Alkoxylated resol type phenolic resin and preparation method thereof

Alkoxylated soluble phenolic resin was prepared by reacting phenol with p-alkylphenol in the presence of alkaline compounds and further processing with alcohol compounds, which solved the risk and resistance of endocrine disruptors of bisphenol A type epoxy resin. The problem of insufficient corrosion is achieved, and the excellent corrosion resistance and color characteristics of the bisphenol A-free epoxy resin coating film are achieved.

CN113646349BActive Publication Date: 2024-11-01KOLON INDUSTRIES INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202180002672.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-06
Filing Date
2021-03-05
Publication Date
2024-11-01
Estimated Expiration
2041-03-05

AI Technical Summary

Technical Problem

The existing endocrine disruptor risks and insufficient corrosion resistance of existing bisphenol A-type epoxy resins in coated films, especially when they come into contact with acidic liquids or hot liquids, which may cause bisphenol A to flow out, affecting the coated films. durability.

Method used

Alkoxylated soluble phenolic resin is prepared by reacting phenol with p-alkylphenol in the presence of alkaline compounds to form soluble phenolic resins, and further reacting with alcohol compounds to replace traditional m-cresol as the raw material. A coating film with excellent corrosion resistance and salt resistance is formed.

Benefits of technology

A coating film with bisphenol A type epoxy resin is realized, with excellent corrosion resistance, salt resistance and color characteristics, suitable for the inner surface coating of beverage cans and food cans, avoiding the risk of endocrine disruptors, and in Keep the initial color unchanged after long-term storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003281548780000021
    Figure BDA0003281548780000021
  • Figure BDA0003281548780000022
    Figure BDA0003281548780000022
  • Figure BDA0003281548780000031
    Figure BDA0003281548780000031
Patent Text Reader

Abstract

The present invention relates to a method for preparing an alkoxylated resol-type phenolic resin and an alkoxylated resol-type phenolic resin. The alkoxylated resol-type phenolic resin prepared by the method can prepare a coating film having excellent corrosion resistance, salt resistance and color characteristics, and a composition containing the alkoxylated resol-type phenolic resin as a curing agent can be suitably used as a varnish for coating the inside of a beverage can.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an alkoxylated soluble phenolic resin type phenolic resin and a preparation method thereof. Background Art

[0002] The inner surfaces of beverage cans and food cans are coated with a coating film that reduces corrosion of the cans caused by the beverages or foods contained therein. Since the coating film is usually deposited on the metal before the can is produced, the coating film needs to have sufficiently good workability to prevent the coating film from falling off the can during the production of the can and at the same time have excellent corrosion resistance and salt resistance after production.

[0003] A known example of a varnish for forming a coating film is a varnish containing a bisphenol A type epoxy resin as a main material and a phenolic resin as a curing agent. The varnish containing the bisphenol A type epoxy resin has high workability, high hydrothermal resistance, and high adhesion to metals.

[0004] However, the bisphenol A type epoxy resin may contain bisphenol A as an unreacted material in the production of the bisphenol A type epoxy resin, which is considered to have an effect of an endocrine disruptor and carries a risk of adversely affecting the brain of a living organism. In addition, when the coating film is cleaned with a detergent or comes into contact with an acidic liquid or a hot liquid, bisphenol A may flow out from a coating film formed of a varnish containing the bisphenol A type epoxy resin. Therefore, a varnish for a coating can that does not contain a bisphenol A type epoxy resin is required.

[0005] Examples of resins used as substitutes for bisphenol A type epoxy resins include acrylic resins containing hydroxyl groups, alkyd resins containing hydroxyl groups, and polyester resins containing hydroxyl groups. In addition, as for curing agents, technologies using alkylphenols including cresol, p-tert-butylphenol, and p-tert-octylphenol as bisphenol-free phenol curing agents applied to epoxy resins and polyester resins as raw materials are being actively developed.

[0006] The properties of the curing agent (phenolic resin) mixed with the coating material have a great influence on the performance of the coating material. The vast majority of conventional methods for preparing bisphenol-free phenolic curing agents include meta-cresol as a raw material. This is because when using meta-cresol, which is more reactive than other raw materials, a phenolic resin with excellent processability and metal adhesion can be easily manufactured. The phenolic resin prepared using the above-mentioned meta-cresol as a raw material is used as a curing agent for varnishes on the inner surface of coating cans, and therefore has excellent processability and metal adhesion. However, there is still a need for improved corrosion resistance and salt resistance of the coating film that is basically required for long-term storage of beverages or foods.

[0007] [Prior Technical Literature]

[0008] Japanese Patent Application Publication No. 2000-336304 Summary of the invention

[0009] Technical issues

[0010] An object of the present invention is to provide an alkoxylated resol type phenolic resin and a method for preparing the same, wherein when the alkoxylated resol type phenolic resin is used, a coating film having excellent corrosion resistance, salt resistance and color characteristics can be obtained. In addition, another object of the present invention is to provide a resin composition comprising the alkoxylated resol type phenolic resin and a varnish for coating the inner surface of a can, the varnish comprising the resin composition.

[0011] Technical Solution

[0012] According to one aspect of the present invention, there is provided a method for preparing an alkoxylated resol-type phenolic resin, the method comprising: (a) reacting a phenolic compound as a mixture of phenol and p-alkylphenol with an aldehyde compound in the presence of an alkaline compound to obtain a resol-type phenolic resin; and (b) reacting the resol-type phenolic resin with an alcohol compound to prepare an alkoxylated resol-type phenolic resin.

[0013] According to another aspect of the present invention, an alkoxylated resol-type phenolic resin is provided, comprising a repeating unit represented by Formula 1 and a repeating unit represented by Formula 2 and at least one group represented by Formula 3.

