Polyimide film and copper clad laminate

By combining non-thermoplastic and thermoplastic polyimide layers in the polyimide film and controlling the thermal expansion coefficient and glass transition temperature, the problem of dimensional changes of copper-clad laminates at high temperatures is solved, achieving excellent dimensional stability and production Stability improves the reliability of the circuit substrate.

CN113527882BActive Publication Date: 2024-10-18NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202110982007.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2017-04-25
Publication Date
2024-10-18
Estimated Expiration
2037-04-25

AI Technical Summary

Technical Problem

The size of existing copper-clad laminates changes greatly during high-temperature processing, resulting in changes in the size of the wiring pattern, affecting the reliability and yield of the circuit substrate, and the dimensional stability is not effectively controlled.

Method used

By introducing non-thermoplastic and thermoplastic polyimide layers into the polyimide film and controlling the thermal expansion coefficient, glass transition temperature and in-plane retardation, a polyimide film with excellent dimensional stability is prepared for manufacturing copper-clad laminates plate.

Benefits of technology

It achieves the suppression of dimensional changes in high-temperature and high-pressure environments, improves the dimensional stability and production stability of copper-clad laminates, enhances the high-density installation capabilities of FPC, and improves the reliability and yield of circuit substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113527882B_ABST
    Figure CN113527882B_ABST
Patent Text Reader

Abstract

The present invention provides a polyimide film capable of reducing dimensional changes during high-temperature processing and a copper-clad laminate using the polyimide film. The polyimide film of the present invention has a thermoplastic polyimide layer on at least one side of a non-thermoplastic polyimide layer, and satisfies the following conditions: (i) the thermal expansion coefficient is within the range of 10 ppm / K to 30 ppm / K; (ii) the glass transition temperature of the thermoplastic polyimide is within the range of 200°C to 350°C; (iii) the in-plane retardation (RO) value is within the range of 5 nm to 50 nm; (iv) the heterogeneity (ΔRO) of RO in the width direction (TD direction) is less than 10 nm.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of the invention patent application with application number 201710279853.7 filed on April 25, 2017 and invention name “Polyimide film and copper-clad laminate”. Technical Field

[0002] The invention relates to a polyimide film and a copper-clad laminate. Background Art

[0003] In recent years, with the development of miniaturization, lightness and space saving of electronic devices, the demand for flexible printed circuits (FPCs) that are thin, light, flexible and durable even when bent repeatedly has been increasing. FPCs can be installed three-dimensionally and at high density even in a limited space, so their use is constantly expanding to wiring or cables, connectors and other parts of movable parts of electronic devices such as hard disk drives (HDDs), digital versatile discs (DVDs), and mobile phones.

[0004] FPC is manufactured by etching the copper layer of copper-clad laminate (Copper-Clad Laminate, CCL) for wiring processing. For FPCs that are continuously bent or bent 180° in mobile phones or smart phones, rolled copper foil is mostly used as the material of the copper layer. For example, Patent Document 1 proposes that the bending resistance of a copper-clad laminate made of rolled copper foil is specified by the number of folding resistances. In addition, Patent Document 2 proposes a copper-clad laminate using rolled copper foil specified by glossiness and the number of bends.

[0005] In the process of photolithography process or installation of FPC to copper-clad laminate, various processes such as bonding, cutting, exposure, etching are performed based on the alignment mark (alignment mark) set in the copper-clad laminate. The processing accuracy in these processes becomes important in maintaining the reliability of the electronic equipment equipped with FPC. However, the copper-clad laminate has a structure in which the copper layer and the resin layer with different thermal expansion coefficients are stacked, so stress is generated between the layers due to the difference in the thermal expansion coefficients of the copper layer and the resin layer. A part or all of this stress is relieved when the etching copper layer is processed for wiring, thereby generating expansion and contraction, resulting in dimensional changes in the wiring pattern. Therefore, dimensional changes eventually occur in the stage of FPC, which becomes the cause of poor contact between wiring or wiring and terminals, and reduces the reliability or yield of the circuit substrate. Therefore, for the copper-clad laminate as a circuit substrate material, dimensional stability is a very important characteristic. However, in the patent document 1 and the patent document 2, no consideration is made about the dimensional stability of the copper-clad laminate.

[0006] As a method for producing a polyimide film, the following method is known: a self-supporting gel film of polyamic acid is subjected to uniaxial stretching and thermal imidization simultaneously or continuously, thereby orienting the polyimide molecular chains to exhibit in-plane birefringence. At this time, in order to control retardation, the conditions such as the heating rate during the uniaxial stretching operation and the thermal imidization, the final curing temperature, and the load are controlled with high precision. For example, Patent Document 3 proposes the following technology: a polyimide film is heated while being uniaxially stretched, thereby controlling retardation.

[0007] [Prior art literature]

[0008] [Patent Document]

[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 2014-15674 (claims, etc.)

[0010] [Patent Document 2] Japanese Patent Application Publication No. 2014-11451 (claims, etc.)

[0011] [Patent Document 3] Japanese Patent Application Publication No. 2000-356713 (claims, etc.) Summary of the invention

[0012] [Problems to be solved by the invention]

[0013] The first aspect of the present invention provides a polyimide film that can reduce dimensional changes during high-temperature processing and a copper-clad laminate using the polyimide film. In addition, the second aspect of the present invention provides a polyimide film that can achieve high dimensional stability accuracy and can be stably produced even in a heating environment above the glass transition temperature of thermoplastic polyimide and a copper-clad laminate using the polyimide film.

[0014] [Technical means to solve the problem]

[0015] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned problems can be solved by controlling the in-plane retardation of a polyimide film, thereby completing the present invention.

[0016] That is, the polyimide film of the present invention has a thermoplastic polyimide layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide layer containing a non-thermoplastic polyimide. The polyimide film of the present invention is characterized by satisfying the following conditions (i) to (iv);

[0017] (i) a coefficient of thermal expansion in the range of 10 ppm / K to 30 ppm / K;

[0018] (ii) the glass transition temperature of the thermoplastic polyimide is within the range of 200° C. to 350° C.;

[0019] (iii) the value of in-plane retardation (RO) is within the range of 5 nm to 50 nm;

[0020] (iv) The non-uniformity (ΔRO) of the in-plane retardation (RO) in the transverse direction (TD direction) is 10 nm or less.

[0021] The polyimide film of the present invention may be formed by heating the film at a temperature of 360°C and a pressure of 340 MPa / m 2 , the change in in-plane retardation (RO) before and after pressurization is less than 20 nm when the holding time is 15 minutes.

[0022] The polyimide film of the present invention may also allow the non-thermoplastic polyimide to contain tetracarboxylic acid residues and diamine residues, wherein the tetracarboxylic acid residues and diamine residues are both aromatic groups, the aromatic groups include biphenyl tetrayl groups or biphenylene groups, and the biphenyl tetrayl groups or biphenylene groups account for 40 molar parts or more relative to 100 molar parts of the total of the tetracarboxylic acid residues and diamine residues.

[0023] The polyimide film of the present invention may also contain a tetracarboxylic acid residue and a diamine residue in the thermoplastic polyimide, wherein the tetracarboxylic acid residue and the diamine residue are both aromatic groups, the aromatic group includes a biphenyl tetrayl group or a biphenylene group, and the biphenyl tetrayl group or the biphenylene group is in a range of 30 mol parts to 80 mol parts based on 100 mol parts in total of the tetracarboxylic acid residue and the diamine residue.

[0024] The polyimide film of the present invention may contain 20 to 70 mol parts of tetracarboxylic acid residues derived from 3,3′,4,4′-biphenyltetracarboxylic dianhydride based on 100 mol parts of all tetracarboxylic acid residues contained in the non-thermoplastic polyimide.

[0025] The polyimide film of the present invention may contain 40 mol parts or more of tetracarboxylic acid residues derived from 3,3′,4,4′-biphenyltetracarboxylic dianhydride based on 100 mol parts of all tetracarboxylic acid residues contained in the thermoplastic polyimide.

[0026] The polyimide film of the present invention may contain 20 parts by mole or more of the diamine residue represented by the following general formula (1) based on 100 parts by mole of all diamine residues contained in the non-thermoplastic polyimide.

[0027] [Chemistry 1]

[0028]

[0029] [wherein, R1 and R2 independently represent an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an alkenyl group having 2 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group]

[0030] The polyimide film of the present invention may contain the diamine residue represented by the following general formula (2) in an amount of 3 to 60 parts by mole per 100 parts by mole of all diamine residues contained in the thermoplastic polyimide.

[0031] [Chemistry 2]

[0032]

[0033] [wherein, R3 and R4 independently represent an alkyl group having 1 to 3 carbon atoms or an alkoxy group or alkenyl group having 1 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group]

[0034] The copper-clad laminate of the present invention comprises an insulating layer and a copper layer located on at least one surface of the insulating layer. Furthermore, the copper-clad laminate of the present invention is characterized in that the insulating layer comprises a thermoplastic polyimide layer in contact with the surface of the copper layer, and a non-thermoplastic polyimide layer laminated indirectly,

[0035] The insulating layer includes any one of the polyimide films.

[0036] The copper-clad laminate of the present invention may have a dimensional change in the longitudinal direction (machine direction, MD direction) and a dimensional change in the width direction (TD direction) of the copper layer before and after etching that is 2% or less.

[0037] [Effects of the Invention]

[0038] Even if the polyimide film of the present invention is delayed under high temperature and high pressure, the variation amount is also suppressed, so for example, even if it is the case of thermocompression bonding with copper foil at high temperature, the dimensional stability is also excellent. Therefore, by using the polyimide film of the present invention, the time of the manufacturing process of the copper-clad laminate can be shortened, and the production stability is excellent. Especially in the case of processing the wide polyimide film in a roll-to-roll manner, laminating copper foil and manufacturing the copper-clad laminate, the full width of the film is also low in dimensional change rate, and the dimension is stable, so the FPC obtained by the copper-clad laminate can be installed at a high density. Therefore, by using the polyimide film of the present invention and the copper-clad laminate using the polyimide film as FPC material, the improvement of reliability and yield rate can be realized to the circuit substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a perspective view showing a schematic configuration of a copper-clad laminate and a test piece used in an evaluation method for evaluating the dimensional stability of a copper-clad laminate according to one embodiment of the present invention.

[0040] Figure 2 A diagram illustrating the positions of marks on a test piece.

[0041] Figure 3 This is a partial enlarged view of the central area of ​​the test piece.

[0042] Figure 4 This is a partial enlarged view of the corner area of ​​the test piece.

[0043] Figure 5 This is a diagram for explaining the amount of dimensional change in the interval between holes.

[0044] Figure 6 It is a figure which shows the evaluation sample for explaining an Example.

[0045] Figure 7 It is a figure for explaining the preparation of the evaluation sample of Example.

[0046] [Explanation of Symbols]

[0047] 10: Test piece

[0048] 20: Imaginary regular quadrilateral

[0049] 20a: Center

[0050] 20b: Corner

[0051] 21: Central Area

[0052] 23a, 23b: Corner area

[0053] 30: Hole

[0054] 30a: Center of hole 30

[0055] 100: Copper clad laminate

[0056] L0, L1: distance

[0057] MD, TD: Direction

[0058] Δ1, Δ1+Δ2: Dimension change DETAILED DESCRIPTION

[0059] Secondly, make appropriate reference to the attached Figure 1 Embodiments of the present invention will be described.

[0060] <Polyimide film>

[0061] The polyimide film of this embodiment has a thermoplastic polyimide layer on at least one side of the non-thermoplastic polyimide layer. That is, the thermoplastic polyimide layer is provided on one side or both sides of the non-thermoplastic polyimide layer. For example, in the case of a copper-clad laminate composed of the polyimide film of this embodiment and a copper layer, the copper layer is laminated on the surface of the thermoplastic polyimide layer.

[0062] The non-thermoplastic polyimide here generally refers to a polyimide that does not show adhesiveness even when it is softened by heating, and in the present invention, it refers to a polyimide having a storage modulus of 1.0×10 at 30°C as measured by a dynamic viscoelasticity measuring device (dynamic mechanical analysis (DMA)). 9 Pa or more, and the storage modulus at 360°C is 1.0×10 8 Thermoplastic polyimide is generally a polyimide whose glass transition temperature (Tg) can be clearly confirmed, but in the present invention, it means a polyimide whose storage modulus at 30°C measured by DMA is 1.0×10 9 Pa or more, and the storage modulus at 360°C is less than 1.0×10 8 Polyimide of Pa.

