Pure isobutylene superposition synthesis preparation process and superposition application catalyst thereof
By using special copolymer resin balls as catalysts to control the isobutylene superposition reaction conditions, the problems of violent reactions and side reactions during the isobutylene superposition process are solved, and the production of high-purity isobutylene and a safe industrialization process are achieved.
Patent Information
- Application Number
- CN202110705635.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-06-24
AI Technical Summary
In the process of isobutylene superimposed synthesis, the reaction is violent, the heat release is huge, there are many side reactions, and the reaction depth is difficult to control, resulting in catalyst burnout and safety hazards. There is a lack of suitable high-purity isobutylene superimposed synthetic resin catalysts and safe preparation processes.
Mixed C4 is used as industrial lamination raw material, and is made of polymerized monomers such as styrene, methyl methacrylate, p-ethylstyrene, m-ethylstyrene, p-divinylbenzene and m-divinylbenzene. The copolymer resin balls are used as cation exchange resin catalysts. Through pore-forming, sulfonation and washing treatments, they form a composite application catalyst with high selectivity and stability. The reaction temperature and pressure are controlled to achieve high conversion rate and low isomerization of isobutylene. change.
The high-purity overlay synthesis of isobutylene has been achieved, with a conversion rate of 100% and diisobutylene selectivity greater than 99.5%, avoiding side reactions and catalyst deactivation, and improving reaction safety and industrial economic benefits.
Abstract
Description
Technical Field
[0001] The present patent application relates to a polymer copolymer resin catalyst, a preparation method thereof and its catalytic synthesis application in the field of petrochemical industry, and in particular to a catalyst for the synthesis of mixed carbon four isobutylene and a preparation method thereof. Background Art
[0002] Ethanol and MTBE are both oxygen-containing gasoline cleaning additives. However, according to the "Implementation Plan on Expanding the Production of Biofuel Ethanol and Promoting the Use of Ethanol Gasoline for Vehicles" jointly issued by the National Development and Reform Commission and other 15 ministries and commissions, it is required that oxygen-containing compounds shall not be artificially added to ethanol gasoline, that is, etherified components such as MTBE and etherified light gasoline can no longer be used as gasoline blending components. Therefore, one of the technical directions for the transformation of the original MTBE preparation system is to implement the industrial production of diisobutylene, i.e., isooctene, by isobutylene superposition. However, the superposition synthesis of high-purity isobutylene faces technical difficulties such as violent reaction, huge heat release, many side reactions such as trimerization, and difficult to control the reaction depth, especially the technical difficulties such as the easy occurrence of polymerization hot spots and burning of catalysts, and the easy occurrence of danger. The existing technology lacks resin catalysts suitable for the preparation of high-purity isobutylene superposition synthesis and mixed and safe preparation processes. Summary of the invention
[0003] The invention purpose of this patent application is to use mixed carbon four as industrial superposition raw material, implement low isomerization rate of n-butene and high conversion rate of isobutene, so as to obtain sufficient raw materials for subsequent n-butene production, make n-butene production have industrial economic benefits, and provide a pure isobutene superposition synthesis preparation process method and its superposition application catalyst.
[0004] The technical solution of the pure isobutylene superposition synthesis preparation process provided by the present patent application is as follows: a pure isobutylene superposition synthesis preparation process, the method uses pure isobutylene as raw material, in a fixed bed reactor filled with a superposition application catalyst, characterized in that the reaction temperature is 60°C-90°C, the reaction pressure is 1.0-1.5Mpa, and the reaction temperature is 0.5-4.0h -1 The superposition reaction is run at an air velocity of , wherein the superposition application catalyst is a cation exchange resin catalyst obtained by extracting, drying, screening, sulfonating and washing copolymer resin balls, wherein the copolymer resin balls are formed by suspension copolymerization of the following polymerization monomers in the presence of a porogen, an initiator and a dispersant: 60-80 parts by weight of styrene, 20-40 parts by weight of methyl methacrylate, 6-12 parts by weight of p-ethylstyrene, 4-8 parts by weight of m-ethylstyrene, the cross-linking agent includes 10-15 parts by weight of p-divinylbenzene and 8-12 parts by weight of m-divinylbenzene, the porogen is propylene glycol diacetate, the initiator is benzoyl peroxide, and the dispersant is alum.
