Compositions comprising comb copolymers

By using the combination of comb copolymer of N-vinyl lactam and vinyl aromatic compounds and carbon-based materials, the problems of dispersant stability and battery pack performance of carbon-based materials are solved, and low viscosity and good stability are achieved carbon-based material dispersion and excellent battery pack performance.

CN113474918BActive Publication Date: 2024-11-15BYK CHEMIE GMBH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202080016075.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-26
Filing Date
2020-02-21
Publication Date
2024-11-15
Estimated Expiration
2040-02-21

AI Technical Summary

Technical Problem

Existing carbon-based material dispersants have difficulty providing stable carbon-based material dispersions and improved rechargeable battery pack performance, especially inadequate charge and discharge cycle stability.

Method used

The composition comprising N-vinyl lactam polymerization units and comb copolymers having vinyl aromatic compounds and ethylenically unsaturated polymerizable carboxylic anhydrides as dispersants of the carbon-based material, by mixing with the carbon-based material and The dispersion is prepared by applying shear force.

Benefits of technology

A low viscosity and small particle size carbon-based material dispersion is achieved, which improves the electrode performance and cycle stability of the battery pack, especially in the lithium-ion rechargeable battery pack, which significantly improves the C-rate discharge performance and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003224345970000121
    Figure BDA0003224345970000121
  • Figure BDA0003224345970000131
    Figure BDA0003224345970000131
  • Figure BDA0003224345970000141
    Figure BDA0003224345970000141
Patent Text Reader

Abstract

The present invention relates to a composition comprising a) a polymer a) comprising polymerized units of N-vinyl lactam, b) a comb copolymer b) having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains, and c) a carbon-based material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a composition comprising a polymer having polymerized units of N-vinyl lactam and a comb polymer. The present invention further relates to the use of the composition as a dispersant for carbon-based materials, a method for preparing a carbon-based material dispersion and a rechargeable electric battery.

[0002] EP 2296208 A relates to a composition for producing electrodes for batteries, in particular for lithium secondary batteries. The document relates to the stabilization of dispersions of carbon-based materials and improving battery performance. The inventors propose to add at least one of an organic dye derivative, an anthraquinone derivative with a basic functional group and a triazine derivative as a dispersant for the carbon-based material. The examples describe the use of polyvinyl pyrrolidone as an additive for preparing a carbon black dispersion.

[0003] JP 2011070908 A relates to a liquid dispersion of a conductive material for manufacturing a lithium ion battery. The dispersion contains a conductive material, a dispersant and a dispersion medium. The dispersant is a nonionic polymer. Preferred polymers are polyvinyl alcohol, polyvinyl pyrrolidone, cellulose resin, polyalkylene oxide, polyvinyl acetal, polyvinyl ether, chitin, chitosan and starch. Examples of dispersion media include aprotic polar solvents such as N-methyl-2-pyrrolidone, dimethyl sulfoxide and dimethylformamide.

[0004] JP 2015227406 A describes a carbon black dispersion liquid and a lithium ion battery electrode material paste using the dispersion. A phthalocyanine metal complex is proposed as a dispersant for carbon black.

[0005] TW 201347972 A describes a drilling entry sheet disposed on a metal substrate. The entry sheet is bonded to the metal using a resin composition comprising a comb copolymer based on styrene-maleic anhydride copolymer and polyvinyl pyrrolidone. The comb copolymer is typically prepared by grafting a styrene-maleic anhydride copolymer with a monomethyl ether of polyethylene glycol or polypropylene glycol.

[0006] There is a continuing need for improved carbon-based material dispersants to provide improved stabilization of carbon-based material dispersions and improved battery performance when used to fabricate rechargeable batteries, such as improved charge and discharge cycle stability.

[0007] The present invention provides a composition comprising

[0008] a) a polymer a) comprising polymerized units of N-vinyllactam,

[0009] b) a comb copolymer having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains, and

[0010] c) Carbon-based materials.

[0011] The polymer a) comprises polymerized units of N-vinyl lactam. The polymerized units are N-vinyl lactams to which ethylenically unsaturated vinyl groups have been polymerized. Examples of suitable N-vinyl lactams may have 4-, 5-, 6- or 7-membered rings, also known as β, γ, δ or ε lactams. Preferred examples include N-vinyl pyrrolidone and N-vinyl caprolactam.

[0012] In one embodiment, polymer a) is a copolymer of N-vinyl lactam and other monomers having ethylenically unsaturated polymerizable groups. Examples of other monomers include acrylates and methacrylates, vinyl aromatic compounds and vinyl esters. In a preferred embodiment, polymer a) consists of at least 50%, more preferably at least 80% by weight of polymerized units of N-vinyl lactam.

[0013] In one embodiment, polymer a) comprises polymerized units of one type of N-vinyl lactam. In other embodiments, polymer a) comprises polymerized units of two or more different types of N-vinyl lactam. Preferably, polymer a) comprises or consists of polymerized units of N-vinyl pyrrolidone.

[0014] The molecular weight of polymer a) is not particularly limited. In some embodiments, the weight average molecular weight of polymer a) is in the range of 2000 to 500000 g / mol, preferably in the range of 5000 to 100000 g / mol. It is particularly preferred that polymer a) has a weight average molecular weight in the range of 15000 to 80000 g / mol. Typically, polymer a) is a substantially linear polymer.

[0015] The weight average molecular weight of the polymer a) may suitably be determined by gel permeation chromatography (GPC) using polymethyl methacrylate as calibration standard and N,N-dimethylacetamide as eluent.