[0063] The polyimide film of the present embodiment may be a film (sheet) or a film laminated on a substrate such as a copper foil, a glass plate, a resin sheet such as a polyimide film, a polyamide film, or a polyester film.

[0064] When the polyimide film of the present embodiment is used as an insulating layer of a circuit board, for example, in order to prevent the occurrence of warping or the reduction of dimensional stability, it is important that the coefficient of thermal expansion (CTE) is within the range of 10 ppm / K to 30 ppm / K, preferably within the range of 10 ppm / K to 25 ppm / K. If the CTE is less than 10 ppm / K or exceeds 30 ppm / K, warping occurs or the dimensional stability is reduced. In addition, in the polyimide film of the present embodiment, the CTE of the polyimide film is more preferably within the range of ±5 ppm / K or less, and most preferably within the range of ±2 ppm / K or less, relative to the CTE of the copper layer including copper foil.

[0065] In the polyimide film of the present embodiment, the thickness of the polyimide film can be set to a thickness within a predetermined range according to the purpose of use. The thickness of the polyimide film is preferably, for example, in the range of 8 μm to 50 μm, and more preferably in the range of 11 μm to 26 μm. If the thickness of the polyimide film is less than the lower limit, electrical insulation may not be ensured, or problems such as difficulty in handling in the manufacturing process due to reduced operability may occur. On the other hand, if the thickness of the polyimide film exceeds the upper limit, in order to control the in-plane delay (RO), the manufacturing conditions must be controlled with high precision, resulting in undesirable conditions such as reduced productivity.

[0066] In the polyimide film of the present embodiment, the non-thermoplastic polyimide layer constitutes a polyimide layer of low thermal expansion, and the thermoplastic polyimide layer constitutes a polyimide layer of high thermal expansion. Here, the polyimide layer of low thermal expansion refers to a polyimide layer in the range of thermal expansion coefficient (CTE) preferably above 1ppm / K and below 25ppm / K, more preferably above 3ppm / K and below 25ppm / K. In addition, the polyimide layer of high thermal expansion refers to a polyimide layer in the range of CTE preferably above 35ppm / K, more preferably above 35ppm / K and below 80ppm / K, and then preferably above 35ppm / K and below 70ppm / K. The polyimide layer can be made into a polyimide layer with a desired CTE by appropriately changing the combination, thickness, drying and curing conditions of the raw materials used.

[0067] In addition, in the polyimide film of the present embodiment, it is preferable that the thickness ratio of the non-thermoplastic polyimide layer to the thermoplastic polyimide layer (non-thermoplastic polyimide layer / thermoplastic polyimide layer) is within the range of 1.5 to 6.0. If the value of this ratio is less than 1.5, the non-thermoplastic polyimide layer relative to the overall polyimide film becomes thinner, so the heterogeneity of the in-plane delay (RO) tends to become larger, and if it exceeds 6.0, the thermoplastic polyimide layer becomes thinner, so the bonding reliability of the polyimide film and the copper layer tends to decrease. The control of the in-plane delay (RO) is related to the resin composition and thickness of each polyimide layer constituting the polyimide film. For a thermoplastic polyimide layer that is a resin composition that imparts adhesion, i.e., high thermal expansion or softening, the greater its thickness, the greater the impact on the value of RO of the polyimide film. Therefore, the ratio of the thickness of the non-thermoplastic polyimide layer is increased, and the ratio of the thickness of the thermoplastic polyimide layer is decreased, so that the RO value of the polyimide film and its non-uniformity are decreased.

[0068] In the polyimide film of the present embodiment, the polyimide constituting the thermoplastic polyimide layer can improve adhesion with the copper layer. The glass transition temperature of such thermoplastic polyimide is in the range of 200°C to 350°C, preferably 200°C to 320°C.

[0069] From the point of view of the improvement effect of the dimensional accuracy of the polyimide film of the present embodiment, the polyimide film of the present embodiment is preferably in the range of a film width of more than 490 mm and less than 1100 mm, and the length of the elongated strip is more than 20 m. In the case of continuously manufacturing the polyimide film of the present embodiment, the wider the film in the width direction (hereinafter also referred to as the TD direction), the more obvious the effect of the invention becomes. In addition, it also includes a film obtained by cutting (slit) at a certain value in the length direction (hereinafter also referred to as the MD direction) and the TD direction of the elongated polyimide film after continuously manufacturing the polyimide film of the present embodiment.

[0070] The in-plane retardation (RO) value of the polyimide film of the present embodiment is within the range of 5 nm to 50 nm, preferably within the range of 5 nm to 20 nm, and more preferably within the range of 5 nm to 15 nm. In addition, the heterogeneity (ΔRO) of RO in the TD direction is 10 nm or less, preferably 5 nm or less, and more preferably 3 nm or less. Since the control is performed within this range, the dimensional accuracy is improved even for a film with a thickness of 25 μm or more.

[0071] The polyimide film of the present embodiment is preferably subjected to a temperature of 360° C. and a pressure of 340 MPa / m 2, the change in the in-plane retardation (RO) before and after the pressurization for 15 minutes is less than 20 nm, more preferably less than 10 nm, and further preferably less than 5 nm. The polyimide film of this embodiment controls the change in RO to be less than the upper limit value even at a temperature exceeding the glass transition temperature of the polyimide constituting the thermoplastic polyimide layer. Therefore, for example, before and after the process of laminating the polyimide film of this embodiment to the copper foil by thermal lamination, RO is not easy to change, so it becomes a polyimide film with excellent dimensional stability.

[0072] In addition, the tensile modulus of the polyimide film of the present embodiment is preferably within the range of 3.0GPa to 10.0GPa, more preferably within the range of 4.5GPa to 8.0GPa. If the tensile modulus of the polyimide film is less than 3.0GPa, the strength of the polyimide itself is reduced, and thus the copper-clad laminate is processed into a circuit substrate, and sometimes the cracking of the film and other operational problems are generated. On the contrary, if the tensile modulus of the polyimide film exceeds 10.0GPa, the rigidity of the copper-clad laminate for bending increases, and as a result, when the copper-clad laminate is bent, the bending stress applied to the copper wiring increases, and the bending resistance decreases. By setting the tensile modulus of the polyimide film to within the range, the strength and flexibility of the polyimide film can be ensured.

[0073] The embodiments of the method for producing the polyimide film of the present embodiment include, for example: [1] a method for producing a polyimide film by coating a solution of polyamic acid on a supporting substrate, drying the solution, and then imidizing the solution; and [2] a method for producing a polyimide film by coating a solution of polyamic acid on a supporting substrate, drying the solution, peeling off a gel film of polyamic acid from the supporting substrate, and imidizing the polyimide film. In addition, the polyimide film of the present embodiment is a polyimide film comprising a plurality of polyimide layers, and therefore the embodiments of the method for producing the polyimide film include, for example: [3] a method for repeatedly coating a solution of polyamic acid on a supporting substrate, drying the solution, and then imidizing the solution (hereinafter referred to as a casting method); and [4] a method for simultaneously coating polyamic acid in a multi-layered state by multi-layer extrusion, drying the polyamic acid, and then imidizing the polyimide film (hereinafter referred to as a multi-layer extrusion method).

[0074] The method [1] may include, for example, the following steps 1a to 1c;

[0075] (1a) coating a polyamic acid solution on a supporting substrate and drying the solution;

[0076] (1b) a step of heat-treating polyamic acid on a supporting substrate to imidize the polyamic acid, thereby forming a polyimide layer; and

[0077] (1c) A step of separating the supporting substrate and the polyimide layer to obtain a polyimide film.

[0078] The method [2] may include, for example, the following steps 2a to 2c;

[0079] (2a) coating a polyamic acid solution on a supporting substrate and drying the solution;

[0080] (2b) a step of separating the supporting substrate from the gel film of polyamic acid; and

[0081] (2c) A step of heat-treating the gel film of the polyamic acid to imidize the film to obtain a polyimide film.

[0082] The method [3] can be carried out in the same manner as the method [1] or [2], except that step 1a or step 2a is repeated a plurality of times in the method [1] or [2] to form a laminated structure of polyamic acid on a supporting substrate.

[0083] The method [4] can be carried out in the same manner as the method [1] or the method [2], except that in step 1a of the method [1] or step 2a of the method [2], the laminated structure of polyamic acid is simultaneously coated by multilayer extrusion and then dried.

[0084] The polyimide film manufactured in the present invention is preferably imidized with polyamic acid on a supporting substrate. Since imidization is performed under the state that the resin layer of polyamic acid is fixed on the supporting substrate, the expansion and contraction change of the polyimide layer during the imidization process can be suppressed, and the thickness or dimensional accuracy of the polyimide film can be maintained.

[0085] However, for the polyimide film that completes the imidization of polyamic acid on the supporting substrate, the polyimide film is extended due to the tension applied to the polyimide film when separating the polyimide film from the supporting substrate, or the stress of the polyimide film generated when peeling using a knife edge, etc. Therefore, it is easy to produce the inhomogeneity of the in-plane delay (RO) of the polyimide film, especially the more the film width is more than 490mm, the more obvious the inhomogeneity of RO becomes. For the polyimide film of the present embodiment, the polyimide constituting the non-thermoplastic polyimide layer and the thermoplastic polyimide layer is easily set in a manner to form an ordered structure, thereby dispersing the stress necessary for peeling to each layer of the polyimide film, thereby controlling RO.

[0086] In addition, the in-plane retardation (RO) can also be controlled by separating the gel film of polyamic acid on the supporting substrate, uniaxially stretching or biaxially stretching the gel film of polyamic acid, and simultaneously or continuously imidizing. At this time, in order to more precisely and highly control the RO, it is preferred to appropriately adjust the conditions such as the heating rate during the stretching operation and imidization, the completion temperature of the imidization, and the load.

[0087] (Non-thermoplastic polyimide)

[0088] In the polyimide film of the present embodiment, it is preferred that the non-thermoplastic polyimide contains tetracarboxylic acid residues and diamine residues, and these residues are all aromatic groups and contain biphenyl tetrakis or biphenylene. Here, biphenyl tetrakis or biphenylene has the same meaning as the diphenyl skeleton, and for example, a halogen atom, an alkyl group, an alkoxy group, an alkenyl group or other substituents may be bonded to the biphenyl tetrakis or biphenylene, but from the viewpoint of reducing the amount of change in the in-plane retardation (RO) under a high temperature environment, for example, it is more preferred that the carbon number of the substituents such as the alkyl group, the alkoxy group, and the alkenyl group is set within the range of 1 to 3.

[0089] In the present invention, the tetracarboxylic acid residue refers to a tetravalent group derived from tetracarboxylic dianhydride, and the diamine residue refers to a divalent group derived from a diamine compound. In addition, the diamine compound is a compound having two amino groups, but the hydrogen atom in each amino group may be substituted by an arbitrary substituent.

[0090] The tetracarboxylic acid residue and diamine residue contained in the non-thermoplastic polyimide are both aromatic groups. By setting them as aromatic groups, the change amount of the in-plane retardation (RO) of the polyimide film in a high temperature environment can be reduced. Furthermore, it is preferred that the biphenyl tetrakisyl group or the biphenylene group is set to 40 molar parts or more, and more preferably 50 molar parts or more, relative to 100 molar parts of the total of the tetracarboxylic acid residue and the diamine residue, thereby easily forming an ordered structure obtained by the biphenyl tetrakisyl group or the biphenylene group, which can reduce the change amount of the RO of the polyimide film in a high temperature environment and suppress the heterogeneity of the RO.

[0091] In addition, the tetracarboxylic acid residues contained in the non-thermoplastic polyimide can preferably include tetracarboxylic acid residues derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride (Biphenyltetracarboxylic dianhydride, BPDA), 2,2',3,3'-biphenyltetracarboxylic dianhydride, etc. Among these tetracarboxylic acid residues, the tetracarboxylic acid residues derived from BPDA (hereinafter also referred to as BPDA residues) are easy to form an ordered structure, which can reduce the change in the in-plane delay (RO) under high temperature environment, and are therefore particularly preferred. In addition, although the BPDA residue can impart self-supporting properties to the gel film of the polyamic acid as a polyimide precursor, it tends to increase the CTE after imidization. From this point of view, the BPDA residue is preferably in the range of 20 to 70 mole parts, and more preferably in the range of 20 to 60 mole parts, relative to 100 mole parts of all tetracarboxylic acid residues contained in the non-thermoplastic polyimide.