[0005] One of the preferred options of the above overall technical solution is that the concentration of the pure isobutylene is not less than 99%.
[0006] In one preferred embodiment of the overall technical solution, the amount of the porogen used is 20-30% of the total mass of the monomer phase.
[0007] One of the preferred options of the above overall technical solution is that the copolymer resin balls as the sulfonated matrix have a moisture content of 5-10% after drying and a particle size screening range of 0.3-0.9 mm.
[0008] One of the preferred options of the above-mentioned overall technical solution is that the water content of the superimposed catalyst is 50%±2%.
[0009] One preferred option of the above overall technical solution, the sulfonation is as follows: the copolymer resin balls are immersed in a sulfonating agent in a saturated solution of dichloroethane or dichloropropylene in sulfur trioxide, wherein the mass ratio of the copolymer resin balls to sulfur trioxide is 1:2~5, stirred for 0.5~2h to fully mix the copolymer resin balls and the sulfonating agent, then reacted at a temperature of 100°C~120°C for 8~20h, cooled, and washed with water until neutral.
[0010] The present patent application also provides a superposition application catalyst for the above-mentioned pure isobutylene superposition synthesis preparation process. The superposition application catalyst is a cation exchange resin catalyst obtained by extracting, drying, screening, sulfonating and washing copolymer resin balls, wherein the copolymer resin balls are formed by suspension copolymerization of the following polymerization monomers in the presence of a porogen, an initiator and a dispersant: 60-80 parts by weight of the main monomer styrene, 20-40 parts by weight of methyl methacrylate, 6-12 parts by weight of p-ethylstyrene, 4-8 parts by weight of m-ethylstyrene, and the cross-linking agent includes 10-15 parts by weight of p-divinylbenzene and 8-12 parts by weight of m-divinylbenzene, and is obtained by heating suspension polymerization in a copolymerization system in which the porogen is propylene glycol diacetate, the initiator is benzoyl peroxide and the dispersant is alum.
[0011] The present patent application provides a technical solution for the preparation process of pure isobutylene superposition synthesis. The superposition catalyst is prepared by copolymerization and sulfonation of mixed monomers. In addition to conventional styrene, the polymerized monomers also include methyl methacrylate in corresponding weight portions. The addition of methyl methacrylate has one effect, which makes the polymerization more uniform, avoids the situation where styrene remains unpolymerized after all the cross-linking agent divinylbenzene is polymerized, so that the later polymerization is mainly styrene, resulting in uneven distribution of sulfonate groups, high local catalytic activity, and the isomerization of n-butene, and the occurrence of local reaction hot spots and side reactions. Another key effect is that methyl methacrylate, as a component of the polymerized monomer, interacts with the porogen in the copolymerization, so that the ester group is concentrated in the pores of the resin ball, and its steric hindrance is used to increase the difficulty of isobutylene superposition, thereby effectively inhibiting the intensity of the isobutylene superposition reaction, controlling the reaction depth, avoiding the occurrence of reaction hot spots, improving selectivity, and inhibiting the production of trimers, thereby avoiding the technical problems of high polymerization products blocking the catalyst pores and causing catalyst deactivation. The implementation of the patented technical solution of the present invention has high selectivity in the superposition synthesis preparation, and the content of trimers and higher polymers is less than 0.5%. DETAILED DESCRIPTION
[0012] Example 1
[0013] The preparation device of the pure isobutylene superposition synthesis preparation process of the present patent application is a fixed bed reactor. 400 ml of superposition application catalyst is loaded into a fixed bed reactor with an inner diameter of 50 mm and a length of 1000 mm. Pure isobutylene is used as a raw material, and the temperature is 60°C, the pressure is 1.0 MPa, and the space velocity is 0.5 h -1 The reaction is run. The concentration of pure isobutylene is not less than 99%. The composite application catalyst A used is obtained through the following preparation steps:
[0014] polymerization
