Binder composition for enhancing adhesion of catalyst support coatings

By using a variety of adhesive compositions with different average particle sizes, the problem of adjusting the bond strength of the catalyst support coating on the substrate is solved, the uniformity and stability of the support coating are improved, and efficient nitrogen oxide removal is achieved.

CN113557089BActive Publication Date: 2024-11-01BASF MOBILE EMISSIONS CATALYSTS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080020355.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-20
Filing Date
2020-03-12
Publication Date
2024-11-01
Estimated Expiration
2040-03-12

AI Technical Summary

Technical Problem

The adhesive strength of the existing catalyst support coating on the substrate is difficult to adjust, resulting in uneven coating and loss of the support coating, making it difficult to obtain a suitable adhesive content for long-term use.

Method used

Using a variety of adhesive compositions, including first, second and third adhesive materials with different average particle sizes, a carrier coating slurry is formed to improve adhesion and viscoelasticity by defining their ratios and concentrations, Ensure uniformity and long-term stability of the carrier coating.

Benefits of technology

The adhesive strength and uniformity between the catalyst support coating and the substrate are improved, the service life of the support coating is extended, the total mass loss of the support coating is reduced, and more efficient nitrogen oxide removal is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113557089B_ABST
    Figure CN113557089B_ABST
Patent Text Reader

Abstract

The present disclosure provides an adhesive composition formed by a variety of adhesive materials with different average particles, and the adhesive composition can be used to improve the adhesion of carrier coatings on substrates. The improvement of adhesion can be related to increasing the concentration of adhesive without significantly or significantly increasing the associated viscosity. Such adhesive compositions can include a first adhesive material formed by a plurality of particles with a first average particle size and a second adhesive material formed by a plurality of particles with a second average particle size, wherein the ratio of the first average particle size to the second average particle size is about 2 or larger. The present disclosure further provides a catalyst composition, a catalyst product and an emission system incorporated with the adhesive composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 818378, filed on March 14, 2019, and to European Application No. 19175283.1, filed on May 20, 2019, in its entirety. Technical Field

[0003] The present invention relates generally to the field of compositions useful in forming catalysts, and to the field of catalytic articles comprising such compositions and methods of making and using such catalytic articles. Background Art

[0004] Over time, nitrogen oxides (NO x ) cause atmospheric pollution. Exhaust gases from internal combustion engines (e.g., in cars and trucks), combustion plants (e.g., power stations heated by natural gas, oil, or coal), and nitric acid production facilities contain NO x .

[0005] Various treatment methods have been used to treat NO x A gas mixture is used to reduce atmospheric pollution. One treatment involves catalytic reduction of nitrogen oxides. There are two methods: (1) a non-selective reduction method, in which carbon monoxide, hydrogen or lower hydrocarbons are used as reducing agents; and (2) a selective reduction method, in which ammonia or an ammonia precursor is used as a reducing agent. In the selective reduction method, a high degree of nitrogen oxide removal can be achieved with a small amount of reducing agent.

[0006] Catalytic articles useful for providing such catalytic reduction are typically prepared by applying the catalyst material to a substrate, typically in the form of a washcoat composition. To ensure durability of the catalytic article, it is beneficial for the washcoat composition to remain substantially adhered to the substrate with minimal loss throughout the useful life of the catalytic article.

[0007] In order to enhance the bonding strength between the catalyst carrier coating and the substrate, one or more adhesives can be added to the carrier coating composition. However, improving the bonding of the carrier coating to the substrate by using an adhesive may be problematic. Increasing the total adhesive content in the carrier coating composition can significantly increase the total viscosity of the composition, which in turn can hinder the uniform coating of the carrier coating composition along the substrate. The unevenness of the coating can then cause the carrier coating to be lost over time. On the other hand, reducing the total adhesive content in the carrier coating composition may undesirably reduce the bonding strength of the carrier coating to the substrate. The reduction in bonding strength can then cause the carrier coating to be lost over time. Therefore, it may be difficult to obtain the appropriate adhesive content required to achieve a suitable loss curve, and the art still needs another adhesive composition for forming a catalytic product. Summary of the invention

[0008] The present disclosure relates to compositions that can be used to form catalyst articles. The compositions include multiple binders having different average particle sizes, the multiple binders being present in defined ratios. The compositions including the multiple binders are useful for enhancing the adhesion of catalyst support coatings on substrates. The combination of multiple binders specifically described herein can increase the total binder content, which can be utilized without undesirably increasing the viscosity of the support coating. Likewise, the combination of multiple binders can improve the viscoelastic behavior of the support coating with which it is adhered to the substrate.

[0009] In one or more embodiments, the present disclosure may relate to an adhesive composition comprising a plurality of adhesive materials having a defined ratio and size. For example, the adhesive composition may include: a first adhesive material, the first adhesive material being formed by a plurality of particles having a first average particle size; and a second adhesive material, the second adhesive material being formed by a plurality of particles having a second average particle size; wherein the ratio of the first average particle size to the second average particle size is about 2 or greater. In further embodiments, the adhesive composition may be defined with respect to one or more of the following statements, which may be combined in any number and order.

[0010] The first binder material and the second binder material are independently selected from the group consisting of an alumina-containing material, a silica-containing material, a zirconia-containing material, a ceria-containing material, a lanthanum-containing material, a yttria-containing material, and combinations thereof.

[0011] The first binder material is an alumina-containing material, and the second binder material is a zirconia-containing material.

[0012] The adhesive composition further includes a third adhesive material formed from a plurality of particles having a third average particle size, wherein a ratio of the third average particle size to the first average particle size is about 2 or greater, or wherein a ratio of the second average particle size to the third average particle size is about 2 or greater.

[0013] The adhesive composition further includes a third adhesive material formed of a plurality of particles having a third average particle size, wherein a ratio of the first average particle size to the third average particle size is about 2 or greater.

[0014] The first average particle size is about 50 nm to about 1000 nm.

[0015] The second average particle size is from about 10 nm to about 500 nm.

[0016] The first binder material and the second binder material are present in a concentration ratio of about 0.01 to about 0.5.

[0017] One or both of the first binder material and the second binder material are catalytic.

[0018] In one or more embodiments, the present disclosure may be directed to a washcoat slurry. For example, such washcoat slurry may include: a liquid medium; and a binder composition as otherwise described herein. In further embodiments, the washcoat slurry may be defined with respect to one or more of the following statements, which may be combined in any number and order.

[0019] The adhesive composition is about 0.01 to about 1.0 g / in 3 and wherein the washcoat slurry is present in an amount of about 300 s -1 The viscosity of the above-mentioned compositions is about 100 cP or less.

[0020] The carrier coating slurry is heated for about 300 s. -1 The viscosity of the above-mentioned compositions is about 50 cP or less.

[0021] The washcoat slurry further includes a catalyst material.

[0022] In one or more embodiments, the present disclosure may be directed to a catalyst article. For example, a catalyst article may include a catalyst substrate having a plurality of channels suitable for gas flow, the wall surface of each channel being adhered to a catalytic coating comprising an adhesive composition described further herein. In further embodiments, the catalyst article may be defined with respect to one or more of the following statements, which may be combined in any number and order.

[0023] The catalytic coating includes a catalyst material in combination with the binder composition.

[0024] The catalyst substrate is a honeycomb including a wall flow filter substrate or a flow-through substrate.

[0025] The catalytic coating has a concentration of at least about 1.0 g / in 3 A loading of is present on the substrate.

[0026] The catalyst substrate comprises a first coating of the catalytic coating and comprises a second coating having a different overall composition, the second coating being disposed overlying at least a portion of the first coating of the catalytic coating.

