Method for judging shear strength of composite layer of pipe
By measuring the length of steel wire throughput under the cyclic changes of high and low temperatures, the problem of the failure of the existing technology to detect the shear strength of steel wire and bonding resin in composite pipes is solved, rapid detection and process adjustment are achieved, and the comprehensive performance of composite pipes is improved and Service life.
Patent Information
- Application Number
- CN202110602798.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-05-31
AI Technical Summary
The prior art cannot effectively detect the shear strength of the steel wire layer and the adhesive resin layer in the steel wire mesh reinforced polyethylene composite pipe, resulting in stress release and weakening of the bonding strength, affecting service life.
By measuring the length of the steel wire under the cyclic changes of high and low temperatures, calculating the percentage of the steel wire, judging the shear strength of the composite layer, and quickly detecting the shear strength of the steel wire and the bonding resin in the manufactured composite pipe.
It realizes rapid detection of the shear strength of steel wire and adhesive resin in composite pipes, timely adjusts the manufacturing process, improves the internal quality of the product, and improves service life and performance stability.
Smart Images

Figure CN113533083B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite pipes, and in particular to a method for judging the shear strength of a composite layer of a pipe. Background Art
[0002] The statements in this section merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] The steel mesh reinforced polyethylene composite pipe is a composite pipe formed by melting and compounding, with pipe-grade polyethylene as the matrix, steel wires coated with adhesive resin are continuously wound left and right to form a mesh structure as the reinforcement, and the polyethylene of the matrix and the steel wire of the reinforcement are connected as a whole by adhesive resin. The polar chemical bonds in the molecular chain of the adhesive resin form van der Waals force with the surface of the steel wire, which restrains the steel wire from moving in the pipe. The apparent test of this van der Waals force is the shear strength of the composite layer.
[0004] During the production process of wire mesh reinforced polyethylene composite pipes, the steel wires are arranged tightly and orderly, and are in a relatively tight state when wound, resulting in stress between the steel wires and the adhesive resin layer. Due to the existence of interlayer van der Waals force, the steel wires and the adhesive layer do not move. If the adhesive resin coating effect is not good (such as coating temperature difference, wind ring wind speed and other factors), resulting in weak adhesion between the composite layers, stress release will occur between the steel wire and the adhesive resin as time and environment change. This stress release causes different degrees of steel wire movement, thereby weakening the bonding strength of the bonding layer of the wire mesh skeleton polyethylene composite pipe and causing failure.
[0005] In the prior art, there is only a method for verifying the shear strength between steel wire and adhesive resin raw materials, but there is no mention of a method for testing the shear strength between steel wire and adhesive resin in the finished composite pipe. There is no method for testing the bonding strength between the steel wire layer and the adhesive resin layer in the finished steel wire mesh skeleton polyethylene composite pipe. Summary of the invention
[0006] In order to solve the technical problems existing in the above-mentioned background technology, the present invention provides a method for judging the shear strength between the steel wire layer and the polyethylene composite layer in a steel wire mesh reinforced polyethylene composite pipe. By cyclically changing high and low temperatures, the stress change between the steel wire and the adhesive resin is accelerated, the length of the protruding steel wire is obtained, and the steel wire mesh reinforced polyethylene composite pipes of the same specification are compared horizontally to reflect the shear strength of the composite layer.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] A first aspect of the present invention provides a method for determining the shear strength of a composite layer of a pipe, comprising the following steps:
[0009] Cutting a composite pipe sample with a set length of L;
[0010] The temperature of the environment in which the composite pipe sample is located is changed according to the set upper and lower temperature limits and cycle period, and the steel wire extension lengths b and c at both ends of the composite pipe sample are obtained;
[0011] The steel wire extension lengths b and c and the composite pipe sample L are used to obtain the steel wire penetration percentage at the end of the composite pipe sample and determine the shear strength of the composite layer of the pipe.
[0012] The composite pipe specimens include a test group and a control group; the specimen length of the test group is L, and the length of the control group is: L±1% of the length of the test group.
[0013] The set upper temperature limit is not higher than 80°C, and the set lower temperature limit is not lower than -30°C; the cycle period is a fixed interval period.
[0014] The wire extension lengths b and c are the average values of the extension lengths of four points at a circumferential distance of 1 / 4 of the circumference of the same end face of the composite pipe sample.
