A coal-based hard carbon negative electrode material for sodium ion batteries and its preparation method and application

The ash content in coal is removed through deaze treatment and high-temperature carbonization methods, and the structure of coal-based hard carbon materials is regulated, which solves the problem of reduced sodium storage performance caused by low deterioration coal, and achieves a high energy density and safety negative electrode material of sodium ion battery.

CN113381013BActive Publication Date: 2024-11-15DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110630727.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-07
Publication Date
2024-11-15
Estimated Expiration
2041-06-07

AI Technical Summary

Technical Problem

In the prior art, coal with low deterioration degree is processed at high temperature, the inorganic minerals contained in the coal will be converted into ash residue, resulting in the sodium storage performance of the hard carbon anode material of sodium ion battery, and the ash conductivity is poor, which will catalyze the decomposition of the electrolyte. and cause self-discharge problems.

Method used

The coal-based hard carbon negative electrode material is prepared by deaze treatment and high-temperature carbonization. The ash is removed by pickling treatment, and the material structure is controlled by program cooling to form a coal-based hard carbon material with high sodium storage capacity and rapid sodium storage properties.

Benefits of technology

It effectively improves the energy density and safety of the battery, realizes the preparation of high-performance coal-based hard carbon negative electrode materials, and is suitable for industrial scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003103331870000071
    Figure BDA0003103331870000071
  • Figure BDA0003103331870000111
    Figure BDA0003103331870000111
  • Figure BDA0003103331870000112
    Figure BDA0003103331870000112
Patent Text Reader

Abstract

The present invention relates to the technical field of sodium ion batteries, and provides a method for preparing coal-based hard carbon negative electrode materials for sodium ion batteries, comprising the following steps: first, deashing the raw coal to obtain a carbon precursor; then placing the carbon precursor in an inert atmosphere for high-temperature carbonization, and obtaining a coal-based hard carbon material after programmed cooling. The present invention removes ash from coal by deashing means but retains volatile matter and heteroatoms such as N, S, and O, thereby improving the safety of the material while taking into account its conductivity. The coal-based hard carbon material prepared according to the method of the present invention is used as a negative electrode material for a sodium ion battery, and has both high sodium storage capacity and first coulomb efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a coal-based hard carbon negative electrode material for sodium ion batteries, and a preparation method and application thereof. Background Art

[0002] Sodium has the advantages of abundant reserves, wide distribution and low price, which can solve the problem of high price and limited resources of lithium-ion batteries. At the same time, the experience accumulated by lithium-ion batteries in battery processes and technologies can be used as a reference for sodium-ion batteries. Therefore, sodium-ion batteries are considered to be one of the most promising large-scale electrochemical energy storage systems.

[0003] As the key material of sodium-ion batteries, the development of high-performance and low-cost negative electrode materials is an important step in promoting the commercialization of sodium-ion batteries. At present, sodium negative electrode materials are divided into alloys (phosphorus, silicon, tin, lead, etc.), conversions (metal oxides, metal sulfides, etc.) and embeddings (titanium-based oxides and carbon materials) according to different energy storage mechanisms. However, alloy and conversion materials have volume expansion problems, resulting in continuous capacity decay during the charge and discharge cycle; titanium-based materials have poor conductivity, and the electrochemical rate performance of the materials needs to be improved. These inherent limitations caused by the properties of the materials themselves make them difficult to commercialize. Carbon materials have become one of the most practical negative electrode materials for sodium ions due to their abundant sources, low prices, low potential, strong conductivity, and strong structural stability. Because the ionic radius of sodium ions is larger than that of lithium ions, the sodium storage capacity of lithium-ion graphite negative electrodes and highly ordered graphite-based soft carbon negative electrodes is low. Hard carbon materials have abundant defects and heteroatoms, graphite crystallites with large interlayer spacing, and a large number of pores, which are active sites for sodium storage and are suitable as negative electrode materials for sodium ion batteries.

[0004] Hard carbon is mainly produced by high-temperature carbonization of biomass, high-molecular polymers, coal and other raw materials. Among them, coal is a high-quality raw material for preparing carbon materials due to its high carbon content, developed aromatic structure, low price and abundant resources. Moreover, there are many types of coal, which can be divided into anthracite, bituminous coal (sub-bituminous coal), lignite and peat according to the degree of metamorphism. Anthracite has a carbon content of more than 90%, and the carbon material obtained by carbonization is soft carbon with a small graphite interlayer spacing and a low heteroatom content. Coal with a low degree of metamorphism can be formed into a coal-based hard carbon material with a larger graphite interlayer spacing, richer heteroatom content and defect structure after high-temperature carbonization, which is more suitable as a negative electrode material for sodium ion batteries. Summary of the invention

[0005] The problem solved by the present invention is that in the prior art, when low-grade coal is treated at high temperature, the inorganic minerals contained in it will be converted into ash residue, and the ash generally has poor conductivity and no electrochemical activity, resulting in reduced sodium storage performance of the material. Ash components such as Fe2O3 and Cr2O3 will dissolve from the hard carbon negative electrode in the sodium ion battery, which not only catalyzes the decomposition of the electrolyte and reduces the coulomb efficiency, but also easily causes problems such as self-discharge effect.

[0006] Specifically, the present invention proposes the following technical solutions:

[0007] In the first aspect, the embodiment of the present invention provides a coal-based hard carbon negative electrode material for a sodium ion battery, wherein the coal-based hard carbon material for a sodium ion battery is granular, and the interplanar spacing d 002 The value is 0.2nm or more, and the preferred interplanar spacing d 002 The value is 0.2-0.5nm, and the more preferred interplanar spacing d 002 The value is 0.364-0.384nm.

[0008] Preferably, the coal-based hard carbon material A for sodium ion battery G / A D The value is 0.1-0.6, and the more preferred A G / A D The value is 0.21-0.49.

[0009] Preferably, the sodium ion battery coal-based hard carbon material L c The value is 1-4nm, and the more preferred L c The value is 2.11-2.60nm; L a The value is 0.5-2.5nm, and the more preferred L a The value is 1.75-2.18nm.

