Method for increasing the adhesion strength between metal and organic material
By using specific zolisilane compounds or oligomers to contact the metal surface, the problem of insufficient adhesion strength between metal and dielectric materials in integrated circuits is solved, and efficient adhesion and bonding is achieved, avoiding signal loss and suitable for high-frequency signals transmission.
Patent Information
- Application Number
- CN202080017831.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-01
- Filing Date
- 2020-02-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-02-27
AI Technical Summary
In the production of integrated circuit substrates, it is difficult for the prior art to improve the adhesion strength between metal and dielectric material without etching or roughening the metal surface, especially in high-frequency signal transmission signal integrity and surface There is a strong association between roughening, resulting in the risk of signal loss or slowing down.
By contacting a specific zolisilane compound or zolisilane oligomer with a metal, metal alloy or metal oxide, a silicon-oxy-silane portion is formed, increasing its adhesion strength to the organic material without changing the total of the metal surface Surface area or introduce surface roughening.
It is achieved that the adhesion strength between the metal and the organic material is significantly improved without changing the metal surface area or introducing roughening, avoiding signal loss, and providing stable adhesion bonding, suitable for high-frequency signal transmission.
Smart Images

Figure BDA0003238462920000021 
Figure BDA0003238462920000081 
Figure BDA0003238462920000091
Abstract
Description
Technical Field
[0001] The present invention relates to a method for increasing the adhesion strength between the surface of a metal, a metal alloy or a metal oxide and the surface of an organic material, the method comprising contacting at least a portion of the metal, metal alloy or metal oxide with a specific azole silane compound, a specific azole silane oligomer or a mixture containing the compound and / or the oligomer as a main step. In addition, the present invention relates to the use of the specific azole silane compound, the specific azole silane oligomer or the mixture in the method for increasing the adhesion strength between the surface of a metal, a metal alloy or a metal oxide and the surface of an organic material. Background Art
[0002] In the semi-additive build-up sequence used in the production of integrated circuit (IC) substrates, one of the key tasks is to form a strong adhesive bond between adjacent layers that essentially have no natural adhesion. The basic challenge here is to form a strong bond between the metal traces and the dielectric material used for the build-up layer or the final solder mask coating without adversely affecting the final product performance.
[0003] In the past, the most commonly used adhesion promoter systems were to highly roughen the metal surface; the roughened surface could then serve as the key to forming a mechanical bond with dielectric materials (e.g., organic resin systems) and metal traces. However, this type of system, based on maximum increase in metal surface area to remove the least amount of metal, is no longer acceptable today. As conductor features become smaller and smaller, it becomes increasingly challenging to form reliable structures with desired line and space tolerances, so introducing an adhesion promotion step based on high surface roughening is simply undesirable.
[0004] In addition, the second challenge now faced is the upcoming 5G system, where there is a strong relationship between signal integrity and surface roughness. As the frequency and rate of data transmission of electrical signals increase, the electrical signal path moves into the outermost layer (outer most skin) of the metal trace. Obviously, if this "skin" is highly roughened to increase adhesion with the buildup layer, the risk of some signal loss or slowdown is much higher. Due to any such losses, the ability to perform in the required high frequency range is also compromised.
[0005] To overcome these challenges, it would be desirable to develop a method for treating metal surfaces and / or dielectric materials in which adhesion between the two materials is increased without etching and / or roughening the metal surface.
[0006] Azosilane compounds are frequently used in the manufacture of electronic components, in particular in surface treatment solutions, for example for the treatment of metal surfaces and surfaces of organic materials as a preparation for further processing steps.
[0007] US 2016 / 0368935 A1 relates to an azole silane compound, and a surface treatment solution, a surface treatment method and uses thereof using the azole silane compound.
[0008] JP 2018016865 A discloses a triazole surface treatment agent containing a silane compound.
[0009] JP 2014240522 A relates to a copper surface treatment liquid, a surface treatment method and uses thereof.
[0010] JP H06279461 A relates to a surface treatment agent for copper foil of a copper-clad laminate for a printed circuit board.
[0011] The article "3-amino-5-mercapto-1,2,4-triazole doped 3-glycidoxypropyltrimethoxysilane based sol-gel coating for corrosion protection of copper", Journal of Research on Chemical Intermediates, Vol. 42, No. 2, pp. 1315 to 1328, 2015 discloses research on corrosion protection of copper in neutral medium by forming a sol-gel coating over a copper surface. It discloses that a 3-amino-5-mercapto-1,2,4-triazole doped 3-glycidoxypropyltrimethoxysilane based sol-gel coating on copper forms a thiolate bond with copper. Summary of the invention
[0012] Based on the above problems, it is therefore an object of the present invention to provide a method for treating a metal surface and / or a dielectric material, wherein the adhesion between the two materials is increased, preferably without etching and / or roughening the metal surface. DETAILED DESCRIPTION
[0013] The above object is solved by a method for increasing the adhesion strength between the surface of a metal, a metal alloy or a metal oxide and the surface of an organic material, the method comprising the following steps in this order:
[0014] (i) providing a substrate, wherein at least one side of the substrate comprises a metal, a metal alloy or a metal oxide,
[0015] (ii) contacting at least a portion of the metal, metal alloy or metal oxide with
[0016] A) Azosilane compound of formula (I)
[0017]
[0018] in
[0019] X stands for NH 2 NH(NH 2 )、NH(NHU)、SH、SCH 3 、OCH 3 , NHU or SU,
[0020] Y represents NH, N(NH 2 ), N(NHU) or S,
[0021] U independently represents CH 2 -CH(OH)-CH 2 -O-(CH 2 ) n -Si(OR) 3 , R is independently (CH 2 -CH 2 -O) m -Z, where independently
[0022] n is an integer between 1 and 12,
[0023] m is 0, 1, 2, 3 or 4, and
[0024] Z represents H or C1 to C5 alkyl,
[0025] and / or
[0026] B) an azole silane oligomer obtained by reacting azole silane compounds of formula (I) with each other in the presence of water, such that the azole silane oligomer comprises at least one silicon-oxygen-silicon moiety,
[0027] Wherein the compound of formula (I) used in the reaction to form the azole silane oligomer
[0028] X represents H, CH 3 NH 2 NH(NH 2 )、NH(NHU)、SH、SCH 3 、OCH 3 , NHU or SU, and
[0029] Y and U have the meanings given above,
[0030] and
[0031] (iii) applying an organic material so that at least a portion of the metal, metal alloy or metal oxide that was in contact with the azole silane compound and / or azole silane oligomer during step (ii) is in contact with the applied organic material.
[0032] Our experiments surprisingly show that the adhesion strength between metal, metal alloy or metal oxide and organic material can be increased without etching or significantly removing the metal, metal alloy or metal oxide. During step (ii) of the inventive method, the total surface area of the metal, metal alloy or metal oxide does not increase but remains constant. In other words, after step (ii), the total surface area of the metal, metal alloy or metal oxide is substantially the same compared to the beginning of step (ii). This distinguishes the inventive method from many known methods (particularly etching methods), the purpose of which is to increase the total surface area by roughening. Therefore, the inventive method is a non-etching method.