[0015] 60 parts by weight of styrene, 20 parts by weight of methyl methacrylate, 6 parts by weight of p-ethylstyrene, 4 parts by weight of m-ethylstyrene, 10 parts by weight of p-divinylbenzene, 8 parts by weight of m-divinylbenzene, porogen propylene glycol diacetate, and 0.4 parts by weight of initiator benzoyl peroxide were weighed and placed in a mixing tank, stirred for 0.5 hours to make the feed liquid evenly mixed to form the oil phase; wherein, the porogen accounts for 20% of the weight of the oil phase. 300 parts by weight of water and 1.0 parts by weight of alum as a dispersant were added to the polymerization kettle, stirred and heated to 40°C, and added to the mixed monomers after they were completely dissolved. The stirring speed was adjusted to 90 rpm according to the dispersion of the monomers, and the temperature was slowly raised to 80°C. After the polymerization reaction lasted for 8 hours, the mixture was cooled and discharged, and the polymer was washed three times with hot water and cold water respectively to separate the copolymer resin balls;
[0016] Extraction, drying and sieving
[0017] Add copolymer resin balls into the extraction kettle, add excess solvent into the distillation kettle and heat it to evaporate the solvent in the kettle and flow into the extraction kettle after condensation. The solvent partially dissolves the porogen in the kettle and the formed mixed solution remains in the extraction kettle. When the liquid level reaches a certain height, it is put into the distillation kettle and heated and evaporated again. This is repeated 6 times and the porogen remaining on the copolymer resin balls is extracted cleanly. Place the extracted copolymer resin balls in a ventilated place and dry them to a water content of 5%. Sieve the copolymer resin balls with a particle size of 0.3~0.9mm as the sulfonated matrix.
[0018] Sulfonation
[0019] The extracted copolymer resin balls were immersed in a saturated sulfur trioxide solution sulfonating agent, wherein the mass ratio of the copolymer resin balls to sulfur trioxide was 1:2, and stirred for 0.5 hours to fully mix the white balls and the sulfonating agent, and then the temperature was controlled to 100°C for 8 hours to terminate the reaction, cool, and place in a water washing column to rinse to neutrality, and separate the resin with a water content of 50%±2%, which is the catalyst for the superposition synthesis of this superposition preparation method. Superposition reaction results: high isobutylene conversion rate is 100%, and diisobutylene selectivity is greater than 99.5%.
[0020] Example 2
[0021] Take 400 ml of the composite application catalyst B and load it into a fixed bed reactor with an inner diameter of 50 mm and a length of 1000 mm. Use pure isobutylene as the raw material and heat it at a temperature of 90°C, a pressure of 1.5 MPa, and a space velocity of 4 h -1 The reaction is run. The concentration of pure isobutylene is not less than 99%. The composite application catalyst B used is obtained by the following preparation steps:
[0022] polymerization
[0023] 80 parts by weight of styrene, 40 parts by weight of methyl methacrylate, 12 parts by weight of p-ethylstyrene, 8 parts by weight of m-ethylstyrene, 15 parts by weight of p-divinylbenzene, 12 parts by weight of m-divinylbenzene, porogen propylene glycol diacetate, and 1.0 part by weight of initiator benzoyl peroxide were weighed and placed in a mixing tank, stirred for 0.5 hours to make the feed liquid evenly mixed to form the oil phase; wherein, the porogen accounts for 30% of the weight of the oil phase. 400 parts by weight of water and 2.0 parts by weight of alum as a dispersant were added to the polymerization kettle, stirred and heated to 50°C, and added to the mixed monomers after they were completely dissolved, and the stirring speed was adjusted to 100 rpm according to the dispersion of the monomers, and the temperature was slowly raised to 80°C. After the polymerization reaction lasted for 18 hours, the material was cooled and discharged, and the polymer was washed three times with hot water and cold water respectively to separate the copolymer resin balls;
[0024] Extraction, drying and sieving
[0025] Add copolymer resin balls into the extraction kettle, add excess solvent into the distillation kettle and heat it to evaporate the solvent in the kettle, and then flow into the extraction kettle after condensation. The solvent partially dissolves the porogen in the kettle, and the formed mixed solution remains in the extraction kettle. When the liquid level reaches a certain height, it is put into the distillation kettle and heated and evaporated again. This is repeated 20 times, and the porogen remaining on the copolymer resin balls is extracted cleanly; the extracted copolymer resin balls are placed in a ventilated place, dried to a water content of 10%, and the copolymer resin balls with a particle size of 0.3~0.9mm are sieved as sulfonated matrix.