[0010] Preferably, the average particle size of the coal-based hard carbon negative electrode material for sodium ion batteries is 28-470 μm.

[0011] Preferably, the coal-based hard carbon negative electrode material for the sodium ion battery is obtained by deashing, carbonizing and programmed cooling the raw coal, wherein the raw coal is one or more of bituminous coal, sub-bituminous coal and lignite, and preferably the coal is lignite.

[0012] Preferably, the programmed cooling treatment refers to a temperature of 1-5°C min -1 The temperature was lowered to 15-30°C at a rate of 1.

[0013] Preferably, the deliming treatment refers to a two-step deliming treatment using an acid, and preferably the two-step deliming treatment refers to a treatment using hydrochloric acid, nitric acid or sulfuric acid, wherein the acids used in the two-step deliming treatment may be the same or different.

[0014] In a second aspect, the present invention provides a method for preparing a coal-based hard carbon negative electrode material for a sodium ion battery, comprising the following steps:

[0015] Step 1: The raw coal is crushed, sieved, placed in a deashing solution for treatment, washed with water until neutral, and dried to obtain a precursor.

[0016] Step 2: The precursor obtained in step 1 is subjected to high-temperature carbonization under the protection of an inert gas, and then programmed to cool to 15-30° C. to obtain a coal-based hard carbon negative electrode material for a sodium ion battery.

[0017] Preferably, the raw coal is one or more of bituminous coal, sub-bituminous coal and lignite, and more preferably the raw coal is lignite.

[0018] Preferably, in the preparation method of the coal-based hard carbon negative electrode material for sodium ion batteries, in step 1, the treatment in the deashing solution refers to a two-step deashing treatment using an acid; preferably, the two-step deashing treatment is performed using hydrochloric acid, hydrofluoric acid, nitric acid or sulfuric acid, wherein the acids used in the two-step deashing treatment may be the same or different.

[0019] Preferably, in the method for preparing the coal-based hard carbon negative electrode material for a sodium ion battery, in step 1, the amount of the deashing solution is: 10-30 mL of acid is used for deashing per gram of coal.

[0020] Preferably, in the method for preparing the coal-based hard carbon negative electrode material for a sodium ion battery, in step 2, the high-temperature carbonization temperature is 1000-1600°C, and a more preferred high-temperature carbonization temperature is 1350-1420°C.

[0021] Preferably, in the method for preparing the coal-based hard carbon negative electrode material for a sodium ion battery, in step 2, the inert gas used for carbonization is at least one of argon and argon.

[0022] Preferably, in the method for preparing the coal-based hard carbon negative electrode material for sodium ion battery, in step 2, the inert gas flow rate used for carbonization is 30-600cc min -1 .

[0023] Preferably, in the method for preparing the coal-based hard carbon negative electrode material for sodium ion battery, in step 2, the temperature is 1-5°C min -1 The temperature is raised to 1000-1600°C at a rate of 1-4 hours, preferably at a rate of 1-5°C min -1 The temperature was raised to 1350-1420°C at a rate of 1.5°C and kept there for 2 h.

[0024] Preferably, in the method for preparing the coal-based hard carbon negative electrode material for sodium ion battery, in step 2, the cooling process adopts programmed cooling at 1-5°C min -1Reduce to 15-30℃.

[0025] In a third aspect, the present invention provides an electrode sheet comprising the coal-based hard carbon negative electrode material described in the second aspect, characterized in that it also includes a conductive agent, a binder and a current collector.

[0026] Preferably, the binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133.

[0027] Preferably, the conductive agent on the negative electrode plate includes one or more of carbon nanotubes, carbon fibers, graphene, acetylene black, and SuperP.

[0028] In a fourth aspect, the present invention provides a sodium ion battery comprising the coal-based hard carbon negative electrode sheet described in the third aspect above.

[0029] The beneficial effects of the present invention include:

[0030] (1) The deashing technology of the present invention can effectively remove ash from coal, which is beneficial to improving the energy density and safety of the battery.

[0031] (2) The carbonization procedure of the present invention can effectively regulate the disorder, defect structure and heteroatom content of coal-based hard carbon, which is conducive to the preparation of high-performance coal-based hard carbon negative electrode materials.

[0032] (3) The preparation method of the coal-based hard carbon negative electrode material for sodium ion batteries of the present invention is simple, the raw materials are easily available, the carbon yield is high and the cost is low, and it is suitable for industrial-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is the XRD spectra of YM-1000, YM-1200, YM-1400 and YM-1600 in Preparation Example 4;

[0034] Figure 2 is the Raman spectra of YM-1000, YM-1200, YM-1400 and YM-1600 in Preparation Example 4;

[0035] Figure 3 is the XRD spectra of CYM-1000, CYM-1200, CYM-1400 and CYM-1600 in Preparation Example 5;

[0036] Figure 4 is the Raman spectra of CYM-1000, CYM-1200, CYM-1400 and CYM-1600 in Preparation Example 5;

[0037] Figure 5is the XRD spectra of HM-1000, HM-1200, HM-1400 and HM-1600 in Preparation Example 6;

[0038] Figure 6 is the Raman spectra of HM-1000, HM-1200, HM-1400 and HM-1600 in Preparation Example 6;

[0039] Figure 7 It is the first charge and discharge curve diagram of EP-YM-1000, EP-YM-1200, EP-YM-1400 and EP-YM-1600 in Application Example 1;

[0040] Figure 8 It is a comparison diagram of the first charge and discharge curves of EP-YM-0-1400 in comparative example 1 and EP-YM-1400 in example 1;

[0041] Fig. 9 is a rate performance diagram of EP-YM-1000, EP-YM-1200, EP-YM-1400 and EP-YM-1600 in Application Example 1;

[0042] Fig.10 It is the first charge and discharge curve diagram of EP-CYM-1000, EP-CYM-1200, EP-CYM-1400 and EP-CYM-1600 in Application Example 2;