[0016] The comb copolymer b) in the composition of the invention is a comb polymer having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains.

[0017] The polymer backbone of polymer b) is generally substantially linear, i.e. it is prepared by polymerization of ethylenically unsaturated polymerizable monomers having one ethylenically unsaturated polymerizable bond. If desired, a small amount of branching may be present in the polymer backbone of polymer b), for example by including monomers having more than one ethylenically unsaturated polymerizable bond.

[0018] The polymer backbone of the comb polymer b) comprises polymerized units of vinyl aromatic compounds. Examples of suitable vinyl aromatic compounds include styrene, vinyl toluene, vinyl xylene, vinyl ethylbenzene and mixtures thereof. The polymer backbone of the comb polymer b) further comprises polymerized units of ethylenically unsaturated polymerizable carboxylic acid anhydrides or ethylenically unsaturated polymerizable dicarboxylic acids. Examples of suitable monomers include maleic anhydride, itaconic anhydride, citraconic anhydride, fumaric acid, esters of the above compounds, and mixtures thereof. The polymer backbone of polymer b) can be suitably prepared by copolymerization of the above two types of monomers. If desired, other monomers, such as acrylic acid or methacrylic acid and esters thereof, may be included in the polymer backbone of polymer b). In a preferred embodiment, the polymer backbone of the comb polymer b) is a copolymer of styrene and maleic anhydride.

[0019] Polymer b) is a comb copolymer. Comb polymers are copolymers having at least two polymeric side chains connected to the polymer backbone. Polymer b) has at least two polyalkylene oxide side chains connected to the polymer backbone. Comb copolymers b) typically have 2 to 100, preferably 2 to 50, more preferably 3 to 25, and most preferably 4 to 12 polyalkylene oxide side chains. Typically, the polyalkylene oxide side chains are polyethers based on polymerized units of epoxides or oxetanes. Typically, the polyalkylene oxide side chains are based on polymerized units of ethylene oxide, propylene oxide, butylene oxide, and mixtures thereof. In the case of mixtures of alkylene oxides, these may be present in the polyalkylene oxide chain in the form of two or more blocks or in random order. Polyalkylene oxide side chains based on ethylene oxide, propylene oxide, and in particular mixtures thereof are preferred.

[0020] The weight average molecular weight of the comb copolymer b) can suitably be determined by gel permeation chromatography (GPC) using polystyrene as calibration standard and THF as eluent.

[0021] The weight average molecular weight of the polyalkylene oxide side chains is typically in the range of 200 to 6000 g / mol, preferably 300 to 4000 g / mol. In some embodiments, the polyalkylene oxide side chains have ether end groups, for example alkyl ether end groups, such as ethyl or methyl ether end groups.

[0022] The polyoxyalkylene oxide side chains can be attached to the polymer backbone by reaction of monofunctional polyoxyalkylene oxides terminated with amines or alcohols with carboxylic anhydride groups of the polymer backbone. The reaction of primary amine groups with carboxylic anhydride groups can produce amide bonds or imide bonds. Preferably, the polyoxyalkylene oxide side chains of the comb copolymer b) are attached to the polymer backbone via amide groups or imide groups, for example by reaction of copolymers of styrene and maleic anhydride with polyether monoamines. Suitable polyether amines are available under the trade name M is available from Huntsman. Alternatively, the polyalkylene oxide side chains may be attached to the polymer backbone via ester bonds. This may be achieved by reacting the carboxylic anhydride groups of the polymer backbone with hydroxyl terminated polyalkylene oxide monoethers.

[0023] In a preferred embodiment, the comb copolymer b) comprises additional functional groups including at least one of hydroxyl groups, carboxylic acids, carboxylic acid salts, tertiary amines, tertiary amine salts, and quaternary ammonium groups.

[0024] Hydroxyl groups can be introduced by reacting the carboxylic acid anhydride groups of the polymer backbone with an alkanolamine such as ethanolamine.

[0025] The carboxylic acid group can be introduced by the ring-opening reaction of the carboxylic acid anhydride group of the polymer backbone with an alcohol or an amine. The carboxylic acid group can be neutralized with a base to form a salt of the carboxylic acid.

[0026] The comb copolymer b) suitably has an acid number in the range of 0 to 300 mg KOH / g. In a preferred embodiment, the acid number of the comb copolymer b) is in the range of 0 to 150 mg KOH / g, more preferably 0 to 100 mg KOH / g or 0 to 70 mg KOH / g.

[0027] Tertiary amine groups can be introduced by reacting the carboxylic anhydride groups of the polymer backbone with diamines having tertiary amine groups and primary or secondary amine groups (such as 3-dimethylaminopropylamine). The tertiary amine can be neutralized with an acid to form its salt. Alternatively, the tertiary amine can be quaternized with a quaternizing agent to form a quaternary ammonium group. Examples of suitable quaternizing agents include alkyl halides or benzyl halides, and epoxides in combination with carboxylic acids. Comb copolymers b) comprising at least one of a tertiary amine, a tertiary amine salt and a quaternary ammonium are preferred.

[0028] The comb copolymer b) suitably has an amine number in the range of 0 to 300 mg KOH / g. In a preferred embodiment, the comb copolymer b) has an amine number in the range of 0 to 150 mg KOH / g, more preferably 0 to 100 mg KOH / g or 0 to 70 mg KOH / g.

[0029] The weight average molecular weight of the comb copolymer b) is suitably in the range from 4000 to 100000 g / mol, preferably in the range from 6000 to 60000 g / mol. The weight average molecular weight can be determined as described above for the comb copolymer b).

