Gas sensor devices based on metal oxide foams
By using metal oxide foam sensing materials with a three-dimensional porous structure, the problems of insufficient sensitivity and long response time in the detection of low-concentration toxic gases in the existing technology are solved, and high sensitivity and rapid detection of toxic gases are achieved.
Patent Information
- Application Number
- CN202080024074.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-26
- Filing Date
- 2020-03-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Existing gas sensors have insufficient sensitivity and long response times when detecting low-concentration toxic gases, and cannot quickly detect the presence and dissipation of gases.
Metal oxide foam with a three-dimensional porous structure is used as the sensing material, and silver paste is attached to the platinum electrode and ruthenium heater on the low-temperature co-fired ceramic substrate to improve the sensitivity and response speed of the sensor.
It achieves high-sensitivity detection and rapid response to extremely low-concentration toxic gases, shortens the gas diffusion reaction path, and is suitable for detecting toxic gases such as ethanol and carbon monoxide.
Smart Images

Figure CN113646264B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This patent application claims the benefit of U.S. Patent Application No. 62 / 824,276, filed on March 26, 2019, which is incorporated by reference along with all other references cited in this application. Background Art
[0003] The present invention relates to the technical field of gas sensing devices. More specifically, the present invention relates to developing a sensitive gas detection device using metal oxide foam to effectively monitor various toxic gases using appropriate gas sensors, which can detect the presence of toxic gases with extremely low particle concentrations to high particle concentrations with higher sensitivity and shorter sensing time.
[0004] The technical difficulty is because most toxic gases exist in relatively low concentrations. It is very important to select appropriate sensing materials that exhibit accurate and sensitive responses to low concentrations of target gases. It is also important to use gas sensor devices with shorter sensing times, where the target gas can enter and exit the gas sensor device as quickly as possible.
[0005] Numerous industrial and private enterprises are in urgent need of advanced gas sensing technology. For example, with the great advancement of modern technology, a large amount of toxic gases are being produced, and there is a growing concern about accidental leaks, which can seriously affect the environment and the health of humans and animals. In addition, a new regulation in the United States requires that every new building should be equipped with a carbon monoxide detector to prevent fires.
[0006] Therefore, there is a need for improved gas sensing device technologies and materials. Summary of the invention
[0007] A new gas sensor device has been prepared, which has a three-dimensional connected metal oxide foam structure with a large surface area and elongated channels within the three-dimensional porous structure for use in gas sensing applications, thereby increasing the surface area of the sensing layer and improving sensitivity and sensor response. The gas sensor device includes a prepared metal oxide foam sensing material, which is attached to a platinum electrode and a ruthenium heater printed on a low-temperature co-fired ceramic substrate via a silver paste. The device provides improved gas sensing performance with improved sensitivity and response time (e.g., faster gas in and out). Gas sensors containing metal oxide foam sensing materials show higher sensitivity to toxic gases such as ethanol and carbon monoxide, because the large surface area achieved by the porous three-dimensional structure provides increased chemical reaction sites and provides larger porous channels that allow gas to pass easily, thereby shortening the gas diffusion reaction path.
[0008] The method is explicitly explained based on the results of tin oxide gas sensing materials, but can be extended to many other metal oxides and includes the preparation of metal oxide foams with pore sizes ranging from a few hundred nanometers to tens of micrometers, and the application of these metal oxide foams as sensing materials in gas sensor applications. When exposed to the target gas, the prepared metal oxide foams react with the toxic gas on their extended surface layer.
[0009] A novel method for preparing three-dimensional metal oxide foams (e.g., tin oxide and copper oxide foams as examples) for use as advanced gas sensing materials. The method consists of preparing tin oxide foams with pore sizes ranging from hundreds of nanometers to several micrometers for use as gas sensing materials, and then patterning two electrode pads with a 200-micrometer pitch on the metal oxide foams using a shadow mask through a lift-off process.
[0010] Gas sensors containing porous tin oxide foams exhibited enhanced sensitivity to toxic gases such as ethanol and carbon monoxide, due to the large surface area achieved through the porous three-dimensional structure providing increased chemical reaction sites and larger porous channels that allow gases to pass easily, thereby shortening the gas diffusion reaction path.