[0043] Fig.11 It is a comparison diagram of the first charge and discharge curves of EP-CYM-0-1400 in comparative example 2 and EP-CYM-1400 in example 2;

[0044] Fig.12 is a rate performance diagram of EP-CYM-1000, EP-CYM-1200, EP-CYM-1400 and EP-CYM-1600 in Application Example 2;

[0045] Fig.13 is the first charge and discharge curve diagram of EP-HM-1000, EP-HM-1200, EP-HM-1400 and EP-HM-1600 in Application Example 3;

[0046] Fig.14 It is a comparison chart of the first charge and discharge curves of EP-HM-0-1400 in comparative example 3 and EP-HM-1400 in example 3;

[0047] Fig.15 This is a rate performance diagram of EP-HM-1000, EP-HM-1200, EP-HM-1400 and EP-HM-1600 in Application Example 3. DETAILED DESCRIPTION

[0048] The present invention relates to the technical field of sodium ion batteries, and provides a method for preparing coal-based hard carbon negative electrode materials for sodium ion batteries, comprising the following steps: first, deashing the raw coal to obtain a carbon precursor; then placing the carbon precursor in an inert atmosphere for high-temperature carbonization, and obtaining a coal-based hard carbon material after programmed cooling. The present invention removes ash from coal by deashing means but retains volatile matter and heteroatoms such as N, S, and O, thereby improving the safety of the material while taking into account its conductivity. The coal-based hard carbon material prepared according to the method of the present invention is used as a negative electrode material for a sodium ion battery, and has both high sodium storage capacity and first coulomb efficiency.

[0049] In the prior art, when coal is used to prepare hard carbon negative electrode materials for sodium ion batteries, low-grade coal will result in residual ash (converted from inorganic minerals in the coal) during high-temperature treatment, which reduces the sodium storage performance of the battery material. In response to this technical problem, the present invention provides a sodium ion battery coal-based hard carbon negative electrode material and its preparation method and application. The present invention adopts deashing and high-temperature carbonization methods to prepare coal-based hard carbon negative electrode materials. After acid washing, the ash in the coal can be effectively removed, which is beneficial to improve the energy density and safety of the battery. High-temperature carbonization can adjust the disorder and heteroatom types of the material, and the coal-based hard carbon can exhibit high reversible specific capacity and rapid sodium storage performance. The material has abundant raw material reserves, low cost and high carbon yield, and is suitable for large-scale production.

[0050] In order to solve the above-mentioned problems of the prior art, in a specific embodiment, the present invention provides a sodium ion battery negative electrode material, characterized in that the material is a coal-based hard carbon material, which is prepared by using coal as raw material, using a deashing solution for deashing, drying, and then high-temperature carbonization under an inert atmosphere.

[0051] The coal includes one or a mixture of bituminous coal, sub-bituminous coal and lignite.

[0052] Wherein, the deashing solution includes one or a mixture of any of hydrochloric acid, hydrofluoric acid, nitric acid and sulfuric acid.

[0053] In another specific embodiment, the present invention also provides a method for preparing a coal-based hard carbon negative electrode for a sodium ion battery, characterized in that the method comprises the following steps:

[0054] (1) First, grind the coal in a mortar and then pass it through a 50-300 mesh sieve.

[0055] (2) The coal obtained in the previous step is treated with acid in two steps for 6-12 hours, wherein the total amount of acid used is in a mass ratio of 10-30 mL g to coal. -1The sample was then vacuum filtered and washed with water until neutral, and then placed in a 50°C forced air oven to dry for 24 hours.

[0056] (3) The sample obtained in the previous step was placed in a graphite boat and placed in a tube furnace. Argon was introduced as an inert gas with a carrier gas flow rate of 60 cc min -1 Then at 3℃min -1 The temperature was raised to 1000-1600°C and kept for 2 hours. The temperature was lowered to 15-30°C by program, and then the material was taken out from the tube furnace to obtain the coal-based hard carbon negative electrode material for sodium ion batteries. The program cooling process makes the stress change caused by temperature change on the material smooth, making the material shrinkage process uniform.

[0057] The present invention provides a coal-based hard carbon negative electrode sheet, wherein the negative electrode sheet comprises the above-mentioned coal-based hard carbon material, a conductive agent, a binder and a current collector.

[0058] The coal-based hard carbon material on the negative electrode plate includes one or more of bituminous coal-based hard carbon, sub-bituminous coal-based hard carbon and lignite-based hard carbon.

[0059] The binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133, but is not limited thereto.

[0060] The conductive agent on the negative electrode plate includes one or more of carbon nanotubes, carbon fibers, graphene, acetylene black, and Super P, but is not limited thereto.

[0061] In addition, the present invention provides a sodium ion battery comprising the above-mentioned coal-based hard carbon negative electrode plate.

[0062] In the following examples and comparative examples, unless otherwise stated, the raw materials used are shown in Table 1 below:

[0063] Table 1 Information of raw materials used in the present invention

[0064]

[0065] In order to better understand the technical solution of the present invention, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0066] I. Preparation Examples

[0067] Preparation Example 1

[0068] First, pour the bituminous coal into a mortar and grind it. After passing it through a 100-mesh sieve, weigh 3 g and pour it into a conical flask. Add 15 mL of 4 mol L -1After continuous stirring in hydrochloric acid for 6 hours, vacuum filtration and water washing until neutral, the sample was placed in a 50°C forced air oven to dry for 24 hours. The dried bituminous coal was then poured into a plastic bottle, 15 mL of 10 wt% hydrofluoric acid was added and stirred for 6 hours, vacuum filtration and water washing until neutral, and placed in a 50°C forced air oven to dry for 24 hours. The obtained sample was named YM-1.