[0014] [Formula 1]

[0015]

[0016] In Formula 1, n is an integer of 1 to 10, R1 is hydrogen or a group represented by Formula 3, and R2 is hydrogen or a C1 to C2 alkyl group.

[0017] [Formula 3]

[0018]

[0019] In formula 3, R 5a and R 5b Each is independently hydrogen or C1 to C2 alkyl, and R6 is hydrogen or C1 to C20 alkyl.

[0020] [Formula 2]

[0021]

[0022] In Formula 2, m is an integer selected from 1 to 10, R3 is a C1 to C8 alkyl group, and R4 is hydrogen or a C1 to C2 alkyl group.

[0023] According to another aspect of the present invention, a resin composition comprising the alkoxylated resol-type phenolic resin is provided.

[0024] According to another aspect of the present invention, a varnish comprising the resin composition is provided.

[0025] Beneficial Effects

[0026] The method for preparing an alkoxylated resol-type phenolic resin according to the present invention enables the preparation of an alkoxylated resol-type phenolic resin which is a curing agent for forming a coating film having excellent corrosion resistance, salt resistance and color characteristics, and a composition containing the alkoxylated resol-type phenolic resin as a curing agent can be suitably used as a varnish which is, for example, a coating material for forming a corrosion-resistant coating. DETAILED DESCRIPTION

[0027] Hereinafter, several aspects and various embodiments of the present invention will now be described in detail.

[0028] The terms or languages ​​used herein should not be interpreted as limited to typical terms or terms defined in a dictionary, but are based on the principle that the inventor can define the terms by himself in an appropriate manner so that the present invention is best understood and thus best described to conform to the technical spirit of the present disclosure.

[0029] The terms used in this article are provided only to describe some of its embodiments, rather than to limit the present disclosure. It should be understood that the singular forms "a", "an" and "said" include plural references unless the context clearly indicates otherwise. It will be further understood that the terms "including" and / or "having" when used in the present invention specify the presence of stated features, integers, steps, operations, components, components, or combinations thereof, but do not exclude the presence or addition of one or more other features, integers, steps, operations, components, components, or combinations thereof.

[0030] Specifically, according to one aspect of the present invention, there is provided a method for preparing an alkoxylated resol-type phenolic resin, the method comprising: (a) reacting a phenolic compound as a mixture of phenol and p-alkylphenol with an aldehyde compound in the presence of an alkaline compound to obtain a resol-type phenolic resin; and (b) reacting the resol-type phenolic resin with an alcohol compound to prepare an alkoxylated resol-type phenolic resin.

[0031] Examples of the p-alkylphenol may include a compound having a structure in which a C1 to C8 alkyl group is substituted on the 4-th carbon atom of the benzene moiety of phenol.

[0032] For example, the p-alkylphenol may include p-cresol, p-ethylphenol, p-propylphenol, p-isopropylphenol, p-n-butylphenol, p-sec-butylphenol, p-tert-butylphenol, p-isobutylphenol, p-n-pentylphenol, p-tert-pentylphenol, p-neopentylphenol, p-isopentylphenol, p-sec-pentylphenol, p-3-pentylphenol, p-sec-isopentylphenol, p-n-hexylphenol, p-isohexylphenol, p-sec-hexylphenol, p-tert-hexylphenol, p-heptylphenol, p-isoheptylphenol, p-sec-heptylphenol, p-tert-heptylphenol, p-octylphenol, p-iso-octylphenol, p-sec-octylphenol, p-tert-octylphenol, or a mixture of at least two thereof.

[0033] According to one embodiment, the p-alkylphenol may be at least one selected from p-cresol, p-tert-butylphenol, p-ethylphenol, and p-tert-octylphenol.

[0034] According to another embodiment, the p-alkylphenol may be at least one selected from p-cresol, p-tert-butylphenol and p-tert-octylphenol. For example, the p-alkylphenol may be p-cresol.

[0035] Since m-cresol has excellent reactivity and thus can easily prepare a resol type phenolic resin, a conventional method includes m-cresol as an essential raw material in preparing a resol type phenolic resin. In the present invention, an alkoxylated resol type phenolic resin is successfully prepared using phenol and p-alkylphenol as raw materials instead of using m-cresol as a raw material, and more specifically, it has been confirmed that the alkoxylated resol type phenolic resin prepared using phenol and p-alkylphenol such as p-cresol as raw materials exhibits excellent corrosion resistance and salt resistance compared to a conventional alkoxylated resol type phenolic resin prepared using phenol and m-cresol as raw materials, thereby completing the present invention.

[0036] In step (a), phenol and p-alkylphenol may be reacted in a molar ratio of 1:1 to 1:10. For example, phenol and p-alkylphenol may be reacted in a molar ratio of 1:2 to 1:6 or in a molar ratio of 1:2 to 1:5. When the molar ratio of phenol to p-alkylphenol exceeds the range of 1:1 to 1:10, the compatibility with the alcohol compound may be insufficient. When the molar ratio of phenol to p-alkylphenol is higher than this range, the degree of alkoxylation may decrease as the molecular weight increases, and thus the corrosion resistance and salt resistance may be insufficient, which is not preferred.

[0037] The aldehyde compound may include at least one selected from paraformaldehyde, formaldehyde, and glyoxal. For example, the aldehyde compound may be paraformaldehyde.

[0038] In step (a), the phenolic compound and the aldehyde compound can react in a molar ratio of 1:1 to 1:10. For example, the phenolic compound and the aldehyde compound can react in a molar ratio of 1:1 to 1:5 or in a molar ratio of 1:3 to 1:5. When the molar ratio of the phenolic compound to the aldehyde compound exceeds the range of 1:1 to 1:10, the reaction cannot be carried out smoothly, which will cause the yield of the final product to be significantly reduced or the molecular structure required in the present invention will not be formed, so it is not preferred. In addition, when the molar ratio of the phenolic compound to the aldehyde compound exceeds the range of 1:3 to 1:5, due to the structural difference of the generated molecule, the alkoxy reaction as a subsequent process cannot be carried out smoothly, so the corrosion resistance, salt resistance and processability will deteriorate.