[0033] Our experiments also surprisingly show that due to the OH group in the side chain (U) of the azole silane compound and the azole silane oligomer of formula (I), the solubility in polar solvents is increased (compared to the compound of formula (I) or the azole silane oligomer in which the OH group is replaced by hydrogen). Therefore, the excess azole silane compound or azole silane oligomer can be removed by conventional wet chemical methods after step (ii), and plasma treatment is not necessary.
[0034] Preference is given to the process according to the invention, wherein in step (i), the metal, metal alloy or metal oxide comprises a metal, metal alloy or metal oxide circuit, preferably a metal, metal alloy or metal oxide circuit. In this case, the metal, metal alloy or metal oxide alloy is structured. This preferably means that the organic material is exposed to non-conductive (preferably organic) areas and conductive metal, metal alloy or metal oxide areas on the same side at the same time. This is most preferred in the case of the process according to the invention.
[0035] Preference is given to the process according to the invention, wherein in step (i) the metal, metal alloy or metal oxide forms at least one layer on the substrate. As mentioned above, this layer or layers may be structured and may form or be a circuit.
[0036] Preferred is the method of the invention, wherein in step (i) (and / or preferably after step (ii)), the metal, metal alloy or metal oxide circuit comprises a line having a line width of 100 μm or less, preferably 75 μm or less, more preferably 55 μm or less. In some cases, preferred is the method of the invention, wherein in step (i) (and / or preferably after step (ii)), the metal, metal alloy or metal oxide circuit comprises a line having a line width of 30 μm or less, preferably 20 μm or less, most preferably 10 μm or less.
[0037] According to the inventive method, it is preferred that an aqueous solution of an azole silane compound of formula (I) and / or an azole silane oligomer is used in step (ii). In this case, it is preferred that the aqueous solution comprises at least 51% by weight of water of the total weight of the aqueous solution. It is preferred that the aqueous solution has a total amount of water in the range of 56% to 88% by weight of the total weight of the aqueous solution, preferably a total amount in the range of 60% to 84.8% by weight, more preferably a total amount in the range of 65% to 82.2% by weight.
[0038] In order to fully dissolve the azole silane compound and the azole silane oligomer in the aqueous solution, one or more water-miscible organic solvents are present. Preferably, the solution of the present invention, wherein the total amount of one or more water-miscible organic solvents present in the solution is in the range of 6 wt % to 44 wt %, preferably in the range of 8 wt % to 43.9 wt %, more preferably in the range of 13 wt % to 39.7 wt %, most preferably in the range of 16 wt % to 34.5 wt %.
[0039] In the context of the present invention, the azole silane compound and the azole silane oligomer and the solution used in step (ii) of the present invention are initially free of halide. On the one hand, this means that the compound and oligomer are respectively free of halogen atoms themselves, because no halogen atom-containing extract is used, and on the other hand, halide ions are not present in the direct synthesis environment. However, in a few cases, it is preferred that the aqueous solution of the present invention contains a precisely defined amount of halide ions. Therefore, in some cases, the aqueous solution used in step (ii) of the present invention preferably additionally contains halide ions, preferably chloride ions.
[0040] However, in other cases, it is preferred that the (aqueous) solution used in step (ii) of the present invention is substantially free of (preferably comprises no) chloride ions, more preferably substantially free of (preferably comprises no) halide ions.
[0041] As mentioned above, the method according to the present invention is preferred, wherein the aqueous solution additionally comprises one or more than one water-miscible organic solvent. In this case, it is preferred that when the one or more than one water-miscible organic solvent comprises a water-miscible organic solvent, it is selected from the group consisting of C1 to C4 alcohols, glycol ethers and mixtures thereof, preferably selected from the group consisting of
[0042] - C1 to C3 alcohols,
[0043] -HO-(CH2-CH2-O) m -Z, where
[0044] m is 1, 2, 3 or 4, preferably 1 or 2, and
[0045] Z represents a C1 to C5 alkyl group, preferably a C3 to C5 alkyl group,
[0046] and mixtures thereof, more preferably
[0047] Selected from the group consisting of methanol, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether and mixtures thereof, even more preferably
[0048] Selected from the group consisting of diethylene glycol monobutyl ether, ethylene glycol monobutyl ether and mixtures thereof.
[0049] In each case, glycol ethers are preferred over alcohols. Glycol ethers generally provide improved stability compared to the alcohols. In addition, alcohols generally exhibit low flash points compared to glycol ethers, which makes alcohols a potential fire hazard. To prevent ignition, a relatively high flash point is generally required. Therefore, glycol ethers generally provide the desired solubility, stability and safety.
[0050] Preference is given to the process according to the invention wherein the total amount of azole silane compound and azole silane oligomer together is 5% by weight or less, based on the total weight of the (aqueous) solution.
[0051] The above term "5 wt% or less" does not include 0 wt%. This means that the total amount is always > 0 wt%, preferably at least 0.1 wt%.
[0052] Preferably, the total amount of all azole silane compounds (as described throughout this document, preferably described as preferred) and all azole silane oligomers (as described throughout this document, preferably described as preferred) together is in the range of 0.1 wt% to 4 wt%, preferably in the range of 0.2 wt% to 3 wt%, more preferably in the range of 0.3 wt% to 2.2 wt%, even more preferably in the range of 0.4 wt% to 2.0 wt%, most preferably in the range of 0.5 wt% to 1.8 wt%, based on the total weight of the aqueous solution.
[0053] Our experiments show that the individual existence of one or more than one azole silane compound and one or more than one azole silane oligomer varies with time. In the freshly prepared aqueous solution, the total weight of the azole silane compound is usually higher than the total weight of the azole silane oligomer. However, as time goes by, when the aqueous solution is used, the total weight of the azole silane oligomer increases sharply, and may even reach the degree that the total weight of the azole silane oligomer is higher than the total weight of the azole silane compound. In addition, the processing of the aqueous solution also affects the total weight of the compound and the oligomer respectively. For example, a large amount of discharge during the use of the aqueous solution and the corresponding supplement of fresh aqueous solution usually lead to a steady state condition with respect to the azole silane compound relative to the azole silane oligomer.
[0054] In step (ii) of the process according to the invention, it is also possible to isolate one or more azole silane oligomers and to use only azole silane oligomers.
[0055] The process according to the invention is preferably carried out in which the pH of the aqueous solution is in the range of 4.8 to 8.6, preferably in the range of 4.8 to 8.0.
[0056] In the context of the present invention, pH is referred to a temperature of 20°C.