[0069] Preparation Example 2

[0070] First, sub-bituminous coal was poured into a mortar for pulverization and passed through a 100-mesh sieve. 3 g was weighed and poured into a conical flask. 15 mL of 4 mol L -1 After continuous stirring in hydrochloric acid for 6 hours, vacuum filtration and water washing until neutral, the sample was placed in a 50°C forced air oven to dry for 24 hours. The dried subbituminous coal was then poured into a plastic bottle, 15 mL of 10 wt% hydrofluoric acid was added and stirred for 6 hours, vacuum filtration and water washing until neutral, and placed in a 50°C forced air oven to dry for 24 hours. The obtained sample was named CYM-1.

[0071] Preparation Example 3

[0072] First, pour the lignite into a mortar and grind it, then pass it through a 100-mesh sieve, weigh 3 g and pour it into a conical flask, add 15 mL of 4 mol L -1 After continuous stirring in hydrochloric acid for 6 hours, vacuum filtration and water washing until neutral, the sample was placed in a 50°C forced air oven to dry for 24 hours. The dried lignite was then poured into a plastic bottle, 15 mL of 10 wt% hydrofluoric acid was added and stirred for 6 hours, vacuum filtration and water washing until neutral, and placed in a 50°C forced air oven to dry for 24 hours. The obtained sample was named HM-1.

[0073] Preparation Example 4

[0074] Weigh 4 g of YM-1 prepared in Example 1 and load them into four graphite boats respectively. Place them in a tube furnace and introduce argon gas at a carrier gas flow rate of 60 cc min. -1 Then at 3℃min -1 The temperature was raised to 1000℃, 1200℃, 1400℃ and 1600℃ respectively, and then kept at 2℃ min -1 The temperature was lowered to room temperature to obtain the bituminous coal-based hard carbon negative electrode material for sodium ion batteries. The obtained samples were named YM-1000, YM-1200, YM-1400 and YM-1600.

[0075] The samples obtained above were characterized by XRD, Raman spectroscopy and XPS. The test results are as follows: Figure 1 , Figure 2 , as shown in Table 2 and Table 3.

[0076] Among them, the XRD test instrument model and test conditions used are as follows:

[0077] The XRD data in this paper were measured on an X'Pert3 Powder X-ray diffractometer produced by PANalytical BV. The test voltage was 40KV, the anode material was Cu target, the excitation was Kα, and the scanning speed (step size 0.02626°, rate 0.1694°s -1 ); scanning range 2θ = 10°~90°.

[0078] Raman spectroscopy test instrument model and conditions are as follows:

[0079] The instrument used for the Raman test in this paper is the DRX micro-Raman spectrometer from Thermo Fisher Scientific, and the visible laser emission wavelength is 532nm.

[0080] XPS test instrument model and conditions are as follows:

[0081] In this paper, the ESCALAB 250 multifunctional surface analyzer of Thermofisher VG Scientific was used to analyze the series of samples. The excitation source was monochromatized Al Kα=1486.6eV, and the energy was 1486.6eV. The binding energy of the samples was corrected by the C1s central peak (284.6eV).

[0082] as follows Figure 1 As shown in Table 2 below, the graphite crystallite interlayer spacing d of the above-mentioned embodiment samples of the present invention is 002 The value is in the range of 0.364-0.381nm, L c The value is 2.13-2.60nm, L a The values ​​are 1.75-2.13nm; among them, the graphite microcrystalline interlayer spacing of YM-1000, YM-1200, YM-1400 and YM-1600 are 0.381, 0.374, 0.370 and 0.364nm respectively. As the carbonization temperature increases, the graphite microcrystalline interlayer spacing gradually decreases. In addition, L a With L c The value gradually increases and the size of graphite crystallite gradually increases.

[0083] as follows Figure 2 As shown in Table 2 below, the A of the samples in the above embodiments of the present invention is G / A D The values ​​are 0.27-0.49. Among them, with the increase of carbonization temperature, the A of YM-1000, YM-1200, YM-1400 and YM-1600 G / A DThey are 0.27, 0.29, 0.44 and 0.49 respectively, showing a gradually increasing trend, and the defect degree of the material gradually decreases.

[0084] Preparation Example 5

[0085] Weigh 4 g of CYM-1 prepared in Example 2 and load them into four graphite boats respectively. Place them in a tube furnace and introduce argon gas. The carrier gas flow rate is 60 cc min. -1 Then at 3℃min -1 The temperature was raised to 1000℃, 1200℃, 1400℃ and 1600℃ respectively, and then kept at 2℃min -1 The temperature was lowered to room temperature to obtain a subbituminous coal-based hard carbon negative electrode material for sodium ion batteries. The obtained samples were named CYM-1000, CYM-1200, CYM-1400 and CYM-1600.

[0086] The samples obtained above were subjected to XRD test, Raman spectrum and XPS test, and the test results are as follows: Figure 3 , Figure 4 , as shown in Table 2 and Table 3. The detection instrument and conditions are the same as those in Preparation Example 4.

[0087] as follows Figure 3 As shown in Table 2 below, the graphite crystallite interlayer spacing d of the above-mentioned embodiment samples of the present invention is 002 The value is in the range of 0.364-0.384nm, L c The value is 2.13-2.56nm, L a The values ​​are 1.77-2.18nm; among them, the graphite microcrystalline interlayer spacing of CYM-1000, CYM-1200, CYM-1400 and CYM-1600 are 0.380, 0.377, 0.372 and 0.365nm respectively. As the carbonization temperature increases, the graphite interlayer spacing gradually decreases. In addition, L a With L c The value gradually increases and the size of graphite crystallite gradually increases.

[0088] as follows Figure 4 As shown in Table 2 below, the A of the samples in the above embodiments of the present invention is G / A D The values ​​were 0.26-0.44. Among them, with the increase of carbonization temperature, the A of CYM-1000, CYM-1200, CYM-1400 and CYM-1600 G / A D They are 0.26, 0.30, 0.38 and 0.44 respectively, showing a trend of gradual increase, and the defect degree of the material gradually decreases.

