Composite superconducting wire and its preparation method and connection method, and a connecting superconducting wire

Composite superconducting wires are formed through heat treatment and stripping technology, and ladder-like exposure and molten diffusion welding are used when connecting. This solves the problems of the multi-layer structure and joint performance of the second-generation high-temperature superconducting wires, improves the current density and preparation efficiency, and enhances the Joint performance.

CN113594348BActive Publication Date: 2024-10-29INST OF ELECTRICAL ENG CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202010367418.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-30
Publication Date
2024-10-29
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

Existing second-generation high-temperature superconducting wires are difficult to achieve multi-layer superconducting layers due to process limitations, which makes it difficult to increase the critical current and current density of a single superconducting wire, and the oxygen diffusion efficiency is low during connection, which affects the preparation efficiency and performance of the joint.

Method used

By heat-treating the silver layer of the silver-containing strip and the silver layer of the second-generation high-temperature superconducting wire, the superconducting layer and buffer layer are peeled off to form a composite superconducting wire, and the stepped exposed superconducting layer and molten diffusion welding are used when connecting. Form efficient oxygen diffusion channels to improve joint performance.

Benefits of technology

The multi-layer superconducting layer structure of the composite superconducting wire is realized, which improves the engineering current density and preparation efficiency, enhances the superconducting performance and mechanical properties of the joint, and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113594348B_ABST
    Figure CN113594348B_ABST
Patent Text Reader

Abstract

The present invention provides a composite superconducting wire and a preparation method and a connection method thereof, and a connected superconducting wire, and belongs to the field of superconducting electrical technology. The present invention connects the silver layer of the second-generation high-temperature superconducting wire through high-temperature heat treatment, thereby completely stripping the superconducting layer from the buffer layer. The superconducting wire after stripping can be silver-plated and stripped repeatedly to prepare a composite superconducting wire with multiple superconducting layers. The silver layer adjacent to the superconducting layer can serve as a fast oxygen diffusion channel, ensuring the recovery of the superconducting performance of the composite superconducting wire and its joints in the later stage. Furthermore, a metal base tape, a buffer layer or a thicker silver tape is used to provide support or isolation for the silver layer and the superconducting layer, thereby ensuring the mechanical properties of the composite superconducting wire and its joints. The preparation method of the present invention enables the composite superconducting wire to have multiple superconducting layers and a higher engineering current density J. e At the same time, it can improve the performance recovery of the superconducting layer after connection and greatly improve the critical current and preparation efficiency of the superconducting joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of superconducting electrical technology, and in particular to a composite superconducting wire and a preparation method and a connection method thereof, and a connected superconducting wire. Background Art

[0002] The general formula of superconducting materials of the second generation high temperature superconducting wire (also called strip, coated conductor and wire, etc.) is ReBa2Cu3O 7-δ , Re includes at least one rare earth metal, and 0≤δ≤0.65. The second generation of high temperature superconducting wires has excellent comprehensive performance, with an irreversible field of 7T at 77K and a critical current density of 10 6 A / cm 2 , breaking through the limitation of the first generation of high-temperature superconducting wires (Bi-based superconducting wires) that they can only be used in weak magnetic fields, and can fully meet the application of high-temperature areas (liquid nitrogen temperature areas) and strong magnetic fields in the field of strong electricity, greatly promoting the practical application of superconducting power technology. However, due to process limitations, it is difficult to make a single superconducting layer very thick, resulting in a single superconducting wire's critical current I c Usually in 10 2 A / cm-w, and its critical current density J c Since the metal base tape and stabilization layer (protective layer) that make up the second-generation high-temperature superconducting wire are relatively thick (the sum of the two is usually more than 0.1 mm), the engineering current density (the ratio of the critical current of the superconducting wire to the cross-sectional area) is J e The traditional method is to continue to deposit buffer layers and superconducting layers on the superconducting layer to continuously increase the number of superconducting layers and improve the current carrying capacity of a single wire. c However, as the number of superconducting layers increases, the quality of the superconducting layers prepared by this method continues to decline. Therefore, the total number of superconducting layers is also limited, usually only a few layers, which has limited improvement on the overall performance of the line and also increases the preparation cost.

[0003] On the other hand, the preparation of superconducting devices often requires very long superconducting wires, especially in the development of large and medium-sized magnets, the amount of superconducting wires may weigh several tons. However, due to process limitations, the prepared superconducting wires cannot take into account both length and overall performance at the same time. When used, it is necessary to prepare joints to connect relatively short wires to meet the length requirements. However, since the buffer layer of the superconducting wire is generally electrically insulating, how to simultaneously lead out the current of each superconducting layer when connecting wires with multiple superconducting layers is also a problem that needs to be considered. At the same time, due to the lack of effective oxygen diffusion channels and the extremely low diffusion coefficient of oxygen in the superconducting layer of the second-generation high-temperature superconducting wire, the oxidation annealing process of the joint when connecting multi-superconducting layer wires is relatively long, which greatly affects the preparation efficiency of the superconducting joint, and thus it is difficult to carry out practical applications. Moreover, the conductivity and mechanical properties of the prepared superconducting wire joints are greatly reduced compared with the original superconducting wires. In order to achieve a resistance-free superconducting joint, it is necessary to directly connect the superconducting layers of the two superconducting wires. Connecting the superconducting layer interface by melt diffusion welding is one of the currently feasible methods. However, the oxygen diffusion efficiency of general melt diffusion welding is too low, resulting in low joint performance and preparation efficiency of multi-superconducting layer wires. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a composite superconducting wire and a preparation method and a connection method thereof, and a connected superconducting wire. The preparation method provided by the present invention enables the composite superconducting wire to have multiple superconducting layers. Theoretically, the number of superconducting layers is not limited, and the composite superconducting wire has a higher engineering current density J e At the same time, it can improve the performance recovery of the superconducting layer after subsequent connection, and greatly improve the critical current and preparation efficiency of the superconducting joint.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a composite superconducting wire, comprising the following steps:

[0007] (1) overlapping the silver layer of the silver-containing strip with the silver layer adjacent to the superconducting layer in a second-generation high-temperature superconducting wire, and performing heat treatment on the overlapping region to obtain a conjoined superconducting wire;

[0008] (2) keeping the silver-containing strip in the conjoined superconducting wire straight, bending and peeling the second-generation high-temperature superconducting wire from one end, separating the superconducting layer and the buffer layer of the second-generation high-temperature superconducting wire, and obtaining a superconducting wire prototype;

[0009] (3) plating a silver layer on the surface of the superconducting layer of the superconducting wire precursor to obtain a superconducting wire intermediate;

[0010] (4) repeating (1), (2) and (3) n times with the superconducting wire intermediate and another second-generation high-temperature superconducting wire, where n≥0, to obtain a composite superconducting wire precursor;

[0011] (5) Performing oxidation annealing on the composite superconducting wire precursor to obtain the composite superconducting wire.