[0011] Tin oxide is a commonly used gas sensing material that can be applied to n-type or p-type gas sensors, depending on its crystal structure. This patent details a new method for preparing tin oxide and other metal oxide foams using combined slurry foaming and powder sintering to provide gas sensing materials with improved sensitivity. The tin oxide foams prepared using the method detailed in this patent show different morphological characteristics depending on the main process parameters, including sintering temperature, sintering time and the amount of powder added. Scanning electron microscopy images identified a dual pore structure within the tin oxide foam, which contained an array of pores of 5.3-10.7 microns and smaller secondary pores with diameters of several microns on the wall surface. The gas sensing performance of the synthesized tin oxide foam in a relatively large laboratory chamber showed a sensitivity of 13.1, a response time of 192 seconds, and a recovery time of 160 seconds for 600 ppm ethanol gas at 300 degrees Celsius, and a sensitivity of 35.9, a response time of 39 seconds, and a recovery time of 27 seconds for 5000 ppm carbon monoxide gas at 200 degrees Celsius. These are remarkable detection results considering that no catalyst was added to the samples prepared according to the patent.
[0012] In addition, the freeze-cast copper oxide foam showed a steadily increasing copper oxide foam sensitivity with increasing carbon monoxide gas concentration at 300 degrees Celsius at low carbon monoxide concentrations of 1000 ppm to 5000 ppm, confirming that the metal oxide sensor structure is beneficial for detecting toxic gases such as carbon monoxide using its enhanced sensing surface area. A metal oxide foam gas sensor device was prepared in which platinum electrodes and ruthenium oxide heaters were printed on a low temperature co-fired ceramic (LTCC) substrate before the metal oxide foam sensor was attached to the top of the heater and electrodes using Ag paste. This sensor device can directly replace existing sensing material components.
[0013] In one embodiment, the gas sensor device comprises a metal oxide foam sensing material coupled to a platinum electrode and a ruthenium heater printed on LTCC via a silver paste. The electrode pattern may include two electrode pads of a suitable metal such as platinum with a separation of a few hundred microns using a lift-off process and a shadow mask to serve as electrodes for the attached metal oxide foam sensor.
[0014] The metal oxide foam has a porosity between about 55% and about 90% and is a gas sensing material in a sensor device that reacts to specific target (e.g., toxic) gases such as ethanol, carbon monoxide, oxygen, nitrogen oxides, hydrogen, toluene, and other gases. The sensing material comprises at least one of: tin oxide foam, or tin oxide foam with at least one of palladium, gold, silver, or platinum catalyst in the range of 0.1 wt % to 3 wt %.
[0015] The sensing material is a metal oxide foam, such as a semiconductor type sensor. The porous sensing material can be any one or a combination of tin oxide (SnO or SnO2), zinc oxide (ZnO), indium oxide (In2O3), tungsten oxide (WO3), titanium oxide (TiO2), nickel oxide (NiO), copper oxide (CuO), cobalt oxide (Co3O4), chromium oxide (Cr2O3) and iron oxide (Fe2O3), or other metal oxides with similar properties.
[0016] The preparation method for forming the porous metal oxide foam sensing material may include at least one of freeze casting, space holder method or dealloying or a combination thereof. The preparation method for forming the porous metal oxide foam sensing material may include a freeze casting method performed as follows: preparing a powder slurry, and a sintering process, wherein the water or camphene-based oxide powder slurry is frozen and dried at low temperature to form a green body, and then sintered at high temperature to form a three-dimensionally connected solid porous structure.
[0017] The sensing material may be a semiconductor type sensor using a metal oxide, and the porous sensing material may be prepared by performing at least one of thermal oxidation or anodizing processes on the surface of a metal foam (e.g., Sn, Zn, In, W, Ti, Ni, Cu, Co, Cr, or Fe) prepared by at least one of freeze casting, a pore former method, or dealloying. The metal oxide sensing material may be constructed on the surface of the prepared metal foam in the form of at least one of an oxide thin layer or a nano needle-shaped oxide.
[0018] Tin oxide foams can be prepared by adding a sintering agent in a composition range of about 0.1 wt % to about 3 wt %, such as Li2O, CuO, MnO2, ZnO, or La2O3, to aid densification by forming a liquid phase during sintering of the tin oxide green body.
[0019] In one embodiment, a method for preparing a metal oxide foam using a freeze casting process comprises: placing a rectangular insulating silicone mold on a copper or aluminum block immersed in liquid nitrogen, controlling the temperature using a thermocouple and a temperature controller, and pouring a metal oxide slurry comprising at least one of deionized water, a dispersant, a binder, a metal or metal oxide powder, and a sintering agent into the mold; freezing the slurry so that dendritic ice crystals form and grow in the slurry, and the metal or metal oxide particles aggregate between the growing ice crystals; and heating the mold by heating the mold at a temperature between about -10 degrees Celsius and about -80 degrees Celsius. Drying the ice crystals of the frozen sample at a sufficiently low temperature and reduced pressure to leave pores at their original positions to form a green metal (oxide) foam; forming a porous metal oxide foam with three-dimensional connections having basic integrity by sintering the porous green body at a sufficiently high temperature between about 800 degrees Celsius and about 1700 degrees Celsius in a controlled furnace under an air or argon atmosphere; and machining the metal oxide foam into a rectangular form that can be directly applied as a sensing material in a gas sensor having a ruthenium heater and a platinum electrode located below the ruthenium heater.