[0089] Preparation Example 6

[0090] Weigh 4 g of HM-1 prepared in Example 3 and load them into four graphite boats respectively. Place them in a tube furnace and introduce argon gas at a carrier gas flow rate of 60 cc min. -1 Then at 3℃min -1 The temperature was raised to 1000℃, 1200℃, 1400℃ and 1600℃ respectively, and then kept at 2℃min -1 The temperature was lowered to room temperature to obtain lignite-based hard carbon anode materials for sodium ion batteries. The obtained samples were named HM-1000, HM-1200, HM-1400 and HM-1600.

[0091] The samples obtained above were subjected to XRD test, Raman spectrum and XPS test, and the test results were Figure 5 , Figure 6 , as shown in Table 2 and Table 3. The detection instrument and conditions are the same as those in Preparation Example 4.

[0092] like Figure 5 As shown in Table 2, the graphite crystallite interlayer spacing d of the above-mentioned embodiment samples of the present invention is 002 The value is in the range of 0.368-0.384nm, L c The value is 2.11-2.46nm, L a The value is 1.80-2.07nm; among them, the graphite microcrystalline interlayer spacing of HM-1000, HM-1200, HM-1400 and HM-1600 are 0.384, 0.381, 0.376 and 0.368nm respectively. As the carbonization temperature increases, the graphite microcrystalline interlayer spacing gradually decreases. In addition, L a With L c The value gradually increases, and the graphite crystallite size gradually increases. In particular, at the same carbonization temperature, the graphite crystallite interlayer spacing of lignite-based hard carbon is always larger than that of bituminous-based hard carbon and sub-bituminous-based hard carbon.

[0093] like Figure 6 As shown in Table 2, the A of the samples in the above embodiments of the present invention is G / A D The value is 0.21-0.40. Among them, with the increase of carbonization temperature, the A of HM-1000, HM-1200, HM-1400 and HM-1600 G / A D They are 0.21, 0.24, 0.28 and 0.40 respectively, showing a trend of gradual increase, and the defect degree of the material gradually decreases. At the same carbonization temperature, compared with the bituminous coal group and the sub-bituminous coal group, the lignite group has the lowest degree of graphitization and has a richer defect structure. This is also related to the low degree of metamorphism of lignite, which contains rich heteroatoms and inhibits the orderly arrangement of graphite crystallites during carbonization.

[0094] Table 2 Structural parameters of YM-1000, YM-1200, YM-1400, YM-1600, CYM-1000, CYM-1200, CYM-1400, CYM-1600, HM-1000, HM-1200, HM-1400 and HM-1600

[0095]

[0096] Table 3 Elemental analysis and XPS analysis results of YM-1000, YM-1200, YM-1400, YM-1600, HM-1000, HM-1200, HM-1400 and HM-1600

[0097]

[0098]

[0099] Preparation Comparative Example 1

[0100] The anthracite was poured into a mortar for pulverization and passed through a 100-mesh sieve. The obtained sample was named WYM-0.

[0101] Preparation Comparative Example 2

[0102] First, pour the anthracite into a mortar and grind it. After passing it through a 100-mesh sieve, weigh 3 g and pour it into a conical flask. Add 15 mL of 4 mol L -1 Stir continuously in hydrochloric acid for 6 hours, vacuum filter and wash with water until neutral, and then place the sample in a 50℃ forced air oven to dry for 24 hours. Pour the dried anthracite into a plastic bottle, add 15mL 10wt% hydrofluoric acid and stir continuously for 6 hours, vacuum filter and wash with water until neutral, and place in a 50℃ forced air oven to dry for 24 hours. The obtained sample is named WYM-1.

[0103] Preparation Comparative Example 3

[0104] The bituminous coal was poured into a mortar for pulverization and passed through a 100-mesh sieve. The obtained sample was named YM-0.

[0105] Preparation Comparative Example 4

[0106] 1 g of YM-0 prepared in Comparative Example 3 was weighed and loaded into four graphite boats respectively and placed in a tube furnace. Argon gas was introduced and the carrier gas flow rate was selected to be 60 cc min -1 Then at 3℃min -1 Raise the temperature to 1400℃, hold for 2h, then heat at 2℃min -1 The temperature was lowered to room temperature to obtain a bituminous coal-based hard carbon negative electrode material for a sodium ion battery, and the obtained material was named YM-0-1400.

[0107] Preparation Comparative Example 5

[0108] The subbituminous coal was poured into a mortar for pulverization and passed through a 100-mesh sieve. The resulting sample was named CYM-0.

[0109] Preparation Comparative Example 6

[0110] 1 g of CYM-0 prepared in Comparative Example 5 was weighed and loaded into four graphite boats respectively and placed in a tube furnace. Argon gas was introduced and the carrier gas flow rate was selected to be 60 cc min -1 Then at 3℃min -1 Raise the temperature to 1400℃, hold for 2h, then heat at 2℃min -1 The temperature was lowered to room temperature to obtain a subbituminous coal-based hard carbon negative electrode material for a sodium ion battery, and the obtained material was named CYM-0-1400.

[0111] Preparation Comparative Example 7

[0112] The lignite was poured into a mortar and pulverized, and passed through a 100-mesh sieve. The obtained sample was named HM-0.

[0113] Preparation Comparative Example 8

[0114] 1 g of HM-0 prepared in Comparative Example 7 was weighed and loaded into four graphite boats respectively and placed in a tube furnace. Argon gas was introduced and the carrier gas flow rate was selected to be 60 cc min -1 Then at 3℃min -1 Raise the temperature to 1400℃, hold for 2h, then heat at 2℃min -1 The temperature was lowered to room temperature to obtain a sodium ion battery lignite-based hard carbon negative electrode material, and the obtained material was named HM-0-1400.