[0030] Examples of suitable comb polymers b) and their preparation are described in detail in European patent application EP 2 125 910 A .

[0031] In the composition of the invention, the weight ratio of polymer a) to comb copolymer b) is preferably in the range from 10:90 to 90:10, more preferably in the range from 25:75 to 75:25.

[0032] In a preferred embodiment, the composition of the invention is provided as a liquid composition. Therefore, the composition preferably comprises at least one solvent. Typically, the solvent is an organic solvent. The choice of solvent is not particularly critical. Suitable solvents are capable of dissolving polymer a) and comb copolymer b). It is also possible to use a combination of solvents. Due to the relatively polar nature of polymer a), it is generally preferred that the solvent comprises an aprotic dipolar solvent, such as dimethyl sulfoxide, dimethylformamide or N-methylpyrrolidone.

[0033] Although the water content of the composition is not particularly critical, it has been found that a high water content caused by the high water absorption of polymer a) can reduce the storage stability and homogeneity of the composition in some embodiments. Therefore, it is preferred that the water content of the composition is in the range of 0.0 to 5.0 wt. % based on the total weight of the composition. It is particularly preferred that the water content of the composition is in the range of 0.0 to 3.0 wt. %, more preferably in the range of 0.0 to 1.5 wt. %.

[0034] The water content may suitably be determined by Karl-Fischer titration.

[0035] Compositions comprising polymer a) and polymer b) are very suitable as dispersants for carbon-based materials. Therefore, the composition of the present invention comprises a carbon-based material. A carbon-based material is a material composed of 90 to 100% by weight of carbon. In order to be used in the field of electrode manufacturing of a battery pack, a conductive carbon-based material is selected. Examples of suitable conductive carbon-based materials include carbon black, carbon nanotubes, graphite, carbon fiber, graphene, fullerene and mixtures thereof. Preferred carbon-based materials are carbon black, graphene and carbon nanotubes. Specific types of suitable carbon black are furnace black and acetylene black.

[0036] The present invention further relates to a method for preparing a carbon-based material dispersion, comprising the steps of

[0037] i) providing a composition comprising: a polymer a) comprising polymerized units of N-vinyllactam and a comb polymer b) having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains,

[0038] ii) providing a carbon-based material,

[0039] iii) mixing the components provided in steps i) and ii) and applying a shear force to prepare a carbon-based material dispersion.

[0040] The shear forces may be provided by known apparatus for dispersing pigments, for example by a ball mill or by a high speed stirrer. Suitably, a total of 1 to 40 wt. % of polymer a) and polymer b) is used in the process, based on the weight of the carbon-based material.

[0041] Dispersions of carbon-based materials in which the composition of the present invention is used as a dispersant exhibit advantageous properties such as low viscosity and small particle size of the carbon-based material.

[0042] The composition of the invention comprising the carbon-based material can be used very advantageously for preparing an electrode paste for a rechargeable battery. Therefore, the invention also relates to a rechargeable battery having an electrode comprising the composition of the invention. The term battery comprises a single electrochemical cell (which contains electrodes, a separator and an electrolyte), as well as a collection of cells or a battery assembly.

[0043] Rechargeable batteries can be made using electrodes as constituent elements, preferably as cathodes. The term cathode refers to the electrode where reduction occurs during a discharge cycle.

[0044] Paste for an electrode contains a dispersion of a carbon-based material, an active electrode material and a binder. The electrode paste can be obtained by kneading. Known devices such as a ribbon mixer, a screw-type kneader, a Spartan granulator, a Loedige mixer, a planetary mixer or a universal mixer can be used for kneading. The electrode paste can be formed into a sheet shape, a pellet shape, etc.

[0045] Examples of the binder used for the electrode paste include known binders such as: fluorine-based polymers such as polyvinylidene fluoride and polytetrafluoroethylene; and rubber-based binders such as styrene-butadiene rubber (SBR).

[0046] The binder is suitably used in an amount of 1 to 50 parts by mass, and particularly preferably in an amount of about 1.5 to 20 parts by mass, relative to 100 parts by mass of nonvolatile matter in the paste.

[0047] A solvent may be used during kneading. Examples of the solvent include known solvents such as dimethylformamide and isopropanol; in the case of fluorine-based polymers, toluene and N-methylpyrrolidone; in the case of SBR, water. In the case of an adhesive using water as a solvent, a thickener is preferably used together. The amount of the solvent is adjusted to obtain a viscosity that allows the paste to be easily applied to a collector.

[0048] The electrode may be formed from a molded product of the electrode paste mentioned above, for example, by applying the electrode paste to a current collector, followed by drying and pressure molding.

[0049] Examples of current collectors include foils and meshes of aluminum, nickel, copper, stainless steel, etc. The coating thickness of the paste is generally 40 to 200 μm. There is no particular limitation on the paste coating method, and one example of the coating method includes a method involving coating with a doctor blade or a rod coater, followed by molding by roll pressing, etc.

[0050] Examples of pressure molding include roll molding, compression molding, etc. The pressure used for pressure molding is preferably about 1 to 3 t / cm 2 As the electrode density increases, the battery capacity per unit volume generally increases. However, if the electrode density increases too much, the cycle characteristics generally deteriorate. If the electrode paste in the preferred embodiment of the present invention is used, the cycle characteristics are less degraded even if the electrode density is increased. Generally, the electrode density is between 1.0 and 4.0 g / cm 3 In some embodiments, the electrode density of the cathode is between 2.0 and 3.5 g / cm 3 The density of the anode is between 1.2 and 2.0 g / cm 3 within the range.