[0057] More preferably, the aqueous solution has a pH in the range of 5.6 to 7.9, more preferably in the range of 5.8 to 7.7, and most preferably in the range of 6.5 to 7.5. The pH in the range of 4.8 to 8.6 supports the oligomerization of the azole silane compound at least to a certain extent, which is desirable. Our experiments have shown that if the pH is significantly lower than pH 4.8 or significantly higher than pH 8.0, undesirable and strong precipitation is usually observed. In addition, the total amount of all azole silane compounds and all azole silane oligomers of 5% by weight or less of the total weight of the solution (and the solution is mainly an aqueous solution) will produce a sufficiently stable solution. This means that precipitation can be significantly avoided at this total amount and this pH in an aqueous environment.
[0058] Since the adhesion strength (e.g. peel strength) between metal and organic material can be increased without any etching cleaning step according to the method of the invention, in some cases, in particular when the surface roughness of the metal surface does not affect the quality of the circuit, another etching cleaning step can be performed. In this case, the adhesion strength between metal and organic material can be even further improved.
[0059] According to the method of the present invention, it is preferred that, before carrying out step (ii), it further comprises the following step: (ia) contacting at least a portion of the metal, metal alloy or metal oxide with an etching cleaning solution, preferably an etching cleaning solution containing one or more than one acid and / or one or more than one oxidizing agent, more preferably an etching cleaning solution containing a mixture of an inorganic acid and a peroxide, preferably a mixture of sulfuric acid and hydrogen peroxide.
[0060] According to the present invention, it is preferred when the oxidizing agent is a peroxide, more preferably when the peroxide is hydrogen peroxide.
[0061] According to the invention, it is preferred when the etching cleaning solution comprises a corrosion inhibitor in addition to the acid and / or one or more than one oxidizing agent.
[0062] According to the method of the present invention, it is preferred that the method further comprises the following step before performing step (ii): (ib) contacting at least a portion of the metal, metal alloy or metal oxide with a (preferably second) etching cleaning solution. In the case where step (ib) is performed after step (ia), the etching cleaning solution used is the second etching cleaning solution. In the case where step ib is performed without performing a previous etching cleaning step, the etching cleaning solution used is the first etching cleaning solution.
[0063] According to the present invention, the second etching cleaning solution comprises an iron (III) salt or an iron (III) complex, and more preferably the second etching cleaning solution comprises iron sulfate (Fe 2 (SO 4 ) 3 ), ferric chloride (FeCl 3 ), ferric bromide (FeBr 3 ), iron nitrate (Fe(NO 3 ) 3 ), ferrous acetate (Fe(OC(O)CH 3 ) 3 、(Fe(OH) 3 ) or a mixture thereof, even more preferably the second etching cleaning solution comprises iron sulfate (Fe 2 (SO 4 ) 3 ). Iron ions are preferably contained in a concentration ranging from 1 to 100 g / l, preferably from 1 to 50 g / l, more preferably from 1 to 30 g / l.
[0064] According to the invention, the second etching cleaning solution preferably comprises an acid, preferably sulfuric acid, in addition to the iron(III) salt or iron(III) complex.
[0065] According to the invention, typical metal, metal alloy or metal oxide removal during steps ia and / or ib is less than 200 nm and the resulting surface roughness is maximally 100 nm.
[0066] According to the method of the present invention, it is preferred that, before carrying out step (ii), it further comprises the following step: (ic) contacting at least a portion of the metal, metal alloy or metal oxide with an alkaline aqueous solution (preferably an aqueous sodium hydroxide solution). It is preferred if the alkaline aqueous solution contains a metal complexing agent.
[0067] In some embodiments of the present invention, it is preferred if the alkaline aqueous solution used in step ic additionally contains sodium chlorite. It is particularly preferred to use sodium chlorite in the alkaline aqueous solution used in step ic if no iron(III) salt or iron(III) complex is used in step ib or if step ib is not performed during the process according to the present invention.
[0068] The order of steps (ia), (ib) and (ic) may vary. The process according to the invention may be carried out in the following order: (ia), (ib), (ic) or (ia), (ic), (ib) or (ib), (ia), (ic) or (ib), (ic), (ia), (ib) or (ic), (ib), (ia). The order (ia), (ib), (ic) is preferred. In the process according to the invention, none, one or both of steps (ia), (ib), (ic) may also be carried out.
[0069] Preference is given to the process according to the invention in which the organic material applied in step (iii) is an organic polymer.
[0070] Preference is given to a method according to the invention in which the organic material is applied in step (iii) by laminating the organic material onto at least the contacting portion of the metal, metal alloy or metal oxide.
[0071] According to the method of the present invention, it is preferred that it comprises, after step (iii), a further step: (iv) subjecting the substrate and the organic material to a heat treatment at a temperature in the range of 142°C to 420°C, preferably in the range of 145°C to 300°C, more preferably in the range of 150°C to 220°C.
[0072] According to the method of the present invention, it is preferred that after step (ii), after step (ia), after step (ib) and / or after step (ic), at least a portion of the metal, metal alloy or metal oxide is rinsed, wherein the metal, metal alloy or metal oxide is preferably rinsed with water. It is preferred that the pH value of the water used during the rinsing after step (ii) is in the range of 4 to 10, preferably in the range of 5 to 9, more preferably in the range of 6 to 8, most preferably in the range of 6.5 to 7.5.
[0073] The process according to the invention is preferred, wherein after step (ii), after step (ia), after step (ib) and / or after step (ic), at least a portion of the metal, metal alloy or metal oxide is dried.
[0074] The process according to the invention is preferred, wherein the metal, metal alloy or metal oxide is copper, aluminum, titanium, nickel, tin, iron, silver, gold, an alloy comprising at least one of the aforementioned metals (or an alloy comprising only the aforementioned metals) or a metal oxide of at least one of the aforementioned metals. The process according to the invention is particularly preferred, wherein the metal is copper, the metal alloy comprises copper and the metal oxide is or comprises copper oxide.