[0115] The samples obtained in the above-mentioned preparation examples 1, 2 and 3 and the preparation comparative examples 1, 2, 3, 5 and 7 were subjected to industrial analysis of the coal samples before and after deashing according to the industrial analysis method of coal in the national standard GBT2122008, and the mineral composition of the above-mentioned products was analyzed by X-ray fluorescence spectrometer (XRF, S8 TIGER, Bruker), and the results are shown in Tables 4 and 5. It can be clearly seen that after the hydrochloric acid and hydrofluoric acid pickling treatment, the ash content of the deashed samples WYM-1, YM-1, CYM-1 and HM-1 was reduced by more than 90% compared with the samples WYM-0, YM-0, CYM-0 and HM-0 that were not deashed, indicating that the treatment method can effectively remove ash. Among them, the structures of HM-0 and CYM-0 are relatively loose, which can make the contact between acid and ash more sufficient, so the deashing efficiency of HM-1 and CYM-1 is relatively high.

[0116] The elements contained in the prepared materials were quantitatively analyzed using an element analyzer (Vario EL) from the German Element Company. The elemental analysis results of the samples obtained by the preparation examples 1, 2, 3 and the preparation comparative example 2 described above are shown in Table 4 below. It can be seen from Table 4 that WYM-1, YM-1, CYM-1 and HM-1 are all mainly carbon elements, and contain small amounts of oxygen, hydrogen, nitrogen and sulfur elements. From anthracite to bituminous coal, sub-bituminous coal and lignite, as the degree of coal metamorphism increases successively, the carbon content of the prepared coal-based hard carbon materials gradually increases, and the oxygen content gradually decreases. Among them, HM-1 has the lowest carbon content and the highest oxygen content, which is mainly attributed to the smaller molecular structure of the aromatic ring of lignite and the larger number of unstable aromatic side chains and oxygen-containing functional groups.

[0117] Table 4 Industrial analysis of coal before and after deashing and elemental analysis results after deashing

[0118]

[0119] Table 5 X-ray fluorescence spectroscopic analysis results of coal before and after deashing

[0120]

[0121] II. Application Examples

[0122] Application Example 1

[0123] YM-1000, YM-1200, YM-1400 and YM-1600 in Preparation Example 4 were used as active materials to prepare sodium ion battery negative electrodes, and their electrochemical charge and discharge performances were tested.

[0124] The specific battery preparation process is as follows: the above-mentioned active material, carbon nanotubes and sodium carboxymethyl cellulose binder are mixed in a mass ratio of 8:1:1 to prepare a slurry. First, the sodium carboxymethyl cellulose binder is weighed into a glass bottle, and then the active material and the carbon nanotubes are mixed and ground and added to the glass bottle, and mechanically stirred for 12 hours to prepare a uniform slurry. The obtained slurry is applied to the copper foil current collector using a coater and then transferred to a blast drying oven for drying at 50°C for 2 hours, and then transferred to a vacuum drying oven for drying at 100°C for 12 hours. The dried electrode piece is cut into a disc with a diameter of 12 mm and named YM-1 electrode. The electrode piece is then transferred to a glove box and assembled into a battery. The assembly of the sodium ion half-cell is carried out in a glove box with an argon atmosphere. A glass fiber membrane (Whatman F) is used as a diaphragm, 1M NaPF6 is dissolved in 1L of ethylene carbonate and diethyl carbonate solution with a volume ratio of 1:1 as an electrolyte, and metallic sodium is used as a counter electrode to assemble a CR2032 button cell. The obtained batteries were named EP-YM-1000, EP-YM-1200, EP-YM-1400 and EP-YM-1600, respectively.

[0125] For the battery prepared in the above-mentioned application example 1, at 0.02A g -1 The first constant current charge and discharge test was carried out at a current density of Figure 7 As shown; at 0.02, 0.05, 0.1, 0.2, 0.5A g -1 The rate performance test was carried out at a current density of , and the charge and discharge voltage window was 0.01-3.00V. The test results are as follows Fig. 9 As shown. Figure 7 It can be seen that at 0.02A g -1 At a current density of 1.34 W, EP-YM-1400 exhibited better electrochemical performance than EP-YM-1000, EP-YM-1200 and EP-YM-1600. The first charge specific capacity of EP-YM-1400 was 317.5 mA h g -1 , the first coulombic efficiency is 80%. Fig. 9 It can be seen that at 1A g -1 At a high current density, the reversible specific capacity of the optimal sample EP-YM-1400 is 57.1 mA h g -1 .

[0126] Application Example 2

[0127] The CYM-1000, CYM-1200, CYM-1400 and CYM-1600 in Preparation Example 5 were used as active materials to prepare the negative electrode of the sodium ion battery, and the electrochemical charge and discharge performance was tested. The obtained batteries were named EP-CYM-1000, EP-CYM-1200, EP-CYM-1400 and EP-CYM-1600, respectively. The preparation process and test method are the same as those in Application Example 1.

[0128] The battery prepared in the above-mentioned application example 2 has the following first constant current charge and discharge test results: Fig.10 As shown; at 0.02, 0.05, 0.1, 0.2, 0.5A g -1 The battery rate performance was tested at a current density of , and the charge and discharge voltage window was 0.01-3.00V. The test results are as follows Fig.12 As shown. Fig.12 It can be seen that compared with EP-CYM-1000, EP-CYM-1200 and EP-CYM-1600, EP-CYM-1400 exhibits better rate performance. Fig.10 It can be seen that at 0.02A g -1 At the current density of 2.5 and 1.3 volts, the first charge specific capacity of EP-CYM-1400 was 326.1 mA h g -1 , the first coulombic efficiency is 79.8%. Fig.12 It can be seen that at 1A g -1 At a high current density, the reversible specific capacity of the optimal sample EP-CYM-1400 is 70.6 mA h g -1 .

[0129] Application Example 3

[0130] HM-1000, HM-1200, HM-1400 and HM-1600 in Preparation Example 6 were used as active materials to prepare sodium ion battery negative electrodes, and electrochemical charge and discharge performance tests were performed on them. The obtained batteries were named EP-HM-1000, EP-HM-1200, EP-HM-1400 and EP-HM-1600, respectively. The preparation process and test method were the same as those in Application Example 1.