[0039] In step (a), examples of alkaline compounds may include metal ion catalysts, non-metal ion catalysts, or mixtures of metal ion catalysts and non-metal ion catalysts. The metal ion catalyst may be NaOH, KOH, Mg(OH)2, Ba(OH)2, or Ca(OH)2, and the non-metal ion catalyst may be NH4OH, N(CH2CH2OH)3, or N(CH2CH3)3.

[0040] According to one embodiment, the alkaline compound may include at least one compound selected from the group consisting of NaOH, KOH, Mg(OH)2, Ba(OH)2, Ca(OH)2, NH4OH, N(CH2CH2OH)3, and N(CH2CH3)3.

[0041] For example, the alkaline compound may include at least one compound selected from the group consisting of NaOH, Ba(OH)2, Ca(OH)2, Mg(OH)2, and KOH.

[0042] In step (a), the reaction may be carried out while maintaining a temperature of 50° C. to 70° C. for 2 to 5 hours and then maintaining a temperature of 75° C. to 90° C. for 5 to 10 hours, and the alkaline compound may be NaOH, and the alkaline compound may be added in an amount of 0.33 mol to 0.3 mol based on 1 mol of the phenolic compound.

[0043] According to one embodiment, in step (a), the reaction may be carried out while maintaining a temperature of 55°C to 65°C for 2 to 4 hours and then maintaining a temperature of 75°C to 85°C for 7 to 9 hours, and the alkaline compound may be NaOH, and the alkaline compound may be added in an amount of 0.05 mol to 0.2 mol based on 1 mol of the phenolic compound.

[0044] When the temperature range, time range, type and amount of the alkaline compound in step (a) are not satisfied, a resol-type phenolic resin having desired properties, for example, excellent corrosion resistance, salt resistance and processability cannot be obtained from the phenolic compound comprising phenol and p-alkylphenol.

[0045] In step (b), the alcohol compound used to replace the hydroxymethyl group of the resol-type phenolic resin with an alkoxy group may be at least one selected from n-butanol, isobutanol and n-pentanol.

[0046] For example, the alcohol compound may be n-butanol.

[0047] The amount of the alcohol compound may be in the range of 100 parts by weight to 500 parts by weight based on 100 parts by weight of the resol-type phenolic resin prepared in step (a).

[0048] For example, considering the reactivity between the resol type phenolic resin and the alcohol compound, the amount of the alcohol compound may be in the range of 200 parts by weight to 400 parts by weight.

[0049] According to one embodiment, the p-alkylphenol may be p-cresol, the aldehyde compound may be paraformaldehyde, the alkaline compound may be NaOH, and the alcohol compound may be n-butanol. Different from the conditions of other types of compounds, the advantage of using each of these types of compounds is that the degree of substitution of methylol groups by butoxy groups is easily controlled, and it has been confirmed that the alkoxylated resol-type phenolic resin prepared using the compounds exhibits excellent processability, corrosion resistance, and salt resistance.

[0050] In step (b), the reaction may be performed at a temperature of 90° C. to 150° C. for 10 to 36 hours. For example, the reaction may be performed at a temperature of 100° C. to 110° C. for 16 to 24 hours.

[0051] 50% to 100% of the methylol groups of the resol-type phenolic resin may be substituted with alkoxy groups. For example, 60% to 100%, 60% to 90%, or 70% to 90% of the methylol groups of the resol-type phenolic resin may be substituted with alkoxy groups. Here, the proportion of the methylol groups substituted with alkoxy groups is calculated based on the weight of the methylol groups. When the reaction of step (b) exceeds the temperature range of 90° C. to 150° C. and the time range of 10 hours to 36 hours, less than 50% of the methylol groups of the resol-type phenolic resin are substituted with alkoxy groups, and thus the tendency of graft polymerization of the alkoxylated resol-type phenolic resin prepared alone may increase, which may have the problem of reduced processability.

[0052] According to one embodiment, since 50% to 100% of the methylol groups of the resol type phenolic resin may be substituted with alkoxy groups, compatibility with the main material is improved by substitution within this range, and thus a coating film having excellent corrosion resistance and salt resistance may be formed.

[0053] Step (b) can be performed by controlling the pH to 3.0 to 4.5 in the presence of at least one acidic compound selected from formic acid, sulfuric acid and phosphoric acid. For example, step (b) can be performed by controlling the pH to 3.5 to 4.0 in the presence of formic acid.

[0054] The weight average molecular weight of the alkoxylated resol type phenolic resin may be in the range of 1000 g / mol to 3000 g / mol. For example, the weight average molecular weight of the alkoxylated resol type phenolic resin may be in the range of 1200 g / mol to 2500 g / mol or 1500 g / mol to 2000 g / mol. When the weight average molecular weight of the alkoxylated resol type phenolic resin is within these ranges, the alkoxylated resol type phenolic resin may have excellent processability, excellent compatibility with the main materials combined to form the coating film, and excellent curing properties.

[0055] Although not specifically described in the following Examples and Comparative Examples, in the method for preparing an alkoxylated resol-type phenolic resin according to the present invention, the characteristics of each alkoxylated resol-type phenolic resin prepared by changing the type of p-alkylphenol, the type of aldehyde compound, the molar ratio of phenol to p-alkylphenol, the molar ratio of phenolic compound to aldehyde compound, reaction temperature and time in step (a), the type of alkaline compound, the amount of alkaline compound added, reaction temperature and time in step (b), the degree of substitution of alkoxy groups of the resol-type phenolic resin, the pH of step (b) and the weight average molecular weight of the alkoxylated resol-type phenolic resin were analyzed and used to form a coating film on aluminum metal using the alkoxylated resol-type phenolic resin for performance analysis.