[0027] One or both of the following conditions may be met: the first binder material is present in an amount of about 0.1 wt % to about 5 wt % of the total dry gain of the first coating of the catalytic coating; the second binder material is present in an amount of about 7 wt % to about 20 wt % of the total dry gain of the first coating of the catalytic coating.

[0028] In one or more embodiments, the present disclosure may be directed to an emission treatment system for treating an exhaust gas stream. For example, the emission treatment system may include: an engine that generates an exhaust gas stream; and a catalyst article as further described herein, the catalyst article being positioned downstream of the engine and in fluid communication with the exhaust gas stream. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] To provide an understanding of embodiments of the invention, reference is made to the accompanying drawings, which are not necessarily drawn to scale and in which reference numerals refer to components of exemplary embodiments of the invention. The drawings are merely exemplary and should not be construed as limiting the invention.

[0030] Figure 1 is a perspective view of a honeycomb-type substrate carrier that may include a washcoat composition according to the present invention;

[0031] Figure 2 is relative to Figure 1 Zoom in and follow the Figure 1 A partial cross-sectional view taken in a plane of an end face of a substrate carrier, the substrate carrier representing an integral flow-through substrate, the figure showing Figure 1 an enlarged view of the plurality of airflow channels shown;

[0032] Figure 3 is relative to Figure 1 A cross-sectional view of an enlarged portion of the Figure 1 The honeycomb-type substrate carrier in the figure represents the entire wall-flow filter substrate;

[0033] Figure 4 is a schematic diagram of an emissions treatment system in which the washcoat composition of the present invention is utilized;

[0034] Figure 5 is a schematic diagram of an emissions treatment system in which the washcoat composition of the present invention is used to form a side-by-side coating;

[0035] Figure 6 is a schematic diagram of an emissions treatment system in which the washcoat composition of the present invention is utilized;

[0036] Figure 7 is a schematic diagram of an emissions treatment system in which the washcoat composition of the present invention is utilized and the emissions treatment system includes an optional particulate filter;

[0037] Figure 8 is a contour plot showing viscosity (cP) of an example washcoat composition according to an embodiment of the present disclosure based on relative loadings of particles of a first binder and particles of a second binder, wherein the second binder (y-axis) and the first binder (x-axis) are loadings normalized to a baseline; and

[0038] Fig. 9 is a contour plot showing percent loss of an example washcoat according to an embodiment of the present disclosure based on relative loadings of particles of a first binder and particles of a second binder used in preparing a composition for forming the washcoat, wherein the second binder (y-axis) and the first binder (x-axis) are loadings normalized to a baseline. DETAILED DESCRIPTION

[0039] The present disclosure will now be described more fully below. However, the present disclosure may be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be thorough and complete and will fully convey the scope of the present disclosure to those skilled in the art.

[0040] As used in the specification and claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0041] The term "about" as used in this specification is used to describe and illustrate small fluctuations. For example, the term "about" may refer to less than or equal to ±5%, such as less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.2%, less than or equal to ±0.1%, or less than or equal to ±0.05%. Whether or not explicitly stated, all numerical values ​​herein are modified by the term "about". Values ​​modified by the term "about" certainly include specific values.

[0042] The present disclosure generally provides a composition that can include multiple adhesives. The composition can include one or more catalysts, and the one or more catalysts can include one or more adhesives in the multiple adhesives or can exist in a form other than an adhesive. The present disclosure further provides a carrier coating composition, a catalyst product, and a catalyst system including such a catalyst product. In one or more embodiments, such products and systems may include a three-way conversion (TWC) catalyst composition, a diesel oxidation catalyst (DOC), SCR, and / or an ammonia oxidation catalyst (AMOx). Thus, in certain embodiments, as further described herein, the present composition can be provided in the form of a coating or multiple coatings on a flow-through substrate. In other embodiments, as further described herein, the present composition can be provided in the form of a coating or multiple coatings on a wall-flow substrate.

[0043] For the purposes of this application, the following terms shall have the corresponding meanings set forth below.

[0044] As used herein, the term "catalyst" or "catalyst composition" refers to a material that promotes a reaction.

[0045] As used herein, the terms "upstream" and "downstream" refer to the relative direction of engine exhaust flow from the engine to the tailpipe, with the engine in an upstream position and the tailpipe and any pollution abatement articles (such as filters and catalysts) downstream of the engine.

[0046] As used herein, the term "stream" broadly refers to any combination of flowing gases that may contain solid or liquid particulate matter. The term "gas stream" or "exhaust stream" means a stream of gaseous components (such as the exhaust gas of a lean burn engine) that may contain entrained non-gaseous components such as liquid droplets, solid particles, etc. The exhaust stream of a lean burn engine typically further includes combustion products, products of incomplete combustion, oxides of nitrogen, combustible and / or carbonaceous particulate matter (soot), and unreacted oxygen and nitrogen.

[0047] As used herein, the term "substrate" refers to a monolithic material on which a catalyst composition is placed, typically in the form of a washcoat containing a plurality of particles of the catalytic composition thereon. The washcoat is formed by preparing a slurry containing the particles at a certain solids content (e.g., 10-80 wt%) in a liquid vehicle, which is then applied to the substrate and dried to provide a washcoat layer.

[0048] As used herein, the term "washcoat" has the general meaning in the art as a thin, adherent coating of catalytic or other material applied to a substrate material (such as a honeycomb-type support structure) that is sufficiently porous to allow the treated gas stream to pass therethrough.

[0049] As used herein, the term "catalyst article" refers to an element used to promote a desired reaction. For example, a catalyst article may include a washcoat containing a catalytic composition on a substrate.

[0050] The term "reduce" means a decrease in amount, and "reduce" means a decrease in amount caused by any means.

[0051] In one or more embodiments, the present disclosure provides an adhesive composition. The adhesive composition is formed by a variety of different adhesive materials. In this way, the adhesive composition may include at least a first adhesive material and a second adhesive material. In other embodiments, other adhesive materials may also be used, and such adhesive materials may be referred to as, for example, a third adhesive material, a fourth adhesive material, etc. The adhesive material may be different in one or more aspects. For example, the adhesive material may be different in the chemical properties of the material. In other examples, the adhesive material may be different in one or more physical properties such as the average size of the particles forming the adhesive material. In a specific embodiment, the adhesive material may be different in both chemical structure and one or more physical properties.

[0052] In some embodiments, it has been found that when the adhesive composition according to the present disclosure includes at least a first adhesive material formed of a plurality of particles having a first average particle size and a second adhesive material formed of a plurality of particles having a second average particle size, a particularly desirable effect can be obtained. In embodiments in which a third adhesive material, a fourth adhesive material, or even more adhesive materials are used, the third adhesive material can be formed of a plurality of particles having a third average particle size, the fourth adhesive material can be formed of a plurality of particles having a fourth average particle size, and so on.

[0053] As used herein, the adhesive particle size can be the D50 particle size, or the adhesive particle size can be the average particle size.Term " average particle size " is defined as the particle size sum of all particles measured divided by the total number of particles.Particle size can be calculated using any suitable means in this area.For example, particle size can be measured using laser diffraction, dynamic light scattering (or photon correlation spectroscopy), sedimentation, image analysis, sonometry, or any other art-recognized method can be used.The particle size of the adhesive component can be measured with a measurement range of 0.04 micron to 500 microns using the liquid mode method recommended by the CILAS1064 laser particle size analyzer according to the manufacturer.For the particle of <40nm, the Malvern Zetasizer Pro can be used to measure particle size, and the Malvern Zetasizer Pro is a high-performance two-angle particle and molecular size analyzer, and the analyzer is used to use dynamic light scattering, utilize 'NIBS' optics to enhance the detection of aggregates and the measurement of small samples or diluted samples and extremely low or extremely high concentration samples.