[0075] Particularly preferred is the method according to the invention which comprises the following steps in the following order:
[0076] (i) providing a substrate, wherein at least one side of the substrate comprises a metal, a metal alloy or a metal oxide,
[0077] (ia) optionally contacting at least a portion of the metal, metal alloy or metal oxide with an etching cleaning solution, preferably an etching cleaning solution comprising one or more than one acid and / or one or more than one oxidizing agent, more preferably an etching cleaning solution comprising a mixture of an inorganic acid and a peroxide, and optionally subsequently rinsing at least a portion of the metal, metal alloy or metal oxide, preferably with water,
[0078] (ib) optionally contacting at least a portion of the metal, metal alloy or metal oxide with a second etching cleaning solution, wherein the second etching cleaning solution preferably comprises iron sulfate and sulfuric acid, and optionally subsequently rinsing at least a portion of the metal, metal alloy or metal oxide, preferably with water,
[0079] (ic) optionally contacting at least a portion of the metal, metal alloy or metal oxide with an alkaline aqueous solution, and optionally subsequently rinsing at least a portion of the metal, metal alloy or metal oxide, preferably with water,
[0080] (ii) contacting at least a portion of the metal, metal alloy or metal oxide with
[0081] A) Azosilane compound of formula (I)
[0082]
[0083] in
[0084] X stands for NH 2 NH(NH 2 )、NH(NHU)、SH、SCH 3 、OCH 3 , NHU or SU,
[0085] Y represents NH, N(NH 2 ), N(NHU) or S,
[0086] U independently represents CH 2 -CH(OH)-CH 2 -O-(CH 2 )n-Si(OR) 3 , R is independently (CH 2 -CH 2 -O) m -Z, where independently
[0087] n is an integer between 1 and 12,
[0088] m is 0, 1, 2, 3 or 4, and
[0089] Z represents H or C1 to C5 alkyl,
[0090] and / or
[0091] B) an azole silane oligomer obtained by reacting azole silane compounds of formula (I) with each other in the presence of water, such that the azole silane oligomer comprises at least one silicon-oxygen-silicon moiety,
[0092] Wherein the compound of formula (I) used in the reaction to form the azole silane oligomer
[0093] X represents H, CH 3 NH 2 NH(NH 2 )、NH(NHU)、SH、SCH 3 、OCH 3 , NHU or SU, and
[0094] Y and U have the meanings given above,
[0095] and optionally subsequently rinsing at least a portion of the metal, metal alloy or metal oxide, preferably with water,
[0096] (iii) applying an organic material so that at least a portion of the metal, metal alloy or metal oxide that was in contact with the azole silane compound and / or azole silane oligomer during step (ii) is in contact with the applied organic material,
[0097] and
[0098] (iv) optionally subjecting the substrate and the organic material to a heat treatment at a temperature in the range of 142° C. to 420° C., preferably in the range of 145° C. to 300° C., more preferably in the range of 150° C. to 220° C.,
[0099] Preferably, the metal is copper, the metal alloy contains copper, and the metal oxide is or contains copper oxide.
[0100] The method according to the invention is preferably wherein the substrate is a non-conductive substrate and / or the organic material is a non-conductive organic material, preferably a non-conductive organic polymer.
[0101] According to the invention the process is preferred in which X represents NH 2 NH(NH 2 ), SH, SCH 3 or OCH 3, preferably NH 2 NH(NH 2 ), SH, SCH 3 or OCH 3 , more preferably NH 2 NH(NH 2 ), SH or SCH 3 , most preferably NH 2 .
[0102] The method according to the invention is preferred, wherein n in U is an integer in the range of 1 to 8, preferably in the range of 2 to 6, more preferably in the range of 3 to 4, and most preferably n is 3.
[0103] In a very preferred method according to the present invention, the azole silane compound is a compound of formula (II) or (I-II)
[0104]
[0105] R is independently (CH 2 -CH 2 -O) m -Z,
[0106] Among them independently
[0107] m is 0, 1 or 2, preferably 0 or 2.
[0108] Z represents H, CH 3 , CH 2 -CH 3 , (CH 2 ) 2 -CH 3 or (CH 2 ) 3 -CH 3 , preferably H, CH 3 or (CH 2 ) 3 -CH 3 ,and
[0109] B is independently selected from H and NH 2 The group consisting of, preferably B is H.
[0110] The compounds of formula (I-II) are particularly preferred.
[0111] In the context of the present invention, the term "independently" (or similar expressions) in combination with a variable means that the selected characteristics of the variable in the first compound are independent of the selected characteristics of the same variable in the second compound (e.g., variable B in (II) and (I-II)), and if a compound contains the same variable at least twice (e.g., variable B in (I-II)), they are selected independently of each other and can therefore be different. For example, in the compound of formula (I-II), B is independently selected from the B in the compound of formula (II). Therefore, the two Bs can be different. In addition, in the compound of formula (I-II), the B connected to the cycloazole nitrogen is independently selected from the B in the external amino group. Therefore, also in this case, the two Bs can be different in the compound of formula (I-II). The same principle applies to other "independently" items.
[0112] In a very preferred method according to the invention, the azole silane compound is a compound of formula (Ia) or (Ib)
[0113]
[0114] R is independently (CH 2 -CH 2 -O) m -Z,
[0115] Among them independently
[0116] m is 0, 1 or 2, preferably 0 or 2, and
[0117] Z represents H, CH 3 , CH 2 -CH 3 , (CH 2 ) 2 -CH 3 or (CH 2 ) 3 -CH 3 , preferably H, CH 3 or (CH 2 ) 3 -CH 3 .
[0118] In the azole silane compound used in the method of the present invention, Y most preferably comprises nitrogen. The azole silane compound used in the method of the present invention is preferably a compound of formula (Ib) and (I-II) as defined above.
[0119] The process according to the invention is preferred, wherein the azole silane oligomer is selected from the group consisting of azole silane dimers, azole silane trimers and azole silane tetramers. Thus, the azole silane oligomer used in the process according to the invention is obtained by reacting an azole silane compound according to formula (I) in the presence of water, preferably as described throughout this document, more preferably as described as preferred. This reaction of azole silane compounds with each other is called oligomerization.
[0120] The above oligomerization reaction requires at least a small amount of water for hydrolysis to form at least some OH groups at each silicon atom. Preferably, the azole silane oligomer is obtained by reacting the azole silane compounds with each other in the presence of at least 2 wt. % of water, based on the total weight of the respective reaction composition.
[0121] In the context of the present invention, the term "azole silane oligomer" includes a combination of at least two monomers, that is, at least two azole silane compounds as described above react with each other. In addition, the term includes three, four, five, six, seven, eight, nine and ten monomers at most. Preferably, the azole silane oligomer as described above, wherein the oligomer is selected from the group consisting of: azole silane dimer, azole silane trimer, azole silane tetramer, azole silane pentamer, azole silane hexamer, azole silane heptamer and azole silane octamer. More preferably, the azole silane oligomer as used in the method of the present invention, wherein the oligomer is selected from the group consisting of azole silane dimer, azole silane trimer and azole silane tetramer. Or, the latter means that the azole silane oligomer is preferably, wherein the oligomer comprises one, two or three silicon-oxygen-silicon parts respectively.
[0122] Based on the azole silane compounds as described above, a vast variety of oligomers of the present invention can be formed. Therefore, the oligomers of the present invention are most preferred and are suitably described by their reaction with each other.
[0123] In the context of the present invention, the term "at least" in combination with a value means the value or more than the value (and can be interchanged with it). For example, the "at least one silicon-oxygen-silicon portion" mentioned above means "one or more than one silicon-oxygen-silicon portion" (and can be interchanged with it). Most preferably, "at least one" means "one, two, three or more than three" (and can be interchanged with it).