[0092] The tetracarboxylic acid residue other than the BPDA residue contained in the non-thermoplastic polyimide can preferably include a tetracarboxylic acid residue derived from pyromellitic dianhydride (PMDA) (hereinafter also referred to as PMDA residue). The PMDA residue is preferably in the range of 0 to 60 mol parts, more preferably in the range of 0 to 50 mol parts, relative to 100 mol parts of all tetracarboxylic acid residues contained in the non-thermoplastic polyimide. The PMDA residue is arbitrary, but is a residue that plays a role in controlling the thermal expansion coefficient and controlling the glass transition temperature.

[0093] Other tetracarboxylic acid residues include, for example, tetracarboxylic acid residues derived from the following aromatic tetracarboxylic acid dianhydrides: 3,3',4,4'-diphenylsulfone tetracarboxylic acid dianhydride, 4,4'-oxydiphthalic anhydride, 2,3',3,4'-biphenyltetracarboxylic acid dianhydride, 2,2',3,3'-benzophenone tetracarboxylic acid dianhydride, 2,3,3',4'-benzophenone tetracarboxylic acid dianhydride or 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, 2,3',3,4'-diphenyl ether tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl) ether dianhydride, 3,3",4,4"-p-terphenyl tetracarboxylic acid dianhydride, 2,3 ,3",4"-terphenyltetracarboxylic dianhydride or 2,2",3,3"-terphenyltetracarboxylic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride or 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride or bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride or bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride or 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-phenanthrene-tetracarboxylic dianhydride, 1 , 2,6,7-phenanthrene-tetracarboxylic dianhydride or 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 2,3,5,6-cyclohexane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6- or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene- 1,4,5,8-tetracarboxylic dianhydride or 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,3,8,9-perylene-tetracarboxylic dianhydride, 3,4,9,10-perylene-tetracarboxylic dianhydride, 4,5,10,11-perylene-tetracarboxylic dianhydride or 5,6,11,12-perylene-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, and the like.

[0094] Among the tetracarboxylic acid residues contained in the non-thermoplastic polyimide, the tetracarboxylic acid residues derived from tetracarboxylic acid dianhydrides of 2,3',3,4'-diphenylether tetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic acid dianhydride, 4,4'-oxydiphthalic anhydride and 2,3',3,4'-diphenyltetracarboxylic acid dianhydride are preferably 20 mol parts or less, and more preferably 15 mol parts or less, relative to 100 mol parts of all tetracarboxylic acid residues contained in the non-thermoplastic polyimide. If these tetracarboxylic acid residues exceed 20 mol parts relative to all tetracarboxylic acid residues contained in the non-thermoplastic polyimide, the orientation of the molecules is reduced, and the control of the in-plane retardation (RO) becomes difficult.

[0095] In the polyimide film of the present embodiment, as the diamine residue contained in the non-thermoplastic polyimide, preferably, for example, a diamine residue represented by the following general formula (1) is mentioned.

[0096] [Chemistry 3]

[0097]

[0098] In the above formula (1), R1 and R2 independently represent an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an alkenyl group having 2 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group.

[0099] The diamine residue represented by the general formula (1) easily forms an ordered structure, and is particularly advantageous in suppressing the change in in-plane retardation (RO) under high temperature environments. From this viewpoint, the diamine residue represented by the general formula (1) is preferably in an amount of 20 mol parts or more, more preferably 50 mol parts or more, and further preferably in a range of 60 mol parts to 90 mol parts, relative to 100 mol parts of all diamine residues contained in the non-thermoplastic polyimide.

[0100] Preferred specific examples of the diamine residue represented by the general formula (1) include diamine residues derived from the following diamine compounds: 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-diethyl-4,4'-diaminobiphenyl (m-EB), 2,2'-diethoxy-4,4'-diaminobiphenyl (m-EOB), 2,2'-dipropoxy-4,4'-diaminobiphenyl (m-POB), 2,2'-n-propyl-4,4'-diaminobiphenyl (m-NPB), 2,2'-divinyl-4,4'-diaminobiphenyl (VAB), 4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl (TFMB), etc. Among these diamine compounds, 2,2′-dimethyl-4,4′-diaminobiphenyl (m-TB) is particularly preferred because it easily forms an ordered structure and can reduce the amount of change in in-plane retardation (RO) under a high temperature environment.

[0101] The diamine residue other than the diamine residue represented by the general formula (1) may preferably be a diamine residue derived from p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), etc., and more preferably a diamine residue derived from p-PDA (hereinafter also referred to as PDA residue) is preferred. The PDA residue is preferably in the range of 0 to 80 mol parts, more preferably in the range of 0 to 50 mol parts, relative to 100 mol parts of all tetracarboxylic acid residues contained in the non-thermoplastic polyimide. The PDA residue is arbitrary, but is a residue that plays a role in controlling the thermal expansion coefficient and controlling the glass transition temperature.

[0102] In order to improve the elongation and bending resistance of the polyimide film, the non-thermoplastic polyimide preferably contains at least one diamine residue selected from the group consisting of diamine residues represented by the following general formulae (3) to (5).

[0103] [Chemistry 4]

[0104]

[0105] In the formula (3), R5 and R6 independently represent a hydrogen atom, a halogen atom, or an alkyl or alkoxy or alkenyl group having 1 to 4 carbon atoms which may be substituted by a halogen atom, X independently represents a divalent group selected from -O-, -S-, -CH2-, -CH(CH3)-, -C(CH3)2-, -CO-, -COO-, -SO2-, -NH- or -NHCO-, and m and n independently represent integers of 1 to 4.

[0106] [Chemistry 5]

[0107]

[0108] In the formula (4), R5, R6 and R7 independently represent a hydrogen atom, a halogen atom, or an alkyl or alkoxy or alkenyl group having 1 to 4 carbon atoms which may be substituted by a halogen atom, X independently represents a divalent group selected from -O-, -S-, -CH2-, -CH(CH3)-, -C(CH3)2-, -CO-, -COO-, -SO2-, -NH- or -NHCO-, and m, n and o independently represent integers of 1 to 4.

[0109] [Chemistry 6]

[0110]

[0111] In the formula (5), R5, R6, R7 and R8 each independently represent a hydrogen atom, or a halogen atom, or an alkyl group, alkoxy group or alkenyl group having 1 to 4 carbon atoms which may be substituted by a halogen atom, X1 and X2 each independently represent a single bond or a divalent group selected from -O-, -S-, -CH2-, -CH(CH3)-, -C(CH3)2-, -CO-, -COO-, -SO2-, -NH- or -NHCO-, excluding the case where both X1 and X2 are single bonds, and m, n, o and p independently represent integers of 1 to 4.

[0112] The diamine residues represented by the general formula (3) to the general formula (5) have a bendable part, so they can impart flexibility to the polyimide film. Here, since the diamine residues represented by the general formula (4) and the general formula (5) have 3 or 4 benzene rings, in order to suppress the increase in the coefficient of thermal expansion (CTE), it is preferred that the terminal group bonded to the benzene ring is set to the para position. In addition, from the viewpoint of imparting flexibility to the polyimide film and suppressing the increase in the coefficient of thermal expansion (CTE), the diamine residues represented by the general formula (3) to the general formula (5) are preferably in the range of 10 to 40 mol parts, and more preferably in the range of 10 to 30 mol parts, relative to 100 mol parts of all diamine residues contained in the non-thermoplastic polyimide. If the diamine residues represented by the general formula (3) to the general formula (5) are less than 10 mol parts, the elongation when the film is made is reduced, and the bending resistance is reduced. On the other hand, when the content exceeds 40 parts by mole, the molecular orientation decreases and it becomes difficult to lower the CTE.

[0113] In the general formula (3), preferred examples of the group R5 and the group R6 include: a hydrogen atom or an alkyl group having 1 to 4 carbon atoms which may be substituted by a halogen atom, or an alkoxy or alkenyl group having 1 to 3 carbon atoms. In addition, in the general formula (3), preferred examples of the linking group X include -O-, -S-, -CH2-, -CH(CH3)-, -SO2- or -CO-. Preferred specific examples of the diamine residue represented by the general formula (3) include diamine residues derived from the following diamine compounds: 4,4'-diaminodiphenyl ether (4,4'-DAPE), 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 3,3'-diaminodiphenylpropane, 3,4'-diaminodiphenylpropane, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, and the like.

[0114] In the general formula (4), preferred examples of the group R5, the group R6 and the group R7 include: a hydrogen atom or an alkyl group having 1 to 4 carbon atoms which may be substituted by a halogen atom, or an alkoxy or alkenyl group having 1 to 3 carbon atoms. In addition, in the general formula (4), preferred examples of the linking group X include -O-, -S-, -CH2-, -CH(CH3)-, -SO2- or -CO-. Preferred specific examples of the diamine residue represented by the general formula (4) include diamine residues derived from the following diamine compounds: 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), bis(4-aminophenoxy)-2,5-di-tert-butylbenzene (DTBAB), 4,4-bis(4-aminophenoxy)benzophenone (BAPK), 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, etc.

[0115] In the general formula (5), preferred examples of the group R5, the group R6, the group R7 and the group R8 include: a hydrogen atom or an alkyl group having 1 to 4 carbon atoms which may be substituted by a halogen atom, or an alkoxy group or alkenyl group having 1 to 3 carbon atoms. In addition, in the general formula (5), preferred examples of the linking group X1 and the linking group X2 include a single bond, -O-, -S-, -CH2-, -CH(CH3)-, -SO2- or -CO-. However, from the viewpoint of providing a bending site, the case where both the linking group X1 and the linking group X2 are single bonds is excluded. Preferred specific examples of the diamine residue represented by the general formula (5) include diamine residues derived from the following diamine compounds: 4,4'-bis(4-aminophenoxy)biphenyl (BAPB), 2,2'-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2'-bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]sulfone, etc.

[0116] Other diamine residues include, for example, diamine residues derived from the following aromatic diamine compounds: 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)biphenyl, bis[1-(3-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, )]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-methylenedi-o-toluidine, 4,4'-methylenedi-2,6-dimethylaniline, 4,4'-methylenedi-2,6-diethylaniline, 3,3 '-Diaminodiphenylethane, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 3,3"-diamino-p-terphenyl, 4,4'-[1,4-phenylenebis(1-methylethylidene)]dianiline, 4,4'-[1,3-phenylenebis(1-methylethylidene)]dianiline, bis(p-aminocyclohexyl)methane, bis(p-β-aminotert-butylphenyl)ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl 1,5-Diaminonaphthalene, 2,6-Diaminonaphthalene, 2,4-bis(β-aminotert-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylene diamine, p-xylene diamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, etc.

[0117] In the non-thermoplastic polyimide, by selecting the types of the tetracarboxylic acid residue and the diamine residue, or the respective molar ratios when two or more tetracarboxylic acid residues or diamine residues are used, the thermal expansion coefficient, storage modulus, tensile modulus, etc. can be controlled. In addition, when the non-thermoplastic polyimide has a plurality of polyimide structural units, they can exist in the form of blocks or randomly. From the viewpoint of suppressing the heterogeneity of the in-plane retardation (RO), it is preferred that they exist randomly.

[0118] (Thermoplastic Polyimide)

[0119] In the polyimide film of the present embodiment, it is preferred that the thermoplastic polyimide contains tetracarboxylic acid residues and diamine residues, and these residues are all aromatic groups and contain biphenyl tetrakis or biphenylene. Here, regarding the biphenyl tetrakis or biphenylene, for example, a halogen atom, an alkyl group, an alkoxy group, an alkenyl group or other substituents may be bonded to the biphenyl tetrakis or biphenylene, and from the viewpoint of suppressing the change in the in-plane retardation (RO) under a high temperature environment, for example, the carbon number of the substituents such as the alkyl group, the alkoxy group, the alkenyl group or other substituents is preferably set within the range of 1 to 3.