[0054] The material forming the binder particles can vary according to its specific desired use. For example, in order to prepare a catalyst product, it may be desirable to utilize a binder material that also exhibits catalyst activity. Therefore, in some embodiments, one or more binder materials used in the binder composition can be a catalyst material or can provide functional effects in other ways. Similarly, the binder material used can be particularly suitable for improving the bonding of a specific catalyst material to a substrate. In some embodiments, a rare earth metal oxide can be used as a binder material. In an exemplary embodiment, the first binder material and the second binder material (and an optional third binder material or even another binder material) can be independently selected from the group consisting of: alumina-containing materials, silica-containing materials, zirconium oxide-containing materials, cerium oxide-containing materials, lanthanum oxide-containing materials, yttrium oxide-containing materials and combinations thereof. In other exemplary embodiments, the binder material used in the composition of the present disclosure can include a binder formed by cerium oxide, zirconium oxide, yttrium oxide, lanthanum oxide and combinations thereof.

[0055] In one embodiment, the first binder material is an aluminum oxide-containing material, and the second binder material is a zirconium oxide-containing material. In one embodiment, the binder composition includes: a first binder material, the first binder material is formed of a plurality of particles having a first average particle size; and a second binder material, the second binder material is formed of a plurality of particles having a second average particle size; wherein the ratio of the first average particle size to the second average particle size is about 2 or greater, wherein the first binder material is an aluminum oxide-containing material, and the second binder material is a zirconium oxide-containing material. In another embodiment, the binder composition includes: a first binder material, the first binder material is formed of a plurality of particles having a first average particle size; and a second binder material, the second binder material is formed of a plurality of particles having a second average particle size; wherein the ratio of the first average particle size to the second average particle size is about 2 or greater, wherein the first binder material is an aluminum oxide-containing material, and the second binder material is a zirconium oxide-containing material, wherein the first average particle size is about 50nm to about 1000nm, and wherein the second average particle size is about 10nm to about 500nm. In still another embodiment, the adhesive composition includes: a first adhesive material, the first adhesive material being formed of a plurality of particles having a first average particle size; and a second adhesive material, the second adhesive material being formed of a plurality of particles having a second average particle size; wherein a ratio of the first average particle size to the second average particle size is about 2 or greater, wherein the first adhesive material is an aluminum oxide-containing material, and the second adhesive material is a zirconium oxide-containing material, wherein the first average particle size is about 50 nm to about 1000 nm, wherein the second average particle size is about 10 nm to about 500 nm, and wherein the first adhesive material and the second adhesive material are present in a concentration ratio of about 0.01 to about 0.5.

[0056] In some embodiments, the binder materials used herein are combined in a specific ratio based on the average particle size of the various binder materials. Unless otherwise specified herein, the terms "first", "second", "third", etc. related to various binder materials are used only for clarity, and it should be understood that the description of "first binder material" and "second binder material" or other various binder materials is interchangeable.

[0057] As a non-limiting example, the ratio of the average particle size of the first binder material to the average particle size of the second binder material can be about 2 or more. In other words, the average particle size of the first binder material can be at least 2 times (or more) larger than the average particle size of the second binder material. In other embodiments, the ratio of the first average particle size of the first binder material to the second average particle size of the second binder material can be about 2.5 or more, about 3 or more, about 3.5 or more, about 4 or more, about 5 or more, or about 6 or more. In other example embodiments, the ratio of the first average particle size of the first binder material to the second average particle size of the second binder material can be about 1 to about 7, about 1 to about 5, about 1.5 to about 4, or about 2 to about 3.

[0058] In embodiments where the third binder material is included in the binder composition, the average particle size of the third binder material may be less than the average particle size of the first binder material or may be greater than the average particle size of the third binder material. For example, the ratio of the third average particle size of the third binder material to the first average particle size of the first binder material may be about 1.5 or more, about 2 or more, about 2.5 or more, about 3 or more, about 4 or more, or about 5 or more, such as about 1 to about 7, about 1.5 to about 6, or about 2 to about 5. Further, the ratio of the second average particle size of the second binder material to the third average particle size of the third binder material may be about 1.5 or more, about 2 or more, about 2.5 or more, about 3 or more, about 4 or more, or about 5 or more, such as about 1 to about 5, about 1 to about 5, about 1.5 to about 4, or about 2 to about 3.

[0059] In embodiments where the third binder material is included in the binder composition, the average particle size of the third binder material may be less than the average particle size of the first binder material or may be greater than the average particle size of the third binder material. For example, the ratio of the first average particle size of the first binder material to the third average particle size of the third binder material may be about 1.5 or greater, about 2 or greater, about 2.5 or greater, about 3 or greater, about 4 or greater, or about 5 or greater, such as about 1 to about 7, about 1.5 to about 6, or about 2 to about 5.

[0060] In some embodiments, the second binder material is a combination of two or more different binder materials that each have a certain average particle size. In this embodiment, the second binder material will have an average particle size.

[0061] In some embodiments, at least one binder material can have an average particle size of about 50 nm to about 1000 nm, about 50 nm to about 750 nm, about 50 nm to about 500 nm, about 50 nm to about 400 nm, about 50 nm to 300 nm, or about 50 nm to about 250 nm. In some embodiments, a binder material having particles within such a range can be referred to as particles having a relatively large average particle size.

[0062] In other embodiments, the average particle size of at least one binder material can be about 10 nm to about 750 nm, about 10 nm to about 500 nm, about 10 nm to about 250 nm, about 10 nm to about 150 nm, about 15 nm to about 150 nm, or about 20 nm to about 120 nm. In some embodiments, a binder material having particles within such a range can be referred to as particles having a relatively small average particle size.

[0063] In an example embodiment, the first binder material may be formed of a plurality of particles having a first average size, and the second binder material may be formed of a plurality of particles having a second average size. The first average size may be relatively larger than the second average size, and conversely the second average size may be relatively smaller than the first average size. Preferably, the relative sizes of the particles of the first binder material and the particles of the second binder material exhibit a ratio described further herein, independent of the absolute average size of the first binder particles and the absolute average size of the second binder particles.

[0064] If present, the third binder material can be a plurality of particles that are larger in size than the first binder material particles according to the ratios provided above, or can be a plurality of particles that are smaller in size than the second binder material particles according to the ratios provided above. Alternatively, if present, the third binder material can be a plurality of particles that are sized to be smaller in size than the first binder material particles and larger in size than the second binder material particles, as long as the overall size ratios conform to the ratios provided above. More specifically, the relative average size of the binder material particles can be according to any of the following, wherein B1 is the average particle size of the first binder material, B2 is the average particle size of the second binder material, and B3 is the average particle size of the third binder material, and wherein the relative average size is within the ratio range otherwise described above: B1>B2; or B2>B1; or B1>B2>B3; or B2>B1>B3; or B2>B3>B1; or B3>B2>B1; or B1>B3>B2. In a particular embodiment, B1>B2; or B1>B2>B3; or B1>B3>B2.

[0065] Except size ratio, in certain embodiments, can define adhesive composition according to the concentration ratio of the various binder materials that exist.In a particular embodiment, the binder material with relatively small mean particle size may be desired to exist with a concentration higher than the binder material with relatively large mean particle size.For example, the binder material with relatively large mean particle size and the binder material with relatively small mean particle size can exist with a concentration ratio of approximately 0.01 to approximately 0.95, approximately 0.01 to approximately 0.9, approximately 0.01 to approximately 0.8, approximately 0.02 to approximately 0.6, approximately 0.02 to approximately 0.5 or approximately 0.3 to approximately 0.5.This type of concentration ratio can be applicable to employed every kind of other binder material with relatively large or relatively small mean particle size successively.