[0056] As a result, unlike other conditions and other numerical ranges, it has been confirmed that when all of the following conditions are satisfied, the compatibility of the alkoxylated resol type phenolic resin with the main material is improved, thereby having the effect of forming a coating film having excellent corrosion resistance and salt resistance. In addition, it has been confirmed that when the alkoxylated resol type phenolic resin is applied in a coating film for coating the inner surface of a can, excellent color characteristics such as easy realization of a desired color, maintenance of the initial color after long-term storage of the contents, and no blushing phenomenon are exhibited.

[0057] ① the p-alkylphenol is p-cresol, ② the aldehyde compound is paraformaldehyde, ③ the phenol in step (a) reacts with the p-alkylphenol in a molar ratio of 1:2 to 1:5, ④ the phenol compound in step (a) reacts with the aldehyde compound in a molar ratio of 1:3 to 1:5, ⑤ the step (a) is carried out by maintaining a temperature of 50°C to 70°C for 2 to 4 hours, and then maintaining a temperature of 75°C to 90°C for 7 to 9 hours, ⑥ the alkaline compound is NaOH, ⑦ the amount of the alkaline compound added is in the range of 0.05 mol to 0.2 mol based on 1 mol of the phenol compound, ⑧ the step (b) is carried out at a temperature of 100°C to 110°C for 16 to 24 hours, ⑨ the alcohol compound is n-butanol, ⑩ 80% to 90% of the hydroxymethyl groups of the resol type phenolic resin are substituted with alkoxy groups, Step (b) is carried out by controlling the pH to 3.5 to 4.0 in the presence of formic acid, The weight average molecular weight of the alkoxylated resol type phenolic resin is in the range of 1000 g / mol to 3000 g / mol.

[0058] When at least one of these conditions is not satisfied, it has been confirmed that there is a problem of reduced processability of the alkoxylated resol type phenolic resin due to an increased tendency of graft polymerization of only the alkoxylated resol type phenolic resin, and it has also been confirmed that the color characteristics of the alkoxylated resol type phenolic resin are deteriorated, such as a coating film formed using the alkoxylated resol type phenolic resin cannot maintain the initial color or exhibits a whitening phenomenon.

[0059] According to another aspect of the present invention, an alkoxylated resol-type phenolic resin is provided, comprising a repeating unit represented by Formula 1 and a repeating unit represented by Formula 2 and at least one group represented by Formula 3.

[0060] [Formula 1]

[0061]

[0062] In Formula 1, n is an integer of 1 to 10, R1 is hydrogen or a group represented by Formula 3, and R2 is hydrogen or a C1 to C2 alkyl group.

[0063] [Formula 3]

[0064]

[0065] In formula 3, R 5a and R 5b Each is independently hydrogen or C1 to C2 alkyl, and R6 is hydrogen or C1 to C20 alkyl.

[0066] [Formula 2]

[0067]

[0068] In Formula 2, m is an integer from 1 to 10, R3 is a C1 to C8 alkyl group, and R4 is hydrogen or a C1 to C2 alkyl group.

[0069] For example, in Formula 2, R3 may be a methyl group, an ethyl group, a tert-butyl group, or a tert-octyl group.

[0070] In Formulae 1 to 3, * represents a bonding site with an adjacent atom.

[0071] According to one embodiment, the alkoxylated resol-type phenolic resin may include at least one repeating unit represented by Formula 1, wherein R1 is represented by Formula 3.

[0072] As described with respect to the alkoxylated resol-type phenolic resin, an alkoxylated resol-type phenolic resin comprising a repeating unit derived from phenol (a repeating unit represented by Formula 1) and a repeating unit having a C1 to C8 alkyl group at the para position (a repeating unit represented by Formula 2) instead of using m-cresol as a raw material can exhibit excellent corrosion resistance and salt resistance, compared to an alkoxylated resol-type phenolic resin conventionally prepared by including m-cresol as a raw material.

[0073] The alkoxylated resol-type phenolic resin may further include a repeating unit represented by Formula 4 and a repeating unit represented by Formula 5.

[0074] [Formula 4]

[0075]

[0076] In Formula 4, n1 is an integer of 1 to 10, R7 is hydrogen or a group represented by Formula 3, and R8 and R9 are each independently hydrogen or a C1 to C2 alkyl group.

[0077] [Formula 3]

[0078]

[0079] In formula 3, R 5a and R 5b Each is independently hydrogen or C1 to C2 alkyl, and R6 is hydrogen or C1 to C20 alkyl.

[0080] The alkoxylated resol-type phenolic resin comprises at least one repeating unit represented by Formula 4, wherein R7 is represented by Formula 3.

[0081] [Formula 5]

[0082]

[0083] In Formula 5, m1 is an integer from 1 to 10, R 10 is a C1 to C8 alkyl group, R 11 and R 12 is hydrogen or C1 to C2 alkyl.

[0084] The repeating unit represented by Formula 1 and the repeating unit represented by Formula 2 refer to the repeating unit contained in the alkoxylated resol-type phenolic resin according to the present invention, and may also contain a typical resol-type phenolic resin structure having an ether group in the repeating unit represented by Formula 4 or Formula 5, regardless of the ratio of existence. This corresponds to the resultant formed by the reaction between phenol or p-alkylphenol as a monomer and an aldehyde compound to form a hydroxyalkyl group directly bonded to the benzene ring during the preparation process.

[0085] The repeating unit represented by Formula 1 may be a repeating unit represented by one or a combination of at least two selected from Formulae 1-1 to 1-3.

