Reflective Materials

A layered reflective material with specific resin compositions and voids addresses uneven brightness and contamination issues in thin liquid crystal displays, maintaining display performance and component integrity.

CN113631967BActive Publication Date: 2024-12-03MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080025485.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-23
Filing Date
2020-03-26
Publication Date
2024-12-03
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing reflective materials used in thin liquid crystal displays suffer from issues such as uneven brightness and component contamination, particularly when using polyolefin resins, due to particle detachment and stress concentration, which can damage the light guide plate and backlight units.

Method used

A reflective material with a layered structure comprising resin layers (A), (B), and (C), where layer (B) contains polyolefin resin and fine powder filler, layer (A) contains polyolefin resin and organic particles, and layer (C) does not contain organic particles larger than 10 μm, with voids in at least one layer to prevent particle detachment and enhance mechanical stability.

Benefits of technology

The layered structure enhances reflective properties while preventing uneven brightness and component contamination, supporting the thinning of liquid crystal displays and ensuring durability of backlight units.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003283917350000411
    Figure BDA0003283917350000411
  • Figure BDA0003283917350000412
    Figure BDA0003283917350000412
Patent Text Reader

Abstract

The present invention provides a reflective material having good reflective properties. When used in a backlight unit, the reflective material can suppress the occurrence of uneven brightness and the detachment of particles contained in the surface layer of the reflective material, and can cope with the thinning of liquid crystal displays. The reflective material has a structure in which a resin layer (B), a resin layer (A) and a resin layer (C) are stacked in sequence, wherein the resin layer (B) contains a polyolefin resin and a fine powder filler, the resin layer (A) contains a polyolefin resin and organic particles, and the resin layer (C) contains a polyolefin resin and does not contain organic particles with a particle size of 10 μm or more, and at least one of the resin layers (A) to (C) has voids.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a reflective material. More specifically, the present invention relates to a reflective material that can be suitably used as a component of a liquid crystal display, a lighting fixture, an illuminated sign, and the like. Background Art

[0002] Reflective materials have been used in many fields, including liquid crystal displays, lighting fixtures, and illuminated signs. Recently, in the field of liquid crystal displays, the size of the device has been increased and the display performance has been improved. It is required to supply as much light as possible to the liquid crystal to improve the performance of the backlight unit, and reflective materials are also required to have better light reflectivity (also referred to as "reflectivity").

[0003] As such a reflective material, a reflective film for a liquid crystal display using, for example, a white polyester film containing an aromatic polyester resin as a main raw material is known (see Patent Document 1).

[0004] However, when an aromatic polyester resin is used as a reflective material, since the aromatic ring contained in the molecular chain absorbs ultraviolet light, there is a problem that the film deteriorates and turns yellow due to ultraviolet light emitted from a light source such as a liquid crystal display device, resulting in a decrease in the light reflectivity of the reflective film.

[0005] In addition, there are also known: a reflective material in which a film formed by adding a filler to a polypropylene resin is stretched to form fine voids in the film, thereby generating light scattering reflection (see Patent Document 2); and a polyolefin resin light reflector having a laminated structure consisting of a base layer containing a polyolefin resin and a filler, and a layer containing a polyolefin resin (see Patent Document 3).

[0006] Such a reflective film using a polyolefin resin has a feature that there are few problems of film degradation and yellowing due to ultraviolet rays.

[0007] In addition, a biaxially stretched reflective sheet with reduced heat shrinkage is known, the reflective sheet comprising a polypropylene resin and at least one resin incompatible with the polypropylene resin (see Patent Document 4). The reflective sheet has a characteristic of showing a higher reflectivity than a conventional reflective sheet with the same weight per unit area and density even if it does not contain a large amount of inorganic powder.

[0008] In recent years, there has been a demand for further thinning of liquid crystal displays, and there has also been a demand for thinning of backlights included in liquid crystal displays.

[0009] When the backlight is thinned, it is necessary to make components such as the back box and the light guide plate thinner. However, if these components are thinned, the mechanical strength of the backlight will be reduced. Therefore, when external force is applied to the display body, the light guide plate and the reflective material will have a local strong contact, which will cause uneven brightness and uneven color (hereinafter collectively referred to as "uneven brightness"). For this reason, for the backlight used in the thinned liquid crystal display, it is required to have a reflective material that is further endowed with the function of preventing uneven brightness.

[0010] As a means of overcoming such a problem of uneven brightness, a reflective material in which particles are contained in the surface layer of the reflective material has been proposed (see Patent Documents 5 and 6).

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 04-239540

[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 11-174213

[0015] Patent Document 3: Japanese Patent Application Publication No. 2005-031653

[0016] Patent Document 4: Japanese Patent Application Publication No. 2008-158134

[0017] Patent Document 5: Japanese Patent Application Publication No. 2015-163986

[0018] Patent Document 6: Japanese Patent Application Publication No. 2015-001596 Summary of the invention

[0019] Problem that the invention aims to solve

[0020] The present inventors have confirmed through research that, although the reflective materials disclosed in Patent Documents 5 and 6 can overcome the problem of uneven brightness, there are cases where the light guide plate is scraped and damaged, or components such as the backlight unit are contaminated. It has also been confirmed that such a phenomenon is more likely to occur in a reflective material using a polyolefin resin.

[0021] Therefore, an object of the present invention is to provide a reflective material, which relates to a reflective material using a polyolefin resin, which has good reflective properties and can suppress the occurrence of brightness unevenness and contamination of components when used in components such as backlight units, and can cope with the thinning of liquid crystal displays.

[0022] Solutions to the problem

[0023] The present invention provides a reflective material having a structure in which a resin layer (B), a resin layer (A) and a resin layer (C) are sequentially stacked, wherein the resin layer (B) contains a polyolefin resin and a fine powder filler, the resin layer (A) contains a polyolefin resin and organic particles, and the resin layer (C) contains a polyolefin resin and does not contain organic particles having a particle size of 10 μm or more, and at least one of the resin layers (A) to (C) has voids.

[0024] Effects of the Invention

[0025] The reflective material provided by the present invention has good reflective properties, and when used in components such as backlight units, it can suppress the occurrence of uneven brightness and contamination of components. The reflective material provided by the present invention can correspond to the thinning of liquid crystal displays. Therefore, the reflective material provided by the present invention can be suitably used as a reflective material for liquid crystal displays, lighting fixtures, or lighting signs. DETAILED DESCRIPTION

[0026] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the embodiments described below, and can be implemented with arbitrary modifications within the scope of the present invention.

[0027] 《Reflective material》

[0028] A reflective material according to an example of an embodiment of the present invention (also referred to as "the present reflective material") comprises a resin layer (B), a resin layer (A) and a resin layer (C) stacked in this order, wherein the resin layer (B) contains a polyolefin resin and a fine powder filler, the resin layer (A) contains a polyolefin resin and organic particles, the resin layer (C) contains a polyolefin resin and does not contain organic particles having a particle size of 10 μm or more, and any one or more of the resin layers (A) to (C) has voids.

[0029] Here, the technical concept for designing the present reflector will be described, but the present invention is not limited to the scope of the following technical concept.

[0030] As mentioned above, as a countermeasure to prevent uneven brightness, a countermeasure has been adopted in the past to make the reflective material a stacked structure and to make its surface contain particles (especially organic particles with large particle size). This is to form protrusions on the surface by making the surface of the reflective material contain particles. By making the surface of the reflective material have protrusions, it is possible to prevent the light guide plate and the reflective material from having strong local contact, thereby suppressing uneven brightness. Based on this, in the case of making the reflective material contain particles in order to form protrusions on the surface, a solution has been adopted to make the outermost layer of the stacked structure contain particles.

[0031] On the other hand, the inventors of the present invention have confirmed through research that although such reflective materials can be observed to overcome the problem of uneven brightness, there are cases where these reflective materials damage the light guide plate and contaminate components such as the backlight unit, depending on the material selection of the reflective material, the layer structure of the reflective material, the manufacturing conditions, etc. It is inferred that when the light guide plate is damaged or the components are contaminated, the liquid crystal display equipped with such components will have defects in the liquid crystal screen.

[0032] It has also been found that such a phenomenon is more likely to occur in a reflective material using a polyolefin resin.

[0033] The results of this study have confirmed that one of the main causes is the detachment of particles contained in the reflective material from the surface layer. Furthermore, the detachment of particles may occur not only during the manufacture of the reflective material, but also during the storage of the reflective material after manufacture, the backlight unit assembly process, and the vibration caused by product handling after assembly.

[0034] If the detached particles are attached to the surface of the reflective material and then assembled in the backlight unit, or if the particles detach from the reflective material in the backlight unit, the particles will aggregate and further increase in size, and will be sandwiched between the reflective material and the light guide plate. If deformation stress is applied to the backlight unit in this state, it is estimated that stress concentration will occur at the condensed particle portion, causing the light guide plate and the reflective material itself to be scraped and damaged, resulting in a defect in the LCD screen.

[0035] From this point of view, it can be understood that problems are more likely to occur in soft (low elastic modulus) polyolefin resin-based reflective materials than in relatively rigid (high elastic modulus) polyester resin-based reflective materials.

[0036] Based on this, the inventors of the present invention have discovered that even if a reflective material using a polyolefin resin is used, by not making the layer containing organic particles used to form the protrusions the outermost layer, but by providing a layer equivalent to the outer layer on the surface side of the layer containing organic particles, it is possible to suppress the detachment of particles present on the surface of the reflective material while exerting the effect of suppressing uneven brightness, and based on this discovery, the present reflective material was designed.

[0037] Furthermore, since the functions of the resin layer (A), the resin layer (B), and the resin layer (C) can be separated by the present reflective material, the following effects (i) to (iii) can be obtained, for example. However, the present reflective material is not limited to these effects.

[0038] (i) the resin layer (B) can be made light reflective and the resin layer (A) and the resin layer (C) can be made heat resistant; or,

[0039] (ii) the resin layer (B) can be made light reflective, while the resin layer (A) and the resin layer (C) can be made rigid as a reflective material; or,

[0040] (iii) It is possible to reflect light on the surface of the resin layer (C) and, on the other hand, to reflect light that has passed through the resin layer (C) within the resin layer (A) or the resin layer (B).

[0041] Since the functions of the resin layer (A), the resin layer (B), and the resin layer (C) can be separated in this manner, higher reflective performance can be obtained while achieving more excellent heat resistance and folding resistance.

[0042] <Resin layer (A)>

[0043] The resin layer (A) is a layer containing a polyolefin resin and organic particles.

[0044] In the resin layer (A), the polyolefin resin is preferably the main component resin. The resin layer (A) can have affinity with the resin layer (B) or the resin layer (C) by using the polyolefin resin as the main component resin, thereby improving the interlayer adhesion. In addition, the resin layer (A) can form appropriate protrusions on the surface of the present reflective material, usually on the side surface of the resin layer (C), by containing organic particles, thereby suppressing uneven brightness.

[0045] It should be noted that in the present invention, "main component resin" refers to the resin with the largest mass ratio among the resins constituting each layer, and other resins may be contained within a range that does not hinder the function of the main component resin. In this case, the content ratio of the main component resin accounts for 50 mass% or more of the resins constituting each layer, preferably 70 mass% or more, and particularly preferably 90 mass% or more (including 100 mass%).

[0046] (Polyolefin resin)

[0047] The type of the polyolefin resin used as the main component resin of the resin layer (A) is not limited. Examples thereof include at least one polyolefin resin selected from the group consisting of polypropylene resins such as polypropylene, propylene-ethylene copolymers, and propylene-α-olefin copolymers; polyethylene resins such as high-density polyethylene, low-density polyethylene, and ethylene-α-olefin copolymers; α-olefin resins such as polymethylpentene, and cyclic olefin resins such as ethylene-cyclic olefin copolymers; olefin elastomers such as ethylene-propylene rubber (EPR) and ethylene-propylene-diene terpolymer (EPDM), etc.

[0048] Among these polyolefin resins, polypropylene resin, cycloolefin resin, or a combination of the two is preferred from the perspective of mechanical properties, flexibility, etc. Among them, cycloolefin resin is particularly preferred as the main component resin. Cycloolefin resin has little absorption of visible light and is heat-resistant, so it is suitable as the main component resin of the resin layer (A).

[0049] The content of the polyolefin resin in the resin layer (A) is not limited, and is usually 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. When the content of the polyolefin resin is above the above lower limit, it is preferred because it can impart good flexibility to the present reflective material.

[0050] In addition, the upper limit of the content of the polyolefin resin in the resin layer (A) is also not limited, and it can be all polyolefin resin except the organic particles. It is preferably 99% by mass or less, more preferably 98% by mass or less, and further preferably 97% by mass or less. When the content of the polyolefin resin is below the above upper limit, the fracture resistance, bending resistance, brightness unevenness prevention function of the present reflective material become good, so it is preferred.

[0051] Here, the content of the polyolefin resin refers to the total amount of all polyolefin resins in the resin layer (A).

[0052] (Cycloolefin resin)

[0053] Next, as the main component resin of the resin layer (A), a cycloolefin resin which is particularly preferred among the above-mentioned polyolefin resins will be described.

[0054] Cycloolefin resin refers to a polymer compound whose main chain is composed of carbon-carbon bonds and at least a part of the main chain has a cyclic hydrocarbon structure. The cyclic hydrocarbon structure can be introduced by using a compound (cycloolefin) having at least one olefinic double bond in the cyclic hydrocarbon structure represented by norbornene and tetracyclododecene as a monomer.

[0055] Cycloolefin resins can be divided into addition polymers of cycloolefins or hydrogenated products thereof, addition polymers of cycloolefins and α-olefins or hydrogenated products thereof, and ring-opening polymers of cycloolefins or hydrogenated products thereof, all of which can be used as cycloolefin resins. In addition, the cycloolefin resin can be any form of cycloolefin homopolymers and cycloolefin copolymers.

[0056] Specific examples of the cycloolefin resin include:

[0057] Monocyclic cycloolefins such as cyclopentene, cyclohexene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene;

[0058] Bicyclo[2.2.1]hept-2-ene (common name: norbornene), 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, 5 -bicyclic cycloolefins such as hexyl-bicyclo[2.2.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, and 5-propenyl-bicyclo[2.2.1]hept-2-ene;

[0059] Tricyclic cycloolefins such as tricyclo[4.3.0.12,5]deca-3,7-diene (common name: dicyclopentadiene);

[0060] Tetracyclic cycloalkenes such as tetracyclo[4.4.0.12,5.17,10]dodec-3-ene (also referred to as tetracyclododecene);

[0061] 8-cyclopentyl-tetracyclo[4.4.0.12,5.17,10]dodec-3-ene, tetracyclo[8.4.14,7.01,10.03,8]pentadeca-5,10,12,14-tetraene (also called 1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene); polycyclic cycloolefins such as tetramers of cyclopentadiene, etc.

[0062] These cycloolefin resins can be used alone or in combination of two or more to form a copolymer.

[0063] Specific examples of α-olefins copolymerizable with cycloolefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, and the like, and ethylene or α-olefins having 2 to 20 carbon atoms, preferably 2 to 8 carbon atoms. These α-olefins may be used alone or in combination of two or more.

[0064] The cycloolefin resin refers to a resin containing a cycloolefin component as a main component, and is a resin containing preferably 50% by mass or more, more preferably 60% by mass or more.

[0065] In this case, the above-mentioned "main component" means the component with the largest mass ratio among the components constituting the cycloolefin resin, and other components are allowed to be contained within the range that does not hinder the function of the main component. In this case, the content ratio of the main component accounts for 50 mass% or more of the components constituting the cycloolefin resin, preferably 70 mass% or more (including 100 mass%). It should be noted that the same applies to the main components of other resins.

[0066] When the cycloolefin resin is a copolymer of a cycloolefin such as norbornene and an α-olefin, the content of the cycloolefin component in the cycloolefin resin is preferably 60 to 90% by mass, and more preferably 65% ​​by mass or more and 80% by mass or less, from the viewpoint of being able to obtain a well-balanced effect of improving processing properties such as stretching by using the α-olefin as a copolymer component and an effect of heat resistance by using the cycloolefin as a main component of the copolymer component.

[0067] The polymerization method of cycloolefin or cycloolefin and α-olefin and the hydrogenation method of the obtained polymer are not particularly limited and can be carried out according to known methods.

[0068] The melt flow rate (MFR) of the cycloolefin resin is not limited, but is preferably 0.1 to 20 g / 10 min, more preferably 0.5 g / 10 min or more and 10 g / 10 min or less, as measured at 230° C. and under a load of 21.18 N in accordance with JIS K7210.

[0069] The cycloolefin resin may be crystalline or amorphous, and among them, amorphous is preferred.

[0070] The glass transition temperature (Tg) of the cycloolefin resin is not limited, but is preferably 70°C or higher, more preferably 80°C or higher, and further preferably 85°C or higher, and is preferably 170°C or lower, more preferably 160°C or lower, and further preferably 150°C or lower from the viewpoint of heat resistance.

[0071] When the glass transition temperature of the cycloolefin resin is within the above range, stretching processability tends to be good.

[0072] Here, the "glass transition point (Tg)" is a value read by using a differential scanning calorimeter after heating from -50°C to 250°C at a rate of 10°C / min, holding isothermally for 1 minute, cooling to -50°C at a rate of 10°C / min, holding isothermally for 1 minute, and then heating to 250°C at a rate of 10°C / min again.

[0073] In addition, you may combine and mix two or more cycloolefin resins, and you may adjust the glass transition point (Tg) of a mixed resin to the said range.

[0074] The cycloolefin resin may be used alone or in combination of two or more cycloolefin resins having different compositions, physical properties, etc. For example, two or more cycloolefin resins may be combined and mixed to adjust the MFR and Tg of the mixed resin to the above ranges.

[0075] The content of the cycloolefin resin in the resin layer (A) is not limited. It is preferably 30% by mass or more, more preferably 35% by mass or more, and further preferably 40% by mass or more. When the content of the cycloolefin resin is above the above lower limit, it can impart good heat resistance to the present reflective material, and therefore is preferred.

[0076] The upper limit of the content of the cycloolefin resin in the resin layer (A) is also not limited, but is preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less.

[0077] When the content of the cycloolefin resin is not more than the above upper limit, the fracture resistance, bending resistance, brightness unevenness prevention function, and the like of the present reflective material become good, which is preferred.

[0078] As cycloolefin resins, commercially available products can be used. Examples include: "ZEONOR (registered trademark)" manufactured by Japan Zeon Co., Ltd. (a hydrogenated product of a ring-opening polymer of a cyclic olefin), "APEL (registered trademark)" manufactured by Mitsui Chemicals, Inc. (an addition copolymer of ethylene and tetracyclododecene), and "TOPAS (registered trademark)" manufactured by Polyplastics (an addition copolymer of ethylene and norbornene). Among them, "ZEONOR" and "TOPAS" are preferred because they have little light absorption and can therefore provide a reflective material with high reflective performance.

[0079] (Other polyolefin resins)

[0080] When a cycloolefin resin is used as the main component resin of the resin layer (A), that is, a polyolefin resin, the folding resistance and heat resistance can sometimes be further improved by forming the resin layer (A) by blending a polyolefin resin other than the cycloolefin resin (hereinafter referred to as "other polyolefin resin").

[0081] In addition, instead of using the cycloolefin resin as the main component resin of the resin layer (A), only "other polyolefin resin" may be used as the main component resin.

[0082] The melt flow rate (MFR) of the "other polyolefin resin" is not limited, but is preferably 0.1 to 20 g / 10 min, more preferably 0.5 g / 10 min or more or 10 g / 10 min or less, as measured at 230°C and a load of 21.18 N in accordance with JIS K7210.

[0083] When the cycloolefin resin is used in combination with "other polyolefin resins", it is preferred that the MFR of the cycloolefin resin is also adjusted to the above range. When the MFR of both is adjusted in this way, the mechanical properties as a reflective material tend to be improved.

[0084] As the "other polyolefin resin", one or more of the polyolefin resins exemplified as the main component resin of the resin layer (A) mentioned above can be used in combination. Among them, polyethylene resins and polypropylene resins are preferred, and polypropylene resins are preferred from the viewpoint of high melting point, excellent heat resistance, and high mechanical properties such as elastic modulus. However, it is not limited to these resins.

[0085] When the "other polyolefin resin" is a polypropylene resin, from the viewpoint of extrusion moldability, the melt flow rate (MFR) is preferably 0.1 to 20 g / 10 minutes, more preferably 0.2 g / 10 minutes or more or 10 g / 10 minutes or less, and even more preferably 0.5 g / 10 minutes or more or 5 g / 10 minutes or less, as measured at 230°C and a load of 21.18 N in accordance with JIS K7210.

[0086] When a cycloolefin resin is used in combination with "other polyolefin resins" as the resin component constituting the resin layer (A), the relationship between the MFR of the cycloolefin resin ("MFR(CO)") and the MFR of the "other polyolefin resin" ("MFR(PO)") is preferably MFR(CO):MFR(PO)=1:0.05 to 1:20, and more preferably 1:0.1 to 1:10.

[0087] When the relationship between the MFRs of the two is within the above range, the “other polyolefin resin” is preferably oriented in the cycloolefin resin, and the mechanical properties as a reflective material tend to be improved.

[0088] The content of "other polyolefin resin" in the resin layer (A) is not limited. When used in combination with a cycloolefin resin, it is preferably 2% by mass or more (relative to 100% by mass of the resin layer (A)), more preferably 5% by mass or more, and further preferably 10% by mass or more. In addition, there is no upper limit. It is preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 25% by mass or less.

[0089] When the content of the "other polyolefin resin" is at least the above lower limit, the resin layer (A) can be more effectively prevented from breaking during stretching, and the interlayer adhesion between the resin layer (A) and the resin layer (B), or between the resin layer (A) and the resin layer (C) can be maintained at a higher level, which is preferred. On the other hand, when the content of the "other polyolefin resin" is at most the above upper limit, there is a tendency that the heat resistance and the brightness unevenness prevention function can be improved.

[0090] Furthermore, if the polyolefin resin as the main component resin of the resin layer (A) is the same as the polyolefin resin as the main component resin of the resin layer (C), the adhesion between the resin layer (A) and the resin layer (C) will be improved, which is preferred. However, they are not limited to being the same.

[0091] In addition, if the polyolefin resin as the main component resin of the resin layer (A) is the same as the polyolefin resin preferably contained as the main component resin of the resin layer (B), the adhesion between the resin layer (A) and the resin layer (B) will be improved, which is preferred. However, they are not limited to being the same.

[0092] (Organic particles)

[0093] The resin layer (A) of the present reflective material contains organic particles.

[0094] Here, as for "organic particles", any particulate material with organic matter as the main component belongs to "organic particles". In this case, "main component" refers to the component with the largest mass ratio among the components constituting the organic particles, and other components are allowed to be contained within the range that does not hinder the function of the main component. In this case, the content ratio of the main component accounts for 50 mass% or more, preferably 70 mass% or more (including 100 mass%) among the components constituting the organic particles.

[0095] As the organic particles, resin particles are preferred, and examples thereof include so-called polymer beads and polymer hollow particles.

[0096] The type of organic particles as the resin particles is not limited, and examples thereof include (meth)acrylate resin particles, styrene resin particles, silicone resin particles, nylon resin particles, polyethylene resin particles, benzoguanamine resin particles, and urethane resin particles.

[0097] These organic particles may be homopolymers or copolymers, and any one of these organic particles may be used alone or in combination of two or more.

[0098] Among these organic particles, (meth)acrylate resin particles are preferred, methyl methacrylate resin particles or butyl methacrylate resin particles are preferred, and methyl methacrylate resin particles are particularly preferred. In these cases, copolymers containing methyl methacrylate or butyl methacrylate as a main component may also be used.

[0099] Here, the "(meth)acrylate" refers to acrylate or methacrylate.

[0100] The shape of the organic particles contained in the resin layer (A) is not limited, and may be, for example, spherical, rod-shaped, flat, or crushed, agglomerated, or irregularly shaped particles having no specific shape. Among these, spherical organic particles are preferred.

[0101] Here, the term "spherical" does not necessarily mean a perfect sphere, but is considered "spherical" as long as it is visually approximately spherical. Specifically, for example, a particle having a cross-sectional shape that is circular, approximately circular, elliptical, approximately elliptical, or a shape surrounded by an arc with curvature is considered "spherical".

[0102] By making the resin layer (A) contain organic particles, it is possible to form appropriate protrusions on the surface of the adjacent resin layer (C), and further, even when "other layers" are stacked on the surface of the resin layer (C), it is possible to form appropriate protrusions on its surface, that is, on the side surface of the resin layer (C) of the present reflector. At this time, when the organic particles contained in the resin layer (A) are spherical, the height, size, shape, etc. of the above-mentioned protrusions can be made more uniform compared to the case where the organic particles are irregularly shaped particles. By making the height, size, shape, etc. of the protrusions formed on the surface of the resin layer (C) and further on the side surface of the resin layer (C) of the present reflector consistent in this way, it is possible to further suppress uneven brightness, particle detachment, etc.

[0103] The organic particles are preferably crosslinked particles (referred to as "crosslinked particles"). The crosslinked organic particles can easily maintain their shape even when deformation stress is applied in a heated state during extrusion film formation.

[0104] Whether the organic particles are cross-linked particles can be confirmed, for example, by swelling when immersed in a solvent (good solvent) that would dissolve when not cross-linked, but not dissolving. At this time, appropriate heating may also be performed. In addition, nuclear magnetic resonance spectroscopy (NMR), infrared absorption spectroscopy (IR), etc. may be used to confirm.

[0105] The solvent (good solvent) that dissolves the organic particles when not crosslinked varies depending on the type of resin constituting the organic particles, and in the case of (meth)acrylate resin particles, examples thereof include acetone, toluene, ethyl acetate, and methyl ethyl ketone.

[0106] In order to make the organic particles into cross-linked particles, for example, a compound having a polyfunctional polymerizable group such as divinylbenzene, polyacrylate, pentaerythritol, trimellitic acid, etc. may be used as a polymerization raw material.

[0107] The glass transition point (also referred to as "Tg") of the organic particles contained in the resin layer (A) is preferably 120°C or higher. By including organic particles having a Tg of 120°C or higher in the resin layer (A), appropriate hardness can be imparted to the surface of the present reflective material, and uneven brightness can be suppressed. For the same reasons as above, the lower limit of the Tg of the organic particles is preferably 125°C or higher, more preferably 130°C or higher.

[0108] In addition, the upper limit of Tg of the organic particles is not limited, but is preferably 260°C or less. By setting the Tg to 260°C or less, there is a tendency that the hardness of the surface of the present reflective material can be suppressed from becoming too high. For the same reasons as above, the upper limit of Tg of the organic particles is preferably 240°C or less, and more preferably 200°C or less.

[0109] Here, the glass transition point (Tg) is set to the value of the glass transition point read when the temperature is increased at a heating rate of 30°C / min using a differential scanning calorimeter, and the particles themselves are measured. It should be noted that, in the case of having multiple glass transition points (Tg), as long as at least one glass transition point (Tg) is within the above range.

[0110] As a method for making the Tg of organic particles within the above range, the organic particles can be used as resin particles, and the Tg can be adjusted according to the type of resin skeleton (for example, a (meth)acrylate skeleton or a styrene skeleton, etc.), the type of monomer (including the type and composition ratio of the monomer in the case of copolymerization), the molecular weight (the degree of cross-linking in the case of cross-linked particles), etc.

[0111] It should be noted that the Tg of organic particles usually changes due to crosslinking. This is because the molecular motion of the polymer chain is restricted by the crosslinking points.

[0112] In the present invention, the organic particles are crosslinked particles, and it is particularly preferred that the Tg thereof is within the above range in terms of suppressing uneven brightness.

[0113] The heat capacity (ΔCp) of the organic particles contained in the resin layer (A) at the glass transition point is preferably 0.75 J / (g·°C) or less. When the resin layer (A) contains organic particles having a ΔCp of 0.75 J / (g·°C) or less, the brightness unevenness of the reflective material can be further suppressed.

[0114] For the same reasons as above, the upper limit of ΔCp of organic particles is preferably 0.50 J / (g·°C) or less, more preferably 0.45 J / (g·°C) or less, further preferably 0.40 J / (g·°C) or less, and further preferably 0.35 J / (g·°C) or less.

[0115] The lower limit of ΔCp of organic particles is not limited, but is preferably 0.10 J / (g·°C) or more, more preferably 0.15 J / (g·°C) or more, more preferably 0.20 J / (g·°C) or more, further preferably 0.25 J / (g·°C) or more, and further preferably 0.30 J / (g·°C) or more.

[0116] Here, the heat capacity (ΔCp) at the glass transition point is set to the value of ΔCp at the glass transition point read when the temperature is increased at a heating rate of 30°C / min using a differential scanning calorimeter, and the particles themselves are measured. It should be noted that in the case of having multiple Tgs, the heat capacity (ΔCp) value at the lowest temperature Tg in the range of 115 to 260°C is set.

[0117] As a method for making the ΔCp of organic particles within the above range, the organic particles can be resin particles, and the type of resin skeleton (for example, a (meth)acrylate skeleton or a styrene skeleton, etc.), the type of monomer (including the type and composition ratio of monomers in the case of copolymerization), the molecular weight (the degree of crosslinking in the case of crosslinked particles), etc. can be adjusted. Among them, the degree of crosslinking has a significant influence.

[0118] The glass transition point is the temperature at which the polymer material starts microscopic Brownian motion, and the heat capacity (ΔCp) is equivalent to the amount of motion at this time. That is, even for resins with similar compositions, the ΔCp value becomes smaller because the molecular chains are constrained when the degree of crosslinking is high. Therefore, a low ΔCp value means that the molecules are constrained and the degree of crosslinking is high.

[0119] The average particle size of the organic particles is preferably 5 to 50 μm. When the average particle size of the organic particles is 5 μm or more, there is a tendency that protrusions of a height effective for suppressing uneven brightness can be effectively formed on the surface. On the other hand, when the average particle size of the organic particles is 50 μm or less, there is a tendency that the detachment of the particles can be suppressed.

[0120] From the above viewpoints, when the present reflective material is used as a component of a liquid crystal display, lighting fixture or illuminated signboard, the average particle size of the organic particles is preferably 15 to 50 μm, more preferably 18 μm or more or 45 μm or less, further preferably 21 μm or more or 39 μm or less, and still further preferably 23 μm or more or 37 μm or less.

[0121] In addition, when the present reflective material is used as a component of a liquid crystal display of a portable information processing terminal such as a smartphone or a tablet terminal, the average particle size of the organic particles is preferably 5 to 20 μm, more preferably 8 μm or more or 19 μm or less, further preferably 10 μm or more or 18 μm or less, and still further preferably 12 μm or more or 15 μm or less.

[0122] The average particle size of the organic particles can be measured as follows.

[0123] The average particle size of the organic particles as a raw material can be measured as an average particle size (D50) obtained from a volume-based particle size distribution measured by a dynamic light scattering method or the like.

[0124] The average particle size of the organic particles contained in the resin layer (A) can be obtained as follows: the surface of the resin layer (A) or the cross section of the present reflective material is observed using an optical microscope or a scanning electron microscope (SEM), the diameters of 3 or more particles, preferably 10 or more particles, are measured, and the average value thereof is obtained. In this case, when the cross-sectional shape is not circular (for example, when it is elliptical, etc.), the average value of the longest diameter and the shortest diameter can be measured as the diameter of each particle.

[0125] It should be noted that, when no significant deformation is observed in the shape of the organic particles contained in the resin layer (A) relative to the shape of the raw organic particles, the average particle size of the raw organic particles can be regarded as the average particle size of the organic particles contained in the resin layer (A).

[0126] The content of organic particles in the resin layer (A) (relative to 100% by mass of the resin layer (A)) is preferably 0.5 to 10% by mass. When the content of organic particles is 0.5% by mass or more, it is easier to achieve specific hardness and roughness on the surface of the present reflective material, so it is preferred. When the content of organic particles is 10% by mass or less, it does not impair the continuous productivity during extrusion film formation, and more efficient production can be achieved, so it is preferred.

[0127] From the above viewpoints, when the present reflective material is used as a constituent member of a liquid crystal display, lighting fixture, illuminated sign, or the like, the content of the organic particles is preferably 0.5 to 5% by mass, more preferably 2% by mass or more and 4% by mass or less.

[0128] When the present reflective material is used as a component of a liquid crystal display of a portable information processing terminal such as a smartphone or a tablet terminal, the content of the organic particles is preferably 3 to 10% by mass, more preferably 3.5% by mass or more and 9% by mass or less.

[0129] (Micro powder filler)

[0130] The resin layer (A) may contain a fine powder filler other than the above-mentioned organic particles (hereinafter referred to as "fine powder filler") in addition to the above-mentioned organic particles.

[0131] By including a micropowder filler in the resin layer (A), the reflective properties of the present reflective material tend to be further improved from the perspective of light scattering caused by the refractive index difference between the polyolefin resin and the micropowder filler, light scattering caused by the refractive index difference between the voids formed around the micropowder filler and the polyolefin resin during the manufacturing process of the present reflective material, and light scattering caused by the refractive index difference between the voids formed around the micropowder filler and the micropowder filler. It should be noted that the resin layer (A) may also include a micropowder filler in the case where sufficient light reflectivity can be ensured by using the resin layer (B).

[0132] Regarding the type, particle size and surface treatment method of the fine powder filler that can be used for the resin layer (A), those described later as the fine powder filler that can be used for the resin layer (B) can also be used, and the preferred examples are the same. Here, the "resin layer (B)" in the matters described later as the fine powder filler for the resin layer (B) is replaced with "resin layer (A)".

[0133] The average particle size of the micropowder filler contained in the resin layer (A) is preferably 0.05 μm or more and 15 μm or less. When the average particle size of the micropowder filler is 0.05 μm or more, the dispersibility in the polyolefin resin will not be reduced, so a more homogeneous reflective material can be obtained. In addition, when the average particle size is 15 μm or less, the interface between the polyolefin resin and the micropowder filler can be densely formed, thereby obtaining a highly reflective reflective material.

[0134] From the above viewpoints, when the present reflective material is used as a constituent member of a liquid crystal display, a lighting fixture, a lighting sign, or the like, the average particle size of the fine powder filler is more preferably 0.1 μm or more and 10 μm or less.

[0135] When the present reflective material is used as a component of a liquid crystal display of a portable information processing terminal such as a smartphone or a tablet terminal, the average particle size of the fine powder filler is preferably 0.05 μm to 5 μm, more preferably 0.1 μm to 2 μm.

[0136] In addition, the average particle size of the fine powder filler can be measured as follows.

[0137] The average particle size of the fine powder filler used as a raw material can be measured as the average particle size (D50) obtained from the volume-based particle size distribution measured by a dynamic light scattering method, or the cumulative (mass-based) 50% particle size in the equivalent spherical distribution measured using a centrifugal sedimentation particle size distribution analyzer can be measured as the average particle size (D50).

[0138] The average particle size of the fine powder filler contained in the resin layer (A) can be obtained as follows: the surface of the resin layer (A) or the cross section of the present reflective material is observed using an optical microscope or a scanning electron microscope (SEM), the diameters of 10 or more particles are measured, and the average value thereof is obtained. At this time, when the cross-sectional shape is not circular, the average value of the longest diameter and the shortest diameter can be measured as the diameter of each particle. The same is true for the fine powder filler contained in the resin layer (B) described later, but in this case, the method of observing the cross section of the present reflective material is appropriate.

[0139] It should be noted that, with respect to the shape of the fine powder filler contained in the resin layer (A), when no obvious deformation relative to the shape of the raw material fine powder filler is observed, the average particle size of the raw material fine powder filler can be regarded as the average particle size of the fine powder filler contained in the resin layer (A).

[0140] When the resin layer (A) contains a micropowder filler, the content of the micropowder filler in the resin layer (A) is not limited. Considering the light reflectivity, mechanical strength, productivity, etc. of the present reflective material, it is preferably 10 to 80% by mass relative to the entire resin layer (A) (i.e., relative to 100% by mass of the resin layer (A)), and more preferably 20% by mass or more or 70% by mass or less. When the content of the micropowder filler is 10% by mass or more, the area of ​​the interface between the resin and the micropowder filler of the resin layer (A) can be fully ensured, and higher reflectivity can be given to the present reflective material. When the content of the micropowder filler is 80% by mass or less, the mechanical strength necessary for the reflective material can be more effectively ensured, so it is preferred.

[0141] (Other ingredients)

[0142] The resin layer (A) may further contain components other than the polyolefin resin, the organic particles and the fine powder filler as "other components".

[0143] Examples of “other components” include resin components other than those mentioned above (including thermoplastic elastomers), antioxidants, light stabilizers, heat stabilizers, dispersants, ultraviolet absorbers, fluorescent whitening agents, compatibilizers, lubricants, and fillers other than fine powder fillers.

[0144] Furthermore, the resin layer (A) may contain recycled raw materials generated in the production process of the present reflector, etc., within a range not impairing the performance of the present reflector.

[0145] The content of the recycled raw material is not limited, but is preferably 1 to 60% by mass relative to the total mass of the resin layer (A) (relative to 100% by mass of the resin layer (A)), and more preferably 10% by mass or more or 50% by mass or less. When the content is 1% by mass or more, there is a cost advantage brought about by the use of recycled raw materials, and when it is 60% by mass or less, there is a tendency that the light reflectivity and mechanical strength necessary for the reflective material will not be impaired.

[0146] However, it should be noted that if the resin layer (A) contains recycled raw materials, the surface roughness of the present reflective material may become unstable and the reflectivity may become unstable. Therefore, in such a case, it is preferably contained in the resin layer (B) as described below.

[0147] <Resin layer (B)>

[0148] The resin layer (B) in the present reflective material is a layer containing a polyolefin resin.

[0149] When the resin layer (B) contains a polyolefin resin, it may contain other resins. Among them, it is preferable to contain a polyolefin resin as a main component resin from the viewpoint of improving the adhesion with the resin layer (A).

[0150] (Polyolefin resin)

[0151] The polyolefin resin used for the resin layer (B) is not limited and can be selected from the resins exemplified as the polyolefin resins of the resin layer (A). For example, at least one polyolefin resin selected from the following group can be cited: polypropylene resins such as polypropylene and propylene-ethylene copolymers, polyethylene resins such as high-density polyethylene, low-density polyethylene, ethylene-α-olefin copolymers, cyclic olefin resins such as ethylene-cyclic olefin copolymers, ethylene-propylene rubber (EPR), ethylene-propylene-diene terpolymer (EPDM) and other olefin elastomers. Among them, polypropylene resins and polyethylene resins are preferred from the perspective of mechanical properties, flexibility, etc., and polypropylene (homopolymer of propylene) is most preferred.

[0152] It should be noted that the polyolefin resin of the resin layer (B) may be a polyolefin resin different from the polyolefin resin as the main component resin of the resin layer (A). Among them, from the viewpoint of improving the adhesion between the resin layers (A) and (B), it is preferred to use a polyolefin resin containing a common monomer unit with the polyolefin resin as the main component resin of the resin layer (A).

[0153] From the viewpoint of extrusion moldability, the melt flow rate (MFR) of the polyolefin resin used for the resin layer (B) is preferably 0.1 to 20 g / 10 minutes, more preferably 0.2 g / 10 minutes or more or 10 g / 10 minutes or less, and even more preferably 0.5 g / 10 minutes or more or 5 g / 10 minutes or less, as measured at 230°C and a load of 21.18 N in accordance with JIS K7210.

[0154] The content of the polyolefin resin in the resin layer (B) is not limited, but is preferably 15% by mass or more (relative to 100% by mass of the resin layer (B)), more preferably 20% by mass or more, and further preferably 25% by mass or more. When the content of the polyolefin resin is above the above lower limit, the strength of the resin layer (B) can be further ensured, which is preferred.

[0155] The upper limit of the content of the polyolefin resin in the resin layer (B) is also not limited, and the layer may consist of the polyolefin resin alone, but is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.

[0156] When the content of the polyolefin resin is not more than the above upper limit, strength can be ensured without causing a decrease in reflectance, which is preferred.

[0157] (Micro powder filler)

[0158] From the viewpoint of obtaining better reflective performance, it is preferred that the resin layer (B) contains a fine powder filler in addition to the polyolefin resin.

[0159] When the resin layer (B) contains a fine powder filler, incident light is diffusely reflected by the fine powder filler to improve the reflection property. Furthermore, when the resin layer (B) is a stretched body, voids are easily formed.

[0160] The fine powder filler contained in the resin layer (B) is not limited, and examples thereof include inorganic fine powder, organic fine powder, etc. It should be noted that the organic fine powder can use the same organic particles as those used for the resin layer (A). Among them, it is preferred that the resin layer (B) contains the inorganic fine powder as the fine powder filler. In addition, the inorganic fine powder and the organic fine powder can also be used in combination.

[0161] Examples of the organic fine powder that can be contained in the resin layer (B) include polymer beads and polymer hollow particles. These organic fine powders can be used alone or in combination of two or more.

[0162] In addition, as described later, the end material produced in the manufacturing process of the reflector can also be used as a recycled raw material to form part of the raw material of the resin layer (B). In this case, the organic particles contained in the resin layer (A) are also contained in the resin layer (B).

[0163] Examples of the inorganic fine powder include calcium carbonate, magnesium carbonate, barium carbonate, magnesium sulfate, barium sulfate, calcium sulfate, zinc oxide, magnesium oxide, calcium oxide, titanium oxide, aluminum oxide, zinc oxide, alumina, aluminum hydroxide, hydroxyapatite, silicon dioxide, magnesium silicate, mica, talc, kaolin, clay, glass powder, asbestos powder, zeolite, silicate clay, etc. These inorganic fine powders may be used alone or in combination of two or more.

[0164] Among these inorganic fine powders, materials with a large refractive index are preferred in view of the difference in refractive index with the resin constituting the resin layer (B), and calcium carbonate, barium sulfate, titanium oxide, or zinc oxide having a refractive index of 1.6 or more is particularly preferably used.

[0165] Among them, titanium oxide has a refractive index significantly higher than other inorganic fine powders and can significantly increase the refractive index difference with the resin constituting the resin layer (B), so compared with the case where other fillers are used, excellent light reflectivity can be obtained with a smaller amount. In addition, by using titanium oxide, high light reflectivity can be obtained even if the thickness of the reflective material is reduced.

[0166] The content of titanium oxide is not limited, but is preferably 30% or more of the total mass of the inorganic fine powder. When organic fine powder and inorganic fine powder are used in combination as fine powder fillers, preferably 30% or more of the total mass is titanium oxide.

[0167] As titanium oxide, commercially available products such as those manufactured by Ishihara Sangyo Co., Ltd., Chemours Co., Ltd., and KRONOS Co., Ltd. can be used.

[0168] In order to improve the dispersibility of these inorganic fine powders in the resin, inorganic fine powders whose surfaces have been treated with silicon compounds, polyol compounds, amine compounds, fatty acids, fatty acid esters, etc. may be used.

[0169] The average particle size of the micropowder filler is preferably 0.05 to 15 μm. When the average particle size of the micropowder filler is 0.05 μm or more, the dispersibility in the resin constituting the resin layer (B) is good, so a more homogeneous reflective material can be obtained. In addition, when the average particle size of the micropowder filler is 15 μm or less, the interface between the resin constituting the resin layer (B) and the micropowder filler can be densely formed, thereby obtaining a reflective material with higher reflectivity.

[0170] From the above viewpoints, when the present reflective material is used as a constituent member of a liquid crystal display, a lighting fixture, a lighting sign, or the like, the average particle size of the fine powder filler is more preferably 0.1 μm or more and 10 μm or less.

[0171] When the present reflective material is used as a component of a liquid crystal display of a portable information processing terminal such as a smartphone or a tablet terminal, the average particle size of the fine powder filler is preferably 0.05 μm to 5 μm, more preferably 0.1 μm to 2 μm.

[0172] Here, the "average particle size" can be measured by the above-mentioned method.

[0173] Considering the light reflectivity, mechanical strength, productivity, etc. of the present reflective material, the content of the fine powder filler contained in the resin layer (B) is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more relative to the mass of the entire resin layer (B) (i.e., relative to 100% by mass of the resin layer (B)). When the content of the fine powder filler is above the above lower limit, the area of ​​the interface between the resin constituting the resin layer (B) and the fine powder filler can be sufficiently ensured, and high reflectivity can be imparted by the reflective material.

[0174] In addition, the upper limit of the content of the fine powder filler is also not limited, preferably 80 mass % or less, more preferably 75 mass % or less, and further preferably 70 mass % or less. When the content of the fine powder filler is below the above upper limit, the mechanical strength required for the reflective material can be more effectively ensured.

[0175] (Other ingredients)

[0176] The resin layer (B) may further contain components other than the polyolefin resin and the fine powder filler as "other components".

[0177] Examples of the “other components” include resin components other than polyolefin resins (including thermoplastic elastomers), crystal nucleating agents, antioxidants, light stabilizers, heat stabilizers, dispersants, ultraviolet absorbers, fluorescent brighteners, compatibilizers, lubricants, and other additives.

[0178] Furthermore, the resin layer (B) may contain recycled raw materials generated in the production process of the present reflective material, etc., as long as the performance of the resin layer (B) is not impaired.

[0179] The content ratio of the recycled raw material is not limited, and is preferably 1 to 60% by mass relative to the mass of the entire resin layer (B) (i.e., relative to 100% by mass of the resin layer (B)), and more preferably 10% by mass or more or 50% by mass or less. When the content is 1% by mass or more, cost advantages due to the use of recycled raw materials are generated, so it is preferred. On the other hand, when the content is 60% by mass or less, it is not easy to damage the light reflectivity and mechanical strength necessary for the reflective material, so it is preferred.

[0180] Generally, the thickness of the resin layer (B) accounts for a relatively high proportion of the total thickness of the present reflector. Therefore, when the resin layer (B) contains recycled raw materials, fluctuations in the properties of the present reflector can be reduced, which is preferred.

[0181] <Resin layer (C)>

[0182] The resin layer (C) is a layer containing a polyolefin resin and containing no organic particles having a particle size of 10 μm or more. In the resin layer (C), the polyolefin resin is preferably used as a main component resin.

[0183] By making the resin layer (C) exist in the form of a layer containing a polyolefin resin and not containing organic particles with a particle size of 10 μm or more, it is possible to suppress the organic particles contained in the resin layer (A) from detaching from the present reflective material. Furthermore, it is possible to reduce the direct effect of the hardness of the organic particles contained in the resin layer (A) on the surface hardness of the present reflective material, so it is expected that the present reflective material will damage the light guide plate when it contacts the light guide plate.

[0184] In order to make the resin layer (C) have such a structure, it is preferable to adjust the type and content ratio (including the case where no organic particles are contained) of the raw material for the resin layer (C), that is, the resin composition C described later. However, the method is not limited to this.

[0185] It is more preferred to apply the same provisions based on replacing the understanding of "organic particles with a particle size of 10 μm or more" in the above record with "organic particles with a particle size of 5 μm or more", further preferred to apply the same provisions based on replacing the understanding with "organic particles with a particle size of 2 μm or more", and particularly preferred to apply the same provisions based on replacing the understanding with "organic particles with a particle size of 1 μm or more".

[0186] Furthermore, the resin layer (C) preferably does not contain a fine powder filler having a particle size of 10 μm or more for the same reason as the above-mentioned organic particles. The fine powder filler has the same meaning as the fine powder filler contained in the resin layer (B).

[0187] In order to make the resin layer (C) have such a structure, it is preferable to adjust the type and content ratio (including the case where no powder filler is contained) of the raw material used for the resin layer (C), that is, the resin composition C described later. However, the method is not limited to this.

[0188] It is more preferred to apply the same provisions based on replacing the "fine powder filler with a particle size of 10 μm or more" in the above description with "fine powder filler with a particle size of 5 μm or more", further preferred to apply the same provisions based on replacing the understanding with "fine powder filler with a particle size of 2 μm or more", and particularly preferred to apply the same provisions based on replacing the understanding with "fine powder filler with a particle size of 1 μm or more".

[0189] It should be noted that "does not contain organic particles or fine powder fillers with a particle size of 10 μm or more" means that it does not substantially contain organic particles or fine powder fillers with a particle size of 10 μm or more, and allows the case where the content of organic particles or fine powder fillers with a particle size of 10 μm or more in the resin layer (C) is 1% by mass or less. In this case, the content ratio of organic particles or fine powder fillers with a particle size of 10 μm or more in the resin layer (C) (relative to 100% by mass of the resin layer (C)) is preferably 0.5% by mass or less, more preferably 0.2% by mass or less, further preferably 0.1% by mass or less, and particularly preferably completely free of them.

[0190] When the content of organic particles or fine powder fillers having a particle size of 10 μm or more in the resin layer (C) is 1 mass % or less, the organic particles or fine powder fillers can be prevented from detaching from the present reflective material, thereby achieving the effects of the present invention.

[0191] The fact that the resin layer (C) "does not contain organic particles or fine powder fillers having a particle size of 10 μm or more" can be confirmed by the following method.

[0192] This can be confirmed by not mixing, as a raw material for the resin layer (C), organic particles or fine powder fillers having an average particle size (D50) of 10 μm or more determined from a volume-based particle size distribution measured by a dynamic light scattering method or the like.

[0193] On the other hand, regarding the organic particles or micropowder fillers in the resin layer (C), it is first necessary to confirm whether the resin layer (C) contains organic particles or micropowder fillers. If contained, select any 10 or more organic particles or micropowder fillers, and measure the diameters of these particles using an optical microscope or a scanning electron microscope (SEM). At this time, in the case where the cross-sectional shape is not circular, the average value of the longest diameter and the shortest diameter can be measured as the diameter of each particle. Furthermore, it is determined whether the measured diameter is greater than 10 μm. If the diameters of not all particles are greater than 10 μm, it can be confirmed that the resin layer (C) "does not contain organic particles or micropowder fillers with a particle size of 10 μm or more.

[0194] It should be noted that “does not contain organic particles or fine powder fillers with a particle size of 5 μm or more”, “does not contain organic particles or fine powder fillers with a particle size of 2 μm or more”, and “does not contain organic particles or fine powder fillers with a particle size of 1 μm or more” can also be similarly confirmed by replacing the above-mentioned “10 μm” with “5 μm”, “2 μm”, and “1 μm” respectively.

[0195] As for the resin layer (C), except that the content ratio of organic particles and fine powder fillers is within the above range relative to the composition of the above resin layer (A), the method is the same as that of the above resin layer (A). That is, regarding the types of polyolefin resins, cycloolefin resins, other polyolefin resins, fine powder fillers, and other components that can be used in the resin layer (C), those described above as polyolefin resins, cycloolefin resins, other polyolefin resins, fine powder fillers, and other components that can be used in the resin layer (A) can be used in the same way, except for the content ratio of organic particles and fine powder fillers, the preferred examples and preferred embodiments are also the same. Here, "resin layer (A)" can be replaced with "resin layer (C)" and applied to the matters described above as the method of the resin layer (A).

[0196] It should be noted that, when the polyolefin resin as the main component resin in the resin layer (A) is the same as the polyolefin resin as the main component resin in the resin layer (C), or when the affinity is high, there will be a situation where the boundary between the resin layer (A) and the resin layer (C) does not exist in the present reflective material or cannot be confirmed. Even in such a case, in the case where the region (layer) containing organic particles and the region (layer) without organic particles can be distinguished, they can also be regarded as the resin layer (A) and the resin layer (C) respectively. Further, even if the content ratio of organic particles changes continuously in the thickness direction, the resin layer (A) and the resin layer (C) can also be regarded as the above-mentioned content ratio of organic particles. Even in such a case, the effect based on the resin layer (A) and the resin layer (C) of the present invention can be shown.

[0197] <Gap>

[0198] In the present reflective material, by providing voids in any layer, the reflective property can be improved.

[0199] The gap may be present in only one of the resin layer (A), the resin layer (B), and the resin layer (C), or in any two of these layers, or in all layers. Alternatively, the gap may be present in a layer (other layer) other than these layers. In the case where the provision of gaps in the resin layer (A) or the resin layer (C) causes a decrease in mechanical properties such as heat resistance and elastic modulus, it is preferred that the gaps are provided only in the resin layer (B). By providing such gaps only in the resin layer (B), the heat resistance of the entire film can be improved.

[0200] The voids can be formed by pre-incorporating a fine powder filler into the composition constituting each layer and stretching, preferably biaxially stretching, or by pre-incorporating an incompatible resin into the polyolefin resin constituting each layer and stretching, preferably biaxially stretching.

[0201] <Reflective material>

[0202] (Layer composition)

[0203] The present reflective material may have any other layers as long as the resin layer (B), the resin layer (A) and the resin layer (C) are sequentially laminated. For example, the reflective material may have an "other layer" on the surface of the resin layer (B) or the resin layer (C), or an "other layer" such as an adhesive layer may be interposed between the resin layer (A) and the resin layer (B) or between the resin layer (A) and the resin layer (C).

[0204] The “other layers” also include layers provided by coating or vapor deposition.

[0205] Alternatively, the composition may be a four-layer or more composition having two or more layers of at least one of the resin layer (A), the resin layer (B), and the resin layer (C). In the case of a composition having four or more layers, the composition preferably has the resin layer (B) as the core layer, and more preferably has the resin layer (A) on both sides of the resin layer (B) and the resin layer (C) on both sides of the two resin layers (A), that is, a five-layer composition of "resin layer (C) / resin layer (A) / resin layer (B) / resin layer (A) / resin layer (C)".

[0206] By sequentially stacking the resin layer (B), the resin layer (A) and the resin layer (C), the functions of the layers can be separated, thereby improving the reflective performance, heat resistance, folding resistance, reduction of uneven brightness, particle detachment, etc. For example, the resin layer (B) can mainly have the function of imparting light reflectivity, the resin layer (A) can have not only heat resistance but also the function of reducing uneven brightness, and the resin layer (C) can have not only heat resistance but also the function of reducing particle detachment.

[0207] The present reflector may have any layer as the outermost layer, but since the resin layer (C) can have the effect of reducing particle detachment, the resin layer (C) is preferably arranged as the surface layer of the present reflector, and more preferably as the outermost layer serving as the reflection surface.

[0208] (Morphologies of Resin Layer (A), Resin Layer (B), and Resin Layer (C))

[0209] The resin layer (A), the resin layer (B) and the resin layer (C) are not limited in any specific shape or production method as long as they are in the form of films, that is, thin films. However, these layers are preferably in the form of films formed by extrusion.

[0210] When each layer is in the form of a film, these layers may be an unstretched film or a uniaxially or biaxially stretched film, among which a stretched film stretched at least 1.1 times in a uniaxial direction is preferred, and a biaxially stretched film is particularly preferred.

[0211] In addition, although it is also possible to make them stick together and obtain a stacked structure after pre-manufacturing the films equivalent to each layer, it is preferably manufactured by a coextrusion method that can form a stacked structure at one time. When stretching after obtaining the stacked structure by the coextrusion method, all layers can be stretched, so it is more preferred.

[0212] (thickness)

[0213] The thickness of the present reflective material is not particularly limited, but is preferably 30 μm to 1500 μm. In consideration of practical operability, the thickness of the present reflective material is preferably about 50 to 1000 μm.

[0214] For example, as a reflective material for liquid crystal displays, the thickness is preferably 50 to 700 μm, and as a reflective material for lighting fixtures and illuminated signs, the thickness is preferably 70 to 1000 μm.

[0215] In addition, when the present reflective material is used as a component of a liquid crystal display of a portable information processing terminal such as a smartphone or a tablet terminal, the thickness is preferably 30 to 200 μm, more preferably 50 μm or more or 150 μm or less, and further preferably 60 μm or more or 110 μm or less.

[0216] The thickness of the resin layer (A) is not particularly limited, but is preferably 0.1 to 100 μm. When the thickness of the resin layer (A) is within the above range, brightness unevenness tends to be more effectively suppressed.

[0217] From the above viewpoints, when the present reflector is used as a constituent member of a liquid crystal display, lighting fixture, illuminated sign, or the like, the thickness of the resin layer (A) is preferably 5 to 100 μm, more preferably 10 μm or more and 80 μm or less.

[0218] In addition, when the present reflective material is used as a constituent member of a liquid crystal display or the like of a portable information processing terminal such as a smartphone or a tablet terminal, the thickness of the resin layer (A) is preferably 0.1 to 20 μm, more preferably 0.5 μm or more or 15 μm or less, and further preferably 1 μm or more or 10 μm or less.

[0219] Here, the thickness of the resin layer (A) indicates an average thickness, which is the thickness obtained by averaging the convex portions caused by the organic particles. In addition, when the present reflective material has a plurality of resin layers (A), the thickness of each layer is indicated.

[0220] The thickness of the resin layer (B) (the total thickness when two or more resin layers (B) are present) is not particularly limited, but is preferably 20 to 1400 μm. When the thickness of the resin layer (B) is within the above range, the reflection characteristics tend to be good.

[0221] From the above viewpoints, when the present reflective material is used as a constituent member of a liquid crystal display, a lighting fixture, an illuminated sign, or the like, the thickness of the resin layer (B) is more preferably 50 μm or more and 600 μm or less.

[0222] In addition, when the present reflective material is used as a constituent member of a liquid crystal display or the like of a portable information processing terminal such as a smartphone or a tablet terminal, the thickness of the resin layer (B) is preferably 20 to 120 μm, more preferably 30 μm or more or 100 μm or less, and further preferably 40 μm or more or 80 μm or less.

[0223] Here, the thickness of the resin layer (B) indicates an average thickness.

[0224] It should be noted that, when the polyolefin resin as the main component resin in the resin layer (A) is the same as the polyolefin resin contained as the main component resin in the resin layer (B), or when the affinity is high, the boundary between the resin layer (A) and the resin layer (B) may not exist or cannot be confirmed in the present reflective material. In such a case, the thickness of each layer and the thickness ratio of each layer described below can be calculated based on the ratio of the raw materials used in each layer and the ratio of the extrusion amount when manufacturing the present reflective material.

[0225] The thickness of the resin layer (C) is not particularly limited, but is preferably 1 to 100 μm. When the thickness of the resin layer (C) is within the above range, there is a tendency for the detachment of particles to be suppressed.

[0226] From the above viewpoints, when the present reflector is used as a constituent member of a liquid crystal display, lighting fixture, illuminated sign, or the like, the thickness of the resin layer (C) is preferably 5 to 100 μm, more preferably 10 μm or more and 80 μm or less.

[0227] In addition, when the present reflective material is used as a component of a liquid crystal display or the like of a portable information processing terminal such as a smartphone or a tablet terminal, the thickness of the resin layer (C) is preferably 1 to 10 μm, more preferably 2 μm or more or 9 μm or less, further preferably 3 μm or more, and even more preferably 4 μm or more.

[0228] Here, the thickness of the resin layer (C) indicates an average thickness. When the present reflective material has a plurality of resin layers (C), the thickness of each layer is indicated.

[0229] It should be noted that, when the polyolefin resin as the main component resin in the resin layer (A) is the same as the polyolefin resin as the main component resin in the resin layer (C), or when the affinity is high, the boundary between the resin layer (A) and the resin layer (C) may not exist or cannot be confirmed in the present reflective material. In such a case, the thickness of each layer and the thickness ratio of each layer described below can be calculated based on the ratio of the raw materials used in each layer and the ratio of the extrusion amount when manufacturing the present reflective material.

[0230] In the present reflective material, the ratio of the thickness of the resin layer (C) to the thickness of the resin layer (A) ((C) / (A)) is preferably 0.5 or more and 5.0 or less. When the thickness ratio is 0.5 or more, the resin layer (C) can cover the organic particles contained in the resin layer (A) with a sufficient thickness, so there is a tendency that the holding force of the particles based on the resin layer (A) and the resin layer (C) is improved and the detachment of the particles can be suppressed. In addition, when the thickness ratio is 5.0 or less, the organic particles contained in the resin layer (A) are not easily buried in the present reflective material, so there is a tendency that the brightness unevenness can be more effectively suppressed.

[0231] For the same reasons as above, the lower limit of the ratio of the thickness of the resin layer (C) to the thickness of the resin layer (A) ((C) / (A)) is preferably 0.6 or more, more preferably 0.8 or more, further preferably 1.0 or more, further preferably 1.5 or more, and particularly preferably 2.0 or more. In addition, for the same reasons as above, the upper limit of the thickness ratio is preferably 4.5 or less, more preferably 4.0 or less, further preferably 3.5 or less, and particularly preferably 3.0 or less.

[0232] In the present reflective material, the ratio of the thickness of the resin layer (B) to the thickness of the resin layer (A) ((B) / (A)) is preferably 1 to 40. When the thickness ratio of the resin layer (B) to the resin layer (A) is 1 or more, there is a tendency for the reflective characteristics to be improved, and further, there is a tendency for the flexibility to be improved, thereby improving the bending processability. In addition, when the thickness ratio of the resin layer (B) to the resin layer (A) is 40 times or less, there is a tendency for the heat resistance to be improved.

[0233] From the above viewpoints, the ratio of the thickness of the resin layer (B) to the thickness of the resin layer (A) ((B) / (A)) is more preferably 2 or more or 30 or less, further preferably 5 or more or 20 or less, and particularly preferably 15 or less.

[0234] In addition, in the case of a structure having two or more resin layers (A) or resin layers (B), the above-mentioned thickness ratio indicates the thickness ratio of the total thickness of each layer.

[0235] In the present reflective material, the ratio of the thickness of the resin layer (B) to the total thickness of the resin layer (A) and the resin layer (C) ((B) / ((A)+(C))) is preferably 2 to 20, more preferably 15 or less. When the ratio of the thickness of the resin layer (B) to the total thickness of the resin layer (A) and the resin layer (C) is 2 times or more, there is a tendency for the reflective characteristics to become better, and further, there is a tendency for the flexibility to become better, thereby improving the bending processability. In addition, when the thickness ratio is 20 times or less, there is a tendency for the heat resistance to become better.

[0236] In the case of a structure having two or more resin layers (A), resin layers (C) or resin layers (B), the thickness ratio refers to the ratio of the total thickness of each layer.

[0237] (Surface protrusions)

[0238] When the present reflective material is used as a component of a liquid crystal display, a lighting fixture, or a lighting sign, the top view diameter of the protrusion on the side surface of the resin layer (C) is preferably 21 μm to 39 μm, more preferably 22 μm or more or 38 μm or less, and further preferably 23 μm or more or 37 μm or less. When the top view diameter of the protrusion on the side surface of the resin layer (C) of the present reflective material is within this range, there is a tendency to suppress brightness unevenness while suppressing the detachment of particles, so it is preferred.

[0239] In addition, when the present reflective material is used as a component of a liquid crystal display or the like of a portable information processing terminal such as a smartphone or a tablet terminal, from the same viewpoint, the top view diameter of the protrusion on the side surface of the resin layer (C) is preferably 5 μm to 20 μm, more preferably 8 μm or more or 19 μm or less, and further preferably 10 μm or more or 18 μm or less.

[0240] Here, the "diameter of the protrusion on the side surface of the resin layer (C) when viewed from above" can be obtained as follows: the surface of the present reflective material is observed from above using an optical microscope or a scanning electron microscope (SEM), i.e., viewed from above, and 10 or more arbitrary protrusions that can be clearly identified as protrusions are selected, and the diameter of the protrusion when viewed from above is measured, i.e., the diameter of the protrusion when viewed from above, and the average value thereof is obtained. In the case where the shape of the protrusion observed from above is not circular, the average value of the shortest diameter and the longest diameter is taken as the diameter of the protrusion when viewed from above.

[0241] It should be noted that, in the case where the "resin layer (C) side surface" is located on both sides of the present reflective material, such as "resin layer (C) / resin layer (A) / resin layer (B) / resin layer (A) / resin layer (C)", the top view diameter of the protrusions on at least one of the surfaces may be within the above range. The same applies to the "protrusion density with a top view diameter of 21 to 39 μm", "protrusion density with a top view diameter of 5 to 20 μm", maximum height Rz, and arithmetic mean roughness Ra described later.

[0242] Since the present reflective material has a resin layer (C) laminated on a resin layer (A) containing organic particles, when the resin layer (C) is the surface layer of the present reflective material, protrusions are generated on the surface of the resin layer (C), i.e., on the surface of the resin layer (C) side of the present reflective material, due to the organic particles in the resin layer (A). In addition, when "another layer" is laminated on the surface of the resin layer (C), protrusions are generated on the surface of the "other layer", i.e., on the surface of the resin layer (C) side of the present reflective material.

[0243] However, it should be noted that when measuring the top view diameter of the protrusions on the side surface of the resin layer (C), not only the protrusions caused by the organic particles in the resin layer (A) are taken as the object. Therefore, it is not necessary to confirm that the protrusions are caused by the organic particles contained in the resin layer (A).

[0244] The method for adjusting the top view diameter of the protrusions on the side surface of the resin layer (C) can be optimized according to the type and proportion of organic particles contained in the resin layer (A), the thickness ratio of the resin layer (A) to the resin layer (C), the type and proportion of polyolefin resins as the main component resins of the resin layer (A) and the resin layer (C), the stretching conditions when manufacturing the reflective material, etc. However, the present invention is not limited to these methods.

[0245] When the present reflective material is used as a component of a liquid crystal display, lighting fixture, or illuminated signboard, the density of protrusions having a diameter of 21 to 39 μm in plan view on the surface of the resin layer (C) is preferably 7 to 40 protrusions / mm 2 , wherein 14 pieces / mm is more preferred 2 Above or 35 / mm 2 Below, among which 21 pieces / mm is more preferred 2 Above and 30 pieces / mm 2 When the protrusions having a plan view diameter of 21 to 39 μm are provided at a density within the above range, brightness unevenness tends to be effectively suppressed, which is preferred.

[0246] In addition, when the present reflective material is used as a component of a liquid crystal display or the like of a portable information processing terminal such as a smartphone or a tablet terminal, from the same viewpoint, the density of protrusions having a diameter of 5 to 20 μm in a plan view on the surface of the resin layer (C) is preferably 10 to 210 mm 2 , wherein 30 pieces / mm is more preferred 2 Above or 180 pieces / mm 2 Below, more preferably 40 / mm 2 Above and 160 pieces / mm 2 the following.

[0247] The density of the protrusions can be adjusted by adjusting the type and blending ratio of the organic particles contained in the resin layer (A), the stretching conditions during the production of the reflective material, and the like.

[0248] (Maximum height Rz)

[0249] The maximum height Rz of the side surface of the resin layer (C) of the present reflective material is not particularly limited, but is preferably 3.0 μm or more, more preferably 3.1 μm or more, further preferably 3.2 μm or more, further preferably 3.4 μm or more, more preferably 3.5 μm or more, and further preferably 4.0 μm or more. When the maximum height Rz of the side surface of the resin layer (C) of the present reflective material is greater than the above lower limit, there is a tendency that the reflection characteristics are good and the brightness unevenness can be further suppressed, so it is preferred.

[0250] In addition, the upper limit of the maximum height Rz of the side surface of the resin layer (C) of the present reflective material is also not limited, and is preferably 7.0 μm or less, more preferably 6.8 μm or less, further preferably 6.5 μm or less, further preferably 6.0 μm or less, and more preferably 5.5 μm or less. When the maximum height Rz of the side surface of the resin layer (C) of the present reflective material is below the above upper limit, there is a tendency that the reflection characteristics are good and the detachment of particles can be suppressed, so it is preferred.

[0251] The method for adjusting the maximum height Rz of the side surface of the resin layer (C) can be optimized based on the thickness ratio of the resin layer (A) to the resin layer (C), the type and mixing ratio of the polyolefin resin as the main component resin of the resin layer (A) and the resin layer (C), the type and mixing ratio of the organic particles contained in the resin layer (A), the stretching conditions when manufacturing the reflective material, etc.

[0252] In addition, the maximum height Rz is measured in accordance with JIS B0601, more specifically, based on the method of the examples described later.

[0253] (Arithmetic mean roughness Ra)

[0254] The arithmetic mean roughness Ra of the surface on the side of the resin layer (C) of the present reflective material is not particularly limited, but is preferably 0.3 μm or more, more preferably 0.35 μm or more, further preferably 0.4 μm or more, and particularly preferably 0.5 μm or more, more preferably 0.6 μm or more, and further preferably 0.7 μm or more. When the arithmetic mean roughness Ra of the surface on the side of the resin layer (C) of the present reflective material is above the above lower limit, there is a tendency that the reflection characteristics are good and the brightness unevenness can be further suppressed, so it is preferred.

[0255] In addition, the upper limit of the arithmetic mean roughness Ra of the side surface of the resin layer (C) of the present reflective material is also not limited, and is preferably 1.0 μm or less, more preferably 0.9 μm or less, and further preferably 0.8 μm or less. When the arithmetic mean roughness Ra of the side surface of the resin layer (C) of the present reflective material is below the above upper limit, there is a tendency that the reflection characteristics are good and the detachment of particles can be suppressed, so it is preferred.

[0256] The method for adjusting the arithmetic mean roughness Ra of the side surface of the resin layer (C) can be optimized based on the thickness ratio of the resin layer (A) to the resin layer (C), the type and mixing ratio of the polyolefin resin as the main component resin of the resin layer (A) and the resin layer (C), the type and mixing ratio of the organic particles in the resin layer (A), the stretching conditions when manufacturing the reflective material, etc.

[0257] In addition, the measurement of arithmetic mean roughness Ra complies with JIS B0601, and more specifically, is based on the method of the Example mentioned later.

[0258] (Reflectivity)

[0259] The present reflective material may have high reflective properties.

[0260] The reflective performance of the present reflective material is not limited, and the average reflectivity of at least one surface can be 95% or more, further 96% or more, further 97% or more, further 98% or more, and particularly 99% or more. If the reflective material has such reflective performance, a liquid crystal display or the like equipped with the present reflective material can achieve sufficient brightness of the screen.

[0261] Here, the "reflectance" refers to the average reflectance to light of wavelength 420 to 700 nm, and a more specific measurement method is described in the Examples described later.

[0262] (Porosity)

[0263] The present reflective material preferably has voids to improve reflective performance.

[0264] The presence of voids in the present reflective material can be confirmed by, for example, observing a cross section of the present reflective material using a microscope (electron microscope, optical microscope).

[0265] The porosity of the present reflective material is not limited, but is preferably 10% or more, more preferably 20% or more. On the other hand, the upper limit is preferably 80% or less, more preferably 70% or less.

[0266] When the porosity of the present reflector is above the lower limit, the whitening of the present reflector is sufficiently performed, so there is a tendency to have high light reflectivity. In addition, when the porosity of the present reflector is below the upper limit, there is a tendency to have appropriate mechanical strength of the present reflector.

[0267] The porosity of the resin layer (B) is not limited, but is preferably 20% or more, more preferably 25% or more, and further preferably 30% or more. On the other hand, the upper limit is preferably 80% or less, more preferably 75% or less, and further preferably 70% or less. When the porosity of the resin layer (B) is above the lower limit, the whitening of the present reflective material is fully carried out, so there is a tendency to have higher light reflectivity. In addition, when the porosity of the resin layer (B) is below the upper limit, there is a tendency for the mechanical strength of the present reflective material to become more suitable.

[0268] It should be noted that the porosity of the present reflective material is essentially based on the resin layer (A), the resin layer (B) and the resin layer (C). When there are other layers between these layers, the porosity of the other layers is also included. On the other hand, when there are other layers such as resin plates and metal plates outside the resin layers (A), the resin layers (B) and the resin layers (C), these layers are not included in the calculation of the porosity of the reflective material.

[0269] The porosity of the present reflective material can be determined by the following method.

[0270] (1) When the voids are formed by stretching, the density of the reflective material before and after stretching can be measured and determined using the following formula.

[0271] Void ratio (%) = {(density of film before stretching - density of film after stretching) / density of film before stretching} × 100

[0272] (2) When the density and blending ratio of each raw material are clear, the density without voids can be calculated from the density and blending ratio of each raw material and determined using the following formula.

[0273] Void ratio (%) = {(density without voids - density of reflective material) / density without voids} × 100

[0274] (3) Furthermore, the density of the reflective material may be determined by measuring the density of the reflective material and then calculating the density after the reflective material is melted, decompressed, cooled and solidified to remove voids.

[0275] <Method for producing the present reflective material>

[0276] Hereinafter, as an example of a method for producing the present reflective material, a five-layer structure of "resin layer (C) / resin layer (A) / resin layer (B) / resin layer (A) / resin layer (C)" produced by a co-extrusion method will be described, but the present reflective material is not limited to the following production method. For example, a laminated structure may be obtained by coating, extrusion lamination, hot melt bonding, adhesives, etc. instead of the co-extrusion method.

[0277] It should be noted that, as a method for setting a layer containing a large number of organic particles with large particle sizes, the coating method has been mainly used in the past. However, when the layer containing organic particles is set by the coating method, although the surface roughness increases, problems such as particle detachment and reduced reusability (self-recyclability) sometimes occur, and not only that, problems such as peeling of the coating layer from the substrate, curling (winding problem), and reduced manufacturing efficiency sometimes occur.

[0278] In contrast, in the manufacturing method of the present reflective material, by making the main component resin constituting the layer containing organic particles (resin layer (A)) the same type as the resin constituting the resin layer (B) and the resin layer (C), that is, a polyolefin resin, a structure suitable for the co-extrusion method can be obtained. Since it is no longer necessary to set the layer containing organic particles by coating when manufacturing the present reflective material by the co-extrusion method, it is possible to suppress the detachment of particles while improving the surface roughness, thereby improving the reusability (self-reusability), and the surface layer will not peel off or curl from the substrate, and the manufacturing efficiency can be greatly improved. On the other hand, compared with the above-mentioned structure of the present reflective material, for example, when the main component resin of the resin layer (A) or the resin layer (A) and the resin layer (C) is an acrylic resin, it is difficult to adopt the co-extrusion method and it is difficult to exert the above-mentioned effect.

[0279] (Resin composition A)

[0280] As a raw material of the resin layer (A), a resin composition A containing a polyolefin resin, organic particles, and other additives as required is prepared. Specifically, after mixing these raw materials using a ribbon mixer, a tumbler, a Henschel mixer, etc., kneading is performed at a temperature higher than the flow starting temperature of the resin (for example, 220° C. to 270° C.) using a Banbury mixer, a single screw or a twin screw extruder, etc., thereby obtaining the resin composition A.

[0281] In addition, each raw material can be added in a given amount using a respective feeder or the like to obtain a resin composition A. Alternatively, a portion of the raw materials can be used as a masterbatch in advance and used as a raw material. Alternatively, a portion of the raw materials can be used to prepare a resin composition in advance, and the resin composition can be kneaded with other raw materials to obtain a resin composition A.

[0282] (Resin composition B)

[0283] As a raw material for the resin layer (B), a fine powder filler and other additives as needed are mixed with a polyolefin resin to prepare a resin composition B. Specifically, after mixing these raw materials using a ribbon mixer, a tumbler, a Henschel mixer, etc., kneading is performed at a temperature higher than the melting point of the resin (for example, 190° C. to 270° C.) using a Banbury mixer, a single-screw or twin-screw extruder, etc., thereby obtaining the resin composition B.

[0284] In addition, similarly to the resin composition A, the resin composition may be produced using a feeder or the like, using part of the raw materials as a master batch, or using part of the raw materials to prepare a resin composition in advance.

[0285] (Resin composition C)

[0286] As a raw material for the resin layer (C), a resin composition C containing a polyolefin resin and other additives as required is prepared. Specifically, after mixing these raw materials using a ribbon mixer, a tumbler, a Henschel mixer, etc., kneading is performed at a temperature higher than the flow starting temperature of the resin (for example, 220° C. to 270° C.) using a Banbury mixer, a single screw or a twin screw extruder, etc., to obtain the resin composition C.

[0287] In addition, the resin composition C can be obtained by adding a given amount of each raw material using a respective feeder or the like. Alternatively, a part of the raw materials can be prepared as a masterbatch in advance and used as a raw material. Alternatively, a part of the raw materials can be used to prepare a resin composition in advance, and the resin composition can be kneaded with other raw materials to obtain the resin composition C.

[0288] In addition, when only a polyolefin resin is used for the resin layer (C), it corresponds to the resin composition C without any blending or the like.

[0289] Next, the resin composition A, resin composition B, and resin composition C thus obtained are dried as necessary, and then supplied to separate extruders, respectively, and heated to a predetermined temperature or higher to be melted.

[0290] The conditions such as the extrusion temperature are arbitrary. For example, it is preferred that the extrusion temperature of the resin composition A and the resin composition C is 220°C to 270°C, and the extrusion temperature of the resin composition B is 190°C to 270°C.

[0291] Thereafter, the melted resin composition A, resin composition B and resin composition C were combined in a three-type five-layer T-die and extruded from the slit-shaped outlet of the T-die in a stacked state and cast on a cooling roll.

[0292] The obtained cast sheet is preferably stretched in at least one uniaxial direction. By stretching, the interface between the polyolefin resin and the fine powder filler in the resin layer (B) is peeled off to form voids, and the sheet is whitened, thereby improving the light reflectivity of the film.

[0293] Furthermore, it is more preferred that the cast sheet is stretched in two directions. When only uniaxial stretching is performed, the voids formed will only be formed into a fibrous form stretched in one direction, but by biaxial stretching, the voids become voids stretched in both the vertical and horizontal directions, forming a disc-like form.

[0294] That is, by biaxial stretching, the peeling area of ​​the interface between the polyolefin resin and the fine powder filler inside the resin layer (B) increases, the whitening of the sheet further proceeds, and as a result, the light reflectivity of the film can be further improved. In addition, when biaxial stretching is performed, the anisotropy of the shrinkage direction of the film decreases, so the heat resistance of the film can be improved, and the mechanical strength of the film can also be increased.

[0295] The stretching temperature when stretching the cast sheet is preferably a temperature in the range of not less than the glass transition temperature (Tg) of the polyolefin resin contained in the resin layer (A) or the resin layer (C) and not more than (Tg+50)°C.

[0296] When the stretching temperature is above the glass transition temperature (Tg), the stretching can be stably performed without breaking the film. In addition, when the stretching temperature is below (Tg+50)°C, the stretching orientation becomes high, and as a result, the porosity becomes large, so it is easy to obtain a film with high reflectivity.

[0297] The stretching sequence of biaxial stretching is not particularly limited, and for example, it may be synchronous biaxial stretching or stepwise stretching. After forming a molten cast sheet, it may be stretched in the traveling direction (MD) by roller stretching, and then stretched in the transverse direction (TD) by tenter stretching, or biaxial stretching may be performed by tubular stretching or the like.

[0298] The stretching ratio in the case of biaxial stretching is not limited. The area ratio is usually 4 times or more, preferably 5 times or more, more preferably 6 times or more, and the upper limit is usually 25 times or less, preferably 20 times or less, more preferably 15 times or less. By making the area ratio within the above range, the void ratio of the reflective material can be controlled in an appropriate range, and excellent reflective performance can be exerted, so it is preferred.

[0299] When performing stepwise biaxial stretching, the ratio of the primary stretching is preferably 1.1 to 5.0 times, more preferably 1.5 to 3.5 times, and the ratio of the secondary stretching is preferably 1.1 to 5.0 times, more preferably 2.5 to 4.5 times.

[0300] After stretching, the reflective material is preferably heat-set to provide dimensional stability (void morphological stability). The treatment temperature for heat-setting the film is preferably 130 to 165° C., more preferably 160° C. or less. The treatment time required for heat-setting is preferably 1 second to 3 minutes.

[0301] In addition, the stretching equipment and the like are not particularly limited, but it is particularly preferred to perform tenter stretching that can be subjected to a heat fixation treatment after stretching.

[0302] <Application>

[0303] The application of the present reflective material is not limited. The present reflective material is useful as a reflective member used in liquid crystal display devices such as liquid crystal displays, lighting fixtures, illuminated signs, and the like because of its excellent reflective performance.

[0304] Generally speaking, a liquid crystal display is composed of a liquid crystal panel, a polarizing reflector, a diffuser, a light guide plate, a reflector, a light source, a light source reflector, etc.

[0305] The present reflective material can be suitably used as a reflective material that allows light from a light source to be efficiently incident on a liquid crystal panel or a light guide plate, and can also be suitably used as a light source reflector that focuses irradiated light from a light source arranged at an edge portion and allows it to be incident on a light guide plate.

[0306] The present reflective material is suitable as a reflective material provided in a backlight unit of a liquid crystal display. When the present reflective material is used, the occurrence of uneven brightness and the detachment of particles can be reduced. There is no restriction on the material of the light guide plate. For example, it can be suitably used in a backlight unit equipped with various light guide plates made of polymethyl methacrylate (PMMA) resin, methyl methacrylate-styrene copolymer (MS resin), cycloolefin resin, etc., and is particularly suitable for a backlight unit equipped with a light guide plate made of MS resin.

[0307] Thus, a backlight unit including the present reflective material and a light guide plate made of polymethyl methacrylate (PMMA) resin, methyl methacrylate-styrene copolymer (MS resin), cycloolefin resin, or the like can be provided.

[0308] The present reflective material can also be used directly as a reflective material having the above-mentioned layer structure.

[0309] Furthermore, it can also be made into a structure stacked on a metal plate or a resin plate (collectively referred to as "metal plate, etc.") and used, which is useful for the above-mentioned uses, that is, as a reflector plate of a component of liquid crystal display devices such as liquid crystal displays, lighting fixtures, illuminated signs, etc.

[0310] Therefore, a liquid crystal display device, a lighting fixture, or a lighting sign can be provided using the present reflective material as a constituent member.

[0311] Incidentally, examples of the metal plate on which the present reflective material is to be laminated include an aluminum plate, a stainless steel plate, a galvanized steel plate, and the like.

[0312] The method of laminating the present reflective material on a metal plate or the like is not particularly limited, and examples thereof include a method using an adhesive, a method of hot-melt bonding, a method of bonding via an adhesive sheet, and a method of extrusion coating.

[0313] More specifically, a polyester-based, polyurethane-based, epoxy-based adhesive or the like may be applied to the surface of a metal plate or the like on which the reflective material is to be attached, and the reflective material may be attached thereto.

[0314] Next, the coated surface is dried and heated using an infrared heater and a hot air heating furnace, and the surface of the metal plate or the like is maintained at a predetermined temperature, and immediately covered with a reflective material using a roll laminator and cooled, thereby obtaining a reflective plate.

[0315] In addition, the present reflective material can be used for purposes other than those described above, for example, various industrial materials, packaging materials, optical materials, electrical materials, and the like.

[0316] <Explanation of terms>

[0317] In the present invention, when referred to as a "film", it is deemed to include a "sheet", and when referred to as a "sheet", it is deemed to include a "film".

[0318] The "reflection" in the present invention, unless otherwise specified, refers to the reflection of light, and in a further limitation, refers to the reflection of visible light.

[0319] In the present invention, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", and also includes the meaning of "preferably greater than X" and "preferably less than Y".

[0320] In addition, when expressed as "X or more" (X is an arbitrary number), it includes the meaning of "preferably greater than X" unless otherwise specified, and when expressed as "Y or less" (Y is an arbitrary number), it includes the meaning of "preferably less than Y" unless otherwise specified.

[0321] Example

[0322] The present invention will be described in more detail below with reference to the following embodiments, but the present invention is not limited to these embodiments and can be applied in various ways without departing from the technical concept of the present invention.

[0323] <Measurement and evaluation methods>

[0324] Hereinafter, the measuring methods and the evaluation methods of the samples obtained in the examples and comparative examples will be described.

[0325] (Heat capacity of organic particles at glass transition temperature and glass transition point (ΔCp))

[0326] The glass transition point (inflection point between baseline shifts) and the heat capacity at the glass transition point when the organic particles were heated to 250° C. at a heating rate of 30° C. / min were measured using a differential scanning calorimeter (manufactured by Perkin Elmer Japan, model name: DSC8500).

[0327] (Thickness of reflective material)

[0328] The thickness of all layers of the reflective material was measured using a film thickness meter.

[0329] The total thickness of the resin layer (A) and the resin layer (C), and the thickness of the resin layer (B) were confirmed by cross-sectional observation of the reflective material using an electron microscope.

[0330] It should be noted that in the three types of five-layer reflective materials (samples), since it is difficult to distinguish the layer interfaces of the resin layer (A) and the resin layer (C) under a microscope, the thickness was calculated by multiplying the total thickness of the resin layer (A) and the resin layer (C) by the extrusion amount ratio during sheet molding.

[0331] (Shape of Organic Particles in Resin Layer (A))

[0332] When observing the cross section of the reflective material (sample) for measuring the thickness, it was confirmed whether the organic particles were deformed, and the deformation was determined based on the following criteria.

[0333] Undeformed: The particle shape is substantially the same as that of the raw material. It should be noted that "substantially the same" means that the ratio of the long side to the short side (L / D) of the organic particles is less than 1.8 times when the resin layer (A) of the reflective material is observed using an optical microscope. In this case, the average particle size of the raw material particles is regarded as the average particle size of the particles in the resin layer (A).

[0334] Deformed: The particle shape is deformed relative to the raw material. When the ratio of the long side to the short side (L / D) of the organic particles exceeds 1.8 times when the resin layer (A) of the reflective material is observed under an optical microscope, it is judged as "deformed". In this case, the average particle size of the raw material particles cannot be regarded as the average particle size of the particles in the resin layer (A).

[0335] (Average particle size of organic particles)

[0336] The average particle size of the organic particles in the resin layer (A) is as follows.

[0337] When the shape of the organic particles is “not deformed” in the above-mentioned confirmation of the shape, the value of the average particle size of the raw material particles is used.

[0338] When the shape of the organic particles is "deformed", the resin layer (A) surface of the reflective material is observed using an optical microscope, and the diameters of three or more particles are measured and the average value is obtained. At this time, when the cross-sectional shape is not circular, the average value of the longest diameter and the shortest diameter is used.

[0339] (Porosity)

[0340] The density of the laminated sheet before stretching (unstretched sheet density) and the density of the laminated sheet after stretching (stretched sheet density) were measured, and the porosity (%) of the reflective material (sample) composed of the laminated sheet was calculated by the following formula.

[0341] Void ratio (%) = {(unstretched sheet density - stretched sheet density) / unstretched sheet density} × 100

[0342] (Surface roughness)

[0343] While the reflective material (sample) is left stationary on a flat surface, Rz and Ra are measured on the resin layer (C) side surfaces (either the front or back surface) at three randomly selected locations, and the average values ​​are taken as Rz (μm) and Ra (μm) of the reflective material (sample).

[0344] The measurement was performed using "Surftest SJ-210" manufactured by Mitutoyo Corporation in accordance with JIS B0601 (2001) with λc: 0.8 mm and λs: 2.5 mm.

[0345] (Diameter of protrusion when viewed from above)

[0346] The top view diameter of the protrusion on the resin layer (C) side surface (either the front or the back surface) of the reflective material (sample) is measured as follows: the surface of the reflective material, that is, the resin layer (C) side surface of the reflective material is observed from above using a scanning electron microscope (SEM, observation magnification of about 300 to 500 times), and the diameters of three or more arbitrary protrusions are measured, and the average value thereof is calculated. It should be noted that in Examples 1 to 8, the top view shape of the protrusion observed on the resin layer (C) side surface is circular.

[0347] (Average reflectivity)

[0348] The reflectance of the reflective material (sample) was measured at 0.5 nm intervals in the wavelength range of 420 to 700 nm using an integrating sphere installed in a spectrophotometer ("U-3900H" manufactured by Hitachi High-Technologies) with an alumina white plate as 100%. The average of the measured values ​​was calculated to obtain an average reflectance (%).

[0349] (Evaluation of Brightness Unevenness of Examples 1 and 2 and Comparative Examples 2 and 3)

[0350] An evaluation model of an edge-light type backlight unit was prepared using a material made of methyl methacrylate-styrene copolymer (MS resin) and having a thickness of about 2 mm as a light guide plate.

[0351] A light guide plate was placed on the resin layer (C) side (either the front or back side) of the reflective material (sample), and a weight (2 kg) was placed on top of the light guide plate, and the edge light was turned on. A camera installed on the top of the light guide plate was used to check whether uneven brightness occurred near the weight, and the judgment was made according to the following criteria.

[0352] ○ (good): No uneven brightness occurs and the material is suitable as a reflective material for a thin backlight or the like.

[0353] × (poor): Uneven brightness occurs, and the material is not suitable as a reflective material for thin backlights and the like.

[0354] (Evaluation of Brightness Unevenness of Examples 3 to 8 and Comparative Examples 1 and 4)

[0355] An evaluation model with a light guide plate as the outermost layer was produced using an edge-light type backlight unit. A reflective material (sample) was placed between a 0.5 mm thick metal sheet and the light guide plate, with the resin layer (C) side (either the front or back side) on the light guide plate side, and a weight (300 g) was placed on top of the reflective material (sample) and the edge light was turned on. A camera installed on the top of the light guide plate was used to check whether uneven brightness occurred near the metal sheet, and the judgment was made according to the following criteria.

[0356] ⊚ (excellent): No brightness unevenness from the end of the metal piece was observed.

[0357] ○ (good): Brightness unevenness from the edge of the metal piece slightly occurs, but it is suitable as a reflective material for a thin backlight or the like.

[0358] × (poor): Clear brightness unevenness occurred from the edge of the metal piece, and the metal piece was not suitable as a reflective material for a thin backlight or the like.

[0359] (Tape Peeling Evaluation of Examples 1 and 2, Comparative Examples 2 and 3)

[0360] After affixing an adhesive tape (manufactured by Nichiban Co., Ltd., CELLOTAPE (registered trademark) CT15) to the side surface (either the front or the back) of the resin layer (C) of the reflective material (sample), the adhesive tape was peeled off, and the peeled reflective material (sample) surface and the adhesive surface of the adhesive tape were observed using an optical microscope, and judged according to the following criteria. It should be noted that the transfer to the adhesive tape is a surrogate indicator of the degree of contamination of the constituent members.

[0361] ◎ (excellent): Peeling of the reflective material (sample) surface and transfer of the reflective material (sample) surface to the adhesive tape were hardly observed.

[0362] ○ (better): There is little peeling of the reflective material (sample) surface and transfer of the reflective material (sample) surface to the adhesive tape.

[0363] Δ (good): Peeling of the reflective material (sample) surface and transfer of the reflective material (sample) surface to the adhesive tape were slightly observed.

[0364] × (poor): There was much peeling of the reflective material (sample) surface and transfer of the reflective material (sample) surface to the adhesive tape.

[0365] (Tape peeling evaluation of Examples 3 to 8 and Comparative Examples 1 and 4)

[0366] After a pressure-sensitive adhesive tape (manufactured by 3M Japan Co., Ltd., trade name "SCOTCH Super Clear Tape S BK-18") was attached to the resin layer (C) side surface (either the front or the back side) of the reflective material (sample), the pressure-sensitive adhesive tape was peeled off, and the surface of the reflective material (sample) after peeling was visually observed and judged according to the following criteria.

[0367] ◎ (excellent): Almost no peeling of the reflective material (sample) surface was observed by naked eye.

[0368] ○ (better): A small amount of peeling of the reflective material (sample) surface was confirmed by visual observation.

[0369] △ (good): Local peeling of the reflective material (sample) surface was confirmed.

[0370] × (poor): Large-scale peeling or a large amount of local peeling was observed on the surface of the reflective material (sample).

[0371] <Raw materials>

[0372] Hereinafter, the raw materials used in Examples and Comparative Examples will be described.