[0012] Preferably, the silver-containing ribbon comprises a silver ribbon or a second-generation high-temperature superconducting wire.

[0013] Preferably, when the silver-containing strip is a silver strip, the (1) is: both sides of the silver strip overlap with the silver layers adjacent to the superconducting layer in the second-generation high-temperature superconducting wire, and the overlapping area is heat treated to obtain a conjoined superconducting wire.

[0014] Preferably, the thickness of the silver strip is 20-200 μm.

[0015] Preferably, the heat treatment is performed at a temperature of 660 to 960° C. and a pressure of 0.1 to 100 MPa.

[0016] Preferably, the radius of the bend is >5 mm.

[0017] Preferably, the parameters of the oxidation annealing include: oxygen partial pressure of 0.1-15 MPa, temperature of 400-600° C., and time of 0.5-300 h.

[0018] The present invention also provides a composite superconducting wire obtained by the preparation method described in the above technical solution, wherein the composite superconducting wire has multiple superconducting layers.

[0019] The present invention also provides a method for connecting the composite superconducting wires described in the above technical solution, comprising the following steps:

[0020] (A) dividing the regions to be connected of the two composite superconducting wires into regions 1 to m in sequence from the ends according to the number of superconducting layers, wherein m≥1, and defining the superconducting layers as regions 1 to m in sequence starting from the silver layer or the buffer layer; removing the surface material of the first region of the two composite superconducting wires until the first superconducting layer is exposed, and so on until the surface material of the mth region is removed until the mth superconducting layer is exposed, thereby obtaining the composite superconducting wires to be connected; the exposed superconducting layers in the regions to be connected of the composite superconducting wires to be connected are distributed in a stepped manner;

[0021] (B) overlapping the regions to be connected of the composite superconducting wires to be connected, sequentially performing melt diffusion welding and oxidation annealing treatment on the overlapping regions, and forming a protective layer on the outer surface of the resulting joint.

[0022] The present invention also provides a connected superconducting wire obtained by the connection method described in the above technical solution.

[0023] The present invention provides a method for preparing a composite superconducting wire, wherein the silver layer of a silver-containing strip is connected to the silver layer of a second-generation high-temperature superconducting wire by high-temperature heat treatment, thereby completely stripping the superconducting layer from the buffer layer. The stripped superconducting wire can be silver-plated on the superconducting layer again and the stripping process can be repeated, thereby preparing a composite superconducting wire with multiple superconducting layers. The silver layer adjacent to the superconducting layer can serve as a fast oxygen diffusion channel, ensuring that the composite superconducting wire has a high engineering current density J e , electromechanical properties; and the superconducting properties of the joints obtained when they are later connected to each other are easy to recover. Furthermore, the metal base tape, buffer layer or thicker silver tape is used to provide support or isolation for the silver layer and the superconducting layer, thereby ensuring the mechanical properties of the composite superconducting wire and its joints.

[0024] The present invention also provides a method for connecting composite superconducting wires. The method provided by the present invention exposes the superconducting layer of the composite superconducting wire in the area to be connected in a stepped form, and then connects the two composite superconducting layers together through melt diffusion welding and oxidation annealing treatment. The superconducting performance of the obtained joint is easy to restore and has excellent mechanical properties; at the same time, the connection efficiency is high.

[0025] The present invention also provides a connected superconducting wire obtained by the connection method described in the above technical solution. The connected superconducting wire of the present invention has a sufficient length and the joint also has good mechanical properties and superconductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram of the structure of the second-generation high-temperature superconducting wire and silver ribbon; Figure 1 In the figure, (a) is a schematic diagram of the structure of a second-generation high-temperature superconducting wire with a protective layer, wherein 1 is a protective layer, 2 is a silver layer, 3 is a superconducting layer, 4 is a buffer layer, and 5 is a metal base tape; (b) is a schematic diagram of the structure of a second-generation high-temperature superconducting wire without a protective layer, wherein: 2 is a silver layer, 3 is a superconducting layer, 4 is a buffer layer, and 5 is a metal base tape; (c) is a schematic diagram of the structure of a silver tape 6;

[0027] Figure 2 Schematic diagram of the process of preparing a composite superconducting wire from two second-generation high-temperature superconducting wires, wherein: 2-1a and 2-1b are two second-generation high-temperature superconducting wires, 2-2 is a conjoined superconducting wire, 2-3 is a buffer layer-metal base tape-silver layer composite obtained after bending and peeling, 2-4 is a superconducting wire prototype, 2-5 is a superconducting wire intermediate, and 2-6 is a composite superconducting wire;

[0028] Figure 3Schematic diagram of the process of preparing composite superconducting wires from silver ribbons and second-generation high-temperature superconducting wires, wherein 3-1 is the second-generation high-temperature superconducting wire, 6 is the silver ribbon, 3-2 is the conjoined superconducting wire, 3-3 is the buffer layer-metal base tape-silver layer composite obtained after bending and peeling, 3-4 is the superconducting wire prototype, 3-5 is the superconducting wire intermediate, and 3-6 is the composite superconducting wire;

[0029] Figure 4 Schematic diagram of the process of preparing a composite superconducting wire from two silver ribbons and a second-generation high-temperature superconducting wire, wherein 6 is a silver ribbon, 4-1a and 4-2b are two second-generation high-temperature superconducting wires, 4-2 is a conjoined superconducting wire, 4-3a and 4-3b are a buffer layer-metal base tape-silver layer composite obtained after bending and peeling, 4-4 is a superconducting wire prototype, 4-5 is a superconducting wire intermediate, and 4-6 is a composite superconducting wire;

[0030] Figure 5 Schematic diagram of the process of the composite superconducting wire connection method in Example 10, wherein 5-1a and 5-1b are two superconducting wires with exposed superconducting layers in the area to be connected and distributed in a step-like manner, and 5-2 is a connecting superconducting wire;