[0120] The tetracarboxylic acid residue and diamine residue contained in the thermoplastic polyimide are both aromatic groups. By setting them as aromatic groups, the variation of the in-plane retardation (RO) under the high temperature environment of the polyimide film can be suppressed. Furthermore, relative to the total of 100 molar parts of the tetracarboxylic acid residue and the diamine residue, the biphenyl tetrayl or biphenylene is set to be within the range of more than 30 molar parts and less than 80 molar parts. If the biphenyl tetrayl or biphenylene is less than 30 molar parts, it is difficult to form an ordered structure obtained by the biphenyl tetrayl or biphenylene, and the variation of RO under the high temperature environment of the polyimide film increases. On the other hand, if the biphenyl tetrayl or biphenylene exceeds 80 molar parts, the thermoplasticity is impaired.

[0121] In addition, the tetracarboxylic acid residue contained in the thermoplastic polyimide can preferably include tetracarboxylic acid residues derived from BPDA, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, etc. Among these tetracarboxylic acid residues, the BPDA residue is particularly preferred because it is easy to form an ordered structure and can suppress the change in the in-plane delay (RO) under a high temperature environment. Therefore, relative to 100 mol parts of all tetracarboxylic acid residues contained in the thermoplastic polyimide, the BPDA residue is preferably 40 mol parts or more, more preferably 50 mol parts or more.

[0122] The tetracarboxylic acid residue other than the BPDA residue contained in the thermoplastic polyimide can preferably include a PMDA residue. The PMDA residue is preferably in the range of 0 to 60 molar parts, more preferably in the range of 0 to 50 molar parts, relative to 100 molar parts of all tetracarboxylic acid residues contained in the thermoplastic polyimide. The PMDA residue is arbitrary, but is a residue that plays a role in controlling the thermal expansion coefficient and controlling the glass transition temperature.

[0123] Other tetracarboxylic acid residues include, for example, tetracarboxylic acid residues derived from the following aromatic tetracarboxylic acid dianhydrides: 3,3',4,4'-diphenylsulfone tetracarboxylic acid dianhydride, 4,4'-oxydiphthalic anhydride, 2,2',3,3'-benzophenone tetracarboxylic acid dianhydride, 2,3,3',4'-benzophenone tetracarboxylic acid dianhydride or 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, 2,3',3,4'-diphenyl ether tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl) ether dianhydride, 3,3",4,4"-p-terphenyl tetracarboxylic acid dianhydride, 2,3,3",4"-p-terphenyl tetracarboxylic acid dianhydride or 2,2 ',3,3'-terphenyltetracarboxylic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride or 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride or bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride or bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride or 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-phenanthrene-tetracarboxylic dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride or 1,2,9,10 -phenanthrene-tetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 2,3,5,6-cyclohexane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6- or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride or 1,4,5,8-tetrachloronaphthalene -2,3,6,7-tetracarboxylic dianhydride, 2,3,8,9-perylene-tetracarboxylic dianhydride, 3,4,9,10-perylene-tetracarboxylic dianhydride, 4,5,10,11-perylene-tetracarboxylic dianhydride or 5,6,11,12-perylene-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, etc.

[0124] In the polyimide film of the present embodiment, as the diamine residue contained in the thermoplastic polyimide, preferably, for example, a diamine residue represented by the following general formula (2) is mentioned.

[0125] [Chemistry 7]

[0126]

[0127] In the above formula (2), R3 and R4 independently represent an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an alkenyl group having 1 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group.

[0128] The diamine residue represented by the general formula (2) is easy to form an ordered structure, and can be particularly advantageous in suppressing the change in the in-plane retardation (RO) under a high temperature environment. From this point of view, the diamine residue represented by the general formula (2) is preferably in the range of 3 to 60 mol parts, and more preferably in the range of 5 to 40 mol parts, relative to 100 mol parts of all diamine residues contained in the thermoplastic polyimide. If the diamine residue represented by the general formula (2) is less than 3 mol parts, it is difficult to form an ordered structure, and the change in the in-plane retardation (RO) of the polyimide film under a high temperature environment increases. If it exceeds 60 mol parts, the thermoplasticity is impaired.

[0129] Preferred specific examples of the diamine residue represented by the general formula (2) include diamine residues derived from the following diamine compounds: 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-diethyl-4,4'-diaminobiphenyl (m-EB), 2,2'-diethoxy-4,4'-diaminobiphenyl (m-EOB), 2,2'-dipropoxy-4,4'-diaminobiphenyl (m-POB), 2,2'-n-propyl-4,4'-diaminobiphenyl (m-NPB), 2,2'-divinyl-4,4'-diaminobiphenyl (VAB), 4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl (TFMB), etc. Among these compounds, 2,2′-dimethyl-4,4′-diaminobiphenyl (m-TB) is particularly preferred because it easily forms an ordered structure and can reduce the amount of change in in-plane retardation (RO) under a high-temperature environment.

[0130] The diamine residues other than the diamine residues represented by the general formula (2) preferably include diamine residues derived from p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), etc., and more preferably diamine residues derived from p-PDA (hereinafter also referred to as PDA residues) are preferred. The PDA residue is preferably in the range of 3 to 60 mol parts, more preferably in the range of 5 to 40 mol parts, relative to 100 mol parts of all diamine residues contained in the thermoplastic polyimide. The PDA residue is arbitrary, but because it has a rigid structure, it has the function of imparting an ordered structure to the polymer as a whole.

[0131] In order to improve the flexibility of the polyimide molecular chain and impart thermoplasticity, the thermoplastic polyimide preferably contains at least one diamine residue selected from the group consisting of diamine residues represented by the following general formulae (6) to (12).

[0132] [Chemistry 8]

[0133]

[0134] In the above formulae (6) to (12), R9 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, the linking group A independently represents a divalent group selected from -O-, -S-, -CO-, -SO-, -SO2-, -COO, -CH2-, -C(CH3)2-, -NH- or -CONH-, and n1 independently represents an integer of 0 to 4. In addition, the formula (8) is excluded from repeating the formula (7), and the formula (10) is excluded from repeating the formula (9). In addition, the term "independently" means that in one or more of the above formulae (6) to (12), multiple linking groups A, multiple R9 or multiple n1 may be the same or different.

[0135] The diamine residues represented by the general formulae (6) to (12) are preferably present in a total amount of at least one of 40 to 97 mol parts relative to 100 mol parts of all diamine residues contained in the thermoplastic polyimide. If the total amount of the diamine residues represented by the general formulae (6) to (12) is less than 40 mol parts, the polyimide has insufficient flexibility and cannot obtain thermoplasticity, while if it exceeds 97 mol parts, the change in the in-plane retardation (RO) of the polyimide film in a high temperature environment tends to increase.

[0136] The diamine residue represented by formula (6) is an aromatic diamine residue having two benzene rings. For the diamine compound that becomes the source of the diamine residue represented by formula (6), it can be considered that the amino group directly bonded to the benzene ring and the divalent linking group A are located in the meta position, and the degree of freedom possessed by the polyimide molecular chain increases and has high bending property, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using the diamine residue represented by formula (6), the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -O-, -CH2-, -C(CH3)2-, -CO-, -SO2-, -S-.

[0137] Examples of the diamine residue represented by formula (6) include diamine residues derived from the following diamine compounds: 3,3'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, 3,3'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,3-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylpropane, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, (3,3'-bisamino)diphenylamine, and the like.

[0138] The diamine residue represented by formula (7) is an aromatic diamine residue having three benzene rings. For the diamine compound that is the source of the diamine residue represented by formula (7), it can be considered that the amino group directly bonded to the benzene ring and the divalent linking group A are located in the meta position, and the degree of freedom of the polyimide molecular chain increases and has high bending property, which helps to improve the flexibility of the polyimide molecular chain. Therefore, if the diamine residue represented by formula (7) is used, the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -O-.

[0139] Examples of the diamine residue represented by formula (7) include diamine residues derived from diamine compounds such as 1,4-bis(3-aminophenoxy)benzene, 3-[4-(4-aminophenoxy)phenoxy]aniline, and 3-[3-(4-aminophenoxy)phenoxy]aniline.

[0140] The diamine represented by formula (8) is an aromatic diamine residue having three benzene rings. For the diamine residue represented by formula (8), it can be considered that the two divalent linking groups A directly bonded to a benzene ring are located at the meta position, and the degree of freedom of the polyimide molecular chain increases and has high bending property, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using the diamine residue represented by formula (8), the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -O-.

[0141] Examples of the diamine residue represented by formula (8) include diamine residues derived from the following diamine compounds: 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), 4,4'-[2-methyl-(1,3-phenylene)bisoxy]bisaniline, 4,4'-[4-methyl-(1,3-phenylene)bisoxy]bisaniline, 4,4'-[5-methyl-(1,3-phenylene)bisoxy]bisaniline, and the like.

[0142] The diamine residue represented by formula (9) is an aromatic diamine residue having four benzene rings. For the diamine compound that is the source of the diamine residue represented by formula (9), it can be considered that at least one amino group directly bonded to the benzene ring and the divalent linking group A are located in the meta position, and have high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using the diamine residue represented by formula (9), the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -O-, -CH2-, -C(CH3)2-, -SO2-, -CO-, -CONH-.

[0143] Examples of the diamine residue represented by formula (9) include diamine residues derived from the following diamine compounds: bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]benzophenone, bis[4,4'-(3-aminophenoxy)]benzanilide, and the like.

[0144] The diamine residue represented by formula (10) is an aromatic diamine residue having four benzene rings. For the diamine residue represented by formula (10), it can be considered that the two divalent linking groups A directly bonded to at least one benzene ring are located at the meta position, and the degree of freedom of the polyimide molecular chain increases and has high bending property, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using the diamine residue represented by formula (10), the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -O-.

[0145] Examples of the diamine residue represented by formula (10) include diamine residues derived from diamine compounds such as 4-[3-[4-(4-aminophenoxy)phenoxy]phenoxy]aniline and 4,4′-[oxybis(3,1-phenyleneoxy)]dianiline.

[0146] The diamine residue represented by formula (11) is an aromatic diamine residue having four benzene rings. Regarding the diamine residue represented by formula (11), it can be considered that the diamine residue has high flexibility by having at least two ether bonds, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using the diamine residue represented by formula (11), the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -C(CH3)2-, -O-, -SO2-, -CO-.

[0147] Examples of the diamine residue represented by formula (11) include diamine residues derived from the following diamine compounds: 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), bis[4-(4-aminophenoxy)phenyl]ketone (BAPK), and the like.

[0148] The diamine residue represented by formula (12) is an aromatic diamine residue having four benzene rings. For the diamine residue represented by formula (12), it can be considered that since there are divalent linking groups A with high bending properties on both sides of the diphenyl skeleton, it helps to improve the flexibility of the polyimide molecular chain. Therefore, by using the diamine residue represented by formula (12), the thermoplasticity of the polyimide is improved. Here, the linking group A is preferably -O-.

[0149] Examples of the diamine residue represented by formula (12) include diamine residues derived from diamine compounds such as bis[4-(3-aminophenoxy)]biphenyl and bis[4-(4-aminophenoxy)]biphenyl.

[0150] In thermoplastic polyimide, by selecting the types of the tetracarboxylic acid residue and the diamine residue, or the respective molar ratios when two or more tetracarboxylic acid residues or diamine residues are used, the thermal expansion coefficient, tensile modulus, glass transition temperature, etc. can be controlled. In addition, when the thermoplastic polyimide has a plurality of polyimide structural units, they can exist in the form of blocks or randomly, preferably randomly.

[0151] The weight average molecular weight of the thermoplastic polyimide is preferably in the range of 10,000 to 400,000, and more preferably in the range of 50,000 to 350,000. If the weight average molecular weight is less than 10,000, the strength of the film is reduced and the film tends to be brittle. On the other hand, if the weight average molecular weight exceeds 400,000, the viscosity is excessively increased, and defects such as uneven film thickness and streaks tend to occur during coating operations.