[0131] The first constant current charge and discharge test results of the battery prepared in the above-mentioned application example 3 are as follows: Fig.13 As shown. Fig.13 It can be seen that at 0.02A g -1At a current density of 1.34 W, EP-HM-1400 exhibited better electrochemical performance than EP-HM-1000, EP-HM-1200 and EP-HM-1600. The first charge specific capacity of EP-HM-1400 was 338.8 mA h g -1 The first coulombic efficiency is 81.1%. The battery prepared in the above application example 3 has a coulombic efficiency of 81.1% at 0.02, 0.05, 0.1, 0.2, and 0.5A g -1 The rate performance was tested at a current density of 1.5 V, and the charge and discharge voltage window was 0.01-3.00 V. The test results are as follows Fig.15 As shown. Fig.15 It can be seen that at 1A g -1 At a high current density, the reversible specific capacity of the optimal sample EP-HM-1400 is 76.0 mA h g -1 .

[0132] The initial charge and discharge conditions of the batteries prepared in the above application examples 1, 2, and 3 are as follows: Figure 7 , 10 , 13. In the following Figure 7 , 10 As can be seen from Figures 1 and 13, compared with the EP-YM-1400 in the above-mentioned Application Example 1 and the EP-CYM-1400 in the above-mentioned Application Example 2, the EP-HM-1400 in Application Example 3 exhibits higher reversible specific capacity and first coulombic efficiency.

[0133] from Figure 7 , 10 As can be seen from 13, the ramp capacity of EP-YM-1400, EP-CYM-1400 and EP-HM-1400 is 138.0mA hg -1 Increased to 158.3 mA hg -1 Therefore, EP-HM-1400 has a higher ramp capacity, which allows it to achieve higher capacity. This is mainly due to the gradual decrease in the metamorphic degree of bituminous coal to sub-bituminous coal to lignite. G / A D The value decreases from 0.44 of YM-1400 to 0.28 of HM-1400, the degree of graphitization decreases, and the defects of the material gradually increase, providing more abundant adsorption active sites.

[0134] In addition, the rate performance of the batteries prepared in the above application examples 1, 2, and 3 is as follows: Fig. 9 , 12 , 15. From Fig. 9 , 1215, it can be seen that compared with EP-YM-1400 prepared in Example 1 and EP-CYM-1400 prepared in Example 2, EP-HM-1400 prepared in Example 3 exhibits better rate performance. This is mainly because lignite has a small degree of metamorphism, the lowest degree of graphitization, and more abundant defective active sites, showing rapid adsorption and sodium storage behavior. Therefore, EP-HM-1400 has a larger sodium storage capacity at high current density.

[0135] The elemental analysis and XPS analysis results of the materials prepared in the above-mentioned preparation examples 4, 5, and 6 are shown in Table 3. It can be seen that HM-1400 has a higher proportion of sp 3 Carbon, indicating that lignite produces more defect structures and a lower degree of graphitization, which is consistent with the results of Raman spectroscopy tests. In addition, the oxygen-containing functional groups of HM-1400 and YM-1400 are mainly -OH and C=O, which provide abundant active sites for the sodium storage of the material. Further exploration of the elemental analysis of samples YM-1400 and HM-1400 showed that the carbon content of HM-1400 is less than that of YM-1400, and it contains more heteroatom defect structures, which is conducive to rapid adsorption and sodium storage. In addition, the oxygen contents of HM-1400 and YM-1400 are 1.86wt% and 1.54wt%, respectively, indicating that HM-1400 has a higher oxygen content.

[0136] In addition, the first charge and discharge conditions of the batteries prepared in the above application examples 1, 2, and 3 are as follows: Figure 7 , 10 、13. Figure 7 , 10 As can be seen from Figure 13, the main reason why EP-HM-1400 has a higher capacity than EP-YM-1400 and EP-CYM-1400 is that the high potential slope is more gentle between 0.5 and 1.0 V. This part of the capacity is related to the oxygen-containing functional groups and Na + This is related to the redox reaction of EP-HM-1400, which is consistent with the richer oxygen content in EP-HM-1400. Therefore, EP-HM-1400 can undergo a rapid sodium adsorption storage reaction and still retain a high specific capacity under high current.

[0137] Application Comparative Example 1

[0138] The YM-0-1400 in the comparative example 4 was used as an active material to prepare a negative electrode of a sodium ion battery, and its electrochemical charge and discharge performance was further tested, and the obtained battery was named EP-YM-0-1400. The preparation process was the same as that in the application example 1.

[0139] The EP-YM-1400 prepared in Example 1 and the EP-YM-0-1400 prepared in Comparative Example 1 were tested at 0.02 A g -1 The constant current charge and discharge curve under current density is as follows Figure 8 As shown in the figure, it can be seen that the deashing treatment can significantly improve the electrochemical performance of bituminous coal-based hard carbon materials. Compared with EP-YM-0-1400 in comparative example 1, the first coulombic efficiency of EP-YM-1400 in example 1 is increased from 76.5% to 80.0%, and the specific capacity is increased from 274.5 mA hg -1 Increased to 317.5mA hg -1 .

[0140] Application Comparative Example 2

[0141] The CYM-0-1400 in Comparative Example 6 was used as an active material to prepare a negative electrode for a sodium ion battery, and the electrochemical charge and discharge performance was tested. The resulting battery was named EP-CYM-0-1400. The preparation process was the same as that in Application Example 1.

[0142] The EP-CYM-1400 prepared in Example 2 and the EP-CYM-0-1400 prepared in Comparative Example 2 were tested at 0.02 A g -1 The charge and discharge curve under current density is constant current, and the results are as follows Fig.11 As shown in the figure, compared with EP-CYM-0-1400 in comparative example 2, the electrochemical performance of EP-CYM-1400 in the application example is significantly improved, the first coulombic efficiency is increased from 69.6% to 79.8%, and the specific capacity is increased from 193.2 mA hg -1 Increased to 326.1mA hg -1 .

[0143] Application Comparative Example 3

[0144] The HM-0-1400 in Preparation Comparative Example 8 was used as an active material to prepare a negative electrode for a sodium ion battery, and an electrochemical charge and discharge test was performed on the negative electrode, and the obtained battery was named EP-HM-0-1400. The preparation process was the same as that in Application Example 1.

