Moving blade positioning and clamping device and laser cladding repair method for blade crown water erosion area

Through the moving blade positioning and clamping device and the laser cladding repair method of HTC1 alloy powder, the problem of large residual stress and deformation after repairing the water-corroded area of ​​the blade is solved, the repair efficiency and performance are improved, and an efficient and economical repair effect is achieved.

CN113510396BActive Publication Date: 2024-10-01HARBIN TURBINE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110930295.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-13
Publication Date
2024-10-01
Estimated Expiration
2041-08-13

AI Technical Summary

Technical Problem

The existing technology has residual stress, deformation and large heat-affected zone when repairing the water-corroded area of ​​the blade, and the comprehensive performance of the laser cladding repair method is poor.

Method used

The moving blade positioning and clamping device and the laser cladding repair method of the water-eroded area of ​​the blade crown are used. HTC1 alloy powder and the moving blade positioning and clamping device are used to clamp the blade. The water-eroded area of ​​the blade is repaired through laser cladding, combined with mechanical processing and fitter work. Grinding, inspection and heat treatment.

Benefits of technology

It significantly reduces the residual stress and deformation of the repaired blade, improves the comprehensive performance of the cladding joint, has low cost, good water erosion resistance, and high repair efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113510396B_ABST
    Figure CN113510396B_ABST
Patent Text Reader

Abstract

A positioning and clamping device for moving blades and a laser cladding repair method for water erosion areas of blade crowns. Specifically, it relates to a laser cladding repair method. The present invention is to solve the problems that the existing methods for repairing water erosion areas of blades have large residual stress, deformation and heat-affected zone of the blades after repair, and the existing laser cladding repair methods have poor comprehensive performance. The mechanical processing procedure removes the water erosion layer in the water erosion area of ​​the blade crown, and the machined area of ​​the blade crown is clad by a laser cladding method and HTC1 alloy powder; the quality of the cladding area and the heat-affected zone of the machined area of ​​the blade crown is tested; the blade is machined and the machined cladding area of ​​the blade crown is bench-ground, and the blade in the machined area is subjected to insulation and aging heat treatment; the hardness of the cladding in the machined area of ​​the blade crown is tested, and the Rockwell hardness of the cladding in the machined area of ​​the blade crown is 35-55, and the processing is completed. Used for repairing water erosion areas of blade crowns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser cladding repair, in particular to a moving blade positioning and clamping device and a laser cladding repair method for a blade crown water erosion area. Background Art

[0002] The existing technology uses common welding methods such as argon arc welding and plasma welding to repair blades with large residual stress, deformation and heat-affected zone. The cost of using alloy powders with high hardness, wear resistance and corrosion resistance such as cobalt-based alloy components is high. In addition, the chemical composition, mechanical properties and physical properties of cobalt-based alloys are very different from those of the blade body. The comprehensive performance of the cladding joint formed after laser cladding is poor. The laser cladding method for repairing the water erosion area of ​​the blade is currently in the research and development stage.

[0003] In summary, the existing methods for repairing water erosion areas of blades have problems such as large residual stress, deformation and heat-affected zone of the blades after repair, and the existing laser cladding repair methods have problems such as poor overall performance. Summary of the invention

[0004] The present invention aims to solve the problems that the prior art methods for repairing the water erosion area of ​​the blade have large residual stress, deformation and heat affected zone after repair, and the prior art laser cladding repair method has poor overall performance. A moving blade positioning and clamping device and a laser cladding repair method for the water erosion area of ​​the blade crown are adopted.

