A manufacturing method for improving the elongation of lithium-ion battery copper foil
By using specific additives to regulate grain growth during the copper foil manufacturing process, the problem of insufficient elongation of copper foil for lithium-ion batteries is solved, the production of high elongation copper foil is achieved, and the safety and performance of lithium batteries are improved.
Patent Information
- Application Number
- CN202111005702.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-08-30
AI Technical Summary
The prior art is difficult to effectively improve the elongation of copper foil of lithium-ion batteries, resulting in the risk of breakage of lithium batteries during charging and discharging, affecting safety and performance.
By adding specific content of organic additives to the copper foil manufacturing process, the number of initial nuclei, grain size and grain growth direction are controlled, and the electrolyte is optimized by combining brighteners, inhibiting nucleation agents, active complexation and leveling agents. The current density distribution in the increase of the elongation of the copper foil.
On the basis of ensuring tensile strength, the elongation of copper foil can be significantly improved, with an elongation of more than 13%, enhancing the winding resistance and flexibility of copper foil, and improving the safety and performance of lithium-ion batteries.
Smart Images

Figure BDA0003237078330000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolytic copper foil, and in particular to a manufacturing method for improving the elongation of copper foil for lithium-ion batteries. Background Art
[0002] Copper foil is a key material for manufacturing negative electrode current collectors of lithium-ion batteries, and its quality directly affects the manufacturing process, performance and production cost of lithium-ion batteries. The important material of lithium-ion battery current collectors is metal foil (such as copper foil and aluminum foil), whose function is to collect the current generated by the active materials of the battery in order to form a larger current output. Therefore, the current collector should be in full contact with the active material, and the internal resistance should be as small as possible, which is also an important reason why lithium-ion batteries use more expensive copper foil and aluminum foil. Lithium battery copper foil with good conductivity, flexibility, and resistance to winding and rolling is the preferred material for negative electrode current collectors of lithium-ion batteries.
[0003] Safety during the use of lithium batteries is of paramount importance. Multiple charge and discharge during the use of lithium batteries will cause the cycle cells to shrink and expand, resulting in battery performance degradation or damage. High elongation copper foil can avoid breakage during the shrinkage and expansion process, thereby increasing the safety of lithium batteries during use. At present, the elongation of copper foil in the industry is generally between 7% and 8%. If the elongation of copper foil can be further improved, it will definitely create new development opportunities for the copper foil manufacturing industry and even the battery manufacturing industry.
[0004] In the actual production of copper foil, additives are usually required to obtain relatively large and uniform grains during the electrolysis of the electrolyte, so as to increase the slip distance of the grains during the stretching process of the copper foil while ensuring the tensile strength, thereby increasing the elongation of the copper foil. In order to obtain electrolytic copper foil with higher elongation and lower profile and surface roughness, specific additives are needed. Different additives play different roles in the process of electrodeposition. For example, leveling agent is a positively charged cation. During the production of copper foil, it occupies the small bumps on the surface of the titanium roller and promotes a smoother surface of the copper foil; brightener is a type of additive that promotes the rapid brightening of the rough surface (M surface) of the copper foil, which can promote grain refinement; positioning agent can, to a certain extent, block the rapid crystallization of copper crystals, thereby making the copper crystals grow larger.
[0005] Different additives combined in different proportions play a vital role in the strength, elongation and roughness of copper foil. Although the prior art has a certain research basis for the efficacy of the above additives, there are few reports on how to reasonably combine the above additives to effectively exert the relevant properties of the additives to prepare copper foil with higher elongation. Summary of the invention
[0006] In view of the above technical problems in the related art, the present invention proposes a manufacturing method for improving the elongation of lithium-ion battery copper foil, which can overcome the above shortcomings of the prior art.