[0066] For a variety of reasons, it may be advantageous to provide a binder material with a relatively small average particle size at a greater concentration. For example, in some embodiments, a binder particle with a relatively small average particle size at a greater concentration may be advantageous to increase the total amount of binder material that can be used. Having a higher total amount of binder material may improve the bonding strength between the catalyst carrier coating and the catalyst substrate. Similarly, a binder particle with a relatively small average particle size at a greater concentration may be advantageous to maintain or even reduce the viscosity of the carrier coating slurry for applying the catalyst carrier coating to the catalyst substrate. This may be advantageous to improve the uniformity of the carrier coating along the length of the substrate, and therefore avoid the catalyst coating region on the substrate being undesirably thicker and / or the catalyst coating region on the substrate being undesirably thicker. Therefore, using the binder composition of the present disclosure may achieve an increase in the amount of binder while maintaining or even reducing the viscosity of the binder carrier coating. This may be beneficial to expanding the operating window to enhance the adhesion of the catalyst to the substrate.

[0067] In further embodiments, the present disclosure may provide a carrier coating slurry formed by a liquid medium and a binder composition as otherwise described herein. The liquid medium used in the carrier coating slurry may be particularly an aqueous medium, and may specifically be water. Binder material particles forming two or more binder materials used in the binder composition may be present in the carrier coating slurry alone or in combination with a dedicated catalyst material. The phrase "dedicated catalyst material" may refer to a catalyst material that is specifically used to exist as a catalyst in forming a catalyst article and is separated from any binder material used in the binder composition, any of which also acts as a catalyst material.

[0068] The binder composition used in the washcoat slurry can be present in a defined amount while maintaining a desired low viscosity. Preferably, the binder composition is present in the washcoat slurry in a concentration sufficient to provide a specified binder loading on the substrate. When describing the amount of material (e.g., binder material and / or catalyst material) present in the washcoat slurry, it is convenient to use the unit of component weight per unit volume of the substrate coated with the washcoat. Thus, the unit grams per cubic inch ("g / in 3 ”) and grams per cubic foot (“g / ft 3 ”) is used herein to refer to the weight of the component per unit volume of the substrate member (including the volume of the void space of the substrate member). In one or more embodiments, the adhesive composition can be used at about 0.01 g / in 3 To about 1.0g / in 3 , about 0.05g / in 3 To about 0.95g / in 3 , about 0.1g / in 3 To about 0.9g / in 3 , about 0.15g / in 3 To about 0.8g / in 3 , or about 0.2g / in 3 To about 0.5g / in 3 The loading amount is present in the carrier coating slurry. In some embodiments, the binder content can be defined as the concentration of the solid content of the whole slurry. For example, it can be expected that the carrier coating composition containing the binder composition includes about 10 wt % to about 60 wt %, about 15 wt % to about 50 wt %, or about 20 wt % to about 40 wt % solids by the total weight of the carrier coating slurry. Preferably, the binder composition accounts for about 1 wt % to about 50 wt %, about 1.5 wt % to about 35 wt %, or about 2 wt % to about 20 wt % of the total solid content of the carrier coating slurry. Therefore, in some embodiments, the binder composition can account for about 0.1 wt % to about 12 wt %, about 0.2 wt % to about 10 wt %, or about 0.4 wt % to about 8 wt % of the carrier coating slurry by the total weight of the carrier coating slurry. In one embodiment, the carrier coating slurry includes: a liquid medium; an adhesive composition as described in addition herein, wherein the adhesive composition is about 0.01 to about 1.0 g / in 3 The amount of the carrier coating slurry is present in about 300s -1 The viscosity of the above-mentioned compositions is about 100 cP or less.

[0069] The present compositions are particularly beneficial in that an increase in binder loading can be achieved without undesirably increasing the viscosity of the washcoat slurry. For example, the viscosity of the washcoat slurry can be measured using a Brookfield viscometer at about 300 s at room temperature. -1 The shear rate is measured in centipoise (cP) as the unit of viscosity. In some embodiments, the viscosity of the carrier coating slurry including the adhesive composition as described herein at the loading amount described above can be about 120cP or less, about 100cP or less, about 80cP or less, about 60cP or less, or about 50cP or less (e.g., wherein the lower limit is greater than one). More specifically, the viscosity of the carrier coating slurry as described above can be about 5cP to about 120cP, about 5cP to about 100cP, about 10cP to about 80cP, or about 15cP to about 60cP.

[0070] As described above, in addition to the binder material, the washcoat slurry described herein may also include one or more catalyst materials. In some embodiments, for example, the binder composition may be combined with a catalyst suitable for use in, for example, a TWC catalyst and / or a four-way conversion (FWC) catalyst. TM ) catalyst composition. According to the requirements of regulatory agencies and / or automobile manufacturers, the catalyst composition with TWC function may include a catalyst composition effective for hydrocarbon (HC), carbon monoxide (CO) oxidation and NOx reduction. In this way, platinum group metal components such as platinum, palladium and rhodium are provided to achieve HC, CO and NOx conversion, and sufficient oxygen storage components (OSC) are provided to achieve sufficient oxygen storage capacity, thereby ensuring appropriate HC, NOx and CO conversion in environments with different A / F (air and fuel) ratios. Sufficient oxygen storage capacity generally means that after aging for the full service life defined by the automobile manufacturer, the catalyst can store and release a minimum amount of oxygen. For example, a useful oxygen storage capacity can be at least 100 mg per liter of oxygen (such as about 200 mg per liter of oxygen after aging for 80 hours at 1050°C exothermic). Examples of suitable oxygen storage components include cerium dioxide and praseodymium oxide, and such materials are provided in the form of mixed oxides. For example, cerium dioxide can be delivered by a mixed oxide of cerium and zirconium and / or a mixed oxide of cerium, zirconium and neodymium. For example, praseodymium oxide can be delivered via mixed oxides of praseodymium and zirconium and / or mixed oxides of praseodymium, cerium, lanthanum, yttrium, zirconium, and neodymium. Suitable TWC catalyst compositions can include those described, for example, in U.S. Pat. Nos. 8,815,189, 9,266,092, and 9,981,258, the disclosures of which are incorporated herein by reference.

[0071] A separate adhesive composition (such as when one or more adhesive materials in the adhesive material also act as a catalyst material) or an adhesive composition in combination with one or more dedicated catalyst materials can be used in a catalyst product, wherein the adhesive composition (alone or in combination with a catalyst material) can be provided on a catalyst substrate. According to one or more embodiments, the substrate can be composed of any material commonly used to prepare automotive catalysts, and will generally include a metal or ceramic honeycomb structure. The substrate generally provides a plurality of wall surfaces, on which a carrier coating comprising at least the adhesive composition is applied and adhered, thereby acting as a carrier for the applied composition.

[0072] Exemplary metal substrates include heat-resistant metals and metal alloys, such as titanium and stainless steel, and other alloys in which iron is a substantial or major component. Such alloys may include one or more of nickel, chromium and / or aluminum, and the total amount of these metals may advantageously account for at least 15 wt.% of the alloy, such as 10-25 wt.% chromium, 3-8 wt.% aluminum, and up to 20 wt.% nickel. The alloy may also contain small or trace amounts of one or more other metals, such as manganese, copper, vanadium, titanium, and the like. The surface or metal support may be oxidized at high temperatures (e.g., 1000° C. or higher) to form an oxide layer on the surface of the substrate, thereby improving the corrosion resistance of the alloy and promoting adhesion of the washcoat layer to the metal surface.

[0073] The ceramic material used to construct the substrate can include any suitable refractory material, for example, cordierite, mullite, cordierite-alpha alumina, silicon carbide, silicon nitride, aluminum titanate, zircon mullite, spodumene, alumina-silica magnesia, zirconium silicate, sillimanite, magnesium silicate, zircon, petalite, alpha alumina, aluminosilicates, and the like.