[0005] The technical solution of the present invention is:

[0006] A moving blade positioning support device comprises a blade crown positioning seat, two hexagonal clamping screws, a blade crown inner diameter positioning block and two hexagon socket screws;

[0007] The blade crown positioning seat is vertically fixed on the machine tool through a pressing plate;

[0008] The leaf crown positioning seat includes a rectangular seat, a trapezoidal seat and a base;

[0009] A rectangular seat and a trapezoidal seat are vertically welded at both ends of the base, and the three are integrated. The vertical surface of the rectangular seat and the inclined surface of the trapezoidal seat are arranged corresponding to each other, and the rectangular seat, the trapezoidal seat and the base form a notch, and the crown of the blade is arranged inside the notch;

[0010] The blade crown inner diameter positioning block is arranged between the rectangular seat and the trapezoidal seat, and the upper end surface of the base is threadedly connected to the blade crown inner diameter positioning block through two hexagon socket screws;

[0011] Two hexagonal clamping screws are arranged in sequence from top to bottom along the vertical direction on the upper part of the rectangular seat, and one end of the two hexagonal clamping screws extends from the outer end surface of the rectangular seat through the inner end surface of the rectangular seat to the inside of the notch.

[0012] A laser cladding repair method for a blade crown water erosion area comprises the following steps:

[0013] Step 1: Pack the leaves;

[0014] Reassemble the disassembled blades in the order of the original blades and mark the blades;

[0015] Step 2, grouping the packaged leaves;

[0016] After marking the leaves in step 1, detect the key morphological dimensions of the water erosion areas of all the leaf crowns, and group the leaves into 1-5 groups according to the key morphological dimensions;

[0017] Step 3: Remove the water erosion layer;

[0018] According to the grouping information of the key morphological dimensions of the water erosion area of ​​the blade crown and the size of the laser cladding nozzle, the morphology and machining program for machining are formulated, the blade crown is clamped by the blade crown positioning seat 1 in the moving blade positioning support device, and then the end of the blade root is placed on the blade root intermediate pad 6, and the water erosion layer of the water erosion area of ​​the blade crown is removed according to the machining program;

[0019] Step 4: Check whether the water erosion layer is completely removed;

[0020] After the water erosion layer in the water erosion area of ​​the blade crown is removed by machining according to the machining procedure in step 3, a penetrant flaw detection method is used to confirm whether the water erosion layer in the water erosion area of ​​the blade crown is completely removed;

[0021] If the erosion layer in the erosion area of ​​the blade crown is completely removed, the erosion depth is 1mm-20mm, the erosion angle is 1°-90°, the remaining thickness of the crown on both sides of the erosion area of ​​the blade crown is 1mm-20mm, the penetration flaw detection standard is NB / T47013.5, and the acceptance level is Level I;

[0022] If the water erosion layer in the water erosion area of ​​the blade crown is not completely removed, repeat step 3 until the water erosion layer in the water erosion area of ​​the blade is completely removed and meets the standard;

[0023] Step 5: Cladding the machined area;

[0024] After the water erosion layer in the water erosion area of ​​the blade crown in step 4 is completely removed and meets the standard, the machined area of ​​the blade crown is clad by using the laser cladding method and HTC1 alloy powder;

[0025] Step 6: Detect the area after cladding;

[0026] After the machined area of ​​the blade crown is clad in step 5, the quality of the clad area and the heat affected zone of the machined area of ​​the blade crown is inspected by using a radiographic flaw detection method and a penetrant flaw detection method;

[0027] The test results are: the radiographic flaw detection standard is NB / T47013.2, the acceptance level is greater than or equal to Level II, the penetrant flaw detection standard is NB / T47013.5, the acceptance level is Level I, then the cladding of the machined area of ​​the blade crown meets the standard;

[0028] Step 7: Perform penetrant testing on the blades in the machining area;

[0029] After the cladding of the machined area of ​​the blade crown in step 6 meets the standard, the blade is machined according to the size of the original blade, the machined cladding area of ​​the blade crown is grinded by benchwork, and the blade in the machined area is subjected to penetrant flaw detection;

[0030] The test results are: According to the NB / T47013.5 standard, the acceptance level is Level I, and the blades in the machining area meet the standards;

[0031] Step 8: Perform heat preservation and aging heat treatment on the blades in the machining area;

[0032] Step nine, testing the hardness of the cladding in the machining area of ​​the blade crown;

[0033] In step eight, after the blade in the machined area is subjected to insulation and aging heat treatment, the hardness of the cladding in the machined area of ​​the blade crown is tested. The Rockwell hardness of the cladding in the machined area of ​​the blade crown is 35-55, which meets the product requirements and the processing is completed.