[0051] The rechargeable battery in the preferred embodiment of the present invention is described by taking a lithium ion rechargeable battery as a specific example. The lithium ion rechargeable battery has a structure in which an anode and a cathode are immersed in an electrolyte.

[0052] In the cathode of lithium-ion rechargeable batteries, lithium-containing transition metal oxides or lithium metal phosphates such as LiFePO are usually used. 4As the cathode active material, it is preferred to use an oxide mainly containing lithium and at least one transition metal element selected from Ti, V, Cr, Mn, Fe, Co, Ni, Mo and W, which is a compound having a lithium / transition metal element molar ratio of 0.3 to 2.2. More preferably, an oxide mainly containing lithium and at least one transition metal element selected from V, Cr, Mn, Fe, Co and Ni is used, which is a compound having a lithium / transition metal molar ratio of 0.3 to 2.2. It should be noted that Al, Ga, In, Ge, Sn, Pb, Sb, Bi, Si, P, B, etc. may be contained in a range of less than 30 mol% relative to the transition metal mainly present. Among the active materials mentioned above, it is preferred to use at least one having the general formula Li x MO 2 (M represents at least one of Co, Ni, Fe and Mn, and x is 0 to 1.2) or Li y N 2 O 4 A material having a spinel structure as shown in (N contains at least Mn, and y is 0 to 2).

[0053] Furthermore, as the cathode active material, it is particularly preferred to use at least one y M a D 1-a O 2 (M represents at least one of Co, Ni, Fe and Mn, D represents at least one of Co, Ni, Fe, Mn, Al, Zn, Cu, Mo, Ag, W, Ga, In, Sn, Pb, Sb, Sr, B and P, provided that the element corresponding to M is excluded, y=0 to 1.2 and a=0.5 to 1) and each having Li z (N b E 1-b ) 2 O 4 The spinel structured material shown (N represents Mn, E represents at least one of Co, Ni, Fe, Mn, Al, Zn, Cu, Mo, Ag, W, Ga, In, Sn, Pb, Sb, Sr, B and P, b = 1 to 0.2, and z = 0 to 2).

[0054] Specifically, take Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co a Ni 1-a O 2 , Li x Co b V1-b O z , Li x Co b Fe 1-b O 2 , Li x Mn 2 O 4 , Li x Mn c Co 2-c O 4 , Li x Mn c Ni 2-c O 4 , Li x Mn c V 2-c O 4 and Li x Mn c Fe 2-c O 4 (wherein x=0.02 to 1.2, a=0.1 to 0.9, b=0.8 to 0.98, c=1.6 to 1.96 and z=2.01 to 2.3). As the most preferred lithium-containing transition metal oxide, Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co a Ni 1-a O 2 , Li x Mn 2 O 4 and Li x Co b V 1-b O z (x=0.02 to 1.2, a=0.1 to 0.9, b=0.9 to 0.98 and z=2.01 to 2.3) It should be noted that the value of x may increase and decrease with charging and discharging.

[0055] Although the average particle size of the cathode active material is not particularly limited, the particle size is preferably 0.1 to 50 μm. Preferably, the volume of particles of 0.5 to 30 μm is 95% or more. More preferably, the volume occupied by a particle group with a particle size of 3 μm or less is 18% or less of the total volume, and the volume occupied by a particle group of 15 μm or more and 25 μm or less is 18% or less of the total volume.

[0056] Although the specific surface area is not particularly limited, the area measured by the BET method is preferably 0.01 to 50 m2 / g, particularly preferably 0.2m 2 / g to 1m 2 / g.

[0057] In a lithium ion rechargeable battery, a separator may be provided between a cathode and an anode. Examples of the separator include nonwoven fabrics, cloths, and microporous films each mainly containing polyolefins such as polyethylene and polypropylene, combinations thereof, and the like.

[0058] As the electrolyte forming the lithium ion rechargeable battery in one preferred embodiment of the present invention, known organic electrolytes, inorganic solid electrolytes and polymer solid electrolytes can be used, but organic electrolytes are preferred in view of ion conductivity.

[0059] As the solvent (non-aqueous solvent) of the organic electrolyte, preferred are solutions of organic solvents, such as: ethers, such as diethyl ether, dibutyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether or ethylene glycol phenyl ether; amides, such as formamide, N-methylformamide, N,N-dimethylformamide, N-ethylformamide, N,N-diethylformamide, N-methylacetamide, N,N -dimethylacetamide, N-ethylacetamide, N,N-diethylacetamide, N,N-dimethylpropionamide or hexamethylphosphoramide; sulfur-containing compounds such as dimethyl sulfoxide or cyclopentane; dialkyl ketones such as methyl ethyl ketone or methyl isobutyl ketone; cyclic ethers such as ethylene oxide, propylene oxide, tetrahydrofuran, 2-methoxytetrahydrofuran or 1,3-dioxolane; carbonates such as ethylene carbonate or propylene carbonate; γ-butyrolactone; N-methylpyrrolidone; acetonitrile; nitromethane, 1,2-dimethoxyethane; etc. In addition, carbonates such as ethylene carbonate, butylene carbonate, diethyl carbonate, dimethyl carbonate, methyl ethyl carbonate, propylene carbonate, vinylene carbonate, and esters such as γ-butyrolactone; ethers such as dioxolane, diethyl ether and diethoxyethane; dimethyl sulfoxide; acetonitrile; tetrahydrofuran; etc. are preferably exemplified. It is particularly preferred to use a carbonate-based nonaqueous solvent such as ethylene carbonate or propylene carbonate.One type of these solvents may be used alone, or two or more types thereof may be used as a mixture.