[0007] To achieve the above technical objectives, the technical solution of the present invention is implemented as follows:
[0008] A manufacturing method for improving the elongation of lithium ion battery copper foil comprises the following steps:
[0009] S1: adding copper metal into a copper dissolving tank containing sulfuric acid, blowing high-temperature air into the tank with a screw blower to dissolve the copper and prepare the main electrolyte;
[0010] S2: filtering the main electrolyte obtained in step S1 through multi-stage filtration (including filtration by a multi-stage filtration system such as diatomaceous earth and activated carbon) and mixing it with a specific additive solution to obtain a copper sulfate electrolyte;
[0011] The additives include agent A, agent B, agent C, agent D, agent E, and chloride ions, wherein agent A is selected from thiol-containing compounds, agent B is selected from alcohol-containing compounds, agent C is selected from sulfur-containing and nitrogen-containing natural or synthetic polymer compounds, agent D is selected from amino-containing compounds, and agent E is selected from oxygen-containing and nitrogen-containing compounds, and the chloride ions are provided by hydrochloric acid or sodium chloride;
[0012] The concentrations of copper ions, sulfuric acid, agent A, agent B, agent C, agent D, agent E, and chloride ions in the copper sulfate electrolyte are 85-100 g / L, 80-140 g / L, 10-80 mg / L, 30-90 mg / L, 3-50 mg / L, 3-50 mg / L, 15-80 mg / L, and 18-30 mg / L, respectively;
[0013] S3: the copper sulfate electrolyte prepared in step S2 is heated to a certain temperature by a heat exchanger, and then injected into an electrolytic cell to perform electrolysis at a certain temperature and a certain current density to prepare raw foil;
[0014] S4 rolls up the original foil prepared in step S3 and cuts it into finished products of different widths.
[0015] Preferably, the cathode of the electrolytic cell is a seamless drum-type titanium roller, and the anode of the electrolytic cell is a dimensionally stable anode.
[0016] Preferably, the agent A is selected from one or more of piperazine dithiocarboxylate propanesulfonate sodium, imidazole dithiocarboxylate propanesulfonate sodium, benzimidazole dithiocarboxylate propanesulfonate sodium, carbazole dithiocarboxylate propanesulfonate sodium, sodium citrate, benzyl acetone, and 2-mercaptobenzimidazole.
[0017] Preferably, the agent B is selected from one or more compounds such as hexynol, 4-butynediol, butynediol monopropoxy ether, butynediol ethoxylate, propynyl alcohol propoxy ether and the like.
[0018] Preferably, the agent C is selected from one or more of sodium isooctyl sulfate, sodium dodecyl sulfate, and sodium dodecyl sulfonate.
[0019] Preferably, the agent D is selected from one or more of aminopropionic acid, glycine, and chloral hydrate.
[0020] Preferably, the E agent is selected from one or more of polyethylene oxide, polypropylene oxide and ethylene oxide.
[0021] Preferably, the content of agent A in the copper ion electrolyte is 10-20 mg / L.
[0022] Preferably, the heat exchange temperature and electrolysis implementation temperature in step S3 are 50-60°C, and the current density in step S3 is 30-100A / dm 2 .
[0023] The beneficial effects of the present invention are as follows: by adding a specific amount of organic additives in the foil production process, the number of initial crystal nuclei, grain size and grain growth direction are controlled, and the elongation of copper foil can be improved while effectively ensuring the tensile strength. By increasing the size of the grains, reducing impurities at the grain boundaries, reducing grain dislocations, and thereby increasing the slip distance of the grains, the elongation of the copper foil can ultimately be improved. In the present invention, agent A is a brightener that allows copper ions to nucleate quickly; agents B and C have a certain inhibitory effect on nucleation, promoting the growth of copper crystals in the electrolyte; agent D plays an active complexing role in the electrolyte, making the current density distribution more uniform during the electrolysis process, thereby making the size of the copper crystals more uniform; agent E is a leveling agent that adheres to the convex points of the cathode, reduces the cathode tip discharge effect, and makes the copper foil surface smoother. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0025] The elongation referred to in the present invention is the percentage of the total deformation ΔL of the gauge length section after the sample is stretched and fractured to the original gauge length L: δ = ΔL / L × 100%. In the present invention, a strip sample with a width of 10 mm and a length of 150 mm is used for testing on a tensile testing machine. The test after heating is a test performed when the sample is heated at 150°C for 10 minutes.
[0026] Example 1
[0027] Add metallic copper to a copper dissolving tank containing sulfuric acid, blow high-temperature air with a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is mixed with an additive solution after multi-stage filtration to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85g / L and an acid content of 100g / L. The composition of other additives is:
[0028] Sodium piperazine dithiocarboxylate propanesulfonate: 10 mg / L;
[0029] Sodium imidazole dithiocarboxylate propanesulfonate: 10 mg / L;
[0030] Sodium benzimidazole dithiocarboxylate propanesulfonate: 10 mg / L;
[0031] Hexynol: 10mg / L;
[0032] 4-Butynediol: 15 mg / L;
[0033] Butynediol monopropoxy ether: 15mg / L; Sodium isooctyl sulfate: 5mg / L;
[0034] Sodium dodecyl sulfate: 5 mg / L;
[0035] Sodium dodecyl sulfate: 5 mg / L;
[0036] Chloral hydrate: 5mg / L;
[0037] Polyethylene oxide: 5 mg / L;
[0038] Polypropylene oxide: 5mg / L;
[0039] Chloride ion: 18mg / L;
[0040] The electrolyte is heated to 54°C by a heat exchanger and then pumped into the electrolytic cell. The cathode of the electrolytic cell is a seamless titanium roller and the anode is a size-limited anode. 2 The raw foil is prepared by electrolysis at 54°C under a current density of , and then rolled and slit into finished products of different widths.
[0041] Example 2
[0042] Add metallic copper to a copper dissolving tank containing sulfuric acid, blow high-temperature air with a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is mixed with an additive solution after multi-stage filtration to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85g / L and an acid content of 100g / L. The composition of other additives is:
[0043] Sodium piperazine dithiocarboxylate propanesulfonate: 20 mg / L;
[0044] Sodium imidazole dithiocarboxylate propanesulfonate: 15 mg / L;
[0045] Sodium benzimidazole dithiocarboxylate propanesulfonate: 15 mg / L;
[0046] Hexynol: 30mg / L;
[0047] 4-Butynediol: 30mg / L; Sodium isooctyl sulfate: 5mg / L;
[0048] Sodium dodecyl sulfate: 2 mg / L;
[0049] Sodium dodecyl sulfate: 2 mg / L;
[0050] Chloral hydrate: 5mg / L;
[0051] Polyethylene oxide: 5 mg / L;
[0052] Polypropylene oxide: 5mg / L;
[0053] Chloride ion: 30mg / L;
[0054] The electrolyte is heated to 50°C by a heat exchanger and then pumped into the electrolytic cell. The cathode of the electrolytic cell is a seamless titanium roller and the anode is a size-limited anode. 2 The raw foil is prepared by electrolysis at 50°C under a current density of , and then rolled and slit into finished products of different widths.
[0055] Example 3
[0056] Add metallic copper to a copper dissolving tank containing sulfuric acid, blow high-temperature air with a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is mixed with an additive solution after multi-stage filtration to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85g / L and an acid content of 100g / L. The composition of other additives is:
[0057] Sodium piperazine dithiocarboxylate propanesulfonate: 15 mg / L;
[0058] Sodium imidazole dithiocarboxylate propanesulfonate: 15 mg / L;
[0059] Sodium benzimidazole dithiocarboxylate propanesulfonate: 15 mg / L;
[0060] Hexynol: 10mg / L;
[0061] 4-Butynediol: 45 mg / L;
[0062] Butynediol monopropoxy ether: 10mg / L; Sodium isooctyl sulfate: 5mg / L;
[0063] Sodium dodecyl sulfate: 5 mg / L;
[0064] Sodium dodecyl sulfate: 5 mg / L;
[0065] Chloral hydrate: 3mg / L;
[0066] Polyethylene oxide: 5 mg / L;
[0067] Polypropylene oxide: 5mg / L;
[0068] Chloride ion: 25mg / L;
[0069] The electrolyte is heated to 50°C by a heat exchanger and then pumped into the electrolytic cell. The cathode of the electrolytic cell is a seamless titanium roller and the anode is a size-limited anode. 2 The raw foil is prepared by electrolysis at 50°C under a current density of , and then rolled and slit into finished products of different widths.
[0070] Example 4
[0071] Add metallic copper to a copper dissolving tank containing sulfuric acid, blow high-temperature air with a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is mixed with an additive solution after multi-stage filtration to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85g / L and an acid content of 100g / L. The composition of other additives is:
[0072] Sodium carbazole dithiocarboxylate propanesulfonate: 10 mg / L;
[0073] Sodium citrate: 20mg / L;
[0074] Benzalcetone: 20mg / L;
[0075] 2-Mercaptobenzimidazole collagen (number average molecular weight 3000-5000): 20 mg / L;
[0076] Butynediol monopropoxy ether: 30 mg / L;
[0077] Butynediol ethoxylate: 30 mg / L;
[0078] Propynyl alcohol propoxy ether: 30 mg / L;
[0079] Sodium dodecyl sulfate: 15 mg / L;
[0080] Sodium dodecyl sulfate: 15 mg / L;
[0081] Alanine: 15 mg / L;
[0082] Glycine: 15 mg / L;
[0083] Polypropylene oxide 15mg / L;
[0084] Polyethylene oxide 15 mg / L;
[0085] Chloride ion: 25mg / L;
[0086] The electrolyte is heated to 50°C by a heat exchanger and then pumped into the electrolytic cell. The cathode of the electrolytic cell is a seamless titanium roller and the anode is a size-limited anode. 2 The raw foil is prepared by electrolysis at 50°C under a current density of , and then rolled and slit into finished products of different widths.
[0087] Example 5
[0088] Add metallic copper to a copper dissolving tank containing sulfuric acid, blow high-temperature air with a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is mixed with an additive solution after multi-stage filtration to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85g / L and an acid content of 100g / L. The composition of other additives is:
[0089] Sodium carbazole dithiocarboxylate propanesulfonate: 30 mg / L;
[0090] Sodium citrate: 30mg / L;
[0091] Benzalcetone: 10mg / L;
[0092] 2-Mercaptobenzimidazole collagen (number average molecular weight 3000-5000): 10 mg / L;
[0093] Butynediol monopropoxy ether: 20 mg / L;
[0094] Butynediol ethoxylate: 20 mg / L;
[0095] Propynyl alcohol propoxy ether: 30 mg / L;
[0096] Sodium dodecyl sulfate: 20 mg / L;
[0097] Sodium dodecyl sulfate: 20 mg / L;
[0098] Alanine: 20mg / L;
[0099] Glycine: 15 mg / L;
[0100] Polypropylene oxide 20mg / L;
[0101] Ethylene oxide 15mg / L;
[0102] Chloride ion: 25mg / L;
[0103] The electrolyte is heated to 50°C by a heat exchanger and then pumped into the electrolytic cell. The cathode of the electrolytic cell is a seamless titanium roller and the anode is a size-limited anode. 2The raw foil is prepared by electrolysis at 50°C under a current density of , and then rolled and slit into finished products of different widths.
[0104] Comparative Example 1
[0105] The electrolytic copper foil was prepared by the same method as in Example 2, except that the polyethylene oxide was removed and other parameters remained unchanged.
[0106] Comparative Example 2
[0107] The electrolytic copper foil was prepared in the same manner as in Example 3, except that chloroacetaldehyde hydrate was omitted and other parameters remained unchanged.