[0031] Figure 6 The voltage-current (VI) curves of the composite superconducting wire and the second-generation high-temperature superconducting wire prepared in Examples 1 and 4 measured by the four-lead method at 77K zero field;

[0032] Figure 7 The voltage-current (VI) curves of the joints prepared in Example 10 and Comparative Example 1 measured by the four-lead method at 77K zero field;

[0033] Figure 8 The cross-sectional optical micrographs of the conjoined superconducting wires obtained in Example 3 and Comparative Example 2 are shown in FIG. (a) is a cross-sectional optical micrograph of the conjoined superconducting wires obtained in Example 3; FIG. (b) is a cross-sectional optical micrograph of the conjoined superconducting wires obtained in Comparative Example 2, and 8-1 is a region where the silver layer is not completely connected;

[0034] Figures 1 to 5 as well as Figure 8 If there is no special explanation in the figure, the numbers 1, 2, 3, 4, 5 and 6 represent the protective layer, silver layer, superconducting layer, buffer layer, metal base tape and silver tape respectively, among which 4 / 5 are the composite layers of buffer layer and metal base tape, among which 4 represents the buffer layer and 5 represents the metal base tape. DETAILED DESCRIPTION

[0035] The present invention provides a method for preparing a composite superconducting wire, comprising the following steps:

[0036] (1) overlapping the silver layer of the silver-containing strip with the silver layer adjacent to the superconducting layer in a second-generation high-temperature superconducting wire, and performing heat treatment on the overlapping region to obtain a conjoined superconducting wire;

[0037] (2) keeping the silver-containing strip in the conjoined superconducting wire straight, bending and peeling the second-generation high-temperature superconducting wire from one end, separating the superconducting layer and the buffer layer of the second-generation high-temperature superconducting wire, and obtaining a superconducting wire prototype;

[0038] (3) plating a silver layer on the surface of the superconducting layer of the superconducting wire precursor to obtain a superconducting wire intermediate;

[0039] (4) repeating (1), (2) and (3) n times with the superconducting wire intermediate and another second-generation high-temperature superconducting wire, where n≥0, to obtain a composite superconducting wire precursor;

[0040] (5) Performing oxidation annealing on the composite superconducting wire precursor to obtain the composite superconducting wire.

[0041] The invention overlaps the silver layer of the silver-containing strip with the silver layer adjacent to the superconducting layer in a second-generation high-temperature superconducting wire, and heat-treats the overlapping area to obtain a conjoined superconducting wire.

[0042] In the present invention, the silver-containing strip preferably includes a silver strip or a second-generation high-temperature superconducting wire.

[0043] In the present invention, the second-generation high-temperature superconducting wire includes a second-generation high-temperature superconducting wire with a protective layer or a second-generation high-temperature superconducting wire without a protective layer; the structure of the second-generation high-temperature superconducting wire with a protective layer is preferably a first protective layer, a first silver layer, a metal base tape, a buffer layer, a superconducting layer, a second silver layer, and a second protective layer stacked in sequence; the structure of the second-generation high-temperature superconducting wire without a protective layer is preferably a first silver layer, a metal base tape, a buffer layer, a superconducting layer, and a second silver layer stacked in sequence. In the present invention, the structure of the second-generation high-temperature superconducting wire with a protective layer is as follows Figure 1 As shown in Figure (a); the structure of the second generation high temperature superconducting wire without protective layer is as follows Figure 1 In the present invention, when the second-generation high-temperature superconducting wire is a second-generation high-temperature superconducting wire with a protective layer, it is preferred to remove the protective layer first when using it. The present invention does not specifically limit the method of removing the protective layer, and the technical means known to those skilled in the art can be used.

[0044] In the present invention, the thickness of the silver ribbon is preferably 20 to 200 μm. The structural schematic diagram of the silver ribbon is as shown in Figure 1 As shown in Figure (c).

[0045] In the present invention, the temperature of the heat treatment is preferably 660-960°C, more preferably 750-850°C, and more preferably 800°C; the pressure is preferably 0.1-100 MPa, more preferably 5-50 MPa, and more preferably 20 MPa; the time is preferably 0.1-120 min, more preferably 1-10 min, and more preferably 2 min.

[0046] The present invention overlaps the silver layer of the silver-containing strip with the silver layer of a second-generation high-temperature superconducting wire and performs heat treatment on the overlapping area at a relatively high temperature and appropriate pressure. In this way, the advantages of silver becoming soft at high temperature and having higher adhesion can be utilized to completely connect the two silver layers into a thicker layer of silver, and at the same time effectively eliminate or reduce the original defects in the silver layer, and improve the interlayer connection strength of the silver and superconducting layers. At the same time, since the thermal expansion coefficient of the silver layer is greater than that of the superconducting layer and the buffer layer, the thermal expansion amount of the silver layer is greater under the same high temperature conditions. Since the heat treatment applies a certain pressure and the silver layer is very thin (the thickness is generally 1 to 2 μm), the internal stress generated by cooling and shrinkage after the heat treatment is mainly concentrated at the interface between the silver layer and the superconducting layer, and the connection strength of the interface is higher than that of the interface between the superconducting layer and the buffer layer. Therefore, the internal stress is partially released by destroying the connection between the interface between the superconducting layer and the buffer layer, which greatly reduces the connection strength of the original interface between the superconducting layer and the buffer layer, thereby effectively promoting the subsequent peeling of the superconducting layer. In addition, the high temperature makes the silver soft, thereby shortening the connection time of the silver layer and improving production efficiency.

[0047] A conjoined superconducting wire is obtained. The present invention keeps the silver-containing strip in the conjoined superconducting wire straight, bends and peels off the second-generation high-temperature superconducting wire from one end, separates the superconducting layer and the buffer layer of the second-generation high-temperature superconducting wire, and obtains a superconducting wire prototype.

[0048] In the present invention, the bending radius is preferably greater than 5 mm, more preferably 50 to 100 mm, and even more preferably 80 mm.

[0049] The method of the present invention keeps the silver-containing strip as a substrate straight, bends and peels off the second-generation high-temperature superconducting wire from one end, and separates the superconducting layer and the buffer layer of the peeled second-generation high-temperature superconducting wire without affecting the integrity of the silver-containing strip as the substrate. On the other hand, the buffer layer of the peeled superconducting wire remains intact and completely exposed, so it can be used again to prepare the same superconducting layer to form a second high-temperature superconducting wire, thereby reducing the cost of superconducting wire preparation.