[0015] Wire penetration percentage Among them, b and c are the steel wire extension lengths at the two end surfaces of the composite pipe sample after cyclic temperature change, and L is the length of the composite pipe sample.
[0016] The composite pipe is a steel wire mesh reinforced polyethylene composite pipe, comprising two groups of coaxially arranged polyethylene layers, a steel wire layer inside the polyethylene layer, and the steel wire layer is connected to the polyethylene layer through an adhesive resin.
[0017] Compared with the prior art, one or more of the above technical solutions have the following beneficial effects:
[0018] 1. It can quickly detect the shear strength of steel wire and bonding resin in the manufactured composite pipe.
[0019] 2. By storing in high and low temperature environments for a short period of time, the shear strength change of the steel wire and the bonding resin is accelerated, thereby accelerating the stress release process of the pipe, so that the cause of the shear strength change can be found in time during the manufacturing process of the composite pipe so as to adjust the manufacturing process, improve the inherent quality of the composite pipe product, and improve the comprehensive performance and performance stability of the steel wire mesh skeleton polyethylene composite pipe, thereby increasing the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0021] Figure 1 is a schematic diagram of the structure of a composite pipe to be inspected provided by one or more embodiments of the present invention;
[0022] Figure 2 is a schematic diagram of the composite pipe structure in a steel wire passing-through state provided by one or more embodiments of the present invention;
[0023] Figure 3 is a schematic diagram of a steel wire penetration length measurement point provided by one or more embodiments of the present invention;
[0024] In the figure: 1. polyethylene layer, 2. steel wire layer, 21. protruding steel wire, 3. bonding resin. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0026] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0027] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0028] As described in the background technology, the wire mesh reinforced polyethylene composite pipe product standard GB / T32439-2015 only requires verification of the shear strength of the steel wire raw materials and the bonding resin raw materials themselves, but does not mention the detection method of the shear strength of the steel wire and the bonding resin in the pipe after the above materials are made into finished pipes. It is impossible to verify the bonding strength between the steel wire layer and the bonding resin layer in the finished wire mesh skeleton polyethylene composite pipe.
[0029] The steel mesh reinforced polyethylene composite pipe is a composite pipe formed by continuously winding steel wires coated with adhesive resin to form a mesh structure as a reinforcement, using pipeline-grade polyethylene as a matrix, connecting the matrix and the reinforcement as a whole using adhesive resin, and then forming the composite pipe through melt compounding.
[0030] During the pipe manufacturing process, the steel wires are arranged tightly and orderly, and are in a relatively tight state when wound. There is stress between the steel wires and the bonding resin layer, which prevents the steel wires and the bonding layer from shifting. If the bonding resin coating effect is not good (such as coating temperature difference, wind ring wind speed and other factors), resulting in weak adhesion between the composite layers, stress release will occur between the steel wires and the bonding resin as time and environment change, which is reflected in different degrees of steel wire movement, resulting in failure of the bonding strength of the bonding layer of the steel wire mesh skeleton polyethylene composite pipe. Intuitively, the steel wire will pass through one end of the end face of the composite pipe, causing difficulties in flange installation and pipe docking during use, thereby affecting the service life of the steel wire mesh reinforced polyethylene composite pipe.
[0031] Therefore, the following embodiment provides a method for judging the shear strength of the composite layer of a pipe. Since the steel wire and polyethylene have different shrinkage rates, the cyclic change of high and low temperatures is used to accelerate the change of stress between the steel wire and the bonding resin. The steel wire mesh reinforced polyethylene composite pipes of the same specification are compared horizontally. By measuring the length of the steel wire protruding from the pipe end of the fixed-length steel wire mesh reinforced polyethylene composite pipe, when the bonding resin has a strong shear resistance to the steel wire, the steel wire and the bonding resin are not easy to be relatively displaced, and the length of the steel wire protruding is small; when the bonding resin has a weak shear resistance to the steel wire, the length of the steel wire protruding is long, so as to detect the shear strength of the steel wire and the bonding resin of the overall pipe. The greater the high and low temperature difference, the more obvious the acceleration effect.
[0032] Embodiment 1:
[0033] The wire mesh reinforced polyethylene composite pipe includes two groups of coaxially arranged polyethylene layers 1, wherein the polyethylene layer 1 has a steel wire layer 2 inside, and the steel wire layer 2 is connected to the polyethylene layer 1 through an adhesive resin 3; after the stress of the steel wire layer 2 is released, it separates from the adhesive resin 3 to form a protruding steel wire 21, and the protruding steel wire 21 is located at the cross sections at both ends of the wire mesh reinforced polyethylene composite pipe.