[0026] Sulfonation
[0027] The extracted copolymer resin balls were immersed in a saturated sulfur trioxide solution sulfonating agent, wherein the mass ratio of the copolymer resin balls to sulfur trioxide was 1:5, and stirred for 2.0 hours to fully mix the white balls and the sulfonating agent, and then the temperature was controlled to be 120°C for reaction for 20 hours, the reaction was terminated, cooled, and placed in a water washing column to be rinsed to neutrality, and the resin with a water content of 50%±2% was separated, which was the catalyst for the superposition synthesis of this superposition preparation method. Superposition reaction results: the isobutylene conversion rate was 100%, and the diisobutylene selectivity was higher than 99.5%.
[0028] Example 3
[0029] Take 400ml of the composite application catalyst C and load it into a fixed bed reactor with an inner diameter of 50mm and a length of 1000mm. Use pure isobutylene as the raw material. The reaction temperature in the fixed bed reactor is 80℃, the pressure is 1.2Mpa, and the space velocity is 2.0h -1 The reaction is run. The concentration of pure isobutylene is not less than 99%. The composite application catalyst C used is obtained through the following preparation steps:
[0030] polymerization
[0031] 70 parts by weight of styrene, 30 parts by weight of methyl methacrylate, 8 parts by weight of p-ethylstyrene, 6 parts by weight of m-ethylstyrene, 12 parts by weight of p-divinylbenzene, 10 parts by weight of m-divinylbenzene, porogen propylene glycol diacetate, and 0.6 parts by weight of initiator benzoyl peroxide were weighed and placed in a mixing tank, stirred for 0.5 hours to make the feed liquid evenly mixed to form the oil phase; wherein, the porogen accounts for 25% of the weight of the oil phase. 350 parts by weight of water and 1.5 parts by weight of alum as a dispersant were added to the polymerization kettle, stirred and heated to 45°C, and added to the mixed monomers after they were completely dissolved. The stirring speed was adjusted to 95 rpm according to the dispersion of the monomers, and the temperature was slowly raised to 80°C. After the polymerization reaction lasted for 12 hours, the material was cooled and discharged, and the polymer was washed three times with hot water and cold water respectively to separate the copolymer resin balls;
[0032] Extraction, drying and sieving
[0033] Add copolymer resin balls into the extraction kettle, add excess solvent into the distillation kettle and heat it to evaporate the solvent in the kettle and flow into the extraction kettle after condensation. The solvent partially dissolves the porogen in the kettle and the formed mixed solution remains in the extraction kettle. When the liquid level reaches a certain height, it is put into the distillation kettle and heated and evaporated again. This is repeated 15 times and the porogen remaining on the copolymer resin balls is extracted cleanly. Place the extracted copolymer resin balls in a ventilated place and dry them to a water content of 8%. Sieve the copolymer resin balls with a particle size of 0.3~0.9mm as the sulfonated matrix.
[0034] Sulfonation
[0035] The extracted copolymer resin balls were immersed in a saturated sulfur trioxide solution sulfonating agent, wherein the mass ratio of the copolymer resin balls to sulfur trioxide was 1:3, and stirred for 1.0h to fully mix the copolymer resin balls and the sulfonating agent, and then the temperature was controlled to 110°C for 15h to terminate the reaction, cool, and place in a water washing column to rinse to neutrality, and separate the resin with a water content of 50%±2%, which is the catalyst for the superposition synthesis of this superposition preparation method. Superposition reaction results: the isobutylene conversion rate is 100%, and the diisobutylene selectivity is higher than 99.5%.