[0050] After obtaining the superconducting wire prototype, the present invention plates a silver layer on the surface of the superconducting layer of the superconducting wire prototype to obtain a superconducting wire intermediate.

[0051] In the present invention, the thickness of the silver-plated layer is preferably 2 μm.

[0052] In the present invention, the method of plating the silver layer preferably includes vacuum evaporation, magnetron sputtering or ion plating, and more preferably magnetron sputtering. The present invention does not specifically limit the parameters of the magnetron sputtering silver layer, and the magnetron sputtering silver layer known to those skilled in the art can be used.

[0053] The present invention plates a silver layer on the surface of the superconducting layer. The diffusion coefficient of oxygen in silver is relatively high (about 10 of the diffusion coefficient in the superconducting layer). 2 ~10 4 times), so oxygen can enter the superconducting layer that loses its superconductivity due to loss of oxygen after heat treatment through the silver layer, which is beneficial to the subsequent superconducting layer to restore its superconducting performance.

[0054] After obtaining the superconducting wire intermediate, the present invention repeatedly overlaps the superconducting wire intermediate with another second-generation high-temperature superconducting wire, performs heat treatment, bending and peeling, and silver plating n times, wherein n≥0, to obtain a composite superconducting wire precursor.

[0055] In the present invention, when the silver-containing strip is a second-generation high-temperature superconducting wire, n is preferably 0≤n≤10, and more preferably 0≤n≤4. In the present invention, when the silver-containing strip is a silver strip, n is preferably 1≤n≤10, and more preferably 1≤n≤4.

[0056] In the present invention, when the silver-containing strip is a second-generation high-temperature superconducting wire, the number of superconducting layers of the composite superconducting wire precursor is preferably n+2; when the silver-containing strip is a silver strip, the number of superconducting layers of the composite superconducting wire precursor is preferably n+1.

[0057] After obtaining the composite superconducting wire precursor, the present invention performs oxidation annealing on the composite superconducting wire precursor to obtain the composite superconducting wire.

[0058] In the present invention, the oxygen partial pressure of the oxidation annealing is preferably 0.1-15 MPa, more preferably 1 MPa; the temperature is preferably 400-600° C., more preferably 500° C.; the time is preferably 0.5-300 h, more preferably 1-50 h, more preferably 5 h.

[0059] In the present invention, when the silver-containing strip is a silver strip, it preferably includes: both sides of the silver strip overlap with the silver layers adjacent to the superconducting layer in the second generation high temperature superconducting wire, and heat-treating the overlapping area to obtain a conjoined superconducting wire.

[0060] In the present invention, the parameters of the heat treatment are preferably consistent with the above technical solution, which will not be repeated here. In the present invention, when the silver tape overlaps with the silver layers adjacent to the superconducting layer in the second-generation high-temperature superconducting wire on both sides, the subsequent steps are consistent with the above technical solution, which will not be repeated here. In the present invention, the n is preferably 0≤n≤10, and more preferably 0≤n≤4. In the present invention, the number of superconducting layers of the composite superconducting wire precursor is preferably 2n+2.

[0061] The present invention completely peels off the superconducting layer and the buffer layer, and the silver layer connected to the exposed superconducting layer can be used as a fast oxygen diffusion channel to ensure the superconductivity of the superconducting wire.

[0062] The present invention also provides a composite superconducting wire obtained by the preparation method described in the above technical solution.

[0063] In the present invention, the structure of the composite superconducting wire may be a first silver layer, a first superconducting layer, a second silver layer, a second superconducting layer and a third silver layer stacked in sequence, or a first silver layer, a metal base tape, a buffer layer, a first superconducting layer, a second silver layer, a second superconducting layer and a third silver layer stacked in sequence. In the present invention, the first silver layer and the second silver layer or the third silver layer may be a composite layer of two silver layers adjacent to the superconducting layer in the second generation high temperature superconducting wire, or a composite layer of a silver layer and a silver-plated layer adjacent to the superconducting layer in the second generation high temperature superconducting wire, or a composite layer of a silver layer and a silver tape adjacent to the superconducting layer in the second generation high temperature superconducting wire, or a composite layer of a silver tape and a silver-plated layer. The specific silver layer is determined according to the actual situation.

[0064] The cross-sectional area of ​​the composite superconducting wire provided by the present invention changes very little, which can greatly improve the engineering current density J of the composite superconducting wire. e .

[0065] The present invention also provides a method for connecting the composite superconducting wires described in the above technical solution, comprising the following steps:

[0066] (A) dividing the regions to be connected of the two composite superconducting wires into the first to m regions starting from the ends according to the number of superconducting layers, and defining the superconducting layers as the first to m superconducting layers starting from the silver layer or the buffer layer; removing the surface material of the first region of the two composite superconducting wires until the first superconducting layer is exposed, and so on until the surface material of the mth region is removed until the mth superconducting layer is exposed, thereby obtaining the composite superconducting wires to be connected; the exposed superconducting layers in the regions to be connected of the composite superconducting wires to be connected are distributed in a stepped manner;

[0067] (B) overlapping the regions to be connected of the composite superconducting wires to be connected, sequentially performing melt diffusion welding and oxidation annealing treatment on the overlapping regions, and forming a protective layer on the outer surface of the resulting joint.

[0068] The present invention divides the areas to be connected of two composite superconducting wires into the first to m areas starting from the ends according to the number of superconducting layers, and defines the superconducting layers as the first to m superconducting layers starting from the silver layer or the buffer layer; removes the surface material of the first area of ​​the two composite superconducting wires until the m superconducting layer is exposed, and so on until the surface material of the m area is removed until the first superconducting layer is exposed, thereby obtaining the composite superconducting wires to be connected; the exposed superconducting layers in the areas to be connected of the composite superconducting wires to be connected are distributed in a stepped manner.

[0069] In the present invention, when the region to be connected of the composite superconducting wire is divided into regions, the length of each region is not specifically limited. In a specific embodiment of the present invention, the length of each region is preferably 0.5 to 2 cm.