[0034] Compared with the prior art, the present invention has the following effects:

[0035] 1. The movable blades in the movable blade positioning and clamping device and the laser cladding repair method for the blade crown water erosion area of ​​the present invention are 0Cr15Ni7Cu2MoNbVN movable blades. The present invention adopts the movable blade positioning and clamping device to clamp the blades, and adopts the laser cladding method to repair the blades. The residual stress, deformation and heat-affected zone mass of the blades are small. The present invention adopts HTC1 alloy powder laser cladding to repair the blades, and the blades obtain a cladding layer with higher hardness than the substrate and better water erosion resistance.

[0036] 2. The chemical composition, mechanical properties and physical properties of the HTC1 alloy powder of the present invention are similar to those of the substrate, and the comprehensive performance of the cladding joint formed after laser cladding is better than that of the cladding joint formed by other alloy powders. The HTC1 alloy powder of the present invention is low-cost compared to the commonly used cobalt-based alloy powder, and the mechanical processing method for removing the water erosion area of ​​the blade is highly efficient.

[0037] 3. The cost of repairing a blade by the method of the present invention is only one tenth of that of a new blade, and the economical efficiency is good. The present invention solves the problem that the repair method of the water erosion area of ​​the blade has large residual stress, deformation and heat affected zone after repair, and the laser cladding repair method of the prior art has poor comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a front view of the moving blade positioning support device of the present invention installed with an unrepaired blade;

[0039] Figure 2 is a top view of the moving blade positioning support device of the present invention installed with an unrepaired blade;

[0040] Figure 3 is a side view of the moving blade positioning support device of the present invention installed with an unrepaired blade;

[0041] Figure 4 This is a front view of the intermediate pad of the blade root of the present invention;

[0042] Figure 5 is a top view of the intermediate pad of the blade root of the present invention;

[0043] Figure 6 is a side view of the blade root intermediate pad of the present invention;

[0044] Figure 7 is a schematic diagram of the water erosion area of ​​the canopy of a blade of the present invention;

[0045] Figure 8 It is a schematic diagram of key morphological dimensions for machining formulated by the present invention based on key morphological dimensions of the water erosion area of ​​the blade crown and size information of the laser cladding nozzle;

[0046] Fig. 9 It is a schematic diagram of the cladding of the water erosion area of ​​the blade crown after laser cladding of the present invention. DETAILED DESCRIPTION

[0047] Specific implementation method 1: Combination Figures 1 to 6 The present embodiment is described as a moving blade positioning support device, which comprises a blade crown positioning seat 1, two hexagonal clamping screws 2, a blade crown inner diameter positioning block 3 and two hexagon socket screws 4;

[0048] The blade crown positioning seat 1 is vertically fixed on the machine tool through a pressing plate;

[0049] The blade crown positioning seat 1 includes a rectangular seat 1-1, a trapezoidal seat 1-2 and a base 1-3;

[0050] The two ends of the base 1-3 are respectively vertically welded with a rectangular seat 1-1 and a trapezoidal seat 1-2, and the three are integrated. The vertical surface of the rectangular seat 1-1 and the inclined surface of the trapezoidal seat 1-2 are arranged corresponding to each other, and the rectangular seat 1-1, the trapezoidal seat 1-2 and the base 1-3 form a notch 1-4, and the crown of the blade is arranged inside the notch 1-4;

[0051] The blade crown inner diameter positioning block 3 is arranged between the rectangular seat 1-1 and the trapezoidal seat 1-2, and the upper end surface of the base 1-3 is threadedly connected to the blade crown inner diameter positioning block 3 through two hexagon socket screws 4;

[0052] Two hexagonal clamping screws 2 are arranged in sequence from top to bottom along the vertical direction on the upper part of the rectangular seat 1-1, and one end of the two hexagonal clamping screws 2 extends from the outer end surface of the rectangular seat 1-1 through the inner end surface of the rectangular seat 1-1 to the inside of the notch 1-4.