[0074] Any suitable substrate can be used, such as a monolithic flow-through substrate having a plurality of fine parallel gas flow channels extending from the inlet of the substrate to the outlet face so that the channel is open to allow the fluid to flow. The channel, which is essentially a straight path from the inlet to the outlet, is defined by a wall, and the wall is coated with a catalytic material as a carrier coating (e.g., comprising an adhesive composition) so that the gas flowing through the channel contacts the catalytic material. The flow channel of the monolithic substrate is a thin-walled channel, which can be any suitable cross-sectional shape, such as a trapezoid, rectangle, square, sinusoidal, hexagonal, elliptical, circular, etc. Such a structure can contain about 60 to about 1200 or more gas inlet openings (i.e., "cells") per square inch of cross section (cpsi), more generally about 300 to 600 cpsi. The wall thickness of the flow-through substrate can vary, with a typical range of 0.002 to 0.1 inches. A commercially available representative flow-through substrate is a cordierite substrate having 400 cpsi, a wall thickness of 6 mils, or 600 cpsi, a wall thickness of 4 mils. However, it will be understood that the present invention is not limited to a particular substrate type, material, or geometry.

[0075] In an alternative embodiment, the substrate can be a wall-flow substrate in which each channel is blocked with a non-porous plug at one end of the substrate body, with alternating channels blocked at the opposite end faces. This requires the gas to flow through the porous walls of the wall-flow substrate to reach the outlet. Such a monolithic substrate can contain up to about 700 or more cpsi, such as about 100 to 400 cpsi, and more typically about 200 to about 300 cpsi. The cross-sectional shape of the unit cell can vary as described above. The wall thickness of the wall-flow substrate is generally between 0.002 inches and 0.1 inches. Representative commercially available wall-flow substrates are composed of porous cordierite, examples of which are 200 cpsi and a wall thickness of 10 mils or 300 cpsi and a wall thickness of 8 mils, and a wall porosity of between 45% and 65%. Other ceramic materials such as aluminum titanate, silicon carbide, and silicon nitride are also used as wall-flow filter substrates. However, it will be understood that the present invention is not limited to a specific substrate type, material, or geometry. It is noted that in the case where the substrate is a wall flow substrate, the catalyst composition (e.g., TWC catalyst and / or FWC TM The catalyst) can, in addition to being disposed on the surface of the wall, also penetrate into the pore structure of the porous wall (ie partially or completely block the pore openings). Figure 1 and 2 An exemplary substrate 2 is shown in the form of a flow-through substrate coated with a washcoat composition as described herein. Figure 1, the exemplary substrate 2 has a cylindrical shape and a cylindrical outer surface 4, an upstream end face 6 and a corresponding downstream end face 8, the downstream end face being identical to the end face 6. The substrate 2 has a plurality of parallel thin gas flow channels 10 formed therein. Figure 2 As seen in FIG. 1 , a flow channel 10 is formed by a wall 12 and extends through the substrate 2 from the upstream end face 6 to the downstream end face 8 , the channel 10 being unobstructed to allow a fluid (e.g., airflow) to flow longitudinally through the substrate 2 through its airflow channel 10 . Figure 2 As can be more easily seen in the figure, the size and configuration of the wall 12 are such that the gas flow channel 10 has a substantially regular polygonal shape. As shown, if desired, the washcoat composition can be applied in multiple, distinct layers. In the illustrated embodiment, the washcoat is composed of a discrete bottom washcoat layer 14 adhered to the wall 12 of the carrier member and a second discrete top washcoat layer 16 coated on the bottom washcoat layer 14. The present invention can be implemented with one or more (e.g., 2, 3, or 4) washcoat layers, and the present invention is not limited to the illustrated two-layer embodiment.

[0076] Figure 3 An exemplary substrate 2 is shown in the form of a wall flow filter substrate coated with a washcoat composition as described herein. Figure 3 As shown, the exemplary substrate 2 has a plurality of channels 52. The channels are tubularly surrounded by the inner wall 53 of the filter substrate. The substrate has an inlet end 54 and an outlet end 56. Alternating channels are plugged with inlet plugs 58 at the inlet end and plugged with outlet plugs 60 at the outlet end to form a relative checkerboard pattern at the inlet 54 and the outlet 56. The gas flow 62 enters through the unplugged channel inlet 64, is blocked by the outlet plug 60, and diffuses to the outlet side 66 through the groove wall 53 (which is porous). The gas cannot return to the inlet side of the wall due to the inlet plug 58. The porous wall flow filter used in the present invention is catalyzed because the wall of the element has or contains one or more catalytic materials. The catalytic material can be present alone on the inlet side of the element wall, alone on the outlet side, on both the inlet side and the outlet side, or the wall itself can be filled with catalytic material in whole or in part. The present invention includes using one or more layers of catalytic material in the wall of the element or on the inlet and / or outlet wall of the element.

[0077] For example, in one embodiment, the catalytic article includes a catalytic material having multiple layers, wherein each layer has a different catalyst composition. Figure 2 The layer 14) may include a first catalyst composition, and the top layer (e.g., Figure 2 The layer 16) may include a second catalyst composition. One or both of the first catalyst composition and the second catalyst composition may include a binder composition as described herein. Figure 2It should be understood that the bottom layer 14 and top layer 16 can each extend completely from the front or inlet end of the substrate to the back or outlet end of the substrate.

[0078] As a non-limiting example, the catalyst material or catalyst composition used to form the catalyst article herein may include any catalyst commonly used, for example, in automotive catalysts. In some embodiments, the catalyst article according to the present disclosure may include a binder composition as described herein and a catalyst article suitable for use as a TWC catalyst, a FWC catalyst, or a catalyst composition ... TM One or more catalyst compositions of a catalyst, a diesel oxidation catalyst (DOC), a gasoline particulate filter (GPF), a lean NOx trap (LNT), an integrated LNT-TWC and / or an ammonia oxidation (AMOx) catalyst.

[0079] In some embodiments, platinum group metals (PGMs) may be used. Specifically, palladium and / or rhodium may be used; however, other PGMs may also (or alternatively) be used. Further, specific PGMs may be explicitly excluded from this disclosure if desired. When present, the PGM may be present at a concentration of at least about 0.5 g / ft 3 or at least about 1.0g / ft 3 The load is about 20 g / ft 3 Thus, when PGM is present, the PGM may be present at a maximum loading of about 20 g / ft 3 In certain embodiments, the total PGM loading may be about 0.5 g / ft 3 To about 20g / ft 3 , about 1g / ft 3 To about 10g / ft 3 , or about 2g / ft 3 To about 10g / ft 3 In certain embodiments, it may be desirable for the catalyst compositions and / or catalyst articles of the present disclosure to be substantially free of PGMs. For this purpose, a catalyst composition may be “substantially free” of PGMs if it comprises less than 0.1 wt % PGMs or less than 0.01 wt % PGMs. Similarly, a catalyst article may be “substantially free” of PGMs if it has a PGM loading of less than 0.1 g / ft 3 or less than 0.01g / ft 3 , then the catalyst product may be "substantially free" of PGM. Preferably, "substantially free" may mean that only trace amounts are present. In some embodiments, if desired, the catalyst composition or catalyst product may be completely free of PGM.

[0080] In one or more embodiments, an ammonia oxidation catalyst (AMOx) may be used. For example, an AMOx catalyst is taught in U.S. Publication No. 2011 / 0271664, the disclosure of which is incorporated herein by reference. An ammonia oxidation (AMOx) catalyst may be a supported precious metal component that is effective in removing ammonia from an exhaust gas stream. The precious metal may include ruthenium, rhodium, iridium, palladium, platinum, silver, or gold. For example, the precious metal component includes a physical mixture of precious metals or a combination of chemical or atomic doping. For example, the precious metal component includes platinum. Platinum may be present in an amount of about 0.008% to about 2wt% in terms of the AMOx catalyst.