[0070] In the present invention, the specific steps of removing the surface material of the first region of the two composite superconducting wires until the mth superconducting layer is exposed, and so on until the surface material of the mth region is removed until the first superconducting layer is exposed preferably include:

[0071] The first region of the composite superconducting wire is immersed in a silver etchant to expose the mth superconducting layer; then the second region and the first region are immersed in the superconducting layer etchant and the silver etchant in turn to expose the m-1th superconducting layer of the first region and the mth superconducting layer of the second region; then the first, second and third regions are immersed in the superconducting layer etchant and the silver etchant in turn to expose the m-2th superconducting layer of the first region, the m-1th superconducting layer of the second region and the mth superconducting layer of the third region, until the mth superconducting layer of the mth region is exposed.

[0072] In the present invention, the silver etchant is preferably SilverEtchant TFS etchant produced by Transene Corporation of the United States. In the present invention, the superconducting layer etchant is preferably diluted phosphoric acid or diluted sulfuric acid with a mass concentration of 5%.

[0073] After obtaining the composite superconducting wires to be connected, the present invention overlaps the areas to be connected of the composite superconducting wires to be connected, performs melt diffusion welding and oxidation annealing treatment on the overlapping areas in sequence, and forms a protective layer on the outer surface of the obtained joint.

[0074] In the present invention, the conditions for melt diffusion welding include: oxygen partial pressure P O2 Preferably ≤1000Pa, the pressure is preferably 1-50MPa, more preferably 20MPa; the temperature is preferably 750-950°C, more preferably 800-900°C, more preferably 850°C; the time is preferably 0.5-120min, more preferably 5min.

[0075] In the present invention, the oxygen partial pressure P O2 It is preferably obtained by filling with an inert gas or evacuating the air.

[0076] In the present invention, the oxygen partial pressure of the oxidation annealing is preferably 0.1-15 MPa, more preferably 1 MPa; the temperature is preferably 400-600° C., more preferably 500° C.; the time is preferably 0.5-300 h, more preferably 100-200 h.

[0077] In the present invention, the material of the protective layer is preferably one of aluminum, copper, silver, gold, nickel, iron, stainless steel, aluminum alloy, copper alloy, silver alloy, nickel alloy and iron alloy, and more preferably copper.

[0078] In the present invention, the method of forming a protective layer on the outer surface of the obtained joint preferably includes laminating and welding metal strips, wrapping the surface with insulating tape or surface coating. In the present invention, the metal strip in the laminating and welding metal strips is preferably a copper strip. The present invention does not specifically limit the method of laminating and welding metal strips, and parameters known to those skilled in the art can be used.

[0079] The present invention also provides a connected superconducting wire obtained by the connection method described in the above technical solution.

[0080] The connecting superconducting wire provided by the invention has excellent superconductivity and mechanical properties.

[0081] The composite superconducting wire and its preparation method and connection method, and the connected superconducting wire provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0082] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0083] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the materials, reagents or instruments used, they are all conventional products that can be obtained commercially.

[0084] Example 1

[0085] A method for preparing a composite superconducting wire, referring to Figure 1 and 2 , including the following steps:

[0086] 1. The silver layers adjacent to the superconducting layers in two second-generation high-temperature superconducting wires are overlapped, and then a pressure of 20 MPa is applied to the overlapping area, and heat-treated at 800°C for 2 minutes to connect the two overlapping silver layers into one, thereby obtaining two superconducting wires connected into one;

[0087] 2. Use any one of the two superconducting wires connected as one in step 1 as a base and keep it straight, and bend the other one from one end with a radius of 80 mm and peel it off, so that the superconducting layer of the peeled superconducting wire is separated from the buffer layer, and obtain a superconducting wire prototype;

[0088] 3. The surface of the superconducting layer of the initial superconducting wire in step 2 is coated with a silver layer by magnetron sputtering to obtain a superconducting wire intermediate;

[0089] 4. The superconducting wire intermediate obtained in step 3 is annealed in an environment of 1 MPa oxygen partial pressure and 500° C. for 5 h to obtain a composite superconducting wire with two superconducting layers.

[0090] Example 2

[0091] A method for preparing a composite superconducting wire, referring to Figure 1 and 2 , including the following steps:

[0092] 1. The silver layers adjacent to the superconducting layers in two second-generation high-temperature superconducting wires are overlapped, and then a pressure of 50 MPa is applied to the overlapping area, and heat-treated at 750°C for 10 minutes to connect the two overlapping silver layers into one, thereby obtaining two superconducting wires connected into one;

[0093] 2. Use any one of the two superconducting wires connected as one in step 1 as a base and keep it straight, and bend the other one from one end with a radius of 50 mm and peel it off, so that the superconducting layer of the peeled superconducting wire is separated from the buffer layer, and obtain a superconducting wire prototype;

[0094] 3. A silver layer is plated on the superconducting layer of the superconducting wire of the initial superconducting wire in step 2 by magnetron sputtering to obtain a superconducting wire intermediate;

[0095] 4. Repeat steps 1, 2 and 3 twice with the superconducting wire intermediate in step 3 and another second-generation high-temperature superconducting wire to obtain a composite superconducting wire precursor having four superconducting layers;

[0096] 5. The composite superconducting wire precursor obtained in step 4 was annealed in an environment of 0.1 MPa oxygen partial pressure and 400° C. for 50 h to obtain a composite superconducting wire.

[0097] Example 3

[0098] A composite superconducting wire was prepared in the same manner as in Example 2, except that the pressure in step 1 was modified to 5 MPa, the temperature was modified to 850°C, and the heat treatment time was modified to 1 min; the bending radius in step 2 was modified to 100 mm; the number of repetitions in step 4 was modified to 4 times to obtain a composite superconducting wire precursor having 6 superconducting layers; and the conditions in step 5 were modified to anneal the composite superconducting wire precursor obtained in step 4 in an environment of 15 MPa oxygen partial pressure and 600°C for 1 h.

[0099] Example 4

[0100] A method for preparing a composite superconducting wire, referring to Figure 1 and 3 , including the following steps:

[0101] 1. A 100 μm thick silver ribbon and a silver layer adjacent to a superconducting layer in a second-generation high-temperature superconducting wire are overlapped with each other, and then a pressure of 20 MPa is applied to the overlapping area, and heat-treated at 800°C for 2 minutes to connect them into one, thereby obtaining a superconducting wire composed of the silver ribbons connected as one;

[0102] 2. The silver tape in the superconducting wire with a layer of silver tape in step 1 is kept straight as a substrate, and the original second-generation high-temperature superconducting wire is bent and peeled off from one end with a radius of 80 mm, so that the superconducting layer of the peeled superconducting wire is separated from the buffer layer, and a superconducting wire prototype is obtained;

[0103] 3. The superconducting layer of the initial superconducting wire in step 2 is coated with a silver layer by magnetron sputtering to obtain a superconducting wire intermediate;

[0104] 4. Repeat steps 1, 2 and 3 once with the superconducting wire intermediate treated in step 3 and another second-generation high-temperature superconducting wire to obtain a composite superconducting wire precursor having two superconducting layers;

[0105] 5. The composite superconducting wire precursor obtained in step 4 was annealed in an environment of 1 MPa oxygen partial pressure and 500° C. for 5 h to obtain a composite superconducting wire.