[0053] This setting can ensure that the spatial position of the blade is basically the same after clamping, the positioning reference is the same, and the morphology of the area to be clad is basically the same after machining, ensuring the repeatability of machining and subsequent laser cladding forming.

[0054] Specific implementation method 2: Combination Figure 1 This embodiment is described. This embodiment also includes a cylindrical pin 5. The cylindrical pin 5 is passed through the lower part of the trapezoidal seat 1-2 in the horizontal direction, and the cylindrical pin 5 is located obliquely above the blade crown inner diameter positioning block 3. This arrangement is to tighten the blade crown of the blade through the cylindrical pin 5, which is conducive to mechanical processing and subsequent laser cladding operations. The rest is the same as the specific embodiment 1.

[0055] Specific implementation method three: Combination Figures 4 to 6 This embodiment is described, and it also includes a blade root intermediate block 6, which is vertically fixed on the machine tool through a pressing plate, and is located on one side of the blade crown positioning seat 1, and the end of the blade root of the blade is placed on the blade root intermediate block 6. Other parts are the same as the specific embodiment 1 or 2.

[0056] Specific implementation method four: Combination Figures 4 to 6 This embodiment is described. The blade root intermediate pad 6 of this embodiment is L-shaped. The upper end surface of the vertical section of the blade root intermediate pad 6 is set to be an arc shape. The blade root end of the blade to be repaired is set on the arc shape. The horizontal section of the blade root intermediate pad 6 is processed with two mutually symmetrical grooves. This arrangement ensures that the blade does not move during the machining process, which is conducive to machining and ensuring the machining size. The rest is the same as the specific embodiment one, two or three.

[0057] Specific implementation method five: Combination Figures 7 to 9The present embodiment is described. The present embodiment is a laser cladding repair method for a blade crown water erosion area, which comprises the following steps:

[0058] Step 1: Pack the leaves;

[0059] Reassemble the disassembled blades in the order of the original blades and mark the blades;

[0060] Step 2, grouping the packaged leaves;

[0061] After marking the leaves in step 1, detect the key morphological dimensions of the water erosion areas of all the leaf crowns, and group the leaves into 1-5 groups according to the key morphological dimensions;

[0062] Step 3: Remove the water erosion layer;

[0063] According to the grouping information of the key morphological dimensions of the water erosion area of ​​the blade crown and the size of the laser cladding nozzle, the morphology and machining program for machining are formulated, the blade crown is clamped by the blade crown positioning seat 1 in the moving blade positioning support device, and then the end of the blade root is placed on the blade root intermediate pad 6, and the water erosion layer of the water erosion area of ​​the blade crown is removed according to the machining program;

[0064] Step 4: Check whether the water erosion layer is completely removed;

[0065] After the water erosion layer in the water erosion area of ​​the blade crown is removed by machining according to the machining procedure in step 3, a penetrant flaw detection method is used to confirm whether the water erosion layer in the water erosion area of ​​the blade crown is completely removed;

[0066] If the erosion layer in the erosion area of ​​the blade crown is completely removed, the erosion depth is 1mm-20mm, the erosion angle is 1°-90°, the remaining thickness of the crown on both sides of the erosion area of ​​the blade crown is 1mm-20mm, the penetration flaw detection standard is NB / T47013.5, and the acceptance level is Level I;

[0067] If the water erosion layer in the water erosion area of ​​the blade crown is not completely removed, repeat step 3 until the water erosion layer in the water erosion area of ​​the blade is completely removed and meets the standard;

[0068] Step 5: Cladding the machined area;

[0069] After the water erosion layer in the water erosion area of ​​the blade crown in step 4 is completely removed and meets the standard, the machined area of ​​the blade crown is clad by using the laser cladding method and HTC1 alloy powder;

[0070] Step 6: Detect the area after cladding;