[0145] The battery EP-HM-1400 prepared in Example 3 and the battery EP-HM-0-1400 prepared in Comparative Example 3 were tested at 0.02 A g -1 The constant current charge and discharge curve under current density is as follows Fig.14As shown in the figure, it can be seen that the electrochemical performance of EP-HM-0-1400 in comparative example 3 is significantly better than that of EP-HM-1400 in example 3. The first coulombic efficiency is increased from 67.9% to 81.1%, and the specific capacity is increased from 137.1 mA hg -1 Increased to 338.8mA hg -1 .

[0146] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the present invention.

Claims

1. A negative electrode plate for a sodium ion battery, characterized in that: The negative electrode plate comprises: a conductive agent, a binder, a current collector and a coal-based hard carbon negative electrode material; the crystal plane spacing d 002 The value is above 0.2nm; A G / A D The value is 0.1-0.6; L c The value is 1-4nm; L a The value is 0.5-2.5nm; The method for preparing the coal-based hard carbon negative electrode material comprises the following steps: Step 1: crushing the raw coal, sieving it, placing it in a deashing solution for treatment, washing it with water until it is neutral, and drying it to obtain a carbon precursor; the treatment in the deashing solution refers to a two-step deashing treatment using an acid; the acid used in the first step of the deashing treatment is hydrochloric acid, and the acid used in the second step of the deashing treatment is hydrofluoric acid; the raw coal is one or more of bituminous coal, sub-bituminous coal and lignite; Step 2: The carbon precursor obtained in step 1 is heated at 1-5°C·min under inert gas protection. -1 The temperature is raised to 1350-1420℃ at a rate of 1-4h and kept for 1-4h. After high-temperature carbonization, the temperature is lowered by a program at 1-5℃·min -1 to 15-30° C., to obtain coal-based hard carbon negative electrode material for sodium ion battery; The conductive agent on the negative electrode plate is carbon nanotubes.

2. The negative electrode plate of the sodium ion battery according to claim 1, characterized in that: In step 1 of the method for preparing the coal-based hard carbon negative electrode material, the raw coal is lignite.

3. The negative electrode plate of the sodium ion battery according to claim 1, characterized in that: In step 1 of the method for preparing the coal-based hard carbon negative electrode material, the amount of the deashing solution is: 10-30 mL of acid is used for deashing per gram of coal.

4. The negative electrode plate of the sodium ion battery according to claim 2, characterized in that: In step 1 of the method for preparing the coal-based hard carbon negative electrode material, the amount of the deashing solution is: 10-30 mL of acid is used for deashing per gram of coal.

5. The negative electrode plate of the sodium ion battery according to claim 1, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization is at least one of nitrogen and argon.

6. The negative electrode plate of the sodium ion battery according to claim 2, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization is at least one of nitrogen and argon.

7. The negative electrode plate of the sodium ion battery according to claim 3, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization is at least one of nitrogen and argon.

8. The negative electrode plate of the sodium ion battery according to claim 1, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization has a flow rate of 30-600 cc·min -1 .

9. The negative electrode plate of the sodium ion battery according to claim 2, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization has a flow rate of 30-600 cc·min -1 .

10. The negative electrode plate of the sodium ion battery according to claim 3, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization has a flow rate of 30-600 cc·min -1 .

11. The negative electrode plate of the sodium ion battery according to claim 5, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the inert gas used for carbonization has a flow rate of 30-600 cc·min -1 .

12. The negative electrode plate of the sodium ion battery according to claim 1, characterized in that: In step 2 of the method for preparing the coal-based hard carbon negative electrode material, the temperature is 1-5 ° C min -1 The temperature was raised to 1350-1420°C at a rate of 1.5°C and kept there for 2 h.

13. The negative electrode sheet of a sodium ion battery according to any one of claims 1 to 12, characterized in that: The interplanar spacing d of the coal-based hard carbon material for sodium ion battery 002 The value is 0.2-0.5nm.

14. The negative electrode plate of the sodium ion battery according to claim 13, characterized in that: The interplanar spacing d of the coal-based hard carbon material for sodium ion battery 002 The value is 0.364-0.384nm.

15. The negative electrode sheet of a sodium ion battery according to any one of claims 1 to 12, characterized in that: A of the coal-based hard carbon material for sodium ion battery G / A D The value is 0.21-0.

49.

16. The negative electrode sheet of a sodium ion battery according to any one of claims 1 to 12, characterized in that: The L of coal-based hard carbon material for sodium ion battery c The value is 2.11-2.60nm; L a The value is 1.75-2.18nm.

17. The negative electrode plate of a sodium ion battery according to any one of claims 1 to 12, characterized in that: The coal-based hard carbon negative electrode material is in granular form, with an average particle size of 28-470 μm.

18. The negative electrode plate of the sodium ion battery according to claim 13, characterized in that: The coal-based hard carbon negative electrode material is in granular form, with an average particle size of 28-470 μm.

19. The negative electrode plate of the sodium ion battery according to claim 15, characterized in that: The coal-based hard carbon negative electrode material is in granular form, with an average particle size of 28-470 μm.

20. The negative electrode plate of the sodium ion battery according to claim 16, characterized in that: The coal-based hard carbon negative electrode material is in granular form, with an average particle size of 28-470 μm.

21. The negative electrode plate of a sodium ion battery according to any one of claims 1 to 12, characterized in that: The binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133.

22. The negative electrode plate of the sodium ion battery according to claim 13, characterized in that: The binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133.

23. The negative electrode plate of the sodium ion battery according to claim 15, characterized in that: The binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133.

24. The negative electrode plate of the sodium ion battery according to claim 16, characterized in that: The binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133.

25. The negative electrode plate of the sodium ion battery according to claim 17, characterized in that: The binder on the negative electrode plate includes one or more of sodium carboxymethyl cellulose, sodium alginate, polyacrylic acid, PVDF, and LA133.