[0106] Example 5

[0107] A method for preparing a composite superconducting wire, referring to Figure 1 and 3 , including the following steps:

[0108] 1. A 20 μm thick silver ribbon and a silver layer adjacent to a superconducting layer in a second-generation high-temperature superconducting wire are overlapped, and then a pressure of 50 MPa is applied to the overlapping area, and heat-treated at 750°C for 10 minutes to connect them into one, thereby obtaining a superconducting wire composed of the silver ribbons connected as one;

[0109] 2. The silver tape in the superconducting wire with a layer of silver tape in step 1 is kept straight as a substrate, and the original second-generation high-temperature superconducting wire is bent and peeled off from one end with a radius of 50 mm, so that the superconducting layer of the peeled superconducting wire is separated from the buffer layer, and a superconducting wire prototype is obtained;

[0110] 3. The superconducting layer of the initial superconducting wire in step 2 is coated with a silver layer by magnetron sputtering to obtain a superconducting wire intermediate;

[0111] 4. Repeating steps 1, 2 and 3 three times with the superconducting wire intermediate in step 3 and another second-generation high-temperature superconducting wire to obtain a composite superconducting wire precursor having four superconducting layers;

[0112] 5. The composite superconducting wire precursor obtained in step 4 was annealed in an environment of 0.1 MPa oxygen partial pressure and 400° C. for 50 h to obtain a composite superconducting wire.

[0113] Example 6

[0114] A composite superconducting wire was prepared in the same manner as in Example 5, except that the thickness of the silver tape in step 1 was modified to 200 μm, the pressure was modified to 5 MPa, the temperature was modified to 850°C, and the heat treatment time was modified to 1 min; the bending radius in step 2 was modified to 100 mm; the number of repetitions in step 4 was modified to 5 times to obtain a composite superconducting wire precursor having 6 superconducting layers; and the conditions in step 5 were modified to anneal the composite superconducting wire precursor obtained in step 4 in an environment of 15 MPa oxygen partial pressure and 600°C for 1 h.

[0115] Example 7

[0116] A method for preparing a composite superconducting wire, referring to Figure 1 and 4 , including the following steps:

[0117] 1. The two surfaces of a 100 μm thick silver ribbon are overlapped with the silver layers adjacent to the superconducting layer in the second-generation high-temperature superconducting wire, and then a pressure of 20 MPa is applied to the overlapping area, and heat-treated at 800 ° C for 2 minutes to connect them into one, thereby obtaining two superconducting wires composited with silver ribbons connected as one;

[0118] 2. The silver tape in the superconducting wire with a layer of silver tape and a double superconducting layer in step 1 is kept straight as a substrate, and the original second-generation high-temperature superconducting wire is bent and peeled off from one end with a radius of 80 mm, so that the superconducting layer of the peeled superconducting wire is separated from the buffer layer, and a superconducting wire prototype is obtained;

[0119] 3. A silver layer is plated on the superconducting layer of the superconducting wire prototype in step 2 by magnetron sputtering to obtain a composite superconducting wire intermediate having two superconducting layers;

[0120] 4. The composite superconducting wire intermediate obtained in step 3 is annealed in an environment of 1 MPa oxygen and 500° C. for 5 h to obtain a composite superconducting wire.

[0121] Example 8

[0122] A method for preparing a composite superconducting wire, referring to Figure 1 and 4 , including the following steps:

[0123] 1. The two surfaces of a 20 μm thick silver ribbon are overlapped with the silver layers adjacent to the superconducting layers in two second-generation high-temperature superconducting wires, and then a pressure of 50 MPa is applied to the overlapping area, and heat-treated at 750 ° C for 10 minutes to connect them into one, thereby obtaining two superconducting wires composited with silver ribbons connected as one;

[0124] 2. The silver tape in the superconducting wire with a layer of silver tape in step 1 is kept straight as a substrate, and the original second-generation high-temperature superconducting wire is bent and peeled off from one end with a radius of 50 mm, so that the superconducting layer of the peeled superconducting wire is separated from the buffer layer, and a superconducting wire prototype is obtained;

[0125] 3. A silver layer is plated on the superconducting layer of the superconducting wire of the initial superconducting wire in step 2 by magnetron sputtering to obtain a superconducting wire intermediate;

[0126] 4. Repeat steps 1, 2 and 3 twice with the superconducting wire intermediate in step 3 and another second-generation high-temperature superconducting wire to obtain a composite superconducting wire precursor having 6 superconducting layers;

[0127] 5. The composite superconducting wire precursor obtained in step 4 was annealed in an environment of 0.1 MPa oxygen and 400° C. for 50 h to obtain a composite superconducting wire.

[0128] Example 9

[0129] A composite superconducting wire was prepared in the same manner as in Example 8, except that the thickness of the silver tape in step 1 was set to 200 μm, the pressure was set to 5 MPa, the temperature was set to 850°C, and the heat treatment time was set to 1 min; the bending radius in step 2 was set to 100 mm; the number of repetitions in step 4 was set to 4 times, and a composite superconducting wire precursor having 10 superconducting layers was obtained; and the conditions in step 5 were changed to annealing the composite superconducting wire precursor obtained in step 4 in an environment of 15 MPa oxygen partial pressure and 600°C for 1 h.