[0071] After the machined area of ​​the blade crown is clad in step 5, the quality of the clad area and the heat affected zone of the machined area of ​​the blade crown is inspected by using a radiographic flaw detection method and a penetrant flaw detection method;

[0072] The test results are: the radiographic flaw detection standard is NB / T47013.2, the acceptance level is greater than or equal to Level II, the penetrant flaw detection standard is NB / T47013.5, the acceptance level is Level I, then the cladding of the machined area of ​​the blade crown meets the standard;

[0073] Step 7: Perform penetrant testing on the blades in the machining area;

[0074] After the cladding of the machined area of ​​the blade crown in step 6 meets the standard, the blade is machined according to the size of the original blade, the machined cladding area of ​​the blade crown is grinded by benchwork, and the blade in the machined area is subjected to penetrant flaw detection;

[0075] The test results are: According to the NB / T47013.5 standard, the acceptance level is Level I, and the blades in the machining area meet the standards;

[0076] Step 8: Perform heat preservation and aging heat treatment on the blades in the machining area;

[0077] Step nine, testing the hardness of the cladding in the machining area of ​​the blade crown;

[0078] In step eight, after the blade in the machined area is subjected to insulation and aging heat treatment, the hardness of the cladding in the machined area of ​​the blade crown is tested. The Rockwell hardness of the cladding in the machined area of ​​the blade crown is 35-55, which meets the product requirements and the processing is completed.

[0079] Specific implementation method six: Combination Figures 1 to 3 To explain this embodiment, in step 5 of this embodiment, the laser cladding method is used to clad the machined area of ​​the blade crown by coaxial powder feeding or lateral powder feeding. This setting is to more comprehensively clad the machined area of ​​the blade crown. The rest is the same as the specific embodiment 5.

[0080] Specific implementation method seven: Combination Figures 7 to 9 To illustrate this embodiment, in step 5 of this embodiment, the laser power is 1000-2000W, the powder feeding amount is 2-15g / min, the protective gas flow rate is 5-25L / min, the powder carrier gas is 2-15L / min, the defocusing amount is 2-20mm, and the linear speed is 100-1000mm / min. The rest is the same as the specific embodiment 5 or 6.

[0081] Specific implementation method eight: Combination Figures 7 to 9To explain this embodiment, in step eight of this embodiment, the blade after machining is kept warm at a temperature of 450-520° C. The rest is the same as that of the fifth, sixth or seventh embodiment.

[0082] Specific implementation method nine: Combination Figures 7 to 9 To explain this embodiment, in step eight of this embodiment, the blade after machining is subjected to aging heat treatment, and the heat preservation time of the aging treatment is 2-10 hours. The rest is the same as the specific embodiments five, six, seven or eight.

[0083] Embodiment 1;

[0084] The specific implementation steps are as follows:

[0085] Step 1: Disassemble 280 blades of the last stage of 4 circles of a unit in a power plant in the order of the original blades and pack them into 8 wooden boxes, with 34-36 blades in each box, and mark them on the box;

[0086] Step 2: Detect the key morphological dimensions of the water erosion area of ​​all blade crowns, and group them according to the key morphological dimensions, dividing the 280 blades into 4 groups;

[0087] Step three, formulate the morphology and machining procedures for mechanical processing according to the grouping information of the key morphological dimensions of the water erosion area of ​​the blade crown and the size of the laser cladding nozzle, use the crown positioning seat 1 in the moving blade positioning support device to clamp the blade crown, then place the end of the blade root on the root intermediate pad 6, and remove the water erosion layer in the water erosion area of ​​the blade crown according to the machining procedure. Use penetrant flaw detection to confirm that the water erosion layer in the water erosion area of ​​the blade crown is completely removed. When the water erosion layer in the water erosion area of ​​the blade crown is completely removed, the water erosion depth is 16mm-20mm, the water erosion angle is 35°--880°, and the remaining thickness of the crown on both sides of the water erosion area of ​​the blade crown is 5mm-15mm. The penetrant flaw detection standard is NB / T47013.5, and the acceptance level is Level I.