[0108] Comparative Example 3
[0109] Electrolytic copper foil was prepared by the same method as in Example 4, except that polyethylene oxide (15 mg / L) and polypropylene oxide (15 mg / L) were replaced with ethylene oxide (15 mg / L) and propylene oxide (15 mg / L), and other parameters remained unchanged.
[0110] The basic physical properties of the electrolytic copper foils prepared in Examples 1-5 and Comparative Examples 1-3 were tested. The basic physical properties testing method is as follows:
[0111] Glossiness test: According to the test method GB / T13891, the glossiness of the copper foil M surface in the length direction is measured at a light incident angle of 60° using a WGG60-EJ gloss meter manufactured by Cosda Optoelectronic Instrument Co., Ltd.
[0112] Tensile strength and elongation test: According to the test method GB / T29847-2013, the tensile strength and elongation of the copper foil were tested at room temperature (about 25°C) using a HY-0230 universal material testing machine manufactured by Shanghai Hengyi Precision Instrument Co., Ltd.
[0113] Roughness test (Rz, ten-point roughness average): According to the test method GB / T29847-2013, the roughness Rz value of the copper foil M surface was tested using a TR200 roughness meter manufactured by Beijing Times Ruida Technology Co., Ltd.
[0114] The basic physical properties test results of the electrolytic copper foils prepared in Examples 1-5 and Comparative Examples 1-3 are shown in Table 1:
[0115] Table 1 Performance test results of high elongation electrolytic copper foil
[0116]
[0117] As shown in Table 1, the physical properties of the copper foil for lithium-ion batteries with high elongation prepared by the technical process provided by the present invention are that on the basis of the tensile strength at room temperature being greater than 320MPa, the elongation at room temperature can be controlled to be above 13%; the elongation after heating (150°C, 10min) is above 10%, and the tensile strength after heating (150°C, 10min) is greater than 310MPa; the roughness of the rough surface Rz≤2μm, and the glossiness is 120-250. Both the roughness and glossiness of the rough surface can meet the application requirements. By comparing Examples 2-4 and Comparative Examples 1-3, it can be seen that agent A is used to refine the grains, and when the amount of agent B used is more than twice that of agent A, it can significantly promote crystal growth, and the complexing effect of agent D makes the copper grain size more uniform, which plays a very important regulatory role in reducing crystal dislocations, improving elongation and ensuring tensile strength. The method of the present invention is suitable for the production of 7μm and 8μm electrolytic copper foils.
[0118] High elongation is the main sign of copper foil's winding resistance and flexibility. Copper foil for lithium-ion batteries is required to have a certain degree of ductility during the stretching process, that is, it must have a high elongation. Copper foil is the current carrier of the negative electrode material of lithium-ion batteries. Lithium-ion batteries will expand and contract during the charging and discharging process. Copper foil with high elongation is not easy to break during the expansion and contraction process, which is beneficial to improve the safety of lithium-ion batteries. Therefore, high elongation is one of the main physical properties of copper foil for lithium-ion batteries.
[0119] The present invention adopts macromolecular alcohols as additive displacement agents to inhibit the crystallization speed of copper crystals and make the copper crystals grow larger. It combines the functions of a brightener, a leveling function and a wetting function to make the copper crystals large and uniform, and increases the slip distance of the copper crystals during the stretching process, thereby effectively improving the elongation of the copper foil.
[0120] In summary, with the above technical solution of the present invention, the present invention can effectively improve the elongation of copper foil while ensuring the tensile strength. The lithium battery copper foil manufactured by the present invention has a tensile strength greater than 320MPa and an elongation of more than 13%, and the copper foil has uniform color and stable brightness.