[0020] In one embodiment, a method of applying the prepared metal oxide foam to a gas sensor includes a patterning process that attaches an electrode pad to the metal oxide foam sensing material in a suitable pattern. The gas sensor may include a metal oxide foam sensing material coupled to a platinum electrode and a ruthenium heater printed on a low temperature co-fired ceramic substrate via a silver paste.
[0021] Other objects, features and advantages of the present invention will become apparent upon consideration of the following detailed description and accompanying drawings, in which like reference numerals represent like features throughout the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figures 1A to 1C The general sensing mechanism of n-type and p-type semiconductor sensors is schematically shown.
[0023] FIG. 2A to FIG. 2B Photographs of tin oxide foam samples before and after sintering are shown.
[0024] Figure 3A X-ray diffraction patterns of tin oxide foam samples heat treated at different temperatures are shown.
[0025] Figure 3B The X-ray absorption near-edge structure spectrum of the tin K-edge of the tin oxide foam is shown.
[0026] Figure 3C X-ray photoelectron spectroscopy measurements of tin oxide are shown.
[0027] Figure 3D The binding energy positions of tin oxide are shown.
[0028] 4A to 4H Scanning electron micrographs of radial cross sections and fracture surfaces of tin oxide foams are shown.
[0029] FIG. 5A to FIG. 5B The results show that the ethanol concentrations ( Figure 5A ) and carbon monoxide gas ( Figure 5B ) of the tin oxide foam at different times.
[0030] FIG. 6A to FIG. 6B The sensing responses of tin oxide foams in ethanol and carbon monoxide gases were compared.
[0031] FIG. 7A to FIG. 7B The changes in resistance and gas sensitivity of tin oxide foams with and without palladium addition at 200 degrees Celsius were compared.
[0032] Figure 8Shown is a comparison of the sensitivity between tin oxide foams with and without added palladium at various temperatures.
[0033] FIG. 9A to FIG. 9B Shown are the changes in resistance and gas sensitivity of tin oxide foam with low concentration of palladium added as a catalyst at 200 degrees Celsius.
[0034] FIG. 10A to FIG. 10C The changes in resistance and gas sensing mechanisms and sensing responses of copper oxide foam at various carbon monoxide concentrations are shown.
[0035] FIG. 11A to FIG. 11G A schematic process flow for fabricating a metal oxide foam gas sensor device is shown, where platinum electrodes and a ruthenium oxide heater are printed on a LTCC substrate.
[0036] Fig.12 A gas sensor product having a tin oxide foam sensor device is shown, which is used to replace an existing much larger commercial sensing module. DETAILED DESCRIPTION
[0037] Metal oxide gas sensors are one of the most commonly used sensing devices for commercial gas sensing applications. The sensor is based on the principle of changing the resistivity (or conductivity) caused by gas adsorption on the surface of the sensing material exposed to the target gas.
[0038] Common sensing materials are tin oxide (SnO or SnO2) and zinc oxide (ZnO), both of which exhibit excellent semiconductor sensing properties. Other metal oxide semiconductors, such as copper oxide (CuO), nickel oxide (NiO), titanium oxide (TiO2), tungsten oxide (WO3), indium oxide (In2O3) and iron oxide (Fe2O3) or their combinations, are also used for new chemical or resistivity functions due to their good response and selectivity to environmental conditions, as well as the simplicity of their material synthesis and sensor device preparation.
[0039] Controlling the (surface) morphology of gas sensing materials is an effective way to enhance the sensing properties. It is important to understand the microstructure of the sensing material because grain size, morphology, surface state and accessible surface area all play an important role in gas sensing performance. Typically, adsorption or desorption processes occur on the surface of the sensing layer and determine the response of the sensor.
[0040] Therefore, there has been a significant increase in recent research and development on the design of gas sensing materials including nanowires, nanoparticles, nanorods, nanotubes, and hollow spheres. However, these efforts have not provided adequate solutions and there is still a need to improve gas sensitivity.
[0041] A new gas sensing device is based on a new metal oxide foam material with enhanced surface area and higher gas permeability. The three-dimensional pore structure on the surface of the metal oxide foam used in the device can improve the adsorption and desorption process of the surface sensing layer, thereby enhancing the sensitivity and response time to the target gas.
[0042] The preparation of the porous structure includes the following steps: (a) freezing a metal or metal oxide slurry having metal or metal oxide powder and a sintering agent powder (e.g., copper oxide) in a silicone mold in contact with a cold surface of a copper rod; (b) sublimating the frozen slurry under reduced pressure and low temperature to form a porous green body; (c) sintering the porous green body to obtain a three-dimensionally connected porous metal oxide foam; (d) cutting the porous metal oxide foam into 10 mm by 20 mm plates to be used as a sensing material; and (e) patterning the porous foam using a lift-off process and a mask, wherein the platinum electrode pads are spaced 200 microns apart.