[0088] Step 4: Use laser cladding method to clad the machined area of ​​the blade crown by coaxial powder feeding or lateral powder feeding, and use radiographic flaw detection and penetrant flaw detection to detect the quality of the cladding area and heat-affected zone of the machined area of ​​the blade crown. The laser power is 1800W, the powder feeding amount is 8g / min, the protective gas flow rate is 20L / min, the powder carrier gas is 10L / min, the defocus is 16mm, and the line speed is 800mm / min. The radiographic flaw detection standard is NB / T47013.2, and the acceptance level is Level II. The penetrant flaw detection standard is NB / T47013.5, and the acceptance level is Level I.

[0089] Step 5: Machine the blade according to the size of the original blade and perform bench grinding on the machined cladding area of ​​the blade crown, and perform penetrant flaw detection on the blade in the machined area. According to the NB / T47013.5 standard, the acceptance level is Level I, and the blade in the machined area meets the standard;

[0090] Step 6: subject the machined blades to aging heat treatment at a holding temperature of 460° C. for 8 hours;

[0091] Step seven: Check the hardness of the cladding in the machined area of ​​the blade crown. The Rockwell hardness of the cladding in the machined area of ​​the blade crown is 35-55, which meets the product requirements and the processing is completed.

[0092] Table 1 shows the composition of HTC1 alloy powder

[0093]

[0094] Table 1

[0095] The present invention has been disclosed as above with preferred implementation cases, but it is not used to limit the present invention. Any simple modification, equivalent changes and modifications made to the above implementation cases by any professional and technical personnel who do not deviate from the content of the technical solution of the present invention and based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A moving blade positioning support device, characterized in that: It comprises a blade crown positioning seat (1), two hexagonal clamping screws (2), a blade crown inner diameter positioning block (3) and two hexagon socket screws (4); The blade crown positioning seat (1) is vertically fixed on the machine tool through a pressing plate; The blade crown positioning seat (1) comprises a rectangular seat (1-1), a trapezoidal seat (1-2) and a base (1-3); A rectangular seat (1-1) and a trapezoidal seat (1-2) are respectively vertically welded at two ends of the base (1-3), and the three are an integral part; a vertical surface of the rectangular seat (1-1) and an inclined surface of the trapezoidal seat (1-2) are arranged corresponding to each other; and the rectangular seat (1-1), the trapezoidal seat (1-2) and the base (1-3) form a notch (1-4), and a blade crown of a blade is arranged inside the notch (1-4); The blade crown inner diameter positioning block (3) is arranged between the rectangular seat (1-1) and the trapezoidal seat (1-2), and the upper end surface of the base (1-3) is threadedly connected to the blade crown inner diameter positioning block (3) via two hexagon socket screws (4); Two hexagonal clamping screws (2) are arranged in sequence from top to bottom along the vertical direction on the upper part of the rectangular seat (1-1), and one end of the two hexagonal clamping screws (2) extends from the outer end surface of the rectangular seat (1-1) through the inner end surface of the rectangular seat (1-1) to the inside of the notch (1-4); It also includes a cylindrical pin (5), which penetrates the lower part of the trapezoidal seat (1-2) in the horizontal direction, and is located obliquely above the blade crown inner diameter positioning block (3); The blade root intermediate pad (6) is vertically fixed on the machine tool through a pressing plate, the blade root intermediate pad (6) is located on one side of the blade crown positioning seat (1), and the end of the blade root of the blade is placed on the blade root intermediate pad (6); The blade root intermediate pad (6) is L-shaped, the upper end surface of the vertical section of the blade root intermediate pad (6) is arranged in an arc shape, the blade root end of the blade is arranged on the arc shape, and the horizontal section of the blade root intermediate pad (6) is processed with two mutually symmetrical grooves.