[0060] Lithium salts are used as solutes (electrolytes) for each of these solvents. Examples of well-known lithium salts include LiClO 4 , LiBF 4 、LiPF 6 、LiAlCl 4 、LiSbF 6 、LiSCN、LiCl、LiCF 3 SO 3 、LiCF 3 CO2 、LiN(CF 3 SO 2 ) 2 wait.

[0061] Examples of the polymer solid electrolyte include polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polycarbonate derivatives, and the like. Example

[0062] Raw materials:

[0063] Potassium carbonate: (Sigma-Aldrich)

[0064] (Dowanol)PMA:1-methoxy-2-propyl acetate (DOW Chemicals)

[0065] SMA 2000: Styrene-maleic anhydride copolymer (styrene / maleic anhydride molar ratio = 2 / 1) (Cray Valley)

[0066] Jeffamine M 2070: Amine terminated EO / PO polyether (Huntsman)

[0067] Lutensol AO11: Fatty alcohol (carbon number: 13–15) ethoxylate (polyethylene glycol repeating unit = 11) (BASF)

[0068] DMAPA: N,N-dimethylaminopropylamine (Huntsman)

[0069] Grilonit RV 1814: Alkyl (C: 13–15) glycidyl ether (EMS-GRILTECH)

[0070] Benzoic acid: (Sigma-Aldrich)

[0071] AMP: 95% aminomethyl propanol and 5% water (Sigma-Aldrich)

[0072] NMP: N-methylpyrrolidone (BASF)

[0073] DISPERBYK-111: Acidic polymer, acid value = 129 mg KOH / g (BYK-Chemie)

[0074] Measurement of non-volatile matter content (solid content)

[0075] The sample (2.0 ± 0.2 g of the test substance) is accurately weighed into a pre-dried aluminum pan and dried in a varnish drying cabinet at 150°C for 20 minutes, cooled in a desiccator and then weighed again. The residue corresponds to the solid content in the sample (ISO 3251).

[0076] Measurement of amine value

[0077] 1.5 to 3.0 g of dispersant was accurately weighed into an 80 mL beaker and dissolved in 50 mL of acetic acid. Using an automatic titration device equipped with a pH electrode, 0.1 mol / L HClO 4 The solution was neutralized and titrated with acetic acid solution. The inflection point of the titration pH curve was used as the titration endpoint, and the amine value (DIN 16945) was obtained by the following equation.

[0078] Amine value [mg KOH / g] = (561 × 0.1 × f × V) / (W × S)

[0079] (where f: coefficient of titrant, V: titration amount at the titration endpoint [mL], W: weighed amount of dispersant sample [g], S: solid matter concentration of dispersant sample [wt%])

[0080] Acid value measurement

[0081] 1.5 to 3.0 g of dispersant was accurately weighed into an 80 ml beaker and dissolved with 50 ml of ethanol. The solution was neutralized and titrated with a 0.1 mol / L ethanol KOH solution using an automatic titration device equipped with a pH electrode. The inflection point of the titration pH curve was used as the titration endpoint, and the amine value (DIN EN ISO 2114) was obtained by the following equation.

[0082] Acid value [mg KOH / g] = (561 × 0.1 × f × V) / (W × S)

[0083] (where f: coefficient of titrant, V: titration amount at the titration endpoint [mL], W: weighed amount of dispersant sample [g], S: solid matter concentration of dispersant sample [wt%])

[0084] Gel Permeation Chromatography (GPC)

[0085] The weight average molecular weight Mw was determined at 40°C according to DIN 55672-1:2007-08 using a high pressure liquid chromatography pump (WATERS 600HPLC pump) and a refractive index detector (Waters 410). As separation columns, a combination of 3 Styragel columns from WATERS was used, with dimensions of 300 mm x 7.8 mm ID / column, a particle size of 5 μm and pore sizes HR4, HR2 and HR1. The eluent used was tetrahydrofuran containing 1% by volume of dibutylamine at an elution rate of 1 ml / min. Polystyrene standards were used for routine calibration.

[0086] Synthesis of Comb Copolymer C-1

[0087] 85 g of PMA was added to the reactor. 21 g of SMA 2000 was added during stirring while the mixture was heated to 70°C. Then, 64 g of Jeffamine M 2070 and 4 g of DMAPA were added dropwise to the reactor. The reaction was carried out at 170°C for 4 hours. PMA was distilled off during the reaction. The Mw of the polymer was 30210 g / mol.

[0088] In the next step, the reactor was cooled to 120° C. Then, 9 g of Grilonit RV 1814 and 4 g of benzoic acid were added to the reactor. The reaction was carried out at 120° C. for 4 hours. Thereafter, the comb copolymer C-1 was obtained.

[0089] The comb copolymer C-1 had a solids content of 100%, an amine value of 18 mg KOH / g and an acid value of 8 mg KOH / g.

[0090] Synthesis of Comb Copolymer C-2

[0091] 85 g of PMA were added to the reactor. 21 g of SMA 2000 were added during stirring while the mixture was heated to 70° C. Then, 79 g of Jeffamine M 2070 were added dropwise to the reactor. The reaction was carried out at 170° C. for 4 hours. After removing the solvent under reduced pressure, comb copolymer C-2 was obtained.