[0373] (COP-A)

[0374] Amorphous cycloolefin resin (MFR (230°C, 21.18N): 1.5 g / 10 min, Tg: 129°C)

[0375] (COP-B)

[0376] Amorphous cycloolefin resin (MFR (230°C, 21.18N): 15g / 10min, Tg: 105°C)

[0377] (PP-A)

[0378] Polypropylene resin ("Novatec PP FY6HA" manufactured by Japan Polypropylene Co., Ltd., MFR (230°C, 21.18N): 2.3 g / 10 min)

[0379] (PP-B)

[0380] Polypropylene resin ("Novatec PP EG6D" manufactured by Japan Polypropylene Co., Ltd., MFR (230°C, 21.18N): 2.0 g / 10 min)

[0381] (Organic Particles-A)

[0382] Methyl methacrylate cross-linked resin particles (Tg: 137°C, ΔCp: 0.34 J / (g·°C), average particle size (D50): 30 μm)

[0383] (Organic Particles-B)

[0384] Methyl methacrylate cross-linked resin particles (Tg: 138°C, ΔCp: 0.20 J / (g·°C), average particle size (D50): 12 μm)

[0385] (Titanium Oxide)

[0386] KRONOS 2450 manufactured by KRONOS Corporation (Rutile titanium oxide manufactured by the chlorine method, surface treated with alumina and silica, TiO2 content 96.0%, average particle size (D50): 0.31 μm)

[0387] (Calcium carbonate)

[0388] "Softon 3200" manufactured by Bihoku Powder Industry Co., Ltd. (average particle size (D50): 0.70 μm)

[0389] <Example 1>

[0390] (Preparation of Resin Composition A)

[0391] COP-A, COP-B, PP-A pellets and organic particles-A were mixed at a mass ratio of COP-A / COP-B / PP-A / organic particles-A=50:25:21:4, and then melt-kneaded using a twin-screw extruder to form pellets, thereby preparing a resin composition A as a raw material for the resin layer (A).

[0392] (Preparation of Resin Composition B)

[0393] PP-A pellets and a fine powder filler were mixed at a mass ratio of PP-A:titanium oxide:calcium carbonate = 55:40:5, and then melt-kneaded at 270° C. using a twin-screw extruder to form pellets to prepare a resin composition B as a raw material for the resin layer (B).

[0394] (Preparation of Resin Composition C)

[0395] Pellets of COP-A, COP-B and PP-A were mixed at a mass ratio of COP-A / COP-B / PP-A=50:25:25, and then melt-kneaded using a twin-screw extruder to form pellets, thereby preparing a resin composition C as a raw material for the resin layer (C).

[0396] (Production of reflective materials)

[0397] The above-mentioned resin compositions A, B and C are respectively supplied in stages to extruders A, B and C which have been heated to 220°C. After being melted in each extruder, the extrusion rates of the resin layer (A) and the resin layer (C) are adjusted so that the extrusion rates are 2.6 kg / h and 2.8 kg / h respectively and the thickness ratio of the resin layer (C) to the resin layer (A) is 1.1. The three types of five-layer T-dies are merged and extruded into sheets in a manner of forming a five-layer structure of resin layer (C) / resin layer (A) / resin layer (B) / resin layer (A) / resin layer (C). The sheets are cooled and solidified using a casting roll at a speed of 1.0 m / min to form an unstretched laminated sheet.

[0398] The obtained laminated sheet was subjected to 2.3 times roll stretching in the traveling direction (MD) of the film at a temperature of 142°C, and then further subjected to 3 times tenter stretching in the orthogonal direction (TD) at 136°C, thereby performing biaxial stretching to obtain a reflective material (sample) consisting of a laminated sheet with a total thickness of 195 μm.

[0399] The obtained reflective material was evaluated for the shape of organic particles, porosity, surface roughness, average reflectivity, brightness unevenness, and tape peeling. The results are shown in Tables 1 and 2.

[0400] <Example 2>

[0401] A reflective material (sample) was obtained in the same manner as in Example 1 except that the extrusion rates of the resin layer (A) and the resin layer (C) were adjusted so that the extrusion rates were 1.4 kg / h and 4.2 kg / h, respectively, and the thickness ratio of the resin layer (C) to the thickness of the resin layer (A) was 3.0. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0402] <Example 3>

[0403] (Preparation of Resin Composition A)

[0404] COP-A, COP-B, PP-A pellets and organic particles-B were mixed at a mass ratio of COP-A / COP-B / PP-A / organic particles-B = 50:25:21:4, and then melt-kneaded at 220° C. using a twin-screw extruder to form pellets, thereby preparing a resin composition A as a raw material for the resin layer (A).

[0405] (Preparation of Resin Composition B)

[0406] As a raw material for the resin layer (B), the same resin composition B as in Example 1 was prepared.

[0407] (Preparation of Resin Composition C)

[0408] Pellets of COP-A, COP-B and PP-A were mixed at a mass ratio of COP-A / COP-B / PP-A=50:25:25, and then melt-kneaded at 220°C using a twin-screw extruder to form pellets, thereby preparing a resin composition C as a raw material for the resin layer (C).

[0409] (Production of reflective materials)

[0410] The above-mentioned resin compositions A, B and C are respectively supplied in stages to extruders A, B and C which have been heated to 220°C. After being melted in each extruder, the extrusion rates of the resin layer (A) and the resin layer (C) are adjusted so that the extrusion rates are 1.1 kg / h and 3.0 kg / h respectively and the thickness ratio of the resin layer (C) to the resin layer (A) is 2. The three types of five-layer T-dies are merged and extruded into sheets in a manner of forming a five-layer structure of resin layer (C) / resin layer (A) / resin layer (B) / resin layer (A) / resin layer (C). The sheets are cooled and solidified using a casting roll at a speed of 2.5 m / min to form an unstretched laminated sheet.

[0411] The obtained laminated sheet was subjected to 2.3 times roller stretching in the traveling direction (MD) of the film at a temperature of 142°C, and then 3 times tenter stretching in the orthogonal direction (TD) at 136°C, thereby biaxially stretched, and then subjected to a heat fixation treatment at 158-162°C for 2 minutes, thereby obtaining a reflective material (sample) consisting of a laminated sheet with a total thickness of 71 μm. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0412] <Example 4>

[0413] A reflective material (sample) was obtained in the same manner as in Example 3 except that the extrusion rates of the resin layer (A) and the resin layer (C) were adjusted so that the extrusion rates were 3.0 kg / h and 2.8 kg / h, respectively, and the thickness ratio of the resin layer (C) to the thickness of the resin layer (A) was 1. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0414] <Example 5>

[0415] The extrusion rates of the resin layer (A) and the resin layer (C) were adjusted to 3.1 kg / h and 1.1 kg / h, respectively, and the thickness ratio of the resin layer (C) to the resin layer (A) was 0.5, and the heat setting treatment temperature was set between 157 and 162° C. A reflective material (sample) was obtained in the same manner as in Example 3. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0416] <Example 6>

[0417] In the preparation of resin composition A, the pellets of COP-A, COP-B, PP-A and organic particles-B were set to a mass ratio of COP-A / COP-B / PP-A / organic particles-B=50:25:17:8, and the extrusion rates of the resin layer (A) and the resin layer (C) were adjusted to 1.0 kg / h and 3.0 kg / h, respectively, and the thickness ratio of the resin layer (C) to the thickness of the resin layer (A) was 4. A reflective material (sample) was obtained in the same manner as in Example 5. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0418] <Example 7>

[0419] A reflective material (sample) was obtained in the same manner as in Example 6 except that the extrusion rates of the resin layer (A) and the resin layer (C) were adjusted so that the extrusion rates were 3.0 kg / h and 2.9 kg / h, respectively, and the thickness ratio of the resin layer (C) to the thickness of the resin layer (A) was 1. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0420] <Example 8>

[0421] A reflective material (sample) was obtained in the same manner as in Example 6 except that the extrusion rates of the resin layer (A) and the resin layer (C) were adjusted to 4.9 kg / h and 2.8 kg / h, respectively, and the thickness ratio of the resin layer (C) to the thickness of the resin layer (A) was 0.5. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0422] <Comparative Example 1>

[0423] Resin composition C was used instead of resin composition A, and the extrusion rates of resin layer (C) were set to 2.6 kg / h and 2.7 kg / h, respectively, so as to form two types of five-layer structures of resin layer (C) / resin layer (C) / resin layer (B) / resin layer (C) / resin layer (C), respectively. A reflective material (sample) was obtained in the same manner as in Example 5. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0424] <Comparative Example 2>

[0425] In the preparation of resin composition A, PP-B pellets and organic particles-A were mixed in a mass ratio of PP-B / organic particles-A=90:10, and then pelletized using a twin-screw extruder to obtain a [PP-B / organic particles-A mixture]. Then, COP-A and COP-B pellets and [PP-B / organic particles-A mixture] were mixed in a mass ratio of COP-A / COP-B / [PP-B / organic particles-A mixture]=50:25:25, and then pelletized using a twin-screw extruder to prepare a resin composition A2 with a mass ratio of COP-A / COP-B / PP-B / organic particles-A=50:25:22.5:2.5 as a raw material for the resin layer (A).

[0426] Instead of using the extruder C, the extruders A and B heated to 250° C. were used in stages, and the extruders were joined at two three-layer T-dies to extrude the sheets into a three-layer structure of resin layer (A) / resin layer (B) / resin layer (A), and the sheets were stretched at 141° C. in the orthogonal direction (TD). A reflective material (sample) was obtained in the same manner as in Example 1. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0427] <Comparative Example 3>

[0428] In the preparation of resin composition A, PP-B pellets and organic particles-A were mixed in a mass ratio of PP-B / organic particles-A=85:15, and then pelletized using a twin-screw extruder to obtain a [PP-B / organic particles-A mixture]. Then, COP-A and COP-B pellets and [PP-B / organic particles-A mixture] were mixed in a weight ratio of COP-A / COP-B / [PP-B / organic particles-A mixture]=50:25:25, and then pelletized using a twin-screw extruder to prepare a resin composition A3 as a raw material of the resin layer (A) with a weight ratio of COP-A / COP-B / PP-B / organic particles-A=50:25:21.25:3.75.

[0429] A three-layer reflective material (sample) was obtained in the same manner as in Comparative Example 2 except that resin composition A3 was used instead of resin composition A2. The obtained reflective material (sample) was evaluated in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0430] <Comparative Example 4>

[0431] Resin composition A was used instead of resin composition C, and the extrusion rates of resin layer (A) were set to 3.0 kg / h and 2.9 kg / h, respectively, so as to form two types of five-layer structures of resin layer (A) / resin layer (A) / resin layer (B) / resin layer (A) / resin layer (A). A reflective material (sample) was obtained in the same manner as in Example 5. The obtained reflective material (sample) was evaluated in the same manner as in Example 1, and the results are shown in Tables 1 and 2.

[0432] [Table 1]

[0433]

[0434] [Table 2]

[0435]

[0436] It is clear from Tables 1 and 2 that the reflective materials of Examples 1 to 8 have a high reflectivity and suppressed brightness unevenness by laminating the resin layer (A) containing organic particles between the resin layer (C) and the resin layer (B). In addition, it was confirmed that the peeling of the reflective material surface and the transfer of the reflective material surface to the adhesive tape were reduced, and the detachment of the organic particles contained in the resin layer (A) was suppressed.

[0437] On the other hand, for the reflective material of Comparative Example 1 not having the resin layer (A), it was confirmed that the brightness unevenness could not be suppressed, and for the reflective materials of Comparative Examples 2 to 4 not having the resin layer (C), it was confirmed that the reflective material surface was peeled off and the transfer of the reflective material surface to the adhesive tape was frequent, so that the particles were easily detached, which caused problems in practical use.

Claims

1. A reflective material comprising a structure of four or more layers in which a resin layer (B), a resin layer (A) and a resin layer (C) are sequentially stacked and at least two layers of at least any one of the resin layer (A), the resin layer (B) and the resin layer (C) are included, wherein the structure of the four or more layers has the resin layer (B) as a core layer, The resin layer (B) contains a polyolefin resin and a fine powder filler. The resin layer (A) contains a polyolefin resin and organic particles. The resin layer (C) contains a polyolefin resin and does not contain organic particles having a particle size of 10 μm or more. The thickness of the resin layer (B) accounts for the highest proportion of the total thickness. The resin layer (C) constitutes the outermost layer, The ratio of the thickness of the resin layer (C) to the thickness of the resin layer (A) is in the range of 0.5 or more and 5.0 or less, At least one of the resin layers (A) to (C) has voids.

2. The reflective material according to claim 1, wherein: The maximum height Rz of the side surface of the resin layer (C) is 3.0 μm to 7.0 μm.

3. The reflective material according to claim 1 or 2, wherein: The heat capacity ΔCp of the organic particles contained in the resin layer (A) at the glass transition point is 0.75 J / (g·° C.) or less.

4. The reflective material according to claim 1 or 2, wherein: The glass transition point of the organic particles is 120° C. or higher.

5. The reflective material according to claim 1 or 2, wherein: The organic particles are cross-linked particles.

6. The reflective material according to claim 1 or 2, wherein: The diameter of the protrusions on the surface of the resin layer (C) side is 21 μm to 39 μm in plan view.

7. The reflective material according to claim 1 or 2, wherein: The diameter of the protrusions on the surface of the resin layer (C) side is 5 μm to 20 μm in plan view.

8. The reflective material according to claim 1 or 2, wherein: The resin layer (A) contains 0.5 to 10% by mass of organic particles.

9. The reflective material according to claim 1 or 2, wherein the porosity thereof is 10 to 80%.

10. The reflective material according to claim 1 or 2, wherein: One or both of the polyolefin resin of the resin layer (A) and the polyolefin resin of the resin layer (C) are polypropylene resins or cycloolefin resins.

11. The reflective material according to claim 1 or 2, wherein: The polyolefin resin of the resin layer (A) and the polyolefin resin of the resin layer (C) are the same resin.

12. The reflective material according to claim 1 or 2, which is used as a constituent member of a backlight unit.

13. The reflective material according to claim 1 or 2, which is used as a component of any of a liquid crystal display, a lighting fixture, and a lighting sign.

14. A liquid crystal display, a lighting fixture or a lighting sign, which uses the reflective material according to claim 1 or 2 as a constituent member.