[0086] [Formula 1-1]

[0087]

[0088] [Formula 1-2]

[0089]

[0090] [Formula 1-3]

[0091]

[0092] In Formula 1-1 to Formula 1-3, n is an integer from 1 to 10,

[0093] R1 is hydrogen or a group represented by Formula 3, and

[0094] R2 is hydrogen or C1 to C2 alkyl.

[0095] [Formula 3]

[0096]

[0097] In formula 3, R 5a and R 5b are each independently hydrogen or C1 to C2 alkyl, and

[0098] R6 is hydrogen or C1 to C20 alkyl.

[0099] In addition, the repeating unit represented by Formula 2 may be a repeating unit represented by Formula 2-1.

[0100] [Formula 2-1]

[0101]

[0102] In formula 2-1, m is an integer from 1 to 10,

[0103] R3 is a C1 to C8 alkyl group, and

[0104] R4 is hydrogen or C1 to C2 alkyl.

[0105] Preferably, in Formula 2-1, R3 may be a methyl group, in which case p-cresol is used as a raw material, which is suitable for use as a varnish for forming a coating film exhibiting the most excellent corrosion resistance and salt resistance, such as a corrosion-resistant varnish. For example, the varnish may be a coating material for coating cans.

[0106] Among the benzene rings contained in the alkoxylated resol type phenolic resin, the ratio of the benzene rings to which the C1 to C8 alkyl group is not directly bonded to the benzene rings to the benzene rings to which the C1 to C8 alkyl group is directly bonded can be in the range of 1:1 to 1:10, for example, 1:2 to 1:6 or 1:2 to 1:5. Here, the ratio of the benzene rings to which the C1 to C8 alkyl group is not directly bonded corresponds to the molar number of the repeating unit represented by Formula 1 or Formula 4, and the ratio of the benzene rings to which the C1 to C8 alkyl group is directly bonded corresponds to the molar number of the repeating unit represented by Formula 2 or Formula 5. The ratios represent the ratios according to the number of benzene rings, respectively. The above ratios can be proportional to the molar ratio of phenol to para-alkylphenol used in the preparation process, and can be specifically analyzed and measured by NMR. The alkoxylated resol type phenolic resin having a ratio within these ranges can not only have excellent corrosion resistance and salt resistance, but also a coating film formed by a varnish containing the alkoxylated resol type phenolic resin can have excellent adhesion.

[0107] The total amount of alkoxy groups in the alkoxylated resol type phenolic resin may be in the range of 50% to 100% of the total amount of alkoxy groups and hydroxyalkyl groups in the alkoxylated resol type phenolic resin. Here, 100% of the total amount of alkoxy groups and hydroxyalkyl groups in the alkoxylated resol type phenolic resin means that the phenolic resin is completely alkoxylated. The amount of alkoxy groups and hydroxyalkyl groups refers to the number of functional groups present therein. The alkoxy groups are derived from the alcohol compound used for alkoxylation in step (b) of the above-mentioned preparation method. When the total amount of alkoxy groups is less than 50% of the total amount of alkoxy groups and hydroxyalkyl groups, the tendency of graft polymerization of the alkoxylated resol type phenolic resin alone increases, and thus there is a problem of reduced processability.

[0108] According to one embodiment, the total amount of alkoxy groups in the alkoxylated resol-type phenolic resin may be 80% to 90% of the alkoxy groups and hydroxyalkyl groups in the alkoxylated resol-type phenolic resin, and in this case, the compatibility with the main material of the resin composition containing the alkoxylated resol-type phenolic resin may be improved, thereby forming a coating film having excellent corrosion resistance and salt resistance.

[0109] The weight average molecular weight of the alkoxylated resol type phenolic resin may be in the range of 1000 g / mol to 3000 g / mol. For example, the weight average molecular weight of the alkoxylated resol type phenolic resin may be in the range of 1200 g / mol to 2500 g / mol or in the range of 1500 g / mol to 2000 g / mol. When the weight average molecular weight of the alkoxylated resol type phenolic resin is within these ranges, the alkoxylated resol type phenolic resin is preferred in terms of having excellent processability, excellent compatibility with the main material used in combination to form the coating film, and excellent curing properties.

[0110] According to one embodiment, in Formula 1, R2 is hydrogen; in Formula 2, R3 is methyl, and R4 is hydrogen; in Formula 3, R 5a and R 5b is hydrogen, and R6 is a C3 to C6 alkyl group; in the alkoxylated resol-type phenolic resin, the ratio of the benzene ring to which the C1 to C8 alkyl group is not directly bonded to the benzene ring to which the C1 to C8 alkyl group is directly bonded is in the range of 1:2 to 1:5; and the total amount of alkoxy groups in the alkoxylated resol-type phenolic resin may be 50% to 100% of the total amount of alkoxy groups and hydroxyalkyl groups in the alkoxylated resol-type phenolic resin. No peeling was observed on the adhesive tape using a coating material comprising an alkoxylated resol-type phenolic resin satisfying all these conditions in a Scribe-Grid test conducted according to ASTM B 571, and thus it was confirmed that the coating film had excellent adhesion. It was confirmed that a portion of the coating film prepared using a varnish comprising an alkoxylated resol-type phenolic resin not satisfying these conditions in the same test was observed on the adhesive tape. In addition, it has been confirmed that when the alkoxylated resol-type phenolic resin is applied in a coating film for coating the inner surface of a can, it has been confirmed to exhibit excellent color characteristics such as easy realization of a desired color, retention of the original color after long-term storage of the contents, and no blushing.

[0111] According to another aspect of the present invention, a resin composition comprising the alkoxylated resol type phenolic resin is provided. The alkoxylated resol type phenolic resin can be used as a curing agent for various resins, and can preferably be used in combination as a curing agent for epoxy resins or polyester resins. The resin composition combined as a curing agent for epoxy resins or polyester resins can be used as a varnish, for example, a varnish for coating the inner surface of a can, as will be described herein to prepare a coating film having excellent corrosion resistance and salt resistance.