[0043] The porous structure of tin oxide foam is used as a sensing material for a gas sensor, providing a higher surface area with directional channel pores (e.g., relative to non-foam materials), which can facilitate the flow of toxic target gases. As schematically shown in Figure 1, this dual pore structure with a large surface area can detect toxic gases such as ethanol, carbon monoxide and other gases with improved sensitivity when exposed to toxic gases.
[0044] A variety of oxide-based gas sensing semiconductor material foams can be made into three-dimensional porous structures, and all can be prepared from the form of starting powders. For example, these foams include tin oxide (SnO or SnO2), zinc oxide (ZnO), indium oxide (In2O3), tungsten oxide (WO3), titanium oxide (TiO2), nickel oxide (NiO), copper oxide (CuO), cobalt oxide (Co3O4), chromium oxide (Cr2O3) and iron oxide (Fe2O3). The initial materials can also be their corresponding metal powders, because the frozen and dried green body composed of metal powders can be sintered at high temperature in a hydrogen atmosphere instead of an air atmosphere to achieve reduction. Tin oxide foam and copper foam are specific examples discussed in this patent, but as mentioned above, other metal oxide materials can also be used in the same way as gas sensing materials, provided that they also have semiconductor materials with wide band gap, high conductivity and good stability.
[0045] Porous metal oxide foams are three-dimensionally connected porous structures with pore sizes ranging from a few hundred nanometers to tens of micrometers, and the pores extend in three dimensions. Three-dimensional metal oxide foams are prepared based on a combination of slurry foaming and powder sintering. This is a relatively simple, low-cost processing method suitable for preparing small or large structures. However, the preparation method of porous metal oxide foams is not limited to this powder processing, and other methods can also be used to prepare metal oxide foam structures for application as sensor devices with improved sensitivity.
[0046] In order to prepare tin oxide foam, sintering agent such as copper oxide can contribute to the densification process by forming a sintering liquid phase.Porous tin oxide with a sintering agent (e.g., copper oxide) can achieve uniform volume shrinkage of foam during sintering, so that cracks will not occur (Fig. 2).We believe that shrinkage is almost isotropic, and the residual stress caused by shrinkage is minimal.As is well known, because the mass transfer mechanism of tin oxide is quite complicated, it is controlled by surface diffusion at low temperatures (e.g., temperatures below 1000 degrees Celsius) and controlled by evaporation condensation at high temperatures (e.g., temperatures above 1300 degrees Celsius), so tin oxide is difficult to densify during sintering.When any one of these two mechanisms is dominant, it is difficult to achieve uniform densification.However, sintering agent (e.g., copper oxide) has a significant effect in promoting bulk or grain boundary diffusion or in forming a liquid phase during tin oxide sintering, or has a significant effect in both aspects.
[0047] Based on the preparation of tin oxide foam, relatively simple modifications can be made to prepare various types of porous metal oxide foams for use as three-dimensional gas sensing materials, such as preparing porous metal oxide foams of titanium oxide, nickel oxide, cobalt oxide, zinc oxide, etc.
[0048] This patent describes some examples of embodiments with specific dimensions, measurements, and values. These examples are not intended to be exhaustive or to limit the invention to the described definite forms. Values, percentages, times, and temperatures are approximate. These values may vary due to, for example, manufacturing variations or measurements of starting powder chemistry or tolerances or other factors. For example, depending on the tightness of manufacturing tolerances and measurement tolerances, values may vary by plus or minus 5%, plus or minus 10%, plus or minus 15%, or plus or minus 20%.
[0049] In addition, the values are for specific embodiments, and other embodiments may have different values, such as certain values being larger for larger-scale processes or products, or smaller for smaller-scale products. By proportionally adjusting the relative measurements (e.g., maintaining the same or approximately the same ratio between different measurements), a device, apparatus, or process may be proportionally made larger or smaller. In various embodiments, these values may be the same as a given value, approximately the same as a given value, at least or greater than a given value, or may be at most or less than a given value, or any combination of these.
[0050] A method for preparing a porous metal oxide foam for use as a gas sensing material, the method may include the following steps:
[0051] 1. A silicone mold is placed on a copper rod or similar high thermal conductivity material immersed in liquid nitrogen, and a metal oxide slurry with a powder size typically in the range of tens or hundreds of nanometers is poured into the mold together with a binder and a sintering agent.
[0052] 2. Freezing the prepared metal oxide slurry, where the metal oxide particles are packed and physically attached between the growing ice crystals.
[0053] 3. Forming a porous green body by drying the ice crystals from the frozen slurry at sufficiently low temperature and reduced pressure to leave pores in the structure and preserve physical attachment.
[0054] 4. Solidification of the metal oxide foam with firmly connected pores by debinding and sintering the porous green body at a sufficiently high temperature in an air atmosphere.
[0055] 5. Cut the porous metal oxide foam into rectangles of 10 mm by 20 mm to be used as the sensing material in the gas sensor.
[0056] 6. The porous foam was patterned by lift-off process using a shadow mask, with two platinum electrode pads separated by 200 μm.
[0057] Exemplary Embodiment 1: Preparation of Tin Oxide Foam
[0058] Tin oxide powder (e.g., 15.5 g) is suspended in 20 ml of a deionized water solution containing a polyvinyl alcohol binder, and a sintering agent (e.g., copper oxide (CuO) powder, less than 3 wt %) is added to improve the densification of the tin oxide powder. The slurry is dispersed for 30 minutes using a manual stirrer and then ultrasonicated for 1 hour. To ensure adequate particle dispersion, the stirring process is repeated twice.
[0059] The slurry is then cooled to a few degrees above the freezing point of water and poured into a cylindrical mold consisting of insulating polytetrafluoroethylene (PTFE), Teflon or silicone, or a combination thereof, placed on a copper rod. Liquid nitrogen is used to cool the copper rod, which is controlled by a thermocouple and a temperature controller.
[0060] Once the freezing process was complete, the frozen tin oxide green foam samples were removed from the mold and -2 Drying at -80 degrees Celsius for 48 hours in a freeze dryer at torr residual pressure was followed by heat treatment in two separate steps: the first treatment was carried out at 300 degrees Celsius for 3 hours to remove the binder, followed by sintering at 1150 degrees Celsius for 10 hours in a box furnace in the atmosphere.
[0061] Exemplary Embodiment 2: Preparation of Sensor Device
[0062] In order to prepare a highly sensitive gas sensor device, two platinum electrode plates and a ruthenium oxide heater are printed on a low temperature co-fired ceramic (LTCC) substrate. A ruthenium oxide (RuO2) heater layer is prepared by punching and filling with silver (Ag) paste, and then two platinum electrodes with a spacing of 200 microns are patterned using a lift-off process and a shadow mask. The gas sensitivity is then measured at 300 degrees Celsius at different ethanol gas concentrations of 20-60 parts per million. For carbon monoxide gas detection performance, the sensor response to low concentrations of 100-500 parts per million and high concentrations of 1000-5000 parts per million is measured at 200-300 degrees Celsius. During the measurement, the gas concentration is balanced and controlled by a mass flow controller (MFC), in which the gas is injected into the sensor chamber and the sensor resistance is continuously measured at a constant microangstrom.
[0063] Figures 1A to 1C The general sensing mechanism of n-type and p-type semiconductor sensors, and in particular the sensing mechanism of the exemplary tin oxide foam sensor proposed in this patent, is schematically illustrated.
[0064] FIG. 2A to FIG. 2B Figure 1 shows a representative tin oxide foam before and after sintering in air. The foam was 45 mm in diameter and 16 mm in height ( Figure 2A , left) is reduced to 31 mm diameter and 11 mm height ( Figure 2B , right), resulting in a volumetric shrinkage of 67%, which is approximately equal to 31% radial and height shrinkage. The sample maintained its integrity after sintering, with no cracking or warping. Therefore, the shrinkage is considered to be nearly isotropic, indicating that the residual stresses due to shrinkage are minimal.
[0065] Figure 3AX-ray diffraction patterns of four tin oxide foam samples heat treated for 10 hours at 1050 degrees Celsius, 1100 degrees Celsius, 1150 degrees Celsius and 1250 degrees Celsius are shown. There is no significant difference between the X-ray diffraction (XRD) peaks of the four foam samples, and they all show typical tin dioxide (SnO2) peaks.
[0066] Figure 3B The tin K-edge X-ray absorption near-edge structure spectrum of tin oxide foam heat-treated at 1150 degrees Celsius for 10 hours is shown compared with commercially available tin monoxide (SnO) and tin dioxide (SnO2) powders; and the three-dimensional X-ray photoelectron spectroscopy spectrum of tin oxide foam after sintering at 1150 degrees Celsius in air for 10 hours ( Figure 3C ) Investigation and three-dimensional metallic tin ( Figure 3D ).
[0067] By obtaining the Sn K-edge X-ray absorption near edge structure (XANES) spectrum ( Figure 3B ) and the absorption edge position of the foam was compared with the absorption edge position of commercial tin oxide (e.g., SnO and SnO2) powder to characterize the oxidation state of tin in the foam. The average tin valence in the foam sample was 3.36, indicating that the oxidation state of tin in the entire foam sample was mainly tin dioxide (SnO2).