[0152] (Synthesis of non-thermoplastic polyimide and thermoplastic polyimide)

[0153] Generally, polyimide can be manufactured by reacting tetracarboxylic dianhydride with a diamine compound in a solvent to generate polyamic acid and then heating for ring closure. For example, tetracarboxylic dianhydride and a diamine compound are dissolved in an organic solvent in approximately equimolar amounts, and the polymerization reaction is carried out by stirring for 30 minutes to 24 hours at a temperature in the range of 0°C to 100°C, thereby obtaining a polyamic acid as a precursor of the polyimide. During the reaction, the reaction components are dissolved in an organic solvent in such a manner that the generated precursor is in the range of 5% by weight to 30% by weight, preferably in the range of 10% by weight to 20% by weight. The organic solvent used in the polymerization reaction can be cited, for example, as follows: N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethyl sulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, cresol, etc. It is also possible to use two or more of these solvents in combination, and further, aromatic hydrocarbons such as xylene and toluene can also be used in combination. In addition, the amount of such an organic solvent used is not particularly limited, and it is preferably adjusted to an amount such that the concentration of the polyamic acid solution obtained by the polymerization reaction becomes about 5% by weight to 30% by weight.

[0154] The synthesized polyamic acid is usually advantageously used in the form of a reaction solvent solution, which can be concentrated, diluted or replaced with other organic solvents as needed. In addition, polyamic acid is generally excellent in solvent solubility, so it can be used advantageously. The viscosity of the polyamic acid solution is preferably in the range of 500cps to 100,000cps. If it deviates from this range, it is easy to produce defects such as uneven thickness and stripes when applying the coating operation using a coating machine. There is no particular limitation on the method for imidizing the polyamic acid, for example, it is suitable to adopt a heat treatment of heating for 1 hour to 24 hours in the solvent under the temperature conditions in the range of 80°C to 400°C.

[0155] <Copper Clad Laminate>

[0156] The copper-clad laminate of the present embodiment has an insulating layer and a copper layer such as copper foil on at least one surface of the insulating layer, and the insulating layer can be formed using the polyimide film of the present embodiment. In addition, in order to improve the adhesion between the insulating layer and the copper layer, the layer of the insulating layer in contact with the copper layer is a thermoplastic polyimide layer. The copper layer is arranged on one side or both sides of the insulating layer. That is, the copper-clad laminate of the present embodiment can be a single-sided copper-clad laminate (single-sided CCL) or a double-sided copper-clad laminate (two-sided CCL). In the case of a single-sided CCL, the copper layer stacked on the single side of the insulating layer is regarded as the "first copper layer" of the present invention. In the case of a two-sided CCL, the copper layer stacked on the single side of the insulating layer is regarded as the "first copper layer" of the present invention, and the copper layer stacked on the surface opposite to the surface stacked with the first copper layer in the insulating layer is regarded as the "second copper layer" of the present invention. The copper-clad laminate of the present embodiment is to etch the copper layer and perform wiring circuit processing to form copper wiring, which is used as FPC.

[0157] The copper-clad laminate can also be produced, for example, by preparing a resin film composed of the polyimide film of the present embodiment, sputtering a metal thereon to form a seed layer, and then forming a copper layer by, for example, copper plating.

[0158] Alternatively, a copper-clad laminate can be produced by preparing a resin film composed of the polyimide film of the present embodiment and laminating a copper foil thereon by a method such as thermocompression bonding.

[0159] Furthermore, a copper-clad laminate can also be produced by casting a coating liquid containing a polyamic acid as a precursor of polyimide on a copper foil, drying the coating liquid to form a coating film, and then performing a heat treatment to imidize the coating film to form a polyimide layer.

[0160] (First copper layer)

[0161] In the copper-clad laminate of the present embodiment, the copper foil used for the first copper layer (hereinafter sometimes referred to as "first copper foil") is not particularly limited, and may be, for example, a rolled copper foil or an electrolytic copper foil.

[0162] The thickness of the first copper foil is preferably less than 13 μm, and more preferably in the range of 6 μm to 12 μm. If the thickness of the first copper foil exceeds 13 μm, the bending stress applied to the copper layer (or copper wiring) when the copper-clad laminate (or FPC) is bent increases, thereby reducing the bending resistance. In addition, from the perspective of production stability and operability, the lower limit of the thickness of the first copper foil is preferably set to 6 μm.

[0163] In addition, the tensile modulus of the first copper foil is preferably within the range of 10GPa to 35GPa, and more preferably within the range of 15GPa to 25GPa. In the present embodiment, when a rolled copper foil is used as the first copper foil, if annealing is performed by heat treatment, the flexibility is easily improved. Therefore, if the tensile modulus of the copper foil is less than the lower limit, in the process of forming an insulating layer on the long first copper foil, the rigidity of the first copper foil itself is reduced due to heating. On the other hand, if the tensile modulus exceeds the upper limit, a greater bending stress is applied to the copper wiring when the FPC is bent, thereby reducing its bending resistance. In addition, the rolled copper foil has a tendency to change its tensile modulus according to the heat treatment conditions when the insulating layer is formed on the copper foil, or the annealing treatment of the copper foil after the insulating layer is formed. Therefore, in the present embodiment, as long as the tensile modulus of the first copper foil in the copper-clad laminate finally obtained is within the range.

[0164] The first copper foil is not particularly limited, and a commercially available rolled copper foil can be used.

[0165] (Second copper layer)

[0166] The second copper layer is laminated on the surface of the insulating layer opposite to the first copper layer. The copper foil (second copper foil) used for the second copper layer is not particularly limited, and may be, for example, a rolled copper foil or an electrolytic copper foil. In addition, a commercially available copper foil may be used as the second copper foil. In addition, the same copper foil as the first copper foil may be used as the second copper foil.

[0167] The copper-clad laminate of the present embodiment preferably has an in-plane non-uniformity of less than ±2% in the test piece, where the ratio of the cumulative converted dimensional change of the wiring pattern of the circuit substrate size (FPC size) of 10 mm to the sum of the wiring width and the wiring spacing obtained by the following evaluation method. The so-called non-uniformity value of less than ±2% means that the dimensional change in the length direction (MD direction) and the dimensional change in the width direction (TD direction) before and after etching are both less than 2%. In the case where the non-uniformity value exceeds ±2%, in the FPC processed by the copper-clad laminate, it becomes a cause of poor contact between wiring or between wiring and terminals, resulting in reduced reliability or yield of the circuit substrate. Here, with reference to Figure 1 to Figure 7Next, a method for evaluating the dimensional stability of the copper-clad laminate used in the present embodiment will be described. The evaluation method includes the following steps (1) to (6).

[0168] (1) Preparation of test pieces:

[0169] In this process, Figure 1 As illustrated, the long copper-clad laminate 100 is cut into a predetermined length to prepare the test piece 10. In addition, in the following description, the length direction of the long copper-clad laminate 100 is defined as the MD direction, and the width direction is defined as the TD direction (the same for the test piece 10). The test piece 10 is preferably formed in a manner close to a square shape so that the width (the length in the TD direction) of the copper-clad laminate 100 is approximately equal to the cutting interval (the length in the MD direction). Although not shown in the figure, the copper-clad laminate 100 has an insulating resin layer and a copper layer stacked on one side or both sides of the insulating resin layer.

[0170] The copper-clad laminate 100 that is the object of this evaluation method can be a copper-clad laminate prepared by any method. For example, the copper-clad laminate 100 can be prepared by preparing a resin film, sputtering a metal thereon to form a seed layer, and then forming a copper layer by plating. In addition, the copper-clad laminate 100 can also be prepared by laminating a resin film and a copper foil by a method such as thermocompression bonding. Furthermore, the copper-clad laminate 100 can also be prepared by coating a resin solution on a copper foil to form an insulating resin layer.

[0171] (2) Step of forming a plurality of marks on a test piece:

[0172] In this process, Figure 2 As shown, first, an imaginary regular quadrilateral 20 (hereinafter sometimes simply referred to as "regular quadrilateral 20") having sides parallel to the MD direction and the TD direction is imagined in the test piece 10. The length of one side of the imaginary regular quadrilateral 20 can be set to a length corresponding to the width of the copper-clad laminate 100 (the length in the TD direction). In addition, regarding the area of ​​the imaginary regular quadrilateral 20, when a plurality of test pieces are taken, the limit of the range of processing into FPC is included in the evaluation object, so it is preferably set to an area that can cover the range of processing into FPC. Therefore, the length of one side of the regular quadrilateral 20 is preferably set to within the range of 60% to 90% of the length of the test piece 10 in the TD direction (the width of the copper-clad laminate 100), and more preferably set to within the range of 70% to 80%. For example, when the width (length in the TD direction) of the copper-clad laminate 100 is 250 mm, the length of one side of the imaginary regular quadrilateral 20 is preferably set within a range of 150 mm to 225 mm, and more preferably within a range of 175 mm to 200 mm.

[0173] Then, like Figure 2 to Figure 4 As shown, in the central area 21 including the center 20a of the imaginary regular quadrilateral 20, and the two corner areas 23a and 23b each including two corners 20b of one side of the TD direction of the common regular quadrilateral 20, a plurality of marks including a linear arrangement are formed. The mark is, for example, a circular hole 30 that passes through the test piece 10. The plurality of holes 30 are preferably formed at equal intervals. In addition, the hole 30 as a mark may be, for example, a polygonal shape such as a triangle or a rectangle. In addition, as long as the mark can identify its position, it is not limited to a through hole, for example, a groove, a cutout, etc. may be formed in the test piece 10, or a pattern printed with ink or the like.

[0174] <Central Area>

[0175] The center 20a of the imaginary regular quadrilateral 20 serves as the reference for the coordinates used to measure the expansion and contraction of the test piece 10. Therefore, in this evaluation method, the central area 21 including the center 20a is used as the measurement object. In the central area 21, the positions of the plurality of holes 30 can be any as long as they include a linear arrangement. For example, they can be arranged in a T-shape, an L-shape, etc. Preferably, they can be arranged in a cross shape evenly in the MD direction and the TD direction from the center 20a of the imaginary regular quadrilateral 20. That is, like Figure 3 As shown in the figure, it is preferred to form a plurality of holes 30 in the MD direction and the TD direction along a cross shape passing through the center 20a of the imaginary regular quadrilateral 20, and it is more preferred to arrange the holes 30 so that the cross-shaped intersection overlaps with the center 20a of the imaginary regular quadrilateral 20. In this case, the holes 30 overlapping with the center 20a are counted repeatedly as the holes 30 constituting the arrangement in both the MD direction and the TD direction.

[0176] In addition, in the central area 21, in order to accurately evaluate the dimensional stability including the dimensional variation non-uniformity within the surface of the test piece 10, the following situation is preferable: starting from the center 20a of the regular quadrilateral 20, a hole 30 is formed in the MD direction and the TD direction in an amount of at least 12.5%, preferably in the range of 12.5% ​​to 32.5%, and more preferably in the range of 12.5% ​​to 25% relative to the length of one side of the regular quadrilateral 20.

[0177] <Corner area>

[0178] exist Figure 1 In the long copper-clad laminate 100 shown in the figure, the area around the two corners 20b of the TD direction side of the regular quadrilateral 20 is the most easily stretched and the area where the dimensional change is likely to be large. Therefore, in this evaluation method, both the two corner areas 23a and the corner area 23b including the two corners 20b of the TD direction side of the regular quadrilateral 20 are measured.

[0179] In the corner regions 23a and 23b, the positions of the holes 30 may be any as long as they include a linear arrangement. For example, it is preferable to form the holes 30 in the manner shown in FIG. Figure 4 As shown, along the two sides of the clamping corner 20b of the imaginary regular quadrilateral 20, a plurality of holes 30 are formed into an L-shape in the MD direction and the TD direction. In this case, the holes 30 overlapped at the corner 20b are counted repeatedly as the holes 30 constituting the arrangement in both the MD direction and the TD direction. Figure 4 Only one corner region 23 b is shown, but the same is true for the other corner region 23 a.

[0180] In order to accurately evaluate the dimensional stability including the dimensional variation non-uniformity within the surface of the test piece 10 in the two corner regions 23a and 23b, the following situation is preferable: holes 30 are formed from both ends of one side of the regular quadrilateral 20 in the TD direction (i.e., the corners 20b of the regular quadrilateral 20) toward the center side in the MD direction, respectively, in an amount of at least 12.5%, preferably in the range of 12.5% ​​to 32.5%, and more preferably in the range of 12.5% ​​to 25% relative to the length of one side in the MD direction.

[0181] In addition, in the two corner areas 23a and 23b, in order to accurately evaluate the dimensional stability including the dimensional variation non-uniformity within the surface of the test piece 10, the following situation is preferable: from the two ends of one side of the regular quadrilateral 20 in the TD direction (i.e., the corner 20b of the regular quadrilateral 20) toward the center side in the TD direction, holes 30 are formed in an amount of at least 12.5%, preferably in the range of 12.5% ​​to 32.5%, and more preferably in the range of 12.5% ​​to 25% relative to the length of one side in the TD direction.