[0124] The method according to the invention is preferably wherein the azole silane oligomer is a compound of formula (II)
[0125]
[0126] (II), where
[0127] R independently represents (CH 2 -CH 2 -O)m -Z,
[0128] in
[0129] m is 0, 1, 2, 3 or 4, preferably 0, 1 or 2, and
[0130] Z represents H or C1 to C5 alkyl,
[0131] k is 1, 2 or 3, preferably 1 or 2, and
[0132] M independently represents a moiety of formula (IIa)
[0133]
[0134] Wherein in formula (IIa)
[0135] X represents H, CH 3 NH 2 NH(NH 2 ), SH, SCH 3 or OCH 3 , preferably CH 3 NH 2 NH(NH 2 ), SH, SCH 3 or OCH 3 , more preferably NH 2 NH(NH 2 ), SH or SCH 3 NH is the most preferred 2 ,
[0136] Y represents NH, N(NH2) or S, preferably NH, and
[0137] n represents an integer in the range of 1 to 12, preferably in the range of 1 to 8, more preferably in the range of 2 to 6, even more preferably in the range of 3 to 4, and most preferably n is an integer of 3.
[0138] In the moiety of formula (IIa) above, the dotted line represents the covalent bond connecting the entire moiety to the silicon atom represented by formula (II).
[0139] Only in a few cases, azole silane oligomers as used in the process of the invention are even preferred in which k is an integer in the range from 1 to 7, preferably in the range from 1 to 5. Most preferably, however, k is 1, 2 or 3, preferably 1 or 2.
[0140] Preferably, the azole silane oligomer as used in the process according to the invention is a homopolymer. This means that preferably identical monomers are combined with one another to form the oligomer.
[0141] Alternatively, preferably, as in the azole silane oligomer used in the method according to the present invention, at least all of the moieties that do not form the silicon-oxygen-silicon backbone (i.e., the azole moiety and the ether moiety connecting the azole moiety to the silicon atom) have the same chemical formula. In this case, it is preferred that m is not independently defined.
[0142] The azole silane compound and the azole silane oligomer used in step (ii) of the method of the present invention may be present in the form of a mixture. Typically, an organic solvent promotes the solubility of the mixture. Therefore, in step (ii) of the method of the present invention, a mixture comprising, preferably consisting of, the following substances may also be used:
[0143] (a) - one or more than one azole silane compound (as described herein throughout, preferably as described as preferably), and / or (preferably and)
[0144] - one or more than one azole silane oligomer (as described herein throughout, preferably as described as preferably), and
[0145] (b) - one or more than one organic solvent and / or water.
[0146] Preferably, the mixture is substantially free of halide ions, preferably comprises no halide ions.
[0147] In the context of the present invention, the term "substantially free" of a target (e.g., compound, material, etc.) means that the target is not present at all or is present only (to) a very small and undisturbed amount (degree) that does not affect the intended purpose of the present invention. For example, this target may be added or used unintentionally, for example, in the form of unavoidable impurities. "Substantially free" preferably means 0 (zero) ppm to 50 ppm (based on the total weight of the mixture (if defined for the mixture)), preferably 0 ppm to 25 ppm, more preferably 0 ppm to 10 ppm, even more preferably 0 ppm to 5 ppm, most preferably 0 ppm to 1 ppm. Zero ppm means that the corresponding respective target is not contained at all, which is most preferred.
[0148] Preferably, the solution or mixture as used in step (ii) of the present invention (as described throughout, preferably as described as preferably), wherein all azole silane compounds (as described throughout, preferably as described as preferably) and all azole silane oligomers (as described throughout, preferably as described as preferably) represent at least 70% by weight, preferably at least 80% by weight, more preferably at least 90% by weight, even more preferably at least 93% by weight, most preferably at least 95% by weight, even most preferably at least 98% by weight, of the total weight of all azole silane compounds and oligomers in the solution, respectively. Most preferably, no other azole silane compounds or oligomers are present except those described throughout, preferably as described as preferably. This also means that the absolute total amount of azole silane compounds and azole silane oligomers together (as defined just above) is very preferably applicable under the condition that no other azole silane compounds and azole silane oligomers are present in the solution. Therefore, the mixture is substantially free of (preferably does not contain) any other azole silane compounds and azole silane oligomers.
[0149] Furthermore, preference is given to mixtures or solutions (as described throughout this document, preferably as described as preferably) in which all azole silane compounds (as described throughout this document, preferably as described as preferably) and all azole silane oligomers (as described throughout this document, preferably as described as preferably) represent at least 51 mol %, preferably at least 60 mol %, more preferably at least 70 mol %, most preferably at least 80 mol %, even most preferably at least 90 mol %, respectively, of all compounds comprising at least one silicon atom in said mixture or solution.
[0150] Preferred is a mixture wherein the one or more than one organic solvent comprises a solvent selected from the group consisting of acetone, 1,3-dioxolane, acetonitrile, 1,4-dioxane, methanol, ethanol, 1-propanol, 2-propanol, tert-butanol, prop-2-en-1-ol, ethyl lactate, ethylene glycol monomethyl ether acetate, N,N-dimethylformamide, 2-butoxyethanol, dipropylene glycol methyl ether, tetrahydrofurfuryl alcohol, N-methyl-2-pyrrolidone, 2-(2-methoxyethoxy)ethanol, γ-butyrolactone, ethylene glycol, propylene glycol, dipropylene glycol, ε-caprolactone, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, tetrahydrothiophene-1-oxide, diethylene glycol monobutyl ether acetate, propylene carbonate, cyclopentane, glycerol, and mixtures thereof.
[0151] Highly preferred is a mixture wherein the one or more than one organic solvent comprises a solvent selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, tert-butanol, di(propylene glycol) methyl ether, ethylene glycol, propylene glycol, dipropylene glycol, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether and mixtures thereof.
[0152] In a few cases, highly preferred is a mixture wherein one or more than one organic solvent comprises a solvent selected from the group consisting of glycol ethers, preferably selected from the group consisting of dipropylene glycol methyl ether, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether and mixtures thereof.
[0153] The above-mentioned azole silane compound of formula (I) can be synthesized by a method comprising the following steps:
[0154] (a) providing an azole compound of formula (III)
[0155]
[0156] in
[0157] X represents H, CH 3 NH 2 NH(NH 2 ), SH, SCH 3 or OCH 3 ,
[0158] Y represents NH, N(NH 2 ) or S,
[0159] (b) providing a silane compound of formula (IV)
[0160]
[0161] Wherein in formula (IV)
[0162] R stands for (CH 2 -CH 2 -O) m -Z, where independently
[0163] m is 0, 1, 2, 3 or 4, and
[0164] Z represents a C1 to C5 alkyl group, and
[0165] n is an integer between 1 and 12,
[0166] (c) reacting the azole compound with the silane compound in a solvent to obtain the compound of the above formula (I), and
[0167] (d) optionally hydrolyzing the compound of formula (I) obtained in step (c) so that at least one of R is (CH 2 -CH 2 -O) m -Z, where m=0 and Z=H.
[0168] Step (d) is optional and comprises the presence of at least some water to hydrolyze the compound obtained in step (d) of the process of the invention. Preferably, the water is added after step (c), in a further step, for example in step (d). If this compound is desired (m=0 and Z=H), step (d) is not optional.
[0169] The solvent in step (c) is one or more than one organic solvent and after step (c) of the process according to the invention a mixture according to the invention is obtained (for the mixture see above). What has been said above about the mixture also applies to the synthesis process according to the invention.