[0092] The comb copolymer C-2 had a solid content of 100% and an acid value of 27 mg-KOH / g. The Mw of the comb copolymer C-2 was 31220 g / mol.

[0093] Synthesis of Comb Copolymer C-3

[0094] 85 g of PMA were added to the reactor. 21 g of SMA 2000 were added during stirring while the mixture was heated to 70° C. After the addition of 0.4 g of potassium carbonate, 43 g of Lutensol AO11 were added dropwise and the reactor was heated to 140° C. for 4 hours.

[0095] In the next step, PMA was distilled off under reduced pressure at 150° C. After cooling to 80° C., 30 g of NMP were added to the reactor. After addition of 6 g of AMP followed by homogenization, comb copolymer C-3 was obtained.

[0096] The comb copolymer C-3 had a theoretical solid content of 70% (solvent: NMP), an amine value of 37 mg KOH / g and an acid value of 27 mg KOH / g. The Mw of the comb copolymer C-3 was 9600 g / mol.

[0097] Synthesis of Comb Copolymer C-4

[0098] 50 g of PMA was added to the reactor. 13 g of SMA 2000 was added during stirring while the mixture was heated to 70°C. Then, 24 g of Jeffamin M 2070 was added dropwise to the reactor and the reaction was carried out at 170°C for 4 hours. PMA was distilled off during the reaction. The Mw of the comb copolymer was 23590 g / mol.

[0099] In the next step, 50 g of NMP were added to the reactor, followed by 11 g of DISPERBYK-111. The salification reaction was carried out at 80° C. for 1 hour to obtain the comb copolymer C-4.

[0100] The comb copolymer C-4 had a solid content of 50% (solvent: NMP), an amine value of 15 mg KOH / g and an acid value of 18 mg KOH / g.

[0101] Production of Carbon Black Dispersions

[0102] Carbon black:Denka Black (granules) (Denka)

[0103] PVP K30: Polyvinylpyrrolidone Sokalan K30P (BASF), Mw 40.000 g / mol

[0104] The dispersion was prepared using a paint shaker Disperser DAS 200 (LAU GmbH) and 150 g of 2 mm zirconium oxide beads. The dispersion time was 3 hours at 30°C.

[0105] General procedure for preparing carbon black dispersions D-1 to D-8

[0106] The comb copolymers (C-1, C-3 and C-4) and PVP K30 stored in sealed boxes were dissolved in NMP in a 140 ml glass bottle. Then, carbon black was added and the mixture was dispersed at 30° C. for 3 hours to obtain respective carbon black dispersions D-1 to D-8 (details are described in Table 1).

[0107] General Procedure for the Preparation of Comparative Carbon Black Dispersions CD-1 to CD-3

[0108] Carbon black dispersions CD-1 to CD-3 were prepared using the same procedure used for carbon black dispersions D-1 to D-8, except that they did not contain PVP K30 (details described in Table 1).

[0109] Procedure for preparing comparative carbon black dispersion CD-4

[0110] Carbon black dispersion CD-4 was prepared using the same procedure used for carbon black dispersions D-1 to D-8, except that it did not contain the comb copolymer (details described in Table 1).

[0111] Table 1 Formulations of carbon black dispersions D-1 to D-8 and CD-1 to CD-4

[0112]

[0113]

[0114] Preparation of Carbon Nanotube (CNT) Dispersion

[0115] CNT:FT7320(C-nano)

[0116] The dispersion was prepared using a paint shaker Disperser DAS 200 (LAU GmbH) and 50 g of 1 mm glass beads. The dispersion time was 12 hours at 30°C.

[0117] General procedure for the preparation of CNT dispersions D-9 to D-11

[0118] The comb copolymers C-1 to C-3 and PVP K30 stored in a sealed box were dissolved in NMP in a 100 ml glass bottle. Then, CNTs were added and the mixture was dispersed at 30° C. for 12 hours to obtain respective CNT dispersions D-9 to D-11 (details described in Table 2).

[0119] General procedure for the preparation of comparative CNT dispersions CD-5 to CD-7

[0120] CNT dispersions CD-5 to CD-7 were prepared using the same procedure used for CNT dispersions D-9 to D-11, except that they did not contain PVP K30 (details described in Table 2).

[0121] General procedure for the preparation of CNT dispersion CD-8

[0122] CNT dispersion CD-8 was prepared using the same procedure used for CNT dispersions D-9 to D-11, except that it did not contain the comb copolymer (details described in Table 2).

[0123] Table 2 Formulation of CNT dispersion

[0124]

[0125] Application test results

[0126] Viscosity of carbon black dispersion and CNT dispersion

[0127] The viscosity of the carbon black dispersion was measured using BROOKFIELD VISCOMETER DV-II+ (BROOKFIELD, upper viscosity limit: 1000 mPa·s).

[0128] Particle size of carbon black dispersion

[0129] The particle size (median diameter: D50) of the carbon black dispersion was measured using a particle size analyzer ELSZ-1000 (Otsuka Electronics).

[0130] Examples 1-6 Viscosity and particle size of carbon black dispersions D-2, D-3 and D-5 to D-8

[0131] The viscosity (at 20° C., rotation speed: 60 rpm) and particle size (D50) of carbon black dispersions D-2, D-3, and D-5 to D-8 are described in Table 3.

[0132] Table 3 Viscosity and particle size of carbon black dispersion

[0133]

[0134]

[0135] Comparative Examples 1-4: Viscosity and Particle Size of Carbon Black Dispersions CD-1–CD-4

[0136] The viscosity (at 20° C., rotation speed: 60 rpm) and particle size (D50) of carbon black dispersions CD-1–CD-4 are described in Table 4.

[0137] Table 4 Viscosity and particle size of carbon black dispersions CD-1–CD-4

[0138]

[0139] *Viscosity greater than 1000mPa·s

[0140] According to the results in Tables 3 and 4, the carbon black dispersions including a mixture of a comb copolymer and PVP (Examples 1-6) exhibit lower viscosity and smaller particle size (D50) than the carbon black dispersions including only a comb copolymer or only PVP (Comparative Examples 1-4).

[0141] Examples 7-9: Viscosity of CNT Dispersions D-9–D-11

[0142] The viscosities (at 20° C., rotation speeds: 1 rpm and 100 rpm) are described in Table 5.

[0143] Table 5 Viscosity of CNT dispersions D-9–D-11

[0144]

[0145] Comparative Examples 5-8: Viscosity of CNT Dispersions CD-5–CD-8

[0146] The viscosities (at 20° C., rotation speeds: 1 rpm and 100 rpm) are described in Table 6.

[0147] Table 6 Viscosity of CNT dispersions CD-5–CD-8

[0148]

[0149] *Viscosity greater than 1000mPa·s

[0150] According to the results in Tables 5 and 6, CNT dispersions including a mixture of comb copolymer and PVP (Examples 7-9) exhibit lower viscosities at different shear rates than CNT dispersions including only comb copolymer or only PVP (Comparative Examples 5-8).

[0151] Evaluation of volume resistivity

[0152] Volume resistivity

[0153] The electrode material Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-x O 2(NCM), polyvinylidene fluoride (PVDF) as a binder, and carbon black (CB) dispersion as a conductive auxiliary agent were added to N-methyl-2-pyrrolidone. In the electrode material paste, the mass ratio of NCM:CB:PVDF was 93:5:2 based on non-volatile materials, and the components were mixed together, thereby preparing an electrode material paste.

[0154] The electrode material paste was applied to the surface of a 180 μm thick PET sheet to form a coating, and the coating was dried to form a cathode layer on the surface of the PET sheet. Thereafter, this PET sheet with the cathode layer was cut into a width of 3 cm to measure the volume resistivity of the cathode layer.

[0155] Furthermore, the volume resistivity of the electrode coating layer was measured by a four-point measurement method at 25°C using a low resistivity meter (product of Mitsubishi Chemical Corporation, model: Loresta-AX).

[0156] Examples 10-12: Volume resistivity of electrode coatings prepared with carbon black dispersions D-4–D-6

[0157] The volume resistivities of the electrode coatings prepared with carbon black dispersions D-4–D-6 are described in Table 7.

[0158] Table 7 Volume resistivity of carbon black dispersions D-4–D-6

[0159]

[0160] Comparative Example 9: Volume resistivity of electrode coating prepared with carbon black dispersion CD-4

[0161] The volume resistivity of the electrode coatings prepared with carbon black dispersion CD-4 is described in Table 8.

[0162] Table 8 Volume resistivity of electrode coatings prepared with carbon black dispersion CD-4

[0163]

[0164] According to the results in Tables 7 and 8, the electrode coatings prepared with the carbon black dispersions including the mixture of the comb copolymer and PVP (Examples 10-12) exhibited lower volume resistivity than the carbon black dispersion including only PVP (Comparative Example 9).

[0165] Battery Assembly

[0166] 90 wt% of Li as cathode active material was combined 1+x (Ni 0.5 Co 0.2 Mn 0.3 )1-x O 2 (NCM), 5.5 wt. % of carbon black (CB) supplied as a dispersion and 4.5 wt. % of PVDF were mixed in a mixer Dispermat CV (VMA Getzmann GmbH) to prepare a cathode mixture. Subsequently, the cathode mixture was coated on an aluminum foil with a thickness of 21 μm, dried and rolled. The cathode mixture was heated to 15.4 mg / cm 2 amount applied.

[0167] 96 wt % of graphite as an electrode active material, 2.0 wt % of carboxymethyl cellulose (CMC) and 2.0 wt % of styrene-butadiene rubber (SBR) were combined and mixed in a mixer to prepare an anode mixture. Subsequently, the anode mixture was coated on a copper foil having a thickness of 17 μm, dried and rolled. The anode mixture was heated to 8.4 mg / cm 2 amount applied.

[0168] As a separator, a microporous film made of polypropylene with a thickness of 16 μm was used. The battery pack structure had the following configuration: cathode / separator / anode. It was assembled in the form of a laminated cell with 1 mol of LiPF dissolved therein. 6 A carbonate electrolytic solution having a volume ratio of ethylene carbonate (EC) to propylene carbonate (PC) of 1:1 was impregnated as an electrolyte to manufacture a battery pack.

[0169] C-rate discharge performance

[0170] For a battery pack with a maximum capacity Q of 22 mAh, "1C current is 22 mA, where the unit C or C-rate is the capacity expressed current in 1 / h, which is multiplied by Q to get the current in amperes.

[0171] The C rate discharge was increased from 0.2 C to 2 C. Then, the C rate discharge capacity was measured as the discharge capacity from 4.3 V to 3.0 V.

[0172] In all these tests, charging was performed at a constant current of 0.067C to a voltage limit of 4.3V and constant voltage to a current limit of 0.03C while gradually increasing the discharge rate. The C-rate performance test was performed at a temperature of 25°C.

[0173] Examples 13-15: C-rate discharge performance of batteries including carbon black dispersions D-4–D-6

[0174] The C-rate discharge performance of the battery pack including carbon black dispersions D-4 - D-6 is described in Table 9. Table 9 C-rate discharge performance of the battery pack including carbon black dispersions D-4 - D-6

[0175]

[0176] Comparative Example 10: C-rate discharge performance of a battery pack including carbon black dispersion CD-4

[0177] The C-rate discharge performance of the battery pack including carbon black dispersion CD-4 is described in Table 10.

[0178] Table 10 C rate discharge performance of battery packs including carbon black dispersion CD-4

[0179]

[0180] According to the results in Tables 9 and 10, the battery packs including the carbon black dispersions containing the mixture of the comb copolymer and PVP (Examples 13-15) exhibited better C rate discharge performance than the battery pack including the carbon black dispersion containing only PVP (Comparative Example 10).

[0181] Cycle test

[0182] For the cycle life evaluation of the battery, the battery was repeatedly charged and discharged 0, 50, 100, 200, 400 and 500 times at a temperature of 25°C.

[0183] Charging was performed at a constant current of 0.067 C to a voltage limit of 4.3 V and constant voltage was performed to a current limit of 0.03 C. Discharging was performed at a constant current of 1 C to a voltage limit of 3.0 V.

[0184] The discharge capacity of the first cycle was set to 100%.

[0185] Examples 16-17: Cyclic testing of battery packs including carbon black dispersions D-5–D-6

[0186] The cycle tests of the battery packs including carbon black dispersions D-5 - D-6 are described in Table 11.

[0187] Table 11 Cyclic tests of battery packs including carbon black dispersions D-5–D-6

[0188]

[0189] Comparative Example 11 Cyclic Test of a Battery Pack Including Carbon Black Dispersion CD-4

[0190] The cycle tests of the battery pack including carbon black dispersion CD-4 are described in Table 12.

[0191] Table 12 Cyclic test of battery packs including carbon black dispersion CD-4

[0192]

[0193] From the results in Tables 11 and 12, it is apparent that the battery packs including the carbon black dispersions containing a mixture of the comb copolymer and PVP (Examples 16-17) exhibited better cycle test performance than the battery pack including the carbon black dispersion containing only PVP (Comparative Example 11).

Claims

1. A composition comprising a) a polymer a) comprising polymerized units of N-vinyllactam, b) a comb copolymer having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains, and c) Carbon-based materials.

2. The composition according to claim 1, wherein the polymer a) comprises or consists of polymerized units of N-vinylpyrrolidone.

3. The composition according to claim 1 or 2, wherein the weight average molecular weight of polymer a) is in the range of 2,000 to 500,000 g / mol.

4. The composition according to claim 1 or 2, wherein the weight average molecular weight of polymer a) is in the range of 5,000 to 100,000 g / mol.

5. The composition according to claim 1, wherein the polyalkylene oxide side chains of the comb polymer b) are linked to the polymer backbone via amide groups or imide groups.

6. The composition according to any one of the preceding claims, wherein the comb copolymer b) comprises additional functional groups comprising at least one of hydroxyl, carboxylic acid, carboxylate, tertiary amine, tertiary amine salt and quaternary ammonium.

7. The composition according to any of the preceding claims, wherein the weight average molecular weight of the comb polymer b) is in the range of 4,000 to 100,000 g / mol.

8. The composition according to any of the preceding claims, wherein the weight ratio of polymer a) to comb copolymer b) is in the range from 10:90 to 90:

10.

9. The composition according to any one of the preceding claims, wherein the composition comprises at least one organic solvent.

10. The composition according to claim 9, wherein the organic solvent comprises N-methylpyrrolidone.

11. A composition according to any one of the preceding claims, wherein the water content of the composition is in the range of 0.0 to 5.0 wt. %, based on the total weight of the composition.

12. The composition according to any one of the preceding claims, wherein the carbon-based material is electrically conductive and comprises at least one of carbon black, carbon nanotubes, graphite, carbon fibers, graphene, and fullerenes.

13. A composition for use as a dispersant for carbon-based materials, the composition comprising a) a polymer a) comprising polymerized units of N-vinyllactam, and b) Comb copolymers b) having a polymer backbone based on vinyl aromatic compounds and ethylenically unsaturated polymerizable carboxylic acid anhydrides and having at least two polyalkylene oxide side chains.

14. The use according to claim 13, wherein the carbon-based material comprises at least one of carbon black and carbon nanotubes.

15. A method for preparing a carbon-based material dispersion, comprising the steps of i) providing a composition comprising: a) a polymer a) comprising polymerized units of N-vinyllactam, and b) a comb polymer having a polymer backbone based on a vinyl aromatic compound and an ethylenically unsaturated polymerizable carboxylic acid anhydride and having at least two polyalkylene oxide side chains, ii) providing a carbon-based material, iii) mixing the components provided in steps i) and ii) and applying a shear force to prepare a carbon-based material dispersion.

16. A rechargeable battery having an electrode comprising the composition according to any one of the preceding claims 1 to 12.

Citation Information

Patent Citations

  • Conductive material dispersion liquid, electrode paste, and conductive material coating active substance

    JP2011070908A

  • Carbon black dispersion liquid

    JP2015227406A

  • Entry board for drilling and production method of water soluble resin composition

    TW201347972A

  • Comb (block) copolymers

    CN101595136A

  • Polymer mixture comprising a comb copolymer

    CN101600744A