[0081] In some embodiments, the substrate may be coated with at least two layers contained in separate washcoat slurries in an axially partitioned configuration. For example, the same substrate may be coated with one layer of washcoat slurry and another layer of washcoat slurry, wherein each layer is different, such as having a different overall composition. The two separate washcoat compositions may contain separate catalyst compositions and may not substantially overlap. For example, with reference to Figure 4 , a first washcoat region 102 comprising a washcoat of a first catalyst composition and a second washcoat region 103 comprising a washcoat of a different second catalyst composition can be positioned side by side along the length of the substrate 100. The first washcoat region 102 of a specific embodiment extends from the front end or inlet end 100a of the substrate 100 in a range of about 5% to about 95%, about 5% to about 75%, about 5% to about 50%, or about 10% to about 35% of the length of the substrate 100. The second washcoat region 103 extends from the rear end or outlet end 100b of the substrate 100 in a range of about 5% to about 95%, about 5% to about 75%, about 5% to about 50%, or about 10% to about 35% of the total axial length of the substrate 100. The catalyst compositions of at least two components in the treatment system according to the present invention can be zoned onto the same substrate.

[0082] In some embodiments, Figure 5 As shown, the substrate 100 can be coated with a first coating 106 and a second coating 107, wherein the first coating extends from the front end or inlet end 100a of the substrate 100 to the rear end or outlet end 100b of the substrate 100, and the second coating is coated on the first coating 106 near the front end or inlet end 100a of the substrate 100 and extends only over a portion of the length of the substrate 100 (i.e., terminates before reaching the rear end or outlet end 100b of the substrate 100).

[0083] In some embodiments, Figure 6As shown, the substrate 100 may be coated with a first coating 115 that is proximate to the rear end or outlet end 100b of the substrate 100 and extends only partially along the length of the substrate 100 (i.e., terminates before reaching the front end or inlet end 100a of the substrate 100). The substrate 100 may be coated with a second coating 114. Figure 6 As shown, the second coating 114 extends from the front or inlet end 100a of the substrate 100 to the rear or outlet end 100b of the substrate 100 (thus being completely coated on the first coating 115). It will be appreciated that the above embodiments are provided by way of example only and further combinations of catalytic coatings are contemplated.

[0084] In one or more embodiments, the catalyst article according to the present disclosure may specifically include a substrate coated with a first coating as a bottom layer and a second coating as a top layer, wherein one or both of the first coating and the second coating include an adhesive composition as described herein. For example, as described above, the first coating or the bottom coating may include at least a first adhesive and a second adhesive (and an optional third adhesive). The second coating or the top layer may include an adhesive composition as described herein, but in some embodiments may include less adhesive than the adhesive present in the first coating.

[0085] In describing the amount of washcoat or catalytic metal component or other components of a composition, it is convenient to use units of weight of the component per unit volume of the catalyst substrate. Thus, the units grams per cubic inch ("g / in 3 ”) and grams per cubic foot (“g / ft 3 ”) refers to the weight of the component per volume of substrate (including the volume of the void spaces of the substrate). Other weight per volume units, such as g / L, are also sometimes used. The total loading of the catalyst composition on the catalyst substrate (such as a monolithic flow-through substrate) is generally from about 0.1 to about 6 g / in 3 , and more typically from about 1 to about 5 g / in 3 It is noted that these weights per unit volume are typically calculated by weighing the catalyst substrate before and after treatment with the catalyst washcoat composition, and because the treatment process involves drying and calcining the catalyst substrate at high temperatures, these weights represent a substantially solvent-free catalyst coating since substantially all of the water of the washcoat slurry has been removed. As such, the foregoing values ​​may represent the dry gain or amount of solids present on the substrate after removal of any solvent or other liquid material present in the original washcoat slurry used to apply the solids to the substrate.

[0086] In some embodiments, it can be beneficial to utilize a first binder and a second binder (and optional additional binders) as described herein in concentrations and ratios for achieving a certain dry gain in one or more coatings, wherein the first binder and the second binder (and any optional additional binders) constitute a desired weight ratio of the total dry gain. For example, in certain embodiments, a first binder having a relatively large average particle size can account for a smaller weight percentage of the dry gain in a given coating (e.g., 0 wt% to about 5 wt%, 0 wt% to about 2.5 wt%, about 0.1 wt% to about 5 wt%, about 0.2 wt% to about 4 wt%, or about 0.25 wt% to about 3 wt%), and a second binder having a relatively small average particle size can account for a larger weight percentage of the dry gain in the same given coating (e.g., about 7 wt% to about 20 wt%, about 10 wt% to about 15 wt%) (all of the above weight percentages are based on the total weight of the dry gain of the given coating). In other examples, the weight percentage of the first binder having a relatively large average particle size present in the coating may be less than 5 wt%, less than 3 wt%, or less than 2.5 wt%, based on the total weight of the dry gain of the coating, which may include zero or may be defined by a minimum value of at least 0.01 wt%. Additionally or alternatively, the weight percentage of the second binder having a relatively small average particle size present in the coating may be greater than 7 wt%, greater than 8 wt%, greater than 9 wt%, or greater than 10 wt% (e.g., up to a maximum of about 25 wt% or about 20 wt%) based on the total weight of the dry gain of the coating.

[0087] The catalyst material may be ground to enhance mixing of the catalyst particles and to form a homogenous material. Grinding may be accomplished in a ball mill, a continuous mill, or other similar equipment. In one embodiment, the catalyst material after grinding is characterized by a D90 particle size of about 5 to about 40 microns, preferably 5 to about 30 microns, and more preferably about 5 to about 10 microns. D90 is defined as the particle size at which 90% of the particles have a finer particle size.

[0088] A washcoat slurry containing a binder material alone or in combination with one or more specialized catalyst materials may be coated on a catalyst substrate using washcoat techniques known in the art. In one embodiment, the catalyst substrate is dipped in the slurry one or more times or otherwise coated with the slurry. Thereafter, the coated substrate is dried at an elevated temperature (e.g., 100-150° C.) for a period of time (e.g., about 10 minutes to about 3 hours), and then calcined by heating (e.g., below 700° C.), typically for about 10 minutes to about 8 hours.

[0089] The temperature during calcination of the coated catalyst substrate is less than about 700° C. In some embodiments, the calcination temperature is in the range of about 300° C. to about 700° C., about 300° C. to about 500° C., about 350° C. to about 500° C., about 400° C. to about 500° C., or about 450° C. to about 500° C. for a period of time. In some embodiments, the calcination temperature is less than about 700° C., about 600° C., about 500° C., about 450° C., about 400° C., or about 350° C., with a lower limit of 300° C. In some embodiments, the calcination time period ranges from about 10 minutes to about 8 hours, about 1 hour to about 6 hours, or 3 hours to about 6 hours (i.e., less than 8 hours, 7 hours, 6 hours, 5 hours, 4 hours, 3 hours, 2 hours, or 1 hour, with a lower limit of about 10 minutes).

[0090] After drying and calcining, the final washcoat coating can be considered to be substantially free of solvent. After calcining, the catalyst loading can be determined by calculating the difference between the coated weight and the uncoated weight of the substrate. As will be apparent to one skilled in the art, the catalyst loading can be modified by changing the slurry rheology. In addition, the coating / drying / calcining process to produce the washcoat can be repeated as needed to build the coating to the desired loading level or thickness, meaning that more than one washcoat layer may be applied. For example, in some embodiments, the catalyst composition can be applied as a single layer or multiple layers. In one embodiment, the catalyst material in combination with the binder material described herein can be applied in a single layer (e.g., only Figure 2 In one embodiment, the catalyst material combined with the binder material described herein can be applied in multiple layers (e.g., Figure 2 The layers 14 and 16 are applied in the form of.