[0068] Figure 3C X-ray photoelectron spectroscopy (XPS) measurements are shown for studying the chemical state of the tin oxide foam surface. Figure 3D The binding energy position of the Sn 3d peak is shown (for 3d 5 / 2 is 486.3 electron volts, and for 3d 3 / 2 is 494.7 electron volts), verifying that the foam surface is also composed of tin oxide (SnO).
[0069] 4A to 4H Scanning electron micrographs of radial cross sections and fracture surfaces of tin oxide foams sintered at different temperatures for 10 hours to produce a dual-pore structure are shown: ( Figure 4A and Figure 4E )1050 degrees Celsius, ( Figure 4B and Figure 4F )1100 degrees Celsius, ( Figure 4C and Figure 4G )1150 degrees Celsius and ( Figure 4D and Figure 4H) 1250 degrees Celsius. Top view image (e.g., FIG. 4A to FIG. 4D ) represent typical junctions during the sintering of metal oxide powders, and the arrows in the fracture surfaces (e.g., FIG. 4E to FIG. 4H ) represents secondary dendrites on the wall struts.
[0070] FIG. 5A to FIG. 5B The results show that the ethanol concentrations ( Figure 5A ) and carbon monoxide ( Figure 5B ) gas with different exposure times, and the change in resistance (gas sensitivity) of the tin oxide foams heat treated at 1150 degrees Celsius for 10 hours. The resistance change confirms that the tin oxide foam samples will operate significantly in gas sensing devices.
[0071] Figure 5A The change in resistance or sensitivity of a tin oxide foam sample relative to measurement time during exposure to ethanol gas at concentrations of 20-60 ppm is shown. The response of the tin oxide foam is a significant increase in resistance as the exposure to ethanol gas increases (e.g., Figure 5A , streaked columns), and the resistance returns to a stable value when the gas is replaced by pure air (e.g. Figure 5A , white column). The tin oxide foam shows a response of 13.1 (unitless) to 60 ppm of ethanol gas at 300 degrees Celsius, which is quite remarkable considering that no catalyst is added. Therefore, the tin oxide foam synthesized by the method embodied in this patent is suitable as an ethanol gas sensing material.
[0072] Figure 5B The change in resistance or sensitivity of the tin oxide foam relative to the measurement time during exposure to carbon monoxide gas at a concentration of 1000-5000 parts per million is shown. Without the addition of a catalyst, the tin oxide foam sensor shows a response value of 35.9 (unitless) at 5000 parts per million of carbon monoxide gas at 200 degrees Celsius. As the concentration of monoxide increases, the sensitivity increases almost linearly. Therefore, the tin oxide foam synthesized by the method embodied in this patent is suitable as a carbon monoxide gas sensing material.
[0073] FIG. 6A to FIG. 6B The sensing response of SnO foam was compared with that of NiO nanoparticles and SnO2 nanowires as a function of ethanol concentration at 300 °C ( Fig. 6A ), and compared with the sensing response of tin oxide thin film samples in carbon monoxide gas at different temperatures ( Figure 6B ). Compared with conventional tin oxide thin films, the tin oxide foam sample successfully detected substantially lower concentrations of carbon monoxide gas.
[0074] like Fig. 6A As shown, the three-dimensional tin oxide foam sensing material prepared as detailed in Examples 1 and 2 achieves higher sensitivity than other sensing materials that do not require additional catalysts. Specifically, Figure 6B It is shown that the three-dimensional tin oxide foam prepared as detailed in this patent detected extremely low concentrations of carbon monoxide gas, which cannot be achieved by conventional tin oxide films. Therefore, this is due to the unique three-dimensional porous tin oxide structure that allows toxic gases to diffuse easily through channel-like pores, and the surface area is increased by adjusting the main process parameters, such as sintering conditions and powder content. Therefore, the tuned pore structure in the tin oxide foam promotes gas diffusion by shortening the reaction path.
[0075] FIG. 7A to FIG. 7B The graph shows the change in resistance (gas sensitivity) of the tin oxide foam with 3.0 wt% palladium added as a catalyst compared with the resistance (gas sensitivity) of the tin oxide foam without palladium added for various carbon monoxide gas concentrations ( Fig. 7A ); and comparison of the sensitivity of tin oxide foams with and without palladium addition as a function of carbon monoxide gas concentration at 200 degrees Celsius ( Figure 7B ).