[0182] In addition, in order to cover the surface of the test piece 10 and accurately grasp the dimensional changes of each part, the arrangement range of the holes 30 at both ends arranged in a straight line in the center area 21 can also overlap with the arrangement range of the holes 30 at both ends arranged in a straight line in the same direction in the corner area 23a and the corner area 23b.

[0183] Specifically, it can also be configured in the following manner: when moving parallel in the TD direction, the positions of the two ends of the multiple holes 30 arranged in the MD direction in at least the center area 21 overlap with the position of the innermost hole 30 (the side away from the corner 20b) among the multiple holes 30 arranged in the MD direction in the two corner areas 23a and the corner area 23b, respectively.

[0184] Similarly, it can also be configured in the following manner: when moving parallel to the MD direction, the position of the hole 30 closest to the corner area 23a and the corner area 23b among the multiple holes 30 arranged in the TD direction in at least the center area 21 overlaps with the position of the hole 30 closest to the inner side (the side away from the corner 20b) among the multiple holes 30 arranged in the TD direction in the two corner areas 23a and the corner areas 23b.

[0185] Considering the above configuration, it is most reasonable to arrange the plurality of holes 30 in a cross shape in the center region 21 , and it is most reasonable to arrange the plurality of holes 30 in an L shape in the two corner regions 23 a and 23 b .

[0186] In the virtual regular quadrilateral 20 of the test piece 10 , the range in which the holes 30 are formed can be adjusted by the size of the holes 30 , the number of the holes 30 , and the length of the interval between the holes 30 .

[0187] In order to improve the detection accuracy of the dimensional change, the size of the hole 30 is preferably set within a range of 20% or less of the length of the interval between the holes 30 .

[0188] For the plurality of holes 30 formed in the central area 21 and the two corner areas 23a and 23b, in order to accurately evaluate the dimensional stability including the dimensional variation heterogeneity within the surface of the test piece 10, it is preferred that at least 11 or more linear arrangements are included in the MD direction and the TD direction, and more preferably at least 20 or more linear arrangements are included. Here, if the number of holes 30 is set to n, the number of intervals between adjacent holes 30 and holes 30 that become the measurement objects in the subsequent steps (3) and (5) becomes n-1. Regarding the intervals between adjacent holes 30 and holes 30, for example, when the number of holes 30 is 10, it becomes 9, and when the number of holes 30 is 21, it becomes 20. In this case, it is preferred that the number of holes 30 in the MD direction and the TD direction is the same.

[0189] In order to improve the detection accuracy of the dimensional change, the distance between the holes 30 is preferably set to 2 mm or more.

[0190] (3) The first measurement process:

[0191] In this process, the positions of the plurality of holes 30 are measured. Then, the distance L0 between the adjacent holes 30 is calculated based on the measurement results of the positions of the holes 30. For example, if the number of holes 30 is 21, the distance L0 is calculated for the intervals of 20 between the adjacent holes 30. Here, Figure 5 As shown, the distance L0 between adjacent holes 30 is the distance from the center 30 a of a certain hole 30 to the center 30 a of the adjacent hole 30 .

[0192] The measurement of the position of the hole 30 is not particularly limited, and can be performed by, for example, a method of detecting the position of the hole 30 based on an image of the test piece 10 .

[0193] The measurement of the position of the hole 30 in this process can be performed after the above-mentioned process (2), but it is preferable to provide a process of adjusting the condition of the test piece 10 before the measurement. An example of adjusting the condition of the test piece 10 is a humidity adjustment process. The humidity adjustment process can be performed by leaving the test piece 10 in a certain environment for a certain period of time (for example, 24 hours in an environment of 23°C and 50RH%).

[0194] (4) Etching process:

[0195] In this process, a part or all of the copper layer of the test piece 10 is etched. In order to evaluate the practical dimensional stability, the etching content is preferably carried out according to the wiring pattern of the FPC formed by the copper-clad laminate 100. In the case where the test piece 10 is prepared by a double-sided copper-clad laminate, the copper layers on both sides may also be etched. In addition, in the case where heat treatment is accompanied in the actual FPC processing, the test piece 10 may also be heated at an arbitrary temperature after etching.

[0196] (5) Second measurement process:

[0197] This step is a step of measuring the positions of the plurality of holes 30 again after the etching in (4). Figure 5 As shown, the distance L1 between the adjacent holes 30 is calculated based on the measurement results of the positions of the holes 30. The positions of the holes 30 in this step can be measured by the same method as in the step (3).

[0198] The measurement of the position of the hole 30 in this step may be performed after the step (4), but it is preferable to provide a step of adjusting the state of the test piece 10 in the same manner as the step (3). In particular, when the state adjustment is performed in the step (3), it is preferable to perform the state adjustment under the same conditions before the measurement in this step.

[0199] (6) Process of calculating the dimensional change:

[0200] In this process, Figure 5 As shown in FIG. 1 , the difference L1-L0 between the distance L0 obtained in the first measurement step and the distance L1 obtained in the second measurement step is calculated for the interval between the same two holes 30 before and after etching. Furthermore, the difference L1-L0 is calculated in the same manner for two or more, preferably ten or more, and more preferably all, intervals between the holes 30 arranged in the same straight line. The difference L1-L0 is referred to as the "dimensional change amount Δ".

[0201] (7) The process of converting to wiring specifications:

[0202] In this step, the dimensional change Δ obtained in step (6) is converted into the specification of the wiring pattern in the FPC formed by the copper-clad laminate 100, and the converted value is expressed as a ratio of the sum of the wiring width and the wiring spacing of the wiring pattern. Through this step, when the copper-clad laminate 100 for testing is actually processed into an FPC, the influence of the dimensional change of the copper-clad laminate 100 on the wiring pattern of the FPC can be easily known and expressed.

[0203] In this process, the dimensional change amount Δ is first converted into the specification of the wiring width / wiring spacing of the L / S wiring pattern in the predetermined FPC formed by the copper-clad laminate 100, and the converted dimensional change amounts are accumulated to obtain the accumulated converted dimensional change amount. For example, when the wiring width and wiring spacing of the wiring pattern in the predetermined FPC are 1 / Y of the distance L0 between the two holes 30 before etching, the dimensional change amount Δ is converted into a value when the specification is downsized to 2×(1 / Y) according to the following formula, and the accumulated converted dimensional change amount of the specification of 2×(1 / Y) is obtained.

[0204] Cumulative conversion size change = [Σ i=1 i (2×Δ i / Y)]

[0205] In the above formula, the symbol Σ i=1 i represents the sum of 1 to i. In addition, the dimensional change Δ represents the value obtained by subtracting the distance L0 between the nth hole 30 and the n-1th hole 30 before etching from the distance L1 between the nth hole 30 and the n-1th hole 30 after etching (here, n is an integer greater than 2). For example, Δ1 is the dimensional change of the length of the first interval (the distance between two adjacent holes 30), Δ i is the dimensional change in the length of the i-th interval (i is a positive integer).

[0206] Then, the displacement ratio of the wiring is calculated from the cumulative converted dimensional change according to the following formula: The displacement ratio of the wiring is expressed as the ratio of the sum of the wiring width (Lmm) and the wiring spacing (Smm) of the planned L / S wiring pattern.

[0207] Wiring displacement ratio (%) =

[0208] {[Σ i=1 i (2×Δ i / Y)] / [L+S]}×100

[0209] The displacement ratio of the wiring of MD and TD in the FPC calculated as above is plotted on a graph, thereby obtaining an approximate straight line corresponding to the size of the FPC (in addition, the diagram is omitted). Here, the so-called "FPC size" refers to the distance between the wirings at the farthest ends of the multiple wirings formed in the FPC. The size of the slope of the graph refers to the size of the wiring displacement, and the size of the non-uniformity of the slope of the graph refers to the size of the in-plane non-uniformity of the wiring displacement.

[0210] Through this process, when the copper-clad laminate 100 to be tested is actually processed into a circuit, the effect of the dimensional change of the copper-clad laminate 100 on the wiring pattern of the FPC can be easily known and expressed. In addition, by making a graph of an approximate straight line, the size of the displacement of the wiring made of the copper-clad laminate 100 as a test piece or the inhomogeneity within the surface can be seen and expressed in correspondence with the FPC size.

[0211] In addition, the dimensional change Δ obtained in the step (6) may be accumulated, and the accumulated dimensional change may be converted into the specification of the wiring width / wiring interval of the L / S wiring pattern in the predetermined FPC formed by the copper-clad laminate 100 to obtain the accumulated converted dimensional change. For example, the dimensional change Δ of each interval is accumulated to obtain the accumulated dimensional change Σ. The accumulated dimensional change Σ can be calculated by the following formula.

[0212] Σ=Δ1+Δ2+Δ3+···+Δ i =Σ i=1 i Δ i

[0213] The cumulative dimensional change Σ can be obtained for either the MD direction or the TD direction of the copper-clad laminate 100, preferably for both directions. Based on the magnitude of the cumulative dimensional change Σ, the dimensional stability of the copper-clad laminate 100 in the MD direction and the TD direction can be evaluated. In addition, an approximate straight line of scale-up can be obtained based on the measured value of the cumulative dimensional change Σ.

[0214] As described above, according to this evaluation method, the dimensional change of the copper-clad laminate 100 including the in-plane non-uniformity can be evaluated with high accuracy through steps (1) to (7). In addition, even when a plurality of test pieces are taken from the copper-clad laminate 100, the dimensional stability of each region processed into the FPC can be evaluated separately.

[0215] <FPC>

[0216] The copper-clad laminate of the present embodiment is mainly useful as an FPC material. That is, the FPC as one embodiment of the present invention can be manufactured by processing the copper layer of the copper-clad laminate of the present embodiment into a pattern to form a wiring layer by a conventional method.

[0217] [Example]

[0218] The following examples are given to more specifically describe the features of the present invention. However, the scope of the present invention is not limited to the examples. In addition, in the following examples, unless otherwise specified, various measurements and evaluations are performed using the following methods.

[0219] [Viscosity measurement]

[0220] The viscosity was measured at 25° C. using an E-type viscometer (Brookfield, trade name: DV-II+Pro). The rotation speed was set so that the torque was 10% to 90%, and the value when the viscosity stabilized was read 2 minutes after the start of the measurement.

[0221] [Determination of weight average molecular weight]

[0222] The weight average molecular weight was measured by gel permeation chromatography (manufactured by Tosoh Corporation, trade name: HLC-8220GPC) using polystyrene as a standard substance and N,N-dimethylacetamide as a developing solvent.

[0223] [Determination of glass transition temperature (Tg)]

[0224] The glass transition temperature was measured using a dynamic viscoelasticity measuring device (DMA: manufactured by UBM, trade name: E4000F) from 30°C to 400°C at a heating rate of 4°C / min and a frequency of 11 Hz on a polyimide film of size 5 mm×20 mm. The temperature at which the elastic modulus change (tanδ) reached the maximum was taken as the glass transition temperature. The storage modulus at 30°C measured using DMA was 1.0×10 9 Pa or more, and the storage modulus at 360°C is less than 1.0×10 8 Pa is considered as "thermoplastic", and the storage modulus at 30°C is 1.0×10 9 Pa and the storage modulus at 360°C is 1.0×10 8 Those above Pa are considered "non-thermoplastic".

[0225] [Determination of coefficient of thermal expansion (CTE)]

[0226] Using a thermomechanical analyzer (manufactured by Bruker, trade name: 4000SA), a load of 5.0 g was applied to a polyimide film of size 3 mm×20 mm, and the temperature was raised from 30°C to 265°C at a certain heating rate. The film was then kept at this temperature for 10 minutes and then cooled at a rate of 5°C / min to determine the average thermal expansion coefficient (thermal expansion coefficient) from 250°C to 100°C.

[0227] [Measurement of Surface Roughness of Copper Foil]

[0228] Regarding the surface roughness of the copper foil, an atomic force microscope (AFM) (manufactured by Bruker AXS, trade name: Dimension Icon SPM) and a probe (manufactured by Bruker AXS, trade name: TESPA (NCHV), tip curvature radius of 10 nm, spring constant 42 N / m) were used to measure the surface of the copper foil in a range of 80 μm×80 μm in tapping mode to determine the ten-point average roughness (Rz).