[0170] The synthesis route is beneficial, wherein the total molar ratio of the compound of formula (III) to the compound of formula (IV) is in the range of 1:0.85 to 1:1.3, preferably in the range of 1:0.90 to 1:1.25, more preferably in the range of 1:0.95 to 1:1.2, and most preferably in the range of 1:1.0 to 1:1.15. If the total molar ratio is significantly higher than 1:1.3, the synthesis product is not stable enough. If the total molar ratio is significantly lower than 1:0.85, there are too many unreacted extracts in the synthesis product, which is undesirable because the desired substance is an azole silane compound containing azole and silane moieties.
[0171] The synthetic route is advantageous wherein in step (c) the temperature is in the range of 50°C to 90°C, preferably in the range of 60°C to 85°C.
[0172] The synthetic route is beneficial, wherein in step (a), the azole compound of formula (III) is provided in the form of a suspension. This means that the azole compound of formula (III) is preferably suspended in at least one solvent so that the azole compound and the at least one solvent form the suspension. For this reason, it is preferred that at least one solvent is one or more than one organic solvent, preferably one or more than one water-miscible organic solvent. Very preferably, at least one solvent used to form the suspension is the same as the solvent used in step (c). Most preferably, the azole compound of formula (III) is suspended in one or more than one solvent, the solvent being selected from the group consisting of C1 to C4 alcohols, glycol ethers and mixtures thereof, preferably selected from the group consisting of:
[0173] -C1 to C3 alcohols,
[0174] -HO-(CH 2 -CH 2 -O) m -Z, where
[0175] m is 1, 2, 3 or 4, preferably 1 or 2, and
[0176] Z represents a C1 to C5 alkyl group, preferably a C3 to C5 alkyl group,
[0177] and mixtures thereof, more preferably
[0178] Selected from the group consisting of methanol, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether and mixtures thereof, most preferably
[0179] Selected from the group consisting of diethylene glycol monobutyl ether, ethylene glycol monobutyl ether and mixtures thereof.
[0180] The synthetic route is advantageous wherein in step (c) the reaction is allowed to proceed for 1 hour to 48 hours, preferably for 3 hours to 24 hours, more preferably for 5 hours to 20 hours.
[0181] The present invention also relates to the specific use of azole silane compounds (as described throughout the text, preferably as described as preferred) and / or azole silane oligomers (as described throughout the text, preferably as described as preferred) in a method for increasing the adhesion strength between the surface of a metal, metal alloy or metal oxide and the surface of an organic material.
[0182] The present invention is further explained by the following non-limiting examples.
[0183] Examples
[0184] A) Synthesis of azole silane compounds:
[0185] 1) Synthesis of azole silane compound of formula (Ia):
[0186]
[0187] In the first step, 3.68 g (27.1 mmol) of 5-amino-1,3,4-thiadiazole-2-thiol (oxazole compound of formula (III), wherein X represents NH 2 and Y represents S) is suspended in 70 ml of methanol and an azole suspension is obtained.
[0188] In the second step, 6.59 g (27.1 mmol) of 3-glycidyloxypropyltrimethoxysilane (silane compound of formula (IV) wherein R represents CH 3 and n is 3) dissolved in 20 ml of methanol was added to the azole suspension. Thus, a reaction suspension was obtained.
[0189] In the third step, the reaction suspension is heated to reflux (temperature of about 65° C.) for 18 hours. During this period, the suspension becomes a clear solution, indicating that the azole compound has been completely used up. Afterwards, the solvent (methanol) is removed and about 10 g (yield 100%) of a yellow, highly viscous substance is obtained as a product, mainly a azole silane compound of formula (Ia). The product thus obtained does not contain any halide and can be used without further purification.
[0190] 1 H NMR: (400 MHz, DMSO-d 6 )δ7.24(s, 2H), 5.22(d, J=5.4Hz, 1H), 3.81(dq, J=7.1, 5.2Hz, 1H), 3.51-3.43(m, 8H), 3.41–3.3 0 (m, 5H), 3.30–3.13 (m, 2H), 3.05 (dd, J=13.1, 7.1Hz, 1H), 1.59–1.44 (m, 2H), 0.68–0.51 (m, 2H)
[0191] ESI-MS: m / z: 369.08 (100.0%), 370.09 (11.9%), 371.08 (9.0%)
[0192] Both NMR and ESI-MS confirmed the presence of the oxadiazole silane compound of formula (Ia). The theoretical molar mass is 369 g / mol.
[0193] 2) Synthesis of azole silane compound of formula (Ib):
[0194]
[0195] In the first step, 3.36 g (28.4 mmol) of 5-amino-4H-1,2,4-triazole-3-thiol (oxazole compound of formula (III) wherein X represents NH 2 and Y represents NH) was suspended in 70 ml of methanol and an azole suspension was obtained.
[0196] In the second step, 6.91 g (28.4 mmol) of 3-glycidyloxypropyltrimethoxysilane (silane compound of formula (IV) wherein R represents CH 3 and n is 3) dissolved in 20 ml of methanol was added to the azole suspension. Thus, a reaction suspension was obtained.
[0197] In the third step, the reaction suspension is heated to reflux (temperature of about 65° C.) for 18 hours. During this period, the suspension becomes a clear solution, indicating that the azole compound has been completely used up. Afterwards, the solvent (methanol) is removed and about 10 g (yield 100%) of a yellow, highly viscous substance is obtained as a product, mainly a silane compound of formula (Ib). The product thus obtained does not contain any halide and can be used without further purification.
[0198] 1 H NMR: (400 MHz, DMSO-d 6 )δ6.03(s, 2H), 5.33–5.08(m, 1H), 3.87–3.75(m, 1H), 3.54–3.25(m, 13H), 3.22–3.08(m, 1H) , 2.97 (dd, J=13.3, 7.0Hz, 1H), 1.55 (dddd, J=12.7, 11.1, 6.6, 3.5Hz, 2H), 0.67–0.50 (m, 2H)
[0199] ESI-MS: m / z: 352.12 (100.0%), 353.13 (11.9%)
[0200] Both NMR and ESI-MS confirmed the presence of the oxadiazole silane compound of formula (Ib). The theoretical molar mass is 352 g / mol.
[0201] The synthesis of the above-described azole silane compounds of formula (Ib) was additionally carried out at varying molar ratios between the azole compound of formula (III) and the silane compound of formula (IV), such as molar ratios of 1:1.1 and 1:0.9.
[0202] 3) Synthesis of azole silane compound of formula (Ib) in DEGBE:
[0203] In the first step, 3.36 g (28.4 mmol) of 5-amino-4H-1,2,4-triazole-3-thiol (oxazole compound of formula (III) wherein X represents NH 2 and Y represents NH) is suspended in 35 ml of diethylene glycol monobutyl ether (DEGBE) and an azole suspension is obtained.
[0204] In the second step, 6.91 g (28.4 mmol) of 3-glycidyloxypropyltrimethoxysilane (silane compound of formula (IV) wherein R represents CH 3 and n is 3) dissolved in 10 ml of DEGBE was added to the azole suspension. Thus, a reaction suspension was obtained.