[0112] The alkoxylated resol type phenolic resin may be present in an amount of 50 to 70 parts by weight based on the total weight of the resin composition. For example, the alkoxylated resol type phenolic resin may be present in an amount of 55 to 65 parts by weight based on the total weight of the resin composition.

[0113] According to another embodiment of the present invention, a varnish, or for example, a corrosion-resistant varnish, comprising the resin composition is provided.

[0114] According to one embodiment, a varnish including the resin composition may be used as a varnish for coating the inner surface of a can.

[0115] The varnish used to coat the interior surface of the can may also contain pigments, solvents or additives.

[0116] Examples of pigments include inorganic pigments and organic pigments. The inorganic pigment may be at least one selected from the following: chromates (chrome yellow and chrome vermilion), ferrocyanides (Prussian blue), sulfides (cadmium yellow and cadmium red), oxides (titanium oxide, red iron oxide, black iron, and zinc oxide), sulfates (barium sulfate and lead sulfate), silicates (dark blue and calcium silicate), carbonates (calcium carbonate and magnesium carbonate), phosphates (cobalt violet), metal powders (aluminum powder and bronze), and carbon (carbon black).

[0117] The organic pigment may be at least one selected from azo organic pigments (benzidine yellow, Hansa yellow, sulphur-resistant orange, permanent red F5R, carmine 6B, lake red C, Kraumoftar red and Kraumoftar yellow), and phthalocyanine organic pigments (phthalocyanine blue and phthalocyanine green).

[0118] Examples of the solvent include aromatic hydrocarbon solvents such as toluene, xylene, Solvesso #100 and Solvesso #150; aliphatic hydrocarbon solvents such as hexane, heptane, octane and decane; and ester solvents such as methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, amyl acetate, ethyl formate and butyl propionate. Other examples of the solvent include the following water-miscible organic solvents: alcohol solvents such as methanol, ethanol, propanol and butanol; ketone solvents such as acetone, methyl ethyl ketone and cyclohexanone; and glycol ether solvents such as ethylene glycol (mono, di) methyl ether, ethylene glycol (mono, di) ethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, monobutyl ether, diethylene glycol (mono, di) methyl ether, diethylene glycol (mono, di) ethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol (mono, di) methyl ether, propylene glycol (mono, di) methyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether and dipropylene glycol (mono, di) methyl ether.

[0119] Examples of the additives include various lubricants, defoamers, levelers, and lubricants. Other curing agents used as curing aids, such as melamine resins, benzoguanamine resins, and isocyanate resins, may also be used in combination with the above additives.

[0120] Hereinafter, the present invention will be described in more detail by way of examples. These examples are provided only to more specifically describe the present invention, and it will be apparent to those skilled in the art that the scope of the present invention is not limited to these examples.

[0121] Example 1: Preparation of Alkoxylated Resole-Type Phenolic Resin

[0122] In a four-necked flask equipped with a stirrer, a condenser and a thermometer, 339.92 g (3.14 mol) of p-cresol, 73.96 g (0.79 mol) of phenol, 385 g (11.79 mol) of 92% paraformaldehyde, 388.5 g (5.24 mol) of n-butanol and 50.27 g of a 50% NaOH aqueous solution were added. The resulting mixture was heated to 60° C. and reacted for 3 hours, then the temperature of the resulting product was raised to 80° C. and reacted until the weight-average molecular weight was 1500 g / mol to 1800 g / mol.

[0123] After the reaction was completed, 777g (10.48mol) of n-butanol was added to the reaction mixture. After the pH inside the system was controlled within the range of 3.5 to 4.0 using formic acid (pKa=3.8), the resulting mixture was reacted at 100°C to 110°C for 20 hours while removing the water produced during the reaction. After the reaction was completed, 800g of ion exchange water was added to the reaction mixture, and the reaction mixture was stirred at 80°C and then allowed to stand. The water layer separated at the bottom was removed. In order to reduce unreacted monomers, the separated water layer was washed with water more than three times. Subsequently, the solvent was removed under reduced pressure. Thus, an alkoxylated soluble phenolic resin type phenolic resin having a solid content of 58% to 62% in the n-butanol solution was obtained. The proportion (degree of alkoxylation) of hydroxymethyl substituted with butoxy contained in the alkoxylated soluble phenolic resin type phenolic resin was 84%. The weight average molecular weight of the alkoxylated resol type phenolic resin is in the range of 1500 g / mol to 1800 g / mol.

[0124] Example 2: Preparation of Alkoxylated Resole-Type Phenolic Resin

[0125] In a four-necked flask equipped with a stirrer, a condenser and a thermometer, 297.01 g (2.75 mol) of p-cresol, 110.94 g (1.18 mol) of phenol, 513.37 g (15.72 mol) of 92% paraformaldehyde, 388.5 g (5.24 mol) of n-butanol and 50.27 g of a 50% NaOH aqueous solution were added. The resulting mixture was heated to 60° C. and reacted for 3 hours, and then the temperature of the resultant was raised to 80° C. and reacted until the weight average molecular weight was 1800 g / mol to 2000 g / mol.

[0126] After the reaction was completed, 777g (10.48mol) of n-butanol was added to the reaction mixture. After the pH inside the system was controlled within the range of 3.5 to 4.0 using formic acid (pKa=3.8), the resulting mixture was reacted at 100°C to 110°C for 25 hours while removing the water produced during the reaction. After the reaction was completed, 800g of ion exchange water was added to the reaction mixture, and the reaction mixture was stirred at 80°C and then allowed to stand. The water layer separated at the bottom was removed. In order to reduce unreacted monomers, the separated water layer was washed with water more than three times. Subsequently, the solvent was removed under reduced pressure. Thus, an alkoxylated soluble phenolic resin type phenolic resin having a solid content of 58% to 62% in the n-butanol solution was obtained. The proportion (degree of alkoxylation) of hydroxymethyl substituted with butoxy contained in the alkoxylated soluble phenolic resin type phenolic resin is 75%. The weight average molecular weight of the alkoxylated resol type phenolic resin is in the range of 1800 g / mol to 2000 g / mol.