[0229] [Determination of peel strength]

[0230] 1) Casting side (resin coating side) of single-sided copper-clad laminate

[0231] After the copper foil of the single-sided copper-clad laminate (copper foil / resin layer) was processed with a width of 1.0 mm, it was cut into 8 cm width × 4 cm length to prepare the measurement sample 1. Regarding the peel strength of the cast side of the measurement sample 1, a tensile tester (Tensilon tester) (manufactured by Toyo Seiki Seisaku-sho, trade name: Universal Testing Machine (Strograph) VE-1D) was used to fix the resin layer side of the measurement sample 1 on the aluminum plate with double-sided tape, and the copper foil was peeled off at a speed of 50 mm / min in the 90° direction to obtain the central strength when the copper foil was peeled off 10 mm from the resin layer. This value was taken as the peel strength 1A.

[0232] 2) Casting side (resin coating side) of double-sided copper-clad laminate

[0233] After the copper foils on both sides of the thermocompression bonding side and the casting side of the double-sided copper-clad laminate (copper foil / resin layer / copper foil) were processed with a width of 0.8 mm (wiring was processed in such a way that the copper foils on both sides were in the same position), they were cut with a width of 8 cm × a length of 4 cm to prepare a measurement sample 2. Regarding the peel strength of the casting side of the measurement sample 2, a tensile tester (Tensilon tester) (manufactured by Toyo Seiki Seisaku-sho, trade name: Universal Testing Machine (Strograph) VE-1D) was used to fix the copper foil surface on the thermocompression bonding side of the measurement sample 2 on an aluminum plate with a double-sided tape, and the copper foil was peeled off at a speed of 50 mm / min in a 90° direction, and the central value strength when the copper foil on the resin-coated side was peeled off 10 mm from the resin layer was obtained. This value was taken as the peel strength 2A.

[0234] [Measurement of in-plane retardation (RO)]

[0235] Regarding the in-plane retardation (RO), the retardation in the in-plane direction of a given sample was determined using a birefringence meter (manufactured by Photonic-Lattice, trade name: wide range birefringence evaluation system WPA-100, measurement area: MD: 140 mm × TD: 100 mm). In addition, the incident angle was 0° and the measurement wavelength was 543 nm.

[0236] [Determination of tensile modulus]

[0237] The tensile modulus of the copper foil was measured by using a universal testing machine (Strograph) R-1 manufactured by Toyo Seiki Seisaku-sho Co., Ltd., at a temperature of 23°C and a relative humidity of 50%, using a copper foil that had been subjected to a heat treatment in a vacuum oven in the same manner as the treatment process for the copper-clad laminate.

[0238] The abbreviations used in Examples and Comparative Examples represent the following compounds.

[0239] NTCDA: 2,3,6,7-Naphthalenetetracarboxylic dianhydride

[0240] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0241] PMDA: Pyromellitic Dianhydride

[0242] m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl

[0243] m-EOB: 2,2'-diethoxy-4,4'-diaminobiphenyl

[0244] TPE-R: 1,3-bis(4-aminophenoxy)benzene

[0245] DAPE: 4,4'-diaminodiphenyl ether

[0246] BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane

[0247] DMAc: N,N-dimethylacetamide

[0248] (Synthesis example 1)

[0249] Under nitrogen flow, 1146.4 parts by weight of m-TB (5.4 parts by mole) and 175.4 parts by weight of TPE-R (0.6 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 706.1 parts by weight of BPDA (2.4 parts by mole) and 965.4 parts by weight of NTCDA (3.6 parts by mole) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 1. The solution viscosity of the polyamic acid solution 1 was 41,100 cps.

[0250] Then, the polyamic acid solution 1 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization, thereby preparing a polyimide film 1 (biphenyl tetrayl and biphenylene: 65 mol%, non-thermoplastic, Tg: 400° C. or more, CTE: 7.7 ppm / K).

[0251] (Synthesis example 2)

[0252] Under nitrogen flow, 743.0 parts by weight of m-TB (3.5 parts by mole) and 672.4 parts by weight of TPE-R (2.3 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 353.1 parts by weight of BPDA (1.2 parts by mole) and 1233.6 parts by weight of NTCDA (4.6 parts by mole) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 2. The solution viscosity of the polyamic acid solution 2 was 41,900 cps.

[0253] Then, the polyamic acid solution 2 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization and prepare a polyimide film 2 (biphenyl tetrayl and biphenylene: 41 mol%, non-thermoplastic, Tg: 391° C., CTE: 19.1 ppm / K).

[0254] (Synthesis example 3)

[0255] Under nitrogen flow, 1040.2 parts by weight of m-TB (4.9 parts by mole), 350.8 parts by weight of TPE-R (1.2 parts by mole), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 529.6 parts by weight of BPDA (1.8 parts by mole), 643.6 parts by weight of NTCDA (2.4 parts by mole), and 392.6 parts by weight of PMDA (1.8 parts by mole) were added, and the mixture was stirred at room temperature for 3 hours to perform a polymerization reaction, thereby obtaining a polyamic acid solution 3. The solution viscosity of the polyamic acid solution 3 was 32,500 cps.

[0256] Then, the polyamic acid solution 3 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization, thereby preparing a polyimide film 3 (biphenyl tetrayl and biphenylene: 55 mol%, non-thermoplastic, Tg: 377° C., CTE: 14.8 ppm / K).

[0257] (Synthesis Example 4)

[0258] Under nitrogen flow, 552.0 parts by weight of m-TB (2.6 parts by mole), 760.9 parts by weight of DAPE (3.8 parts by mole), and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 1716.3 parts by weight of NTCDA (6.4 parts by mole) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 4. The solution viscosity of the polyamic acid solution 4 was 42,300 cps.

[0259] Then, the polyamic acid solution 4 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization and prepare a polyimide film 4 (biphenylene: 20 mol%, non-thermoplastic, Tg: 400° C. or more, CTE: 32.1 ppm / K).

[0260] (Synthesis Example 5)

[0261] Under nitrogen flow, 898.7 parts by weight of m-EOB (3.3 parts by mole) and 660.8 parts by weight of DAPE (3.3 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 1439.6 parts by weight of PMDA (6.6 parts by mole) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 5. The solution viscosity of the polyamic acid solution 5 was 31,700 cps.

[0262] Then, the polyamic acid solution 5 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization, thereby preparing a polyimide film 5 (biphenylene: 25 mol%, non-thermoplastic, Tg: 376° C., CTE: 33.5 ppm / K).

[0263] (Synthesis Example 6)

[0264] Under nitrogen flow, 63.7 parts by weight of m-TB (0.3 molar parts) and 1490.9 parts by weight of TPE-R (5.1 molar parts) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 1118.0 parts by weight of BPDA (3.8 molar parts) and 349.0 parts by weight of PMDA (1.6 molar parts) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 6. The solution viscosity of the polyamic acid solution 6 was 6,700 cps, and the weight average molecular weight was 163,400.

[0265] Then, the polyamic acid solution 6 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization, thereby preparing a polyimide film 6 (biphenyl tetrayl and biphenylene: 38 mol %, thermoplasticity, Tg: 242° C., storage modulus at 30° C.: 4.3×10 9 Pa, storage modulus at 360°C: 1.4×10 7 Pa).

[0266] (Synthesis Example 7)

[0267] Under nitrogen flow, 743.0 parts by weight of m-TB (3.5 parts by mole) and 672.4 parts by weight of TPE-R (2.3 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 1206.3 parts by weight of BPDA (4.1 parts by mole) and 370.8 parts by weight of PMDA (1.7 parts by mole) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 7. The solution viscosity of the polyamic acid solution 7 was 7,200 cps, and the weight average molecular weight was 112,000.

[0268] Then, the polyamic acid solution 7 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization, thereby preparing a polyimide film 7 (biphenyl tetrayl and biphenylene: 66 mol%, thermoplasticity, Tg: 266° C., storage modulus at 30° C.: 4.3×10 9 Pa, storage modulus at 360°C: 7.1×10 7 Pa).

[0269] (Synthesis Example 8)

[0270] Under nitrogen flow, 233.5 parts by weight of m-TB (1.1 parts by mole) and 1344.7 parts by weight of TPE-R (4.6 parts by mole) and DMAc in an amount such that the solid content concentration after polymerization becomes 15% by weight were added to a reaction tank, and stirred at room temperature to dissolve. Then, 676.7 parts by weight of BPDA (2.3 parts by mole) and 741.6 parts by weight of PMDA (3.4 parts by mole) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to obtain a polyamic acid solution 8. The solution viscosity of the polyamic acid solution 8 was 7,400 cps, and the weight average molecular weight was 163,400.

[0271] Then, the polyamic acid solution 8 was uniformly coated on a stainless steel support substrate in such a manner that the thickness after curing was about 25 μm, and then heated and dried at 120° C. to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120° C. to 360° C. within 30 minutes to complete imidization, thereby preparing a polyimide film 8 (biphenyl tetrayl and biphenylene groups were 30 mol%, thermoplasticity, Tg: 279° C., storage modulus at 30° C.: 4.1×10 9 Pa, storage modulus at 360°C: 7.9×10 7 Pa).

[0272] [Example 1-1]

[0273] On an endless belt-shaped stainless steel support substrate, a multi-manifold three-layer co-extrusion multilayer die was used to continuously extrusion-coat a three-layer structure in the order of polyamic acid solution 7 / polyamic acid solution 1 / polyamic acid solution 7, and the solvent was removed by heating and drying at 130°C for 3 minutes. Then, a step-by-step heat treatment was performed from 130°C to 360°C to complete imidization and prepare a polyimide film 1a' with a thickness of 2.5μm / 20μm / 2.5μm for the thermoplastic polyimide layer / non-thermoplastic polyimide layer / thermoplastic polyimide layer. The polyimide film 1a' on the support substrate was peeled off by a knife edge method to prepare a long strip of polyimide film 1a with a length of 1100mm in the width direction.

[0274] <Preparation of samples for evaluation of in-plane retardation (RO)>

[0275] The left and right ends (left and right) and the center (center) of the long polyimide film 1a in the TD direction were cut into A4 size (TD: 210 mm×MD: 297 mm) to prepare sample L1 (Left), sample R1 (Right), and sample C1 (Center).

[0276] <Evaluation of In-Plane Retardation (RO)>

[0277] The in-plane retardation (RO) was measured for each sample L1, sample R1, and sample C1. The maximum value of the measured value of each sample was taken as the "in-plane retardation (RO)", and the difference between the maximum and minimum values ​​in the measured value of the in-plane retardation (RO) was taken as the "inhomogeneity (ΔRO) of the in-plane retardation (RO) in the width direction (TD direction)". In addition, "under the environment of temperature 360°C and pressure 340MPa / m 2 , holding time 15 minutes "Change in the in-plane retardation (RO) before and after pressurization" is set to the difference between the maximum values ​​of the measured values ​​of the in-plane retardation (RO) of sample C1 before and after pressurization.

[0278] In addition, the measurement area in each sample is as follows.

[0279] Sample L1: left end area in TD direction and central area in MD direction

[0280] Sample R1: right end area in TD direction and central area in MD direction

[0281] Sample C1: Central area in TD and MD directions

[0282] The evaluation results of the long polyimide film 1a are as follows.

[0283] CTE: 17ppm / K

[0284] In-plane retardation (RO): 11nm

[0285] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 1 nm

[0286] At a temperature of 360°C and a pressure of 340 MPa / m 2 、Holding time 15 minutes Change in in-plane retardation (RO) before and after pressurization: 3nm

[0287] [Example 1-2]

[0288] A long polyimide film 1 b was prepared in the same manner as in Example 1-1 except that the length in the width direction (TD direction) was 540 mm.

[0289] The evaluation results of the long polyimide film 1b are as follows.