[0034] like Figure 1-3 As shown, the method for determining the shear strength of the composite layer of a pipe comprises the following steps:
[0035] S1: Cut multiple sections of wire mesh reinforced polyethylene composite pipes of the same length and grind both ends of the pipes flat using equipment, such as Figure 1 As shown, measure the sample length L;
[0036] The cut length should be no less than 1 meter, and the length L deviation of the comparison group sample should be controlled within 1%;
[0037] S2: Place the sample in a test chamber with adjustable high and low temperatures for cyclic testing. The intervals are equal. After the test, observe the end surface of the pipe and measure the lengths b and c of the steel wires at both ends of the pipe. Figure 2 ).
[0038] The high temperature should be controlled below 80℃, and the low temperature should be controlled above -30℃, but the temperature difference should be set as high as possible to make the test phenomenon of the steel wire passing through the end face of the pipe more obvious;
[0039] The wire extension length b / c value should be the average of the extension lengths of four points at the same end face, each 1 / 4 of the circumference. Figure 3 ).
[0040] For example Figure 3 In the figure, the color line indicates the horizontal line of the pipe section. The line passes through two points on the outer diameter of the pipe section, namely Figure 3 1.74m and 1.67m in the figure, and then take a line perpendicular to the color line through the other two points on the outer diameter of the pipe section, that is, Figure 3 1.73m and 1.69m.
[0041] S3: Calculate the end wire penetration percentage The shear state of the steel wire and the bonding resin is detected based on the percentage of the results.
[0042] The above method can quickly detect the shear strength of steel wire and adhesive resin in the steel wire skeleton polyethylene composite pipe, accelerate the shear strength change of steel wire and adhesive resin by short-term storage in high temperature and low temperature environments, thereby accelerating the stress release process of the pipe, so that the cause of the shear strength change can be found in time during the manufacturing process of the composite pipe so as to adjust the manufacturing process, improve the intrinsic quality of the composite pipe product, improve the comprehensive performance and performance stability of the steel wire skeleton polyethylene composite pipe, and thus increase the service life.
[0043] The following are several sets of experimental data to reflect the effect of this embodiment:
[0044] Experiment 1:
[0045] Batch A wire mesh skeleton polyethylene composite pipe φ200*3.5MPa model;
[0046] Adhesive resin layer: 100% adhesive resin (Shandong Donghong EN360 adhesive resin);
[0047] The pipe cutting size is 0.5m per pipe, and a total of 6 pipes are cut;
[0048] The test chamber temperature was set at -30°C for low temperature and 80°C for high temperature. The temperature was changed every 6 hours, and the cycle lasted for 12 hours. The test data are shown in Table 1.
[0049] Table 1: Batch A 0.5m long pipe test data
[0050]
[0051] Experiment 2:
[0052] Batch A wire mesh skeleton polyethylene composite pipe φ200*3.5MPa model;
[0053] Adhesive resin layer: 100% adhesive resin (Shandong Donghong EN360 adhesive resin);
[0054] The pipe cutting size is 1.0m per pipe, and a total of 6 pipes are cut;
[0055] The test chamber temperature was set at -30°C for low temperature and 80°C for high temperature. The temperature was changed every 6 hours, and the cycle lasted for 12 hours. The test data is shown in Table 2.
[0056] Table 2: Test data of batch A1m long pipe
[0057]
[0058] Experiment 3:
[0059] Batch A wire mesh skeleton polyethylene composite pipe φ200*3.5MPa model;
[0060] Adhesive resin layer: 100% adhesive resin (Shandong Donghong EN360 adhesive resin);
[0061] The pipe cutting size is 1.5m per pipe, and a total of 6 pipes are cut;
[0062] The test chamber temperature was set at -30°C for low temperature and 80°C for high temperature. The temperature was changed every 6 hours, and the cycle lasted for 12 hours. The test data are shown in Table 3.
[0063] Table 3: Test data of batch A 1.5m long pipe
[0064]
[0065]
[0066] Experiment 4:
[0067] Batch A wire mesh skeleton polyethylene composite pipe φ200*3.5MPa model;
[0068] Adhesive resin layer: 100% adhesive resin (Shandong Donghong EN360 adhesive resin);
[0069] The pipe cutting size is 2.0m per pipe, and a total of 6 pipes are cut;
[0070] The test chamber temperature was set at -30°C for low temperature and 80°C for high temperature. The temperature was changed every 6 hours and the cycle lasted for 12 hours. The test data are shown in Table 4.