[0091] In some embodiments, the calcined coated substrate is aged. Aging can be performed under various conditions, and as used herein, "aging" is understood to cover a range of conditions (e.g., temperature, time, and atmosphere). An exemplary aging scheme involves treating the calcined coated substrate at a temperature of 650° C. in 10% steam for about 50 hours, at a temperature of 750° C. in 10% steam for about 5 hours, or at a temperature of 800° C. in 10% steam for about 16 hours. However, these schemes are not limiting, and the temperature can be lower or higher (e.g., including but not limited to 400° C. and higher temperatures, such as 400° C. to 900° C., 600° C. to 900° C., or 650° C. to 900° C.); the time can be shorter or longer (e.g., including but not limited to a time of about 1 hour to about 50 hours or about 2 hours to about 25 hours); and the atmosphere can be modified (e.g., different amounts of steam and / or other components are present therein).

[0092] The present disclosure also provides an emission treatment system incorporating one or more compositions described herein. The adhesive compositions described herein (alone or in combination with one or more specialized catalyst materials) can be used in an integrated emission treatment system comprising one or more additional components for treating exhaust emissions, such as exhaust emissions from a gasoline engine.

[0093] exist Figure 7 An exemplary emission treatment system is shown in , which depicts a schematic diagram of an emission treatment system 32. As shown, an exhaust gas stream containing gaseous pollutants is transported from an engine 34 to a TWC catalyst assembly 38 through an exhaust conduit 36 ​​and then to a particulate filter assembly 42, which is also optionally coated with a TWC, in a conduit 40. One or both of the TWC catalyst assembly 38 and the particulate filter assembly 42 may include the adhesive composition described herein.

[0094] Exemplary embodiments are as follows.

[0095] 1. An adhesive composition comprising:

[0096] a first binder material formed from a plurality of particles having a first average particle size; and

[0097] a second binder material formed from a plurality of particles having a second average particle size;

[0098] wherein a ratio of the first average particle size to the second average particle size is about 2 or greater.

[0099] 2. The adhesive composition of embodiment 1, wherein the first adhesive material and the second adhesive material are independently selected from the group consisting of: aluminum oxide-containing materials, silicon oxide-containing materials, zirconium oxide-containing materials, ceria-containing materials, lanthanum oxide-containing materials, yttrium oxide-containing materials, and combinations thereof.

[0100] 3. The adhesive composition of any one of embodiments 1 to 2, wherein the first adhesive material is an aluminum oxide-containing material and the second adhesive material is a zirconium oxide-containing material.

[0101] 4. The adhesive composition of any one of embodiments 1 to 3, further comprising a third adhesive material formed by a plurality of particles having a third average particle size, wherein a ratio of the third average particle size to the first average particle size is about 2 or greater, or wherein a ratio of the second average particle size to the third average particle size is about 2 or greater.

[0102] 4a. The adhesive composition of any one of embodiments 1 to 4, further comprising a third adhesive material formed from a plurality of particles having a third average particle size, wherein a ratio of the first average particle size to the third average particle size is about 2 or greater.

[0103] 5. The adhesive composition of any one of embodiments 1 to 4a, wherein the first average particle size is from about 50 nm to about 1000 nm.

[0104] 6. The adhesive composition of any one of embodiments 1 to 5, wherein the second average particle size is from about 10 nm to about 500 nm.

[0105] 7. The adhesive composition of any one of embodiments 1 to 6, wherein the first adhesive material and the second adhesive material are present in a concentration ratio of about 0.01 to about 0.5.

[0106] 8. The adhesive composition of any one of embodiments 1 to 7, wherein one or both of the first adhesive material and the second adhesive material are catalytic.

[0107] 9. A carrier coating slurry comprising:

[0108] Liquid medium;

[0109] The adhesive composition according to any one of embodiments 1 to 8.

[0110] 10. The washcoat slurry of embodiment 9, wherein the binder composition is present in an amount of about 0.01 to about 1.0 g / in 3 and wherein the washcoat slurry is present in an amount of about 300 s -1 The viscosity of the above-mentioned compositions is about 100 cP or less.

[0111] 11. The washcoat slurry of any one of embodiments 9 to 10, wherein the washcoat slurry is heated to about 300 s. -1 The viscosity of the above-mentioned compositions is about 50 cP or less.

[0112] 12. The washcoat slurry of any of embodiments 9 to 11, further comprising a catalyst material.

[0113] 13. A catalyst article comprising a catalyst substrate having a plurality of channels suitable for gas flow, a wall surface of each channel adhered to a catalytic coating comprising the binder composition according to any one of embodiments 1 to 8.

[0114] 14. The catalyst article of embodiment 13, wherein the catalytic coating comprises a catalyst material in combination with the binder composition.

[0115] 15. The catalyst article of any one of embodiments 13 to 14, wherein the catalyst substrate is a honeycomb including a wall flow filter substrate or a flow-through substrate.

[0116] 16. The catalyst article of any one of embodiments 13 to 15, wherein the catalytic coating has a concentration of at least about 1.0 g / in 3 A loading of is present on the substrate.

[0117] 17. The catalyst article of any one of embodiments 13 to 16, wherein the catalyst substrate comprises a first coating of the catalytic coating and comprises a second coating having a different overall composition, the second coating being located over at least a portion of the first coating of the catalytic coating.

[0118] 18. The catalyst article of any one of embodiments 13 to 17, wherein one or both of the following conditions are met:

[0119] said first binder material being present in an amount of about 0.1 wt % to about 5 wt % of the total dry gain of said first coating of said catalytic coating;

[0120] The second binder material is present in an amount of about 7 wt % to about 20 wt % of the total dry gain of the first coating of the catalytic coating.

[0121] 19. An emission treatment system for treating an exhaust gas stream, the emission treatment system comprising:

[0122] i. an engine that produces an exhaust gas flow; and

[0123] ii. The catalyst article of any of embodiments 13 to 18, positioned downstream of the engine and in fluid communication with the exhaust gas stream.

[0124] 20. The catalyst article of any of embodiments 13 to 18, wherein the washcoat total mass loss is less than 6%.

[0125] 21. The adhesive composition of any of embodiments 1 to 8, wherein when the adhesive composition is part of a washcoat, the washcoat has a total mass loss of less than 6%.

[0126] 22. The washcoat slurry of any of embodiments 9 to 12, wherein the washcoat total mass loss is less than 6% when the slurry is coated on a substrate.

[0127] Examples

[0128] Various aspects of the present invention are more fully described by the following examples, which are set forth for the purpose of illustrating certain aspects of the present invention and should not be construed as limiting the present invention.

[0129] Tests were conducted to evaluate the effects of different ratios of binder components on the properties of the carrier coating composition and the performance of the coating formed using the carrier coating composition. The carrier coating composition was prepared using a first binder formed of a plurality of alumina particles having an average particle size of about 78 nm and a second binder formed of a plurality of ceria / zirconia particles having an average particle size of about 28 nm and / or a plurality of zirconia / yttria particles having an average particle size of about 24 nm. That is, the second binder was a plurality of ceria / zirconia particles or a plurality of zirconia / yttria particles, or the second binder was a combination of a plurality of ceria / zirconia particles and a plurality of zirconia / yttria particles. The average particle size of the binder components was measured by dynamic light scattering using a Malvern Zetasizer Pro.