[0127] Example 3: Preparation of Alkoxylated Resole-Type Phenolic Resin

[0128] In a four-necked flask equipped with a stirrer, a condenser and a thermometer, 297.01 g (2.75 mol) of p-cresol, 110.94 g (1.18 mol) of phenol, 641.67 g (19.65 mol) of 92% paraformaldehyde, 388.5 g (5.24 mol) of n-butanol and 25.14 g of a 50% NaOH aqueous solution were added. The resulting mixture was heated to 60° C. and reacted for 3 hours, and then the temperature of the resultant was raised to 80° C. and reacted until the weight average molecular weight was 1800 g / mol to 2000 g / mol.

[0129] After the reaction was completed, 777g (10.48mol) of n-butanol was added to the reaction mixture. After the pH inside the system was controlled within the range of 3.5 to 4.0 using formic acid (pKa=3.8), the resulting mixture was reacted at 100°C to 110°C for 25 hours while removing the water produced during the reaction. After the reaction was completed, 800g of ion exchange water was added to the reaction mixture, and the reaction mixture was stirred at 80°C and then allowed to stand. The water layer separated at the bottom was removed. In order to reduce unreacted monomers, the separated water layer was washed with water more than three times. Subsequently, the solvent was removed under reduced pressure, and the solvent was removed. Thus, an alkoxylated soluble phenolic resin type phenolic resin having a solid content of 58% to 62% in the n-butanol solution was obtained. The proportion (degree of alkoxylation) of hydroxymethyl substituted with butoxy contained in the alkoxylated soluble phenolic resin type phenolic resin was 64%. The weight average molecular weight of the alkoxylated resol type phenolic resin is in the range of 1800 g / mol to 2000 g / mol.

[0130] Comparative Example 1: Preparation of Alkoxylated Resole-Type Phenolic Resin

[0131] An alkoxylated resol-type phenolic resin was prepared in the same manner as in Example 1, except that 85.43 g (0.79 mol) of m-cresol was used instead of 73.96 g (0.79 mol) of phenol. The ratio of methylol groups substituted with butoxy groups contained in the alkoxylated resol-type phenolic resin (degree of alkoxylation) was 82%. The weight average molecular weight of the alkoxylated resol-type phenolic resin was in the range of 1500 g / mol to 1800 g / mol.

[0132] Comparative Example 2: Preparation of Alkoxylated Resole-Type Phenolic Resin

[0133] An alkoxylated resol-type phenolic resin was prepared in the same manner as in Example 3, except that 127.60 g (1.18 mol) of m-cresol was used instead of 110.94 g (1.18 mol) of phenol. The ratio of methylol groups substituted with butoxy groups contained in the alkoxylated resol-type phenolic resin (degree of alkoxylation) was 65%. The weight average molecular weight of the alkoxylated resol-type phenolic resin was in the range of 1800 g / mol to 2000 g / mol.

[0134] Each phenolic resin prepared in Examples 1 to 3 and Comparative Examples 1 and 2 was used to prepare a varnish for a coating film in the following manner. Each varnish was applied to a tin-plated steel plate, followed by a baking treatment. The coating film was tested for workability, autoclave resistance, corrosion resistance, and salt resistance. The test method is as follows.

[0135] Experimental Example 1: Evaluation of coating film performance

[0136] Clear varnish for coating films

[0137] An epoxy resin or polyester resin, n-butanol and xylene were dissolved in a mixed solvent at a weight ratio of 0.6:1:1 to prepare an epoxy resin or polyester resin solution having a solid content of 30%. The epoxy resin or polyester resin solution was mixed with each of the phenolic resins obtained from Examples 1 to 3 and Comparative Examples 1 and 2, respectively, so that the weight ratio of the epoxy resin or polyester resin solution to the phenolic resin was 8 to 2 to obtain a sample varnish composition for a coating film.

[0138] Performance test methods for coating films

[0139] The sample varnishes prepared by the above method were respectively applied to a tin-plated steel plate having a thickness of 0.3 mm using a coating bar so that the thickness of the dry coating film on the steel plate was 5 μm to 7 μm, and the obtained coating film was printed at 205° C. for 10 minutes. Thereafter, the properties of the following coating films were measured, and the results are shown in Table 1.

[0140] (1) Workability: After each sample was treated with steam and high-temperature hydrothermal treatment at 125°C for 30 minutes, the adhesion of the film when the coating film was forcibly peeled off at its side was evaluated according to the following grades: good (◎), fair (○), poor (△).

[0141] (2) Autoclave resistance: After each sample was treated with steam and high-temperature hydrothermal treatment at 125°C for 30 minutes, the whitening state of the adhesive layer was observed with the naked eye and evaluated according to the following grades: good (◎), fair (○), poor (△).

[0142] (3) Corrosion resistance: After treating each sample with a copper sulfate aqueous solution for 3 hours, the state of the adhesive layer was observed with the naked eye and evaluated according to the following grades: good (◎), fair (○), poor (△).

[0143] (4) Corrosion resistance, salt resistance: After each sample was distilled in a 3% sodium chloride, 3% acetic acid and 0.1% cysteine ​​aqueous solution at 125°C for 30 minutes, the state of the adhesive layer was observed by naked eyes and evaluated according to the following grades: good (◎), fair (○), poor (△).

[0144] Table 1

[0145]

[0146] As shown in Table 1, when compared with Comparative Examples 1 and 2, it has been confirmed that the coating films using the alkoxylated resol type phenolic resin prepared in Examples 1 to 3 exhibit equal or superior levels of overall properties such as processability, autoclave resistance, corrosion resistance, and salt resistance.