[0076] Adding a small amount of catalyst such as palladium, platinum or other catalysts does improve the sensitivity of metal oxide foam sensors. Fig. 7A A comparison of the resistance change (gas sensitivity) of tin oxide foam with and without the addition of 3.0 wt. % palladium as a catalyst for various carbon monoxide gas concentrations is shown. Figure 7B As shown in Figure 2, the sensitivity of the tin oxide foam sensor with palladium added is much higher than that of the tin oxide foam sensor without palladium added over the entire range of carbon monoxide gas concentrations at 200 degrees Celsius. In addition, the sensitivity of the tin oxide foam sensor with palladium is higher than that of the tin oxide foam sensor without palladium over the entire temperature range of 200 degrees Celsius to 300 degrees Celsius ( Figure 8 ).
[0077] Figure 8 A sensitivity comparison between tin oxide foams with and without palladium addition at different temperatures at a carbon monoxide gas concentration of 4500 parts per million (ppm) is shown. The palladium-added tin oxide foam exhibits a fairly high sensitivity in all temperature ranges between 200 degrees Celsius and 300 degrees Celsius.
[0078] FIG. 9A to FIG. 9B The resistance (gas sensitivity) of tin oxide foam with palladium as catalyst added in the presence of low concentration (from 100 ppm to 500 ppm) of carbon monoxide gas at 200 degrees Celsius is shown in Figure 2. Fig.9A ); and the sensitivity of palladium-doped tin oxide foam as a function of carbon monoxide gas concentration between 100 parts per million (ppm) and 500 ppm at 200 degrees Celsius ( Fig. 9B ).
[0079] Specifically, for carbon monoxide gas in the low concentration range, the addition of palladium is beneficial. Fig.9A The change in resistance (gas sensitivity) of tin oxide foam with palladium added as a catalyst under low concentration (e.g., 100 ppm to 500 ppm) of carbon monoxide gas at 200 degrees Celsius is shown. In this low concentration range of carbon monoxide gas, at 200 degrees Celsius, the sensitivity of the tin oxide foam with palladium added increases steadily with increasing carbon monoxide gas concentration between 100 ppm and 500 ppm.
[0080] FIG. 10A to FIG. 10C The change in electrical resistance (gas sensitivity) of copper oxide foam at carbon monoxide concentrations ranging from 1000 parts per million (ppm) to 5000 ppm at 300 degrees Celsius is shown. Fig. 10A ); and a schematic diagram of its operating mechanism ( Fig. 10B ); and the sensitivity (response) of the copper oxide foam as a function of carbon monoxide gas concentration between 1000 ppm and 5000 ppm at 300 degrees Celsius ( Fig. 10C ).
[0081] For the preparation of metal foam oxide gas sensor devices, not only tin oxide foam sensors are applicable, but also other metal oxide foam sensors can be applied. Fig. 10A shows the change in electrical resistance (gas sensitivity) of freeze-cast copper oxide foams at relatively low carbon monoxide concentrations of 1000 ppm to 5000 ppm at 300 degrees Celsius, and Fig. 10CIt is shown that at 300 degrees Celsius, with the increase of carbon monoxide gas concentration between 1000 parts per million and 5000 parts per million, the sensitivity of copper oxide foam increases steadily, confirming that the metal oxide sensor structure is beneficial to the use of its enhanced sensing surface area to detect toxic gases such as carbon monoxide. Here, freeze casting is used to prepare copper oxide foam. Copper oxide powder is mixed with polyvinyl alcohol in deionized water using stirring and ultrasonic treatment. The dispersed suspension is poured into a silicone mold located on a cooled copper rod, where the temperature is fixed at -10 degrees Celsius using liquid nitrogen and a heater. After the suspension is completely frozen, the frozen sample is vacuum sublimated in a desiccator at -88 degrees Celsius for 40 hours. Then before sintering, the green body is reduced from copper oxide (CuO) to copper in a hydrogen atmosphere. The reduction and sintering process is carried out in a tubular furnace under a hydrogen mixed gas with a pre-sintering of 250 degrees Celsius for 4 hours and a high-temperature sintering of 800 degrees Celsius for 14 hours.
[0082] FIG. 11A to FIG. 11G A schematic process flow for making a metal oxide foam gas sensor device is shown, where platinum electrodes and a ruthenium oxide heater are printed on a low temperature co-fired ceramic (LTCC) substrate before a silver paste is used to attach the metal oxide foam sensor on top of the heater and electrodes.
[0083] exist FIG. 11A to FIG. 11G An example of making a metal oxide sensor electrode device is described in , which shows a schematic process flow for making a metal oxide foam gas sensor electrode device, where platinum electrodes and ruthenium oxide heaters are printed on a LTCC substrate before the metal oxide foam sensor is attached to the heater and electrode contacts using silver paste. This sensor device is significantly smaller than, for example, Fig.12 The commercially available sensing module 1203 shown can directly replace existing sensing material components.