[0130] Example 10

[0131] A method for connecting a composite superconducting wire, referring to Figure 1 and 5 , including the following steps:

[0132] A. The regions to be connected of the two composite superconducting wires prepared in Example 1 are divided into the first and second regions from the ends, each region is 2 cm long and wrapped with a polyimide tape, and each superconducting layer starting from the buffer layer is defined as the first and second superconducting layers in sequence; the first regions of the two superconducting wires are immersed in a silver etchant to remove the silver layer in the first region by etching to expose the second superconducting layer, and then the first region and the second region are placed in the silver etchant and the superconducting layer etchant in sequence to expose the first superconducting layer in the first region and the second superconducting layer in the second region, so that the superconducting layers exposed in the regions to be connected are distributed in a stepped manner;

[0133] B. Overlap the two superconducting wires to be connected obtained in step A, fix the overlapping area, and evacuate to 50Pa (P O2 The overlapped area is subjected to a pressure of 20 MPa, and the area is heated to 850°C and kept warm for 5 minutes, so that the overlapping superconducting layers are partially melted and diffused into one another to form a joint; the obtained joint is annealed in an environment of 1 MPa oxygen and 500°C for 200 hours to restore the superconductivity of the superconducting layer; the superconducting joint after annealing is laminated and welded with copper tape to form a protective layer on its outer surface to complete the connection of the superconducting wire.

[0134] Embodiment 11

[0135] A method for connecting a composite superconducting wire, referring to Figure 1 and 5 , including the following steps:

[0136] A. The areas to be connected of the two multi-superconducting layer composite superconducting wires prepared in Example 2 are divided into the first to fourth areas in sequence from the ends, each area is 1 cm long and wrapped with a polyimide tape, and each superconducting layer starting from the silver layer is defined as the first to fourth superconducting layers in sequence; the first areas of the two superconducting wires are immersed in a silver etchant to etch away the silver layer in the first area to expose the fourth superconducting layer, and then the first area and the second area are placed in the silver etchant and the superconducting layer etchant in sequence to expose the third superconducting layer in the first area and the fourth superconducting layer in the second area. Then, the first region, the second region and the third region are sequentially placed in the silver etchant and the superconducting layer etchant to expose the second superconducting layer in the first region, the third superconducting layer in the second region and the fourth superconducting layer in the third region. Then, the first region, the second region, the third region and the fourth region are sequentially placed in the silver etchant and the superconducting layer etchant to expose the first superconducting layer in the first region, the second superconducting layer in the second region, the third superconducting layer in the third region and the fourth superconducting layer in the fourth region, so that the superconducting layers exposed in the regions to be connected are distributed in a stepped manner.

[0137] B. Overlap the two superconducting wires obtained in step A and fix the overlapped area, and evacuate to 5000Pa (P O2 The method comprises the following steps: applying a pressure of 50 MPa to the overlapping area, heating the area to 750°C and keeping the temperature for 120 minutes, so that the overlapping superconducting layers are partially melted and diffused into each other to form a joint; annealing the obtained joint in an environment of 0.1 MPa oxygen and 400°C for 300 hours to restore the superconductivity of the superconducting layer; laminating and welding the annealed superconducting joint with copper tape to form a protective layer on its outer surface to complete the connection of the superconducting wire.

[0138] Example 12

[0139] A method for connecting a composite superconducting wire, referring to Figure 1 and 5 , including the following steps:

[0140] A. The areas to be connected of the two composite superconducting wires prepared in Example 3 are divided into the first to sixth areas starting from the ends, each area is 0.5 cm long and wrapped with a polyimide tape, and each superconducting layer starting from the silver layer is defined as the first to sixth superconducting layers in sequence; the first area of ​​the two superconducting wires is immersed in a silver etchant, the silver layer of the first area is etched away, and the sixth superconducting layer is exposed, and then the first area and the second area are sequentially placed in the silver etchant and the superconducting layer etchant to expose the fifth superconducting layer of the first area and the sixth superconducting layer of the second area, and then the first area, the second area and the third area are sequentially placed in the silver etchant and the superconducting layer etchant to expose the fourth superconducting layer of the first area and the sixth superconducting layer of the second area. The 5th superconducting layer is exposed, and the 6th superconducting layer in the 3rd region is exposed, and then the 1st region, the 2nd region, the 3rd region and the 4th region are sequentially placed in the silver etchant and the superconducting layer etchant to expose the 3rd superconducting layer in the 1st region, the 4th superconducting layer in the 2nd region, the 5th superconducting layer in the 3rd region, and the 6th superconducting layer in the 4th region. The 1st region, the 2nd region, the 3rd region, the 4th superconducting layer in the 3rd region are exposed, the 5th superconducting layer in the 4th region are exposed, and the 6th superconducting layer in the 5th region are exposed. The fifth region and the sixth region are sequentially placed in the silver etchant and the superconducting layer etchant, so that the first superconducting layer of the first region is exposed, the second superconducting layer of the second region is exposed, the third superconducting layer of the third region is exposed, the fourth superconducting layer of the fourth region is exposed, the fifth superconducting layer of the fifth region is exposed, and the sixth superconducting layer of the sixth region is exposed, so that the superconducting layers exposed in the regions to be connected are distributed in a stepped manner;

[0141] B. Overlap the areas to be connected of the two superconducting wires obtained in step A, fix the overlapped areas, and fill them with argon gas (P O2 The method comprises the following steps: applying a pressure of 50 MPa to the overlapping area, heating the area to 950°C and keeping the temperature for 0.5 min, so that the overlapping superconducting layers are partially melted and diffused into each other to form a joint; annealing the obtained joint in an environment of 15 MPa oxygen and 600°C for 100 h to restore the superconductivity of the superconducting layer; laminating and welding the annealed superconducting joint with copper tape to form a protective layer on its outer surface to complete the connection of the superconducting wire.

[0142] Embodiment 13

[0143] The composite superconducting wires were connected in the same manner as in Example 10, except that the composite superconducting wire in step A was changed to the composite superconducting wire obtained in Example 4, and the buffer layer was changed to a silver tape.

[0144] Embodiment 14

[0145] The composite superconducting wires were connected in the same manner as in Example 11, except that the composite superconducting wire in step A was changed to the composite superconducting wire obtained in Example 5, and the buffer layer was changed to a silver tape.

[0146] Embodiment 15

[0147] The composite superconducting wires were connected in the same manner as in Example 12, except that the composite superconducting wire described in step A was changed to the composite superconducting wire obtained in Example 6, and the buffer layer was changed to a silver tape.

[0148] Comparative Example 1

[0149] A method for connecting a second generation high temperature superconducting wire comprises the following steps:

[0150] 1. Immerse a 4 cm long second-generation high-temperature superconducting wire in a silver etchant to remove the silver layer and expose the superconducting layer underneath;

[0151] 2. Immerse the 2 cm long area to be connected of the two second-generation high-temperature superconducting wires to be connected in a silver etchant to etch away the silver layer, exposing the superconducting layer underneath, and use laser welding to achieve the connection between the metal base tapes;

[0152] 3. Overlap the superconducting layer of the connector obtained in step 1 and the exposed superconducting layers of the two superconducting wires in step b, fix the overlapping area, and evacuate to 50Pa (P O2 The overlapped area is subjected to a pressure of 20 MPa, and the temperature of the area is raised to 850° C. and kept at this temperature for 5 minutes, so that the overlapping superconducting layers are partially melted and diffused into each other to form a joint;

[0153] 4. Anneal the joint in step 3 in an environment of 1MPa oxygen and 500°C for 200h to restore the superconductivity of its superconducting layer;

[0154] 5. The superconducting joint processed in step 4 is laminated and welded with copper tape to form a protective layer on its outer surface to complete the connection of the superconducting wire.

[0155] Comparative Example 2

[0156] The following provides a method for preparing a composite superconducting wire, referring to Figure 1 and 2 , which comprises the following steps:

[0157] 1. The silver layers adjacent to the superconducting layers in two second-generation high-temperature superconducting wires are overlapped, and then a pressure of 20 MPa is applied to the overlapping area, and heat-treated at 500°C for 60 minutes to obtain a conjoined superconducting wire;

[0158] 2. Any one of the conjoined superconducting wires in step 1 is kept straight as a base, and the other one is bent from one end with a radius of 100 mm and peeled off, and the superconducting layer is not completely peeled off or the superconducting layer is broken.

[0159] Figure 6 The voltage-current (VI) curves of the composite superconducting wires and the second-generation high-temperature superconducting wires prepared in Examples 1 and 4 were measured by the four-lead method at 77K zero field. The critical currents obtained by the 1μV / cm criterion were 183A, 174A and 97A, respectively. Compared with the original second-generation high-temperature superconducting wire, the J of the composite superconducting wire obtained was e The improvement is nearly doubled. This shows that the composite superconducting wire prepared by the method of the present invention can greatly increase the critical current compared with the original second-generation high-temperature superconducting wire, and greatly increase the engineering current density while the cross-sectional area of ​​the superconducting wire remains basically unchanged.

[0160] Figure 7 The voltage-current (VI) curves of the joints prepared in Example 10 and Comparative Example 1 were measured by the four-lead method at 77K zero field. The critical currents of the joints were 98A and 4.5A, respectively, according to the 1μV / cm criterion, indicating that the method of the present invention can not only prepare superconducting joints, but also effectively improve the efficiency of superconducting joint preparation by introducing a fast oxygen channel (silver layer).

[0161] Figure 8The cross-sectional optical micrographs of the conjoined superconducting wires obtained in Example 3 and Comparative Example 2 show that the silver layer after heat treatment at 500°C for 60 minutes has an incompletely connected area (8-1), which leads to the failure of stripping in Comparative Example 2, i.e., the superconducting layer is broken, and a superconducting current path cannot be formed and subsequently utilized; on the contrary, the silver layer after heat treatment at 850°C for 5 minutes is completely connected as a whole. This shows that the method of the present invention can make the silver layer completely connected, which is conducive to completely and effectively stripping the superconducting layer, and thereby efficiently preparing a composite superconducting wire and a superconducting joint.

[0162] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a composite superconducting wire, It is characterized in that The following steps are involved: (1) overlapping the silver layer of the silver-containing strip with the silver layer adjacent to the superconducting layer in a second-generation high-temperature superconducting wire, and performing heat treatment on the overlapping region to obtain a conjoined superconducting wire; (2) keeping the silver-containing strip in the conjoined superconducting wire straight, bending and peeling the second-generation high-temperature superconducting wire from one end, separating the superconducting layer and the buffer layer of the second-generation high-temperature superconducting wire, and obtaining a superconducting wire prototype; (3) plating a silver layer on the surface of the superconducting layer of the superconducting wire precursor to obtain a superconducting wire intermediate; (4) repeating (1), (2) and (3) n times with the superconducting wire intermediate and another second-generation high-temperature superconducting wire, wherein n>0, to obtain a composite superconducting wire precursor; (5) performing oxidation annealing on the composite superconducting wire precursor to obtain the composite superconducting wire; The heat treatment temperature is 660-960°C, the pressure is 0.1-100 MPa, and the time is 0.1-120 min; The parameters of the oxidation annealing include: oxygen partial pressure of 0.1-15 MPa, temperature of 400-600° C., and time of 0.5-50 h.

2. The preparation method according to claim 1, It is characterized in that The silver-containing ribbon comprises a silver ribbon or a second-generation high-temperature superconducting wire.

3. The preparation method according to claim 2, It is characterized in that When the silver-containing strip is a silver strip, the (1) is: both sides of the silver strip overlap with the silver layers adjacent to the superconducting layer in the second-generation high-temperature superconducting wire, and heat-treating the overlapping area to obtain a conjoined superconducting wire.

4. The preparation method according to claim 2 or 3, It is characterized in that The thickness of the silver ribbon is 20-200 μm.

5. The preparation method according to claim 1, 2 or 3, It is characterized in that The radius of the bend is >5 mm.

6. The composite superconducting wire obtained by the preparation method according to any one of claims 1 to 5, It is characterized in that The composite superconducting wire has a plurality of superconducting layers.

7. The method for connecting a composite superconducting wire according to claim 6, It is characterized in that The following steps are involved: (A) dividing the regions to be connected of the two composite superconducting wires into first to m regions starting from the ends according to the number of superconducting layers, where m≥1, and defining the superconducting layers as first to m superconducting layers starting from the silver layer or the buffer layer; The surface material of the first region of the two composite superconducting wires is removed until the first superconducting layer is exposed, and the surface material of the mth region is removed by analogy until the mth superconducting layer is exposed, thereby obtaining the composite superconducting wires to be connected; The exposed superconducting layers in the to-be-connected region of the to-be-connected composite superconducting wires are distributed in a stepped manner; (B) overlapping the regions to be connected of the composite superconducting wires to be connected, sequentially performing melt diffusion welding and oxidation annealing treatment on the overlapping regions, and forming a protective layer on the outer surface of the resulting joint.

8. A connected superconducting wire obtained by the connection method according to claim 7.

Citation Information

Patent Citations

  • ReBCO high temperature superconducting wire bonding device and bonding method using same

    CN105636719A

  • High temperature-superconducting wire having superconducting layer staked thereon and method for manufacturing same

    WO2019198937A1