[0071] Table 4: Test data of batch A2m long pipe
[0072]
[0073]
[0074] Experiment 5:
[0075] Batch A wire mesh skeleton polyethylene composite pipe φ200*3.5MPa model;
[0076] Adhesive resin layer: 100% adhesive resin (Shandong Donghong EN360 adhesive resin);
[0077] The pipe cutting size is 1.5m per pipe, and a total of 6 pipes are cut;
[0078] The test chamber temperature was set at -20°C for low temperature and 60°C for high temperature. The temperature was changed every 6 hours, and the cycle lasted for 12 hours. The test data is shown in Table 5.
[0079] Table 5: Batch A - 20℃ to 60℃ test data
[0080]
[0081] Experiment 6:
[0082] Batch B wire mesh skeleton polyethylene composite pipe φ200*3.5MPa model;
[0083] Adhesive resin layer: 100% polyethylene resin (Qilu Petrochemical DGDB2480 polyethylene resin);
[0084] The pipe cutting size is 1.5m per pipe, and a total of 6 pipes are cut;
[0085] The test chamber temperature was set at -30°C for low temperature and 80°C for high temperature. The temperature was changed every 6 hours, and the cycle lasted for 12 hours. The test data are shown in Table 6.
[0086] Table 6: Batch B 1.5m long pipe test data
[0087]
[0088] By comparing the average values of the four test groups 1 / 2 / 3 / 4, it can be seen that the test data of the same batch of wire mesh skeleton polyethylene composite pipes with different lengths have slight deviations. The longer the pipe, the longer the test acceleration time.
[0089] Comparing the test variances of the four groups of experiments 1 / 2 / 3 / 4, we can see that among the pipes in the same batch, the test variance of the 1.5-meter pipe is the smallest;
[0090] Comparing experiments 3 / 5, it can be seen that in the same batch of pipes, the greater the temperature difference, the more obvious the acceleration effect;
[0091] From the comparison experiment 3 / 6, it can be seen that the worse the bonding effect of the bonding resin is, the smaller the shear force between the steel wire and the resin layer is, and the greater the steel wire penetration rate is.
[0092] The above experiments show that in the process of judging the shear strength of the pipe composite layer by the percentage of steel wire penetration, the length of the pipe sample, the bonding effect of the bonding resin and the temperature conditions are all factors that affect the shear strength of the pipe composite layer.
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for determining the shear strength of a composite layer of a pipe, characterized in that: The following steps are involved: Cutting a composite pipe sample with a set length of L; The temperature of the environment in which the composite pipe sample is located is changed according to the set temperature upper and lower limits and temperature cycle period, and the steel wire extension lengths b and c at both ends of the composite pipe sample are obtained; the set temperature upper limit is not higher than 80°C, and the set temperature lower limit is not lower than -30°C; The steel wire extension length b, c, and the composite pipe sample L are used to obtain the steel wire penetration percentage of the composite pipe sample end face, and the shear strength of the composite layer of the pipe is determined; the steel wire extension length b, c values are the average of the extension lengths of 4 points at a circumferential interval of 1 / 4 of the circumference of the same end face of the composite pipe sample; the steel wire penetration percentage , where b and c are the steel wire extension lengths at both ends of the composite pipe sample after cyclic temperature change, and L is the length of the composite pipe sample; The composite pipe is a steel wire mesh reinforced polyethylene composite pipe.
2. The method for determining the shear strength of a composite layer of a pipe according to claim 1, characterized in that: The composite pipe sample includes a test group and a control group.
3. The method for determining the shear strength of a composite layer of a pipe according to claim 2, wherein: The sample length of the test group is L, and the length of the control group is: the test group length L±1%.
4. The method for determining the shear strength of a composite layer of a pipe according to claim 1, wherein: The cycle period is a fixed interval period.
5. The method for determining the shear strength of a composite layer of a pipe according to claim 1, wherein: The steel wire mesh reinforced polyethylene composite pipe comprises two groups of polyethylene layers arranged coaxially, a steel wire layer is arranged inside the polyethylene layer, and the steel wire layer is connected to the polyethylene layer through an adhesive resin.