[0290] CTE: 17ppm / K

[0291] In-plane retardation (RO): 11nm

[0292] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 1 nm

[0293] At a temperature of 360°C and a pressure of 340 MPa / m 2 、Holding time 15 minutes Change in in-plane retardation (RO) before and after pressurization: 3nm

[0294] [Examples 1-3]

[0295] On the surface of a long strip of copper foil 1 (rolled copper foil, manufactured by JX Metal Co., Ltd., trade name: GHY5-93F-HA-V2 foil, thickness: 12 μm, tensile modulus after heat treatment: 18 GPa, length in the width direction: 540 mm), after uniformly applying a polyamic acid solution 7 in a manner that the thickness after hardening becomes 2.5 μm, the solvent is removed by heating and drying at 120 ° C for 1 minute. After uniformly applying a polyamic acid solution 1 thereon in a manner that the thickness after hardening becomes 20 μm, the solvent is removed by heating and drying at 120 ° C for 3 minutes. Furthermore, after uniformly applying a polyamic acid 7 thereon in a manner that the thickness after hardening becomes 2.5 μm, the solvent is removed by heating and drying at 120 ° C for 1 minute. Then, a staged heat treatment is carried out from 130 ° C to 360 ° C, and after completing imidization, a single-sided copper-clad laminate 1a is prepared.

[0296] The evaluation results of the long polyimide film prepared by etching away the copper foil of the single-sided copper-clad laminate 1a are as follows.

[0297] CTE: 17ppm / K

[0298] In-plane retardation (RO): 11nm

[0299] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 1 nm

[0300] The copper foil 1 is stacked on the polyimide layer side of the single-sided copper-clad laminate 1a, and heated at a temperature of 360°C and a pressure of 340 MPa / m 2 The double-sided copper-clad laminate 1a was prepared by thermal compression bonding for 15 minutes under the conditions of . The in-plane retardation (RO) of the long strip of polyimide film prepared by etching away the copper foil of the double-sided copper-clad laminate 1a was 8 nm.

[0301] The center portion of the prepared double-sided copper-clad laminate 1 a was cut to prepare a long copper-clad laminate 1 a ′ (end width: 250 mm) as a material for a sample for evaluation of dimensional stability.

[0302] <Preparation of samples for evaluation of dimensional stability>

[0303] The copper-clad laminate 1a' is cut into pieces with a length of 250 mm in the MD direction to obtain pieces with a size of 250 mm in MD x 250 mm in TD. Figure 6 As shown in the figure, a hypothetical regular quadrilateral is assumed within the range of MD: 200mm × TD: 200mm of the cut copper-clad laminate. In the left and right corner areas (Left and Right) of the hypothetical regular quadrilateral, each of which includes two corners of a common TD direction, and the central area (Center) including the center of the hypothetical regular quadrilateral, 21 holes are continuously opened at intervals of 2.5mm in the MD and TD directions to prepare a sample for evaluation. In addition, a drill with a diameter of 0.105mm is used for the hole opening process.

[0304] <Evaluation of dimensional stability>

[0305] A non-contact CNC image measuring machine (Mitutoyo, trade name: Quick Vision QV-X404PIL-C) was used to measure the positions of the holes before and after the copper foil layers on both sides of the evaluation sample were completely etched and removed. The dimensional change and cumulative dimensional change of the distance between two adjacent holes before and after etching were calculated based on the measured values.

[0306] Prepare a long copper-clad laminate 1a', such as Figure 7Evaluation samples 1 and 2 were prepared as shown. The positions of the holes before and after etching of the Center, Left, and Right holes were measured for the evaluation samples 1 and 2. The dimensional change of the distance between two adjacent holes before and after etching and the cumulative dimensional change of the total (20 locations) were calculated from the measured values.

[0307] According to the evaluation results of the copper-clad laminate 1a', the cumulative dimensional change and non-uniformity of MD are shown in Table 1. In addition, in Table 1, the cumulative dimensional change rate of Left, Center, and Right and the cumulative converted dimensional change amount converted to the assumed FPC size of 10mm are expressed, and the non-uniformity of the entire range of Left, Center, and Right is also shown. In addition, the "cumulative dimensional change rate" refers to the ratio (%) of the cumulative dimensional change amount to the total value of the distance between the two holes before etching. In addition, the numerical value of the "range" in the table refers to the central value of the entire range of Left, Center, and Right ± the upper and lower range (the same in Table 2 and Table 3).

[0308] [Table 1]

[0309]

[0310] According to the results, it was confirmed that the displacement ratio of the wiring and the non-uniformity of the dimensional change rate within the test piece surface can be evaluated for the circuit wiring substrate (L / S=0.025mm / 0.0025mm) formed by using the copper-clad laminate 1a' as a material, and it was confirmed that the non-uniformity of the displacement ratio of the wiring at each FPC size of the double-sided copper-clad laminate 1a of Examples 1-3 was small. In addition, it was confirmed that in order to achieve high dimensional stability accuracy of the copper-clad laminate that cannot be achieved by controlling the CTE of the polyimide film alone, it is important to control the in-plane delay.

[0311] [Examples 1-4]

[0312] Copper foil 1 was overlapped on both sides of the long strip polyimide film 1b prepared in Example 1-2, and the film was heated at 360°C and 340 MPa / m 2 The double-sided copper-clad laminate 1b was prepared by thermal compression bonding under conditions of 100°C for 15 minutes, and a long copper-clad laminate 1b' (end width: 250 mm) was prepared in the same manner as in Example 1-3, and the dimensional stability was evaluated. The results are shown in Table 2.

[0313] [Table 2]

[0314]

[0315] [Comparative Example 1-1]

[0316] A long polyimide film 1c (thickness: 25 μm, manufactured by Kaneka Corporation, trade name: Pixeo) was prepared.

[0317] The evaluation results of the long polyimide film 1c are as follows.

[0318] CTE: 17ppm / K

[0319] In-plane retardation (RO): 200nm

[0320] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 80nm

[0321] At a temperature of 360°C and a pressure of 340 MPa / m 2 、Holding time 15 minutes Change in in-plane retardation (RO) before and after pressurization: 30nm

[0322] [Comparative Example 1-2]

[0323] Copper foil 1 is laminated on both sides of the long polyimide film 1c and heated at 360°C and 340 MPa / m 2 The double-sided copper-clad laminate 1c was prepared by thermal compression bonding under the conditions of 100°C for 15 minutes, and a long copper-clad laminate 1c' (end width: 250 mm) was prepared in the same manner as in Example 1-3, and the dimensional stability was evaluated. The results are shown in Table 3.

[0324] [Table 3]

[0325]

[0326] [Example 2-1]

[0327] A long polyimide film 2 having a width direction length of 1100 mm was prepared in the same manner as in Example 1-1 except for a three-layer structure of polyamic acid solution 8 / polyamic acid solution 1 / polyamic acid solution 8 in this order.

[0328] The evaluation results of the long polyimide film 2 are as follows.

[0329] CTE: 17ppm / K

[0330] In-plane retardation (RO): 11nm

[0331] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 1 nm

[0332] At a temperature of 360°C and a pressure of 340 MPa / m 2 、Holding time 15 minutes Change in in-plane retardation (RO) before and after pressurization: 5nm

[0333] [Example 3-1]

[0334] A long polyimide film 3 having a width direction length of 1100 mm was prepared in the same manner as in Example 1-1 except for a three-layer structure of polyamic acid solution 6 / polyamic acid solution 2 / polyamic acid solution 6 in this order.

[0335] The evaluation results of the long polyimide film 3 are as follows.

[0336] CTE: 17ppm / K

[0337] In-plane retardation (RO): 17nm

[0338] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 3nm

[0339] At a temperature of 360°C and a pressure of 340 MPa / m 2 、Holding time 15 minutes Change in in-plane retardation (RO) before and after pressurization: 7nm

[0340] [Example 4-1]

[0341] A long polyimide film 4 having a width direction length of 1100 mm was prepared in the same manner as in Example 1-1 except for a three-layer structure of polyamic acid solution 8 / polyamic acid solution 3 / polyamic acid solution 8 in this order.

[0342] The evaluation results of the long polyimide film 4 are as follows.

[0343] CTE: 17ppm / K

[0344] In-plane retardation (RO): 15nm

[0345] In-plane retardation (RO) non-uniformity (ΔRO) in the width direction (TD direction): 2nm

[0346] At a temperature of 360°C and a pressure of 340 MPa / m 2 、Holding time 15 minutes Change in in-plane retardation (RO) before and after pressurization: 10nm

[0347] As mentioned above, although embodiment of this invention was demonstrated in detail for the purpose of illustration, this invention is not limited to the said embodiment, Various deformation|transformation is possible.

[0348] This application claims the benefit of priority based on Japanese Patent Application No. 2016-89514, filed on Apr. 27, 2016, the entire contents of which are incorporated herein by reference.

Claims

1. A polyimide film comprising a thermoplastic polyimide layer comprising a long strip of thermoplastic polyimide on at least one side of a non-thermoplastic polyimide layer comprising a non-thermoplastic polyimide, and The polyimide film has a film width in the range of 490 mm to 1100 mm, and satisfies the following conditions i to iv and vii: iThe thermal expansion coefficient is in the range of 10ppm / K to 30ppm / K; ii. The glass transition temperature of the thermoplastic polyimide is within the range of 200° C. to 350° C.; iii. the value of in-plane retardation is within the range of 5 nm to 50 nm; iv The in-plane retardation non-uniformity in the width direction is less than 10 nm, The tetracarboxylic acid residues derived from 3,3',4,4'-biphenyltetracarboxylic dianhydride are in the range of 20.69 mol parts to 70 mol parts based on 100 mol parts of all tetracarboxylic acid residues contained in the non-thermoplastic polyimide; and vii The thermoplastic polyimide contains a tetracarboxylic acid residue and a diamine residue, both of which are aromatic groups, and the aromatic group includes a biphenyl tetrayl group or a biphenylene group, and the biphenyl tetrayl group or the biphenylene group is in the range of 30 mol parts or more and 80 mol parts or less relative to 100 mol parts in total of the tetracarboxylic acid residue and the diamine residue.

2. The polyimide film according to claim 1, characterized in that: In addition to the above conditions i-iv and vii, the following conditions are further satisfied: vAt a temperature of 360°C and a pressure of 340MPa / m 2 , the change in in-plane retardation before and after pressurization is less than 20 nm when the holding time is 15 minutes.

3. The polyimide film according to claim 1 or 2, characterized in that: In addition to the above conditions i-iv and vii, the following conditions are further satisfied: vi The non-thermoplastic polyimide contains a tetracarboxylic acid residue and a diamine residue, both of which are aromatic groups, and the aromatic group includes a biphenyl tetrayl group or a biphenylene group, and the biphenyl tetrayl group or the biphenylene group is 40 molar parts or more relative to a total of 100 molar parts of the tetracarboxylic acid residue and the diamine residue.

4. The polyimide film according to claim 1 or 2, characterized in that: The tetracarboxylic acid residue derived from 3,3′,4,4′-biphenyltetracarboxylic dianhydride is 40 parts by mole or more based on 100 parts by mole of all tetracarboxylic acid residues contained in the thermoplastic polyimide.

5. The polyimide film according to claim 1 or 2, characterized in that: The diamine residue represented by the following general formula (1) is 20 mol parts or more relative to 100 mol parts of all diamine residues contained in the non-thermoplastic polyimide. In the formula, R1 and R2 independently represent an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an alkenyl group having 2 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group.

6. The polyimide film according to claim 1 or 2, characterized in that: The diamine residue represented by the following general formula (2) is in the range of 3 mol parts or more and 60 mol parts or less relative to 100 mol parts of all diamine residues contained in the thermoplastic polyimide. In the formula, R3 and R4 independently represent an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, or an alkenyl group having 1 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group.

7. A copper-clad laminate comprising an insulating layer and a copper layer located on at least one surface of the insulating layer, wherein: The insulating layer includes a thermoplastic polyimide layer in contact with the surface of the copper layer and a non-thermoplastic polyimide layer laminated indirectly. The insulating layer includes the polyimide film according to any one of claims 1 to 6.

8. The copper-clad laminate according to claim 7, characterized in that: The dimensional change in the length direction and the dimensional change in the width direction of the copper layer before and after etching are both 2% or less.

Citation Information

Patent Citations

  • Polyimide optical wave plate and its production

    JP2000356713A

  • Rolled copper foil, process of manufacturing the same, and laminate sheet

    JP2014011451A

  • Rolled copper foil and copper-clad laminate

    JP2014015674A

  • Water discharge device

    JP2016089514A

  • Adhesive film, flexible metal-clad laminate, and process for producing the same

    JP2005350668A