Claims
1. A pure isobutylene superposition synthesis preparation process, characterized in that: The method uses pure isobutylene as a raw material, is carried out in a fixed bed reactor filled with a superposition application catalyst, and performs superposition reaction at a reaction temperature of 60°C-90°C, a reaction pressure of 1.0-1.5Mpa, and a space velocity of 0.5-4.0h-1, wherein the superposition application catalyst is a cation exchange resin catalyst obtained by extracting, drying, screening, sulfonating, and washing copolymer resin balls, wherein the copolymer resin balls are prepared by the following polymerization monomers in the presence of a crosslinking agent, a porogen, and an initiator: The porogen is prepared by suspension copolymerization with the participation of a dispersant: 60-80 parts by weight of styrene, 20-40 parts by weight of methyl methacrylate, 6-12 parts by weight of p-ethylstyrene, 4-8 parts by weight of m-ethylstyrene, wherein the crosslinking agent comprises 10-15 parts by weight of p-divinylbenzene and 8-12 parts by weight of m-divinylbenzene, the porogen is propylene glycol diacetate, the initiator is benzoyl peroxide, and the dispersant is alum; the porogen is used in an amount of 20-30% of the total mass of the monomer phase.
2. The method for preparing pure isobutylene by superposition synthesis according to claim 1, characterized in that: The concentration of the pure isobutylene is not less than 99%.
3. The method for preparing pure isobutylene by superposition synthesis according to claim 1, characterized in that: The copolymer resin balls as sulfonated matrix have a moisture content of 5-10% after drying and a particle size screening range of 0.3-0.9 mm.
4. The method for preparing pure isobutylene by superposition synthesis according to claim 1 or 3, characterized in that: The water content of the composite catalyst is 50%±2%.
5. The method for preparing pure isobutylene by superposition synthesis according to claim 1 or 3, characterized in that: The sulfonation comprises the following steps: immersing the copolymer resin balls in a sulfonating agent of a saturated solution of dichloroethane or dichloropropylene in sulfur trioxide, wherein the mass ratio of the copolymer resin balls to sulfur trioxide is 1:2-5, stirring for 0.5-2h to fully mix the copolymer resin balls and the sulfonating agent, then reacting at a temperature of 100°C-120°C for 8-20h, cooling, and washing with water until neutral.
6. A catalyst for superposition application in the process for preparing pure isobutylene by superposition synthesis according to any one of claims 1 to 5, wherein the catalyst for superposition application is a cation exchange resin catalyst obtained by extracting, drying, screening, sulfonating and washing copolymer resin balls, characterized in that: The copolymer resin spheres are obtained by suspension copolymerization of the following monomers in the presence of a crosslinking agent, a porogen, an initiator and a dispersant: 60-80 weight parts of main monomer styrene, 20-40 weight parts of methyl methacrylate, 6-12 weight parts of p-ethylstyrene and 4-8 weight parts of m-ethylstyrene, wherein the crosslinking agent comprises 10-15 weight parts of p-divinylbenzene and 8-12 weight parts of m-divinylbenzene, and the copolymer resin spheres are obtained by temperature-raising suspension polymerization in a copolymerization system in which the porogen is propylene glycol diacetate, the initiator is benzoyl peroxide and the dispersant is alum, wherein the amount of the porogen is 20-30% of the total weight of the monomer phase.
Citation Information
Patent Citations
Preparation method and application for supported catalysis / polymerization-inhibition macroporous resin microsphere
CN108855229A
Catalyst for isobutylene hydration reaction and preparation method thereof
CN110665542A
Etherification catalyst for preparing methyl tert-butyl ether from methanol-tert-butyl alcohol and preparation method of etherification catalyst
CN111957346A
Fuel components and their selective manufacturing methods
US20030088134A1