[0130] For each test sample, a first washcoat composition (used as a basecoat) was prepared to have a total solids content of about 2.172 g / in 3 The first washcoat composition contained both particles having a first relatively large average particle size and particles having a second relatively small average particle size at the solid loadings shown in the table below. The second washcoat composition (used as a topcoat) was prepared to have a total solids content of about 1.366 g / in 3 The second carrier coating composition comprises a solid loading of 0.025 g / in 3 The first carrier coating composition (1.83 wt % of the total solids content of the second carrier coating) contained first binder particles (i.e., having a relatively large average particle size), but did not contain any second binder particles having a relatively small average particle size. The viscosity of the first carrier coating composition (used as a basecoat on a substrate) is also shown in the table below.

[0131] The first washcoat composition and the second washcoat composition for each test sample were applied to a flow-through substrate made of cordierite material having a cell density of 600 cells per square inch and having a wall thickness of about 4.3 mm by: dipping the flow-through substrate into the slurry to a defined depth; applying a vacuum to draw the slurry upward into the cells of the flow-through substrate along at least a portion of the length of the substrate in a direction from a first end of the substrate to a second end of the substrate; removing the vacuum; rotating the flow-through substrate 180°; and applying a blast through the cells of the flow-through substrate in a direction from the first end of the substrate to the second end of the substrate so that the slurry was coated across substantially the entire length of the substrate. A suitable method for coating a flow-through substrate is provided in U.S. Pat. No. 7,521,087, the disclosure of which is incorporated herein by reference. The method involves coating the interior of a hollow substrate with a washcoat composition by partially immersing an end of the substrate into a container containing a bath of a coating slurry; and applying a vacuum to the partially immersed substrate at an intensity and for a time sufficient to draw the coating slurry upward from the bath into the interior of the hollow substrate. In a next step, the substrate is rotated and an air blast is applied to the end of the substrate immersed in the slurry to distribute the washcoat composition therein. A basecoat is applied using a first washcoat composition according to the method above, and the basecoat is dried before a topcoat is applied using a second washcoat composition according to the method above.

[0132] The coated flow-through substrate was subjected to a washcoat loss test to evaluate the performance of catalytic coatings containing various ratios of binders. A rigorous multi-step washcoat adhesion test was performed on the catalyst including the binder package. Each catalyst was divided into three sections (top, middle and bottom), and each section was subjected to a thermal shock step, an ultrasonic water bath step and an air blast step to evaluate the adhesion of the catalyst washcoat under different conditions. Specifically, the catalyst section was tested after a heating / quenching cycle of about 850°C. Washcoat adhesion (WCA) is shown in the table below as washcoat loss, which represents the washcoat adhesion loss percentage (based on the difference between the mass of the catalyst section before and after being subjected to the above treatment). Under these conditions, a washcoat total mass percentage loss of less than 6% indicates a robust WCA.

[0133] Figure 8 A contour plot showing the viscosity of the first washcoat composition based on the relative loading of the first binder material formed of particles of relatively larger average size and the second binder material formed of particles of relatively smaller average size is provided. The viscosity of the first washcoat composition was measured using a Brookfield viscometer at room temperature at about 300 s -1 The viscosity is measured at a shear rate of . The graph shows that a preferred lower viscosity is achieved using a defined ratio of first binder particles to second binder particles. Fig. 9 A contour plot showing the percent washcoat loss based on the relative loadings of the first binder particles and the second binder particles is provided. The plot shows that the preferred lower washcoat loss is achieved using a defined ratio of the first binder particles to the second binder particles.

[0134] The following examples were prepared according to the general procedure described above.

[0135]

[0136] + The second binder is a combination of a plurality of ceria / zirconia particles and a plurality of zirconia / yttria particles.

[0137] Many modifications and other embodiments of the subject matter of the present disclosure will occur to those skilled in the art with the benefit of the foregoing description and the teachings presented in the associated drawings. Therefore, it should be understood that the present disclosure should not be limited to the specific embodiments described herein, and modifications and other embodiments are intended to be included within the scope of the appended claims. Although specific terms are employed herein, they are used in a general and descriptive sense only, and not for the purpose of limitation.

Claims

1. An adhesive composition comprising: a first binder material formed of a plurality of particles having a first average particle size, wherein the first average particle size is 50 nm to 1000 nm; as well as a second binder material formed of a plurality of particles having a second average particle size, wherein the second average particle size is from 10 nm to 500 nm; wherein the ratio of the first average particle size to the second average particle size is 2 or greater, The first binder material and the second binder material are present in a concentration ratio of 0.01 to 0.

5.

2. The adhesive composition of claim 1, wherein the first adhesive material and the second adhesive material are independently selected from the group consisting of: an alumina-containing material, a silica-containing material, a zirconia-containing material, a ceria-containing material, a lanthanum-containing material, a yttria-containing material, and combinations thereof. 3 . The adhesive composition of claim 1 , wherein the first adhesive material is an aluminum oxide-containing material and the second adhesive material is a zirconium oxide-containing material. 4 . The adhesive composition according to claim 1 , further comprising a third adhesive material formed of a plurality of particles having a third average particle size, wherein a ratio of the first average particle size to the third average particle size is 2 or more. 5 . The adhesive composition of claim 1 , wherein a ratio of the first average particle size to the second average particle size is 2.5 to 6. 6 . 6 . The adhesive composition of claim 1 , wherein a ratio of the first average particle size to the second average particle size is 2.5 to 3.

5. 7 . The adhesive composition according to claim 1 , wherein a concentration ratio of the adhesive material having a relatively larger average particle size to the adhesive material having a relatively smaller average particle size is 0.02 to 0.

3.

8. The adhesive composition according to any one of claims 1 to 7, wherein at least one adhesive material is a particle having a relatively large average particle size, the average particle size of which is from 50 nm to 250 nm.

9. The adhesive composition according to any one of claims 1 to 7, wherein at least one adhesive material is a particle having a relatively small average particle size, the average particle size of which is from 20 nm to 120 nm.

10. The adhesive composition of claim 1, wherein one or both of the first adhesive material and the second adhesive material are catalytic.

11. A carrier coating slurry comprising: Liquid medium; The adhesive composition according to any one of claims 1 to 10.

12. The washcoat slurry of claim 11, wherein the binder composition is present in an amount of 0.01 to 1.0 g / in 3 The amount of the carrier coating slurry is present in 300s -1 The viscosity of the above-mentioned material is 100 cP or less.

13. The washcoat slurry of claim 12, wherein the washcoat slurry is heated to 300 s. -1 The viscosity of the above-mentioned product is 50 cP or less.

14. The washcoat slurry of claim 11 further comprising a catalyst material.

15. A catalyst article comprising a catalyst substrate having a plurality of channels suitable for gas flow, a wall surface of each channel being adhered to a catalytic coating comprising the binder composition according to any one of claims 1 to 10.

16. The catalyst article of claim 15, wherein the catalytic coating comprises a catalyst material in combination with the binder composition.

17. The catalyst article of claim 15, wherein the catalyst substrate is a honeycomb including a wall flow filter substrate or a flow-through substrate.

18. The catalyst article of claim 15, wherein the catalytic coating has a concentration of at least 1.0 g / in 3 A loading of is present on the substrate.

19. The catalyst article of claim 15, wherein the catalyst substrate comprises a first coating of the catalytic coating and comprises a second coating having a different overall composition, the second coating being disposed overlying at least a portion of the first coating of the catalytic coating.

20. The catalyst product according to claim 19, wherein one or both of the following conditions are met: said first binder material being present in an amount of 0.1 wt % to 5 wt % of the total dry gain of said first coating of said catalytic coating; The second binder material is present in an amount of 7 wt % to 20 wt % of the total dry gain of the first coating of the catalytic coating.

21. An emission treatment system for treating an exhaust gas stream, the emission treatment system comprising: i. an engine that produces an exhaust gas flow; as well as ii. A catalyst article according to any one of claims 15 to 20, positioned downstream of the engine and in fluid communication with the exhaust gas stream.