2. A laser cladding repair method for a blade crown water erosion area, characterized in that: Using the moving blade positioning support device according to claim 1 specifically comprises the following steps: Step 1: Pack the leaves; Reassemble the disassembled blades in the order of the original blades and mark the blades; Step 2, grouping the packaged leaves; After marking the leaves in step 1, detect the key morphological dimensions of the water erosion areas of all the leaf crowns, and group the leaves into 1-5 groups according to the key morphological dimensions; Step 3: Remove the water erosion layer; The morphology and machining procedure for machining are formulated according to the grouping information of the key morphology size of the water erosion area of ​​the blade crown and the size of the laser cladding nozzle, the blade crown is clamped by the blade crown positioning seat (1) in the moving blade positioning support device, and the end of the blade root is placed on the blade root intermediate pad (6), and the water erosion layer of the water erosion area of ​​the blade crown is removed according to the machining procedure; Step 4: Check whether the water erosion layer is completely removed; After the water erosion layer in the water erosion area of ​​the blade crown is removed by machining according to the machining procedure in step 3, a penetrant flaw detection method is used to confirm whether the water erosion layer in the water erosion area of ​​the blade crown is completely removed; If the erosion layer in the erosion area of ​​the blade crown is completely removed, the erosion depth is 1mm-20mm, the erosion angle is 1°-90°, the remaining thickness of the crown on both sides of the erosion area of ​​the blade crown is 1mm-20mm, the penetration flaw detection standard is NB / T47013.5, and the acceptance level is Level I; If the water erosion layer in the water erosion area of ​​the blade crown is not completely removed, repeat step 3 until the water erosion layer in the water erosion area of ​​the blade is completely removed and meets the standard; Step 5: Cladding the machined area; After the water erosion layer in the water erosion area of ​​the blade crown in step 4 is completely removed and meets the standard, the machined area of ​​the blade crown is clad by using the laser cladding method and HTC1 alloy powder; Step 6: Detect the area after cladding; After the machined area of ​​the blade crown is clad in step 5, the quality of the clad area and the heat affected zone of the machined area of ​​the blade crown is inspected by using a radiographic flaw detection method and a penetrant flaw detection method; The test results are: the radiographic flaw detection standard is NB / T47013.2, the acceptance level is greater than or equal to Level II, the penetrant flaw detection standard is NB / T47013.5, the acceptance level is Level I, then the cladding of the machined area of ​​the blade crown meets the standard; Step 7: Perform penetrant testing on the blades in the machining area; After the cladding of the machined area of ​​the blade crown in step 6 meets the standard, the blade is machined according to the size of the original blade, the machined cladding area of ​​the blade crown is grinded by benchwork, and the blade in the machined area is subjected to penetrant flaw detection; The test results are: According to the NB / T47013.5 standard, the acceptance level is Level I, and the blades in the machining area meet the standards; Step 8: Perform heat preservation and aging heat treatment on the blades in the machining area; Step nine, testing the hardness of the cladding in the machining area of ​​the blade crown; In step eight, after the blade in the machined area is subjected to insulation and aging heat treatment, the hardness of the cladding in the machined area of ​​the blade crown is tested. The Rockwell hardness of the cladding in the machined area of ​​the blade crown is 35-55, which meets the product requirements and the processing is completed.

3. The laser cladding repair method for a blade crown water erosion area according to claim 2, characterized in that: In step five, the laser cladding method is used to clad the machined area of ​​the blade crown using coaxial powder feeding or lateral powder feeding.

4. The laser cladding repair method for a blade crown water erosion area according to claim 2 or 3, characterized in that: In step five, the laser power is 1000-2000W, the powder feeding amount is 2-15g / min, the shielding gas flow rate is 5-25L / min, the powder carrier gas is 2-15L / min, the defocusing amount is 2-20mm, and the linear speed is 100-1000mm / min.

5. The laser cladding repair method for a blade crown water erosion area according to claim 2, characterized in that: In step eight, the machined blades are kept warm at a temperature of 450-520°C.

6. The laser cladding repair method for a blade crown water erosion area according to claim 5, characterized in that: In step eight, the machined blades are subjected to aging heat treatment, and the insulation time of the aging treatment is 2-10 hours.