[0205] In the third step, the reaction suspension is heated to 80° C. for 15 hours. During this period, the suspension becomes a clear solution, which indicates that the azole compound has been completely used up. Afterwards, a reaction product with a concentration of about 18% by weight in DEGBE is obtained. The product thus obtained does not contain any halide at all and can be used without further purification. In addition, there is no need to change or remove the solvent as described, for example, in Examples 1 and 2 above.
[0206] ESI-MS confirmed the formation of compounds containing three methoxy groups attached to the silicon atom. In addition, compounds containing one, two or three DEGBE moieties instead of individual methoxy groups have been identified.
[0207] 4) Synthesis of azole silane compound of formula (x) in DEGBE:
[0208]
[0209] The synthetic procedure as described in Example 3 for the synthesis of oxadiazole silane compounds of formula (Ib) was carried out, but using 3-mercapto-1,2,4-triazole instead of 5-amino-4H-1,2,4-triazole-3-thiol.
[0210] 5) Synthesis of azole silane compound of formula (y):
[0211]
[0212] 1.88 g (16.2 mmol) of 5-amino-4H-1,2,4-triazole-3-thiol was added to 30 ml of DMF. Then a solution of 3.5 g (16.2 mmol) (3-isocyanatopropyl) trimethoxysilane in 10 ml of DMF was added dropwise. After addition, the reaction mixture was heated to 60 ° C for 6 hours. The solvent was then removed via vacuum. Thus, 5.4 g of the product was obtained as a light yellow viscous oil, which was subsequently dissolved in 21.6 g of DEGBE to obtain a 20 wt % solution.
[0213] B) Sample preparation
[0214] Samples 1 to 8 (each sample comprising several identical specimens) were prepared as follows (see also summary in Table 1 below):
[0215] Step (i): providing a substrate having at least one surface with a copper surface:
[0216] A copper foil (150 mm x 75 mm x 35 μm, provided by Changchun, China) having a copper surface was used. The copper foil was used without a substrate in the examples under simplified laboratory conditions.
[0217] Step (ia): Clean the copper surface with an etching cleaning solution:
[0218] In the first step, a sulfuric acid / H2O solution containing 180 ml / L SoftClean UC168, 200 ml / L Cupra EtchStarter, 75 ml / L Hydrox (all products from Atotech) and 545 ml / L deionized water was used. 2 O 2 The solution cleaned the copper surfaces of all copper foils of samples 1 to 8 at 30° C. for 30 seconds to obtain an etched clean copper surface. Etching cleaning removes heavy oxides and other compounds, such as protective layers and / or anti-corrosion agents and / or surfactants. After etching cleaning, the etched clean copper surface was rinsed with water for about 30 seconds. Thus, an etched clean and rinsed copper surface was obtained.
[0219] Since commercially available copper foil has a protective layer on the copper surface, this step must be performed under laboratory conditions to remove the protective layer.
[0220] Step (ic): Treat the copper surface with an alkaline aqueous solution:
[0221] In the second step, 100 mL / L The copper surfaces of all substrates of samples 1 to 4, 6, 7 and 8 were treated with an aqueous solution of Cleaner ALK (alkaline aqueous solution, 50°C, 30 seconds). After treatment, the treated copper surfaces of all copper foils were rinsed with cold water for about 30 seconds. The copper surface of the copper foil of sample 5 was not treated in this step.
[0222] Step (ii): contacting the copper surface with an azole silane compound of formula (I) and an azole silane oligomer:
[0223] The copper surfaces of all substrates of samples 2 to 8 were immersed in a freshly prepared coating solution containing about 1 wt% of an azole silane compound and diethylene glycol monobutyl ether (DEGBE) and deionized water as solvents at 25°C for 60 seconds. The pH of the coating solution was 7 (adjusted with sulfuric acid). Three different coating solutions were prepared, each containing a different azole silane compound:
[0224] For samples 2, 5 and 6: the oxadiazole silane compound of formula (Ib) synthesized as in Example 3
[0225] For sample 3: the oxadiazole silane compound of formula (x) synthesized as in Example 4
[0226] For samples 4 and 7: 3-amino-5-[6-(trimethoxysilyl)hexylthio]-1,2,4-triazole as described in Examples 1 to 4 of US 2016 / 0368935 A1
[0227] For Sample 8: the compound of formula (y) as disclosed in formula (Ia-7) of JP 2014-240522 A was used.
[0228] Then, the resulting copper surfaces of all copper foils were rinsed with cold water for about 30 seconds and dried. Thus, the silanized and dried copper surfaces of all copper foils of Samples 2 to 8 were obtained.
[0229] Step (ii-a): Annealing:
[0230] The copper foils of Samples 1 to 8 containing silanized copper surfaces were then annealed at 130° C. for 30 minutes to remove residual moisture from the surface. These substrates containing copper surfaces were subsequently subjected to lamination into build-up films (see below).
[0231] Step (iii): Applying an organic material to the copper surface of the substrate:
[0232] In the lamination step, an insulating film (Ajinomoto stacked film GXT31 in samples 1 to 5 and 8 or Ajinomoto stacked film GZ41 in samples 6 and 7) was vacuum laminated onto the copper foil of all samples by using a vacuum laminator in a clean room at a room temperature in the range of 20 to 25°C and a relative humidity of 50 to 60%.
[0233] The conditions of vacuum lamination were as follows: 100° C., vacuum: 30 seconds at 3 hPa, pressure: 30 seconds at 0.5 MPa.
[0234] After lamination, a laminated copper surface is obtained.
[0235] Table 1. Overview of sample design
[0236]
[0237] * "Silane treatment" is a chemical treatment of the copper surface with an organic compound (attaching silane to the cleaned copper surface)
[0238] # Compare samples
[0239] Adhesion evaluation via peel strength test:
[0240] For each sample (1 to 8) obtained after lamination, the peel strength was determined:
[0241] (1) Initially,
[0242] (2) After 96 hours of HAST (HAST conditions: 130°C, 85% rh, HAST chamber: EHS-221M).
[0243] To determine the peel strength, several strip-shaped segments were prepared from each sample by adhering the respective copper foil to a rigid board (same size as the copper foil) in such a manner that the rigid board faced the insulating film. Thus, a copper surface with a structurally reinforced insulating film was obtained.
[0244] The obtained copper surface with the structurally enhanced insulating film was then cured in an oven at 190° C. for 90 minutes.
[0245] Afterwards, each copper surface with the structurally reinforced insulating film was cut into the strip-shaped segments (10 x 100 mm, Bugard drilling / routing).
[0246] The strip segments were subjected to a peel force measuring machine (Zwick Instruments Z010) to individually evaluate the peel strength required to delaminate the copper surface from its respective structurally reinforced insulating film (angle: 90°, speed: 50 mm / min). In general, the higher the peel strength required to avoid delamination, the better the adhesion.