[0147] From this result, it was confirmed that the properties of the coating film can be improved by using phenol instead of m-cresol as a raw material in the preparation of the alkoxylated resol type phenolic resin.

[0148] Therefore, the method for preparing an alkoxylated resol type phenolic resin according to the present invention can prepare an alkoxylated resol type phenolic resin, which is a curing agent and can form a coating film with excellent corrosion resistance, salt resistance and color characteristics.

[0149] The above embodiments and comparative examples are described herein to illustrate the present invention, and the present invention is not limited thereto. It will be appreciated by those skilled in the art that various modifications may be made without departing from the spirit of the present invention. Therefore, the scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing an alkoxylated resol-type phenolic resin, the method comprising: (a) reacting a phenol compound which is a mixture of phenol and p-alkylphenol with an aldehyde compound in the presence of a basic compound to obtain a resol type phenolic resin; as well as (b) reacting the resol-type phenolic resin with an alcohol compound to prepare an alkoxylated resol-type phenolic resin, Wherein, in step (a), the phenol and the p-alkylphenol are reacted in a molar ratio ranging from 0.79:3.14 to 1:

10.

2. The method of claim 1, wherein: The p-alkylphenol is at least one selected from p-cresol, p-tert-butylphenol, p-ethylphenol and p-tert-octylphenol.

3. The method of claim 1, wherein: The p-alkylphenol is p-cresol.

4. The method of claim 1, wherein: The aldehyde compound is at least one selected from paraformaldehyde, formaldehyde and glyoxal.

5. The method of claim 1, wherein: The alkaline compound is at least one selected from NaOH, Ba(OH)2, Ca(OH)2, Mg(OH)2, KOH, NH4OH, N(CH2CH2OH)3 and N(CH2CH3)3.

6. The method of claim 1, wherein: The alcohol compound is at least one selected from n-butanol, isobutanol and n-pentanol.

7. The method of claim 1, wherein The p-alkylphenol is p-cresol, The aldehyde compound is paraformaldehyde, The alkaline compound is NaOH, and The alcohol compound is n-butanol.

8. The method of claim 1, wherein: In step (a), the phenolic compound and the aldehyde compound are reacted in a molar ratio ranging from 1:1 to 1:

10.

9. The method of claim 1, wherein Step (a) is carried out by maintaining the temperature in the range of 50°C to 70°C for 2 hours to 5 hours, and then maintaining the temperature in the range of 75°C to 90°C for 5 hours to 10 hours, The alkaline compound is NaOH, and The basic compound is added in the range of 0.33 mol to 0.3 mol based on 1 mol of the phenol compound.

10. The method of claim 1, wherein: 50% to 100% of the methylol groups of the resol-type phenolic resin are substituted with alkoxy groups.

11. The method of claim 1, wherein The step (b) is performed by controlling the pH to be 3.0 to 4.5 in the presence of at least one acidic compound selected from the group consisting of formic acid, sulfuric acid and phosphoric acid.

12. The method of claim 1, wherein The p-alkylphenol is p-cresol, The aldehyde compound is paraformaldehyde, The phenol of step (a) reacts with the p-alkylphenol in a molar ratio ranging from 0.79:3.14 to 1:5, The phenolic compound of step (a) reacts with the aldehyde compound in a molar ratio ranging from 1:3 to 1:5, Step (a) is carried out by maintaining the temperature in the range of 50°C to 70°C for 2 hours to 4 hours, and then maintaining the temperature in the range of 75°C to 90°C for 7 hours to 9 hours, The alkaline compound is NaOH, The basic compound is added in the range of 0.05 mol to 0.2 mol based on 1 mol of the phenolic compound, Step (b) is carried out by maintaining the temperature in the range of 100° C. to 110° C. for 16 to 24 hours, The alcohol compound is n-butanol, 80% to 90% of the hydroxymethyl groups of the resol-type phenolic resin are substituted with alkoxy groups, Step (b) is carried out by controlling the pH to 3.5 to 4.0 in the presence of formic acid, and The weight average molecular weight of the alkoxylated resol type phenolic resin is in the range of 1000 g / mol to 3000 g / mol.

13. An alkoxylated resol-type phenolic resin comprising a repeating unit represented by Formula 1 and a repeating unit represented by Formula 2 and comprising at least one group represented by Formula 3, wherein: The repeating unit represented by Formula 1 and the repeating unit represented by Formula 2 are included in the alkoxylated resol-type phenolic resin in a ratio ranging from 0.79:3.14 to 1:10: [Formula 1] Wherein, in Formula 1, n is an integer selected from 1 to 10, R1 is hydrogen or a group represented by Formula 3, and R2 is hydrogen or C1 to C2 alkyl, [Formula 3] Among them, in formula 3, R 5a and R 5b are each independently hydrogen or C1 to C2 alkyl, and R6 is hydrogen or C1 to C20 alkyl, [Formula 2] Wherein, in Formula 2, m is an integer selected from 1 to 10, R3 is a C1 to C8 alkyl group, and R4 is hydrogen or C1 to C2 alkyl.

14. The alkoxylated resol-type phenolic resin according to claim 13, wherein In Formula 2, R3 is methyl, ethyl, tert-butyl, or tert-octyl.

15. The alkoxylated resol-type phenolic resin according to claim 13, wherein The total amount of alkoxy groups contained in the alkoxylated resol-type phenolic resin is 50% to 100% of the total amount of alkoxy groups and hydroxyalkyl groups contained in the alkoxylated resol-type phenolic resin.

16. The alkoxylated resol-type phenolic resin according to claim 13, wherein In Formula 1, R2 is hydrogen, In Formula 2, R3 is methyl, