhaust fan motor is 1000KW with a maximum rated current of 69.3A and a maximum current of 59A in normal operation, and the fan outlet baffle opening is normally about 55%; the kiln tail high-temperature fan motor is 1800KW with a maximum rated current of 123.4A and a maximum current of 95A in normal operation.

[0021] Preferably, the cooler used in the 2500t / d production line for calcining raw materials into clinker in step 4 is a CP cooler, and the effective area of ​​the grate bed of the grate cooler is 76.4m 2 The maximum designed output is 2800t / d, the maximum stroke of the grate bed is 220mm, and the stroke frequency is 0-9 times / minute.

[0022] Preferably, in the process of calcining raw materials into clinker in step 4, the tertiary air temperature is 900-930°C, the secondary air temperature calibration value is 1100-1150°C, and the clinker temperature out of the grate cooler is 80-100°C.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention provides a production process for making cement clinker using pebbles, which solves the problems of low yield, easy grinding and poor burnability of raw materials, and difficulty in calcining clinker when pebbles are used instead of limestone as raw materials for burning clinker. DETAILED DESCRIPTION

[0024] This specific implementation method (Example 1) adopts the following technical solution: Its operation steps are as follows:

[0025] Step 1: crushing and homogenizing the raw materials;

[0026] The pebbles, clay, coal gangue and iron materials are crushed and homogenized by a mill, and the particle size of the pebbles entering the pile is controlled to be 60cm; the specifications of the mill used are as follows: the mill nozzle ring cover is 2.45m 2 , grinding pressure is 7.5-8.0MPa, retaining ring is 90cm, initial value of grinding roller skin is 10mm, initial value of grinding disc liner is 10mm; center feed chute is 470mm; rotary feeder is sealed feeder;

[0027] Step B: Raw material ingredients:

[0028] The raw material is one of a dry-based batch or a wet-based batch, wherein the wet-based batch is composed of the following components in parts by weight: 92 parts by weight of pebbles, 5 parts by weight of clay, 4.5 parts by weight of coal gangue, and 3.8 parts by weight of iron-aluminum materials; the dry-based batch is composed of the following components in parts by weight: 88 parts by weight of pebbles, 4.0 parts by weight of clay, 4.2 parts by weight of coal gangue, and 3.5 parts by weight of iron-aluminum materials;

[0029] Step C: Raw material grinding:

[0030] Grind the raw material obtained in step 2 by using a raw powder grinding system, and control the raw material out of the mill to be ≤18.0% and the moisture content of the raw material to be ≤0.5%;

[0031] The three-fan system configured in the raw material grinding system adopts variable frequency fans;

[0032] Among them: the circulating fan motor is 2500KW with a rated current of 171.7A, and the maximum current of normal operation is 145A;

[0033] The motor of the kiln tail exhaust fan is 1000KW, with a maximum rated current of 69.3A, a maximum current of 59A in normal operation, and a normal opening of the fan outlet damper of about 55%;

[0034] The high-temperature fan motor at the kiln tail is 1800KW, with a maximum rated current of 123.4A and a maximum current of 95A in normal operation;

[0035] Step 4: Calcination of raw materials into clinker:

[0036] The raw material ground in step three is calcined: that is, Yangzhou Shengxu burner is used, and the primary fan pressure is controlled at about 25000Pa, the internal flow opening of the burner is 25%, and the clearance opening of the tertiary air damper is 50cm to extend the flame length and improve the calcination fire intensity in front of the kiln; when Yangzhou Shengxu burner is used, the average KH value of the clinker is 0.895, and the average f-CaO is 0.5%, the calcination fire is strong, and the quality of the clinker is significantly improved.

[0037] During the calcination process, the control indicators are as follows:

[0038] Coal powder fineness: 4.0±2.0%, moisture ≤3.0%, total sulfur ≤1.0%, ash content adjacent ±2.0%;

[0039] Raw materials entering the kiln KH: K±0.02%, SM: K±0.01%, IM: K±0.01%, decomposition rate: 94±3%;

[0040] Kiln clinker KH: K±0.02%, SM: K±0.01%, IM: K±0.01%, f-Ca0≤1.20%, cubic meter weight: 1325±75g / 1, Mgo≤4.0%, C3A≤8.0% when necessary, strength grade 3-day compressive strength ≥30.0%, 28-day compressive strength ≥54.0%, water-soluble chromium (VI) ≤9.00mg / kg;

[0041] The cooler used in the 2500t / d production line is a CP cooler, and the effective area of ​​the grate bed of the grate cooler is 76.4m 2 , the designed maximum output is 2800t / d, the maximum stroke of the grate bed is 220mm, and the stroke frequency is 0-9 times / minute;

[0042] The tertiary air temperature is 900-930℃, the secondary air temperature is calibrated to 1100-1150℃, and the clinker temperature out of the grate cooler is 80-100℃.

[0043] After adopting the above structure, the beneficial effects of this specific implementation are as follows:

[0044] 1. Solve the problems of low output, easy grinding and poor burnability of raw materials, and difficulty in calcining clinker when pebbles replace limestone as raw materials for clinker burning: First, coal gangue is used to replace part of clay for four-component batching, which effectively solves the problem of insufficient AL2O3 in clinker, reduces clinker SM and increases IM, and the burnability of raw materials is significantly improved. After adopting the batching components of the present invention, the clinker granulation is uniform, the fine powder is significantly reduced, the clinker granulation is dense, the physical quality of clinker cement is further improved, and the output per rotary kiln and the economic indicators of coal and electricity consumption are optimized; secondly, the hammer head of the pebble crusher is replaced and regularly After flanging and adjusting the gap between the grate screen, the particle size of the pebbles in the pile was reduced from 80cm in the early stage to 60cm, which improved the grinding efficiency of the mill, increased the mill feed rate from 230t / h to 260t / h, and reduced the process power consumption from 18kwh / t to 16.5kwh / t; with the adjustment of mill parameters, the pebble grinding capacity was increased to match the overall production line, and the length of the central discharge chute was extended to prevent the discharge distillation pipe in the mill from being blocked when the moisture content of the raw materials was high, thereby improving production efficiency; the use of sealed feeders not only reduced the frequency of mill blockage and shutdown failures, but also solved the problem of air leakage and improved the heat recovery efficiency of the mill;

[0045] (2) After the three-fan system of the raw material grinding system adopts variable frequency fans, the power consumption has dropped from the initial 70kwh / t to the current 62.5kwh / t, and the power consumption of the raw material process has dropped to 16.44kwh / t;

[0046] (3) The CP cooler in the process of raw material calcination to clinker is replaced by a step-type cooler. The tertiary air temperature is 50°C higher than that of the previous period, the secondary air temperature is 50°C higher than that of the previous period, and the clinker temperature out of the grate cooler is 50-100°C lower than that of the previous period. At the same time, the heat recovery efficiency of the grate cooler can be as high as 75.0%;

[0047] (4) After the pebbles are used, the primary fan pressure is controlled at about 25000Pa, the burner internal flow opening is 25%, and the tertiary air damper clearance opening is 50cm to extend the flame length and improve the calcination fire intensity in front of the kiln;

[0048] (5) The present invention overcomes multiple technical difficulties in various links in the innovative use of pebbles, so that pebbles can be efficiently used in the production of cement clinker, with very significant economic effects.

[0049] Embodiment 2:

[0050] The difference between this embodiment and the first embodiment is that in step 2, the wet-based ingredients are composed of the following weight parts: 93.68 weight parts of pebbles, 4.65 weight parts of clay, 4.18 weight parts of coal gangue, and 3.62 weight parts of copper waste slag as the iron-aluminum material; the dry-based ingredients are composed of the following weight parts: 89.00 weight parts of pebbles, 3.70 weight parts of clay, 4.00 weight parts of coal gangue, and 3.30 weight parts of copper waste slag as the iron-aluminum material. The remaining process steps are the same as those in the first embodiment.