[0247] The peel strengths of Samples 2 to 8 are shown in Table 2 below.
[0248] Table 2, peel strength, in N / cm:
[0249]
[0250] The initial peel strength of Comparative Samples 4, 7 and 8 is higher than that of Samples 2 and 6 according to the present invention, but the peel strength of the comparative examples drops sharply after HAST, while the peel strength of Samples 2 and 6 remains almost constant.
[0251] The peel strength value of Sample 1 is lower than the peel strength value of Example 2. The peel strength value of Sample 3 is lower than the peel strength values of Examples 2 and 6.
[0252] Although sample 8 shows a relatively acceptable initial peel strength, unacceptable decline is observed after HAST. In addition, formula (y) azole silane compound seems to be generally obviously unstable. After synthesis, obvious precipitation occurs, particularly if the azole silane compound is stored under a strongly alkaline pH condition (e.g., pH 12). For storage purposes, a pH of 12 is generally applied to the formula (I) azole silane compound to minimize the premature polymerization of the silane functional group. However, it seems that under this strongly alkaline condition, the amide functional group (which does not exist in the formula (I) azole silane compound) of the formula (y) azole silane compound undergoes obvious decomposition. In addition, even in pH 7 (generally ensuring stable silane coating) and with the coating solution of the azole silane compound of about 1 % by weight working concentration, obvious precipitation is observed again. Therefore, formula (y) azole silane compound seems to be unsuitable for long-term use in commercial products / applications.
Claims
1. A method for increasing the adhesion strength between the surface of a metal, a metal alloy or a metal oxide and the surface of an organic material, the method comprising the following steps in this order: (i) providing a substrate, at least one side of which comprises the metal, metal alloy or metal oxide, (ii) contacting at least a portion of the metal, metal alloy or metal oxide with A) Azosilane compound of formula (I) in X stands for NH 2 NH(NH 2 )、NH(NHU)、SH、SCH 3 、OCH 3 , NHU or SU, Y represents NH, N(NH 2 ), N(NHU) or S, U independently represents CH 2 -CH(OH)-CH 2 -O-(CH 2 ) n -Si(OR) 3 , R is independently (CH 2 -CH 2 -O) m -Z, where independently n is an integer between 1 and 12, m is 0, 1, 2, 3 or 4, and Z represents H or C1 to C5 alkyl, and / or B) an azole silane oligomer obtained by reacting the azole silane compounds of formula (I) with each other in the presence of water so that the azole silane oligomer comprises at least one silicon-oxygen-silicon moiety, wherein in the compound of formula (I) used in the reaction to form the azole silane oligomer X represents H, CH 3 NH 2 NH(NH 2 )、NH(NHU)、SH、SCH 3 、OCH 3 , NHU or SU, and Y and U have the meanings given above, and (iii) applying the organic material so that the at least a portion of the metal, metal alloy or metal oxide that was in contact with the azole silane compound and / or the azole silane oligomer during step (ii) is in contact with the applied organic material. 2 . The method according to claim 1 , wherein an aqueous solution of the azole silane compound of formula (I) and / or the azole silane oligomer is used in step (ii).
3. The method according to claim 2, wherein the aqueous solution further comprises one or more than one water-miscible organic solvent.
4. The method of claim 3, wherein the one or more than one water-miscible organic solvent comprises a water-miscible organic solvent selected from the group consisting of C1 to C4 alcohols, glycol ethers, and mixtures thereof.
5. The method of claim 3, wherein the one or more than one water-miscible organic solvent comprises a water-miscible organic solvent selected from the group consisting of - C1 to C3 alcohols, -HO-(CH 2 -CH 2 -O) m -Z, where m is 1, 2, 3, or 4, and Z represents a C1 to C5 alkyl group, and mixtures thereof. The method according to claim 5 , wherein m is 1 or 2.
7. The method according to claim 5, wherein said Z represents a C3 to C5 alkyl group.
8. The method of claim 3, wherein the one or more than one water-miscible organic solvent comprises a water-miscible organic solvent selected from the group consisting of methanol, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, and mixtures thereof.
9. The method of claim 3, wherein the one or more than one water-miscible organic solvent comprises a water-miscible organic solvent selected from the group consisting of diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, and mixtures thereof.
10. The method according to any one of claims 2 to 9, wherein the total amount of the azole silane compound and the azole silane oligomer together is 5 wt% or less based on the total weight of the aqueous solution.
11. The method according to any one of claims 2 to 9, wherein the pH of the aqueous solution is in the range of 4.8 to 8.
6.
12. The method according to any one of claims 1 to 9, wherein before step (ii) The following steps are involved: (ia) contacting the at least a portion of the metal, metal alloy or metal oxide with an etch cleaning solution.
13. The method of claim 12, wherein the etching cleaning solution contains one or more than one acid and / or one or more than one oxidizing agent.
14. The method of claim 12, wherein the etch cleaning solution contains a mixture of an inorganic acid and a peroxide.
15. The method according to any one of claims 1 to 9, wherein before step (ii) The following steps are involved: (ib) contacting the at least a portion of the metal, metal alloy or metal oxide with an etching cleaning solution.
16. The method according to any one of claims 1 to 9, wherein before step (ii) The following steps are involved: (ic) contacting the at least a portion of the metal, metal alloy or metal oxide with an alkaline aqueous solution.
17. A method according to any one of claims 1 to 9, wherein the organic material applied in step (iii) is an organic polymer.
18. A method according to any one of claims 1 to 9, wherein in step (iii) the organic material is applied by laminating the organic material onto at least the contact portion of the metal, metal alloy or metal oxide.
19. The method according to any one of claims 1 to 9, comprising after step (iii) the further step of: (iv) subjecting the substrate and the organic material to a temperature in the range of 142°C to 420°C.
20. The method of any one of claims 1 to 9, wherein after step (ii), the at least a portion of the metal, metal alloy or metal oxide is rinsed.
21. The method of claim 12, wherein after step (ia), the at least a portion of the metal, metal alloy or metal oxide is rinsed.
22. The method of claim 15, wherein after step (ib), the at least a portion of the metal, metal alloy or metal oxide is rinsed.
23. The method of claim 16, wherein after step (ic), the at least a portion of the metal, metal alloy, or metal oxide is rinsed.
24. The method of any one of claims 1 to 9, wherein after step (ii), the at least a portion of the metal, metal alloy or metal oxide is dried.
25. The method of claim 12, wherein after step (ia), the at least a portion of the metal, metal alloy, or metal oxide is dried.
26. The method of claim 15, wherein after step (ib), the at least a portion of the metal, metal alloy or metal oxide is dried.
27. The method of claim 16, wherein after step (ic), the at least a portion of the metal, metal alloy, or metal oxide is dried.
28. The method of any one of claims 1 to 9, wherein the metal, metal alloy, or metal oxide is copper, aluminum, titanium, nickel, tin, iron, silver, gold, an alloy comprising at least one of the foregoing metals, or a metal oxide of at least one of the foregoing metals.