[0084] Fig.12 A tin oxide foam sensor device 1212 prepared as described in this patent is shown, which can directly replace an existing sensing module in a commercially available gas sensor product (eg, a carbon monoxide sensor product).
[0085] The description of the present invention is given for the purpose of illustration and description. It is not intended to be exhaustive or to limit the invention to the specific form described, and many modifications and variations are possible in light of the above teachings. The embodiments are selected and described in order to best explain the principles of the invention and its practical application. This description will enable others skilled in the art to best utilize and practice the invention in various embodiments with various modifications suitable for a particular use. The scope of the invention is defined by the following claims.
Claims
1. A gas sensor device, comprising: A metal oxide foam sensing material coupled to a platinum electrode and a ruthenium heater printed on a low temperature co-fired ceramic substrate via a silver paste, The metal oxide foam sensing material contains 0.1 wt % to 3 wt % of at least one of palladium, gold, silver or platinum catalysts. Wherein, the metal oxide foam sensing material is tin oxide SnO or SnO2, and Among them, the preparation method for forming porous metal oxide foam sensing materials is a freeze casting method, in which a water- or camphene-based oxide powder slurry is frozen and dried at low temperature to form a green body, and then sintered at high temperature to form a three-dimensionally connected solid porous structure.
2. A gas sensor device, comprising: A metal oxide foam sensing material coupled to a platinum electrode and a ruthenium heater printed on a low temperature co-fired ceramic substrate via a silver paste, The metal oxide foam sensing material contains 0.1 wt % to 3 wt % of at least one of palladium, gold, silver or platinum catalysts. Wherein, the metal oxide foam sensing material is tin oxide SnO or SnO2, and The metal oxide foam sensing material is prepared on the surface of the metal foam by at least one of thermal oxidation or anodizing processes, and the metal foam is prepared by freeze casting, wherein the metal of the metal foam is Sn.
3. The device according to claim 1 or 2, further comprising an electrode of an attached metal oxide foam sensor, wherein the electrode pattern comprises two electrode pads of a suitable metal having a separation of several hundred microns using a lift-off process and a shadow mask.
4. The device according to claim 3, wherein The suitable metal is platinum.
5. The device of claim 1 or 2, wherein the metal oxide foam has a porosity between 55% and 90% that reacts with a target toxic gas.
6. The device according to claim 5, wherein The target toxic gases are ethanol and carbon monoxide.
7. The device according to claim 2, wherein: The metal oxide foam sensing material is constructed in such a manner that a thin oxide layer is formed on the surface of the prepared metal foam.
8. The device according to claim 7, wherein The metal oxide foam sensing material is constructed in the form of a nano-needle-shaped oxide thin layer formed on the surface of the prepared metal foam.
9. The device according to claim 1, wherein A sintering agent in a composition range of 0.1 wt % to 3 wt % is added during the preparation of the metal oxide foam to aid densification by forming a liquid phase during sintering of the metal oxide green body.
10. The device according to claim 9, wherein The sintering agent is Li2O, CuO, MnO2, ZnO or La2O3.
11. A method for preparing a metal oxide foam, the method being performed using a freeze casting process, the method comprising: placing a rectangular insulating silicone mold on a copper block or an aluminum block immersed in liquid nitrogen, controlling the temperature using a thermocouple and a temperature controller, and pouring a metal oxide slurry containing at least one of deionized water, a dispersant, a binder, a metal or metal oxide powder, and a sintering agent into the mold; freezing the slurry so that dendritic ice crystals form and grow in the slurry and metal oxide particles aggregate between the growing ice crystals; The green metal oxide foam is formed by drying ice crystals of a frozen sample at a sufficiently low temperature between -10 degrees Celsius and -80 degrees Celsius and reduced pressure to leave pores in their original locations; forming a substantially complete three-dimensionally connected porous metal oxide foam by: sintering the green metal oxide foam at a sufficiently high temperature between 800 degrees Celsius and 1700 degrees Celsius in a controlled furnace under an air or argon atmosphere; as well as The metal oxide foam is machined into a rectangular or circular shape, and the metal oxide foam can be directly applied as a sensing material in a gas sensor having a ruthenium heater and a platinum electrode located below the ruthenium heater, wherein the metal oxide foam contains 0.1 wt % to 3 wt % of at least one of palladium, gold, silver or platinum catalysts, and Wherein, the metal oxide foam is tin oxide SnO or SnO2.
12. A method of preparing a metal oxide foam for a gas sensor, the method comprising a patterning process of attaching an electrode pad to the metal oxide foam in a suitable pattern, wherein the metal oxide foam is prepared according to the method of claim 11.
13. The method according to claim 12, wherein: The metal oxide foam was coupled via silver paste to platinum electrodes and ruthenium heaters printed on a low temperature co-fired ceramic substrate.