[0051] Embodiment 3:

[0052] The difference between this embodiment and the first embodiment is that in step 2, the wet-base ingredients are composed of the following weight parts: 94 weight parts of pebbles, 4 weight parts of clay, 44 weight parts of coal gangue, and 3.5 weight parts of iron-aluminum materials; the dry-base ingredients are composed of the following weight parts: 90 weight parts of pebbles, 3.5 weight parts of clay, 3.8 weight parts of coal gangue, and 3 weight parts of iron-aluminum materials. The remaining process steps are the same as those in the first embodiment.

[0053] For those skilled in the art, they can modify the technical solutions described in the aforementioned embodiments and make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A production process for making cement clinker using pebbles, characterized in that: Its operation steps are as follows: Step (1), crushing and homogenizing the raw materials; The pebbles, clay, coal gangue and iron materials are crushed and homogenized by a mill, and the particle size of the pebbles entering the pile is controlled to be 60cm; the specifications of the mill used are as follows: the mill nozzle ring cover is 2.45㎡, the grinding pressure is 7.5-8.0MPa, the inner diameter of the central feed chute used by the mill is 470mm; the rotary feeder used by the mill is a sealed feeder; Step (ii): Raw material ingredients: The raw material is one of a dry-based ingredient or a wet-based ingredient, wherein the wet-based ingredient is composed of the following components in parts by weight: 92-94 parts by weight of pebbles, 4-5 parts by weight of clay, 4-4.5 parts by weight of coal gangue, and 3.5-3.8 parts by weight of iron-aluminum materials, which are mixed and stirred evenly; the dry-based ingredient is composed of the following components in parts by weight: 88-90 parts by weight of pebbles, 3.5-4.0 parts by weight of clay, 3.8-4.2 parts by weight of coal gangue, and 3-3.5 parts by weight of iron-aluminum materials, which are mixed and stirred evenly; Step (iii): Raw material grinding: The raw material obtained in step (ii) is ground by a raw powder grinding system, and the moisture content of the raw material is ≤0.5%; the three-fan system configured in the raw material grinding system adopts a variable frequency fan, and the circulating fan motor of the three-fan system configured in the raw material grinding system is 2500KW, the rated current is 171.7A, and the maximum current of normal operation is 145A; the kiln tail exhaust fan motor is 1000KW, the maximum rated current is 69.3A, the maximum current of normal operation is 59A, and the fan outlet damper opening is normally about 55%; the kiln tail high temperature fan motor is 1800KW, the maximum rated current is 123.4A, and the maximum current of normal operation is 95A; Step (IV): calcining raw materials into clinker: The raw material ground in step (iii) is calcined: that is, a burner is used, and the primary fan pressure is controlled to be about 25000Pa, the burner internal flow opening is 25%, the tertiary air damper clearance opening is 50cm to extend the flame length and increase the calcination fire intensity in front of the kiln; the tertiary air temperature is 900-930℃, the secondary air temperature is calibrated to 1100-1150℃, and the clinker temperature out of the grate cooler is 80-100℃; the control indicators are as follows: coal powder fineness: 4.0±2.0%, moisture ≤3.0%, total sulfur ≤1.0%, ash content adjacent ±2. 0%; Raw material KH: K±0.02%, SM: K±0.01%, IM: K±0.01%, Decomposition rate: 94±3%; Clinker KH: K±0.02%, SM: K±0.01%, IM: K±0.01%, f-CaO≤1.20%, Liter weight: 1325±75g / l, Mgo≤4.0%, Water-soluble chromium≤9.00mg / kg; The cooler used in the 2500t / d production line for calcining raw materials into clinker is CP cooler, and the effective area of ​​grate bed of grate cooler is 76.4m 2 The designed maximum output is 2800t / d, the maximum stroke of the grate bed is 220mm, and the stroke frequency is 0-9 times / minute.

2. The production process for making cement clinker using pebbles according to claim 1, characterized in that: In the wet-based ingredients described in step (ii), pebbles are 93.68 parts by weight, clay is 4.65 parts by weight, coal gangue is 4.18 parts by weight, and the iron-aluminum material is copper waste slag, which is 3.62 parts by weight; in the dry-based ingredients, pebbles are 89.00 parts by weight, clay is 3.70 parts by weight, coal gangue is 4.00 parts by weight, and the iron-aluminum material is copper waste slag, which is 3.30 parts by weight.