[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for improving the elongation of lithium ion battery copper foil, characterized in that: The following steps are involved: The copper metal is added into a copper dissolving tank containing sulfuric acid, and high-temperature air is blown into the copper dissolving tank by a screw fan to prepare an acidic copper sulfate main electrolyte by dissolving the copper. The main electrolyte is mixed with an additive solution after multi-stage filtration to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85 g / L and an acid content of 100 g / L. The composition of other additives is: sodium piperazine dithiocarboxylate propanesulfonate: 10 mg / L; sodium imidazole dithiocarboxylate propanesulfonate: 10 mg / L; sodium benzimidazole dithiocarboxylate propanesulfonate: 10 mg / L; hexynol: 10 mg / L; 4-butynediol: 15 mg / L; butynediol monopropoxy ether: 15 mg / L; sodium isooctyl sulfate: 5 mg / L; sodium dodecyl sulfate: 5 mg / L; Sodium dodecyl sulfonate: 5mg / L; chloroacetaldehyde hydrate: 5mg / L; polyethylene oxide: 5mg / L; polypropylene oxide: 5mg / L; chloride ion: 18mg / L; the obtained electrolyte is heated to 54°C by a heat exchanger and pumped into an electrolytic cell. The cathode of the electrolytic cell is a seamless drum titanium roller, and the anode is a size-limited anode. At 55A / dm 2 The raw foil is prepared by electrolysis at 54°C under a current density of , and then rolled and slit into finished products of different widths.
2. A method for improving the elongation of lithium ion battery copper foil, characterized in that: The following steps are involved: The copper metal is added into a copper dissolving tank containing sulfuric acid, and high-temperature air is blown into the tank by a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is filtered through multiple stages and then mixed with an additive solution to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85 g / L and an acid content of 100 g / L. The composition of other additives is: sodium piperazine dithiocarboxylate propanesulfonate: 20 mg / L; sodium imidazole dithiocarboxylate propanesulfonate: 15 mg / L; sodium benzimidazole dithiocarboxylate propanesulfonate: 15 mg / L ; Hexynol: 30mg / L; 4-butynediol: 30mg / L; Sodium isooctyl sulfate: 5mg / L; Sodium dodecyl sulfate: 2mg / L; Sodium dodecyl sulfonate: 2mg / L; Chloral hydrate: 5mg / L; Polyethylene oxide: 5mg / L; Polypropylene oxide: 5mg / L; Chloride ion: 30mg / L; The obtained electrolyte is heated to 50℃ by a heat exchanger and injected into the electrolytic cell. The cathode of the electrolytic cell is a seamless drum titanium roller, and the anode is a size-limited anode. At 60A / dm 2 The raw foil is prepared by electrolysis at 50°C under a current density of , and then rolled and slit into finished products of different widths.
3. A method for improving the elongation of lithium ion battery copper foil, characterized in that: The following steps are involved: The copper metal is added into a copper dissolving tank containing sulfuric acid, and high-temperature air is blown into the tank by a screw fan to dissolve the copper to prepare an acidic copper sulfate main electrolyte. The main electrolyte is filtered through multiple stages and then mixed with an additive solution to obtain an electrolyte. The obtained electrolyte has a copper ion concentration of 85 g / L and an acid content of 100 g / L. The composition of other additives is: sodium piperazine dithiocarboxylate propanesulfonate: 15 mg / L; sodium imidazole dithiocarboxylate propanesulfonate: 15 mg / L; sodium benzimidazole dithiocarboxylate propanesulfonate: 15 mg / L; hexynol: 10 mg / L; 4-butynediol: 45 mg / L; butynediol monopropoxy ether: 10 mg / L; sodium isooctyl sulfate: 5 mg / L; sodium dodecyl sulfate: 5 mg / L; Sodium dodecyl sulfonate: 5mg / L; chloroacetaldehyde hydrate: 3mg / L; polyethylene oxide: 5mg / L; polypropylene oxide: 5mg / L; chloride ion: 25mg / L; the obtained electrolyte is heated to 50℃ by a heat exchanger and pumped into an electrolytic cell. The cathode of the electrolytic cell is a seamless drum titanium roller, and the anode is a size-limited anode. At 60A / dm 2 The raw foil is prepared by electrolysis at 50°C under a current density of , and then rolled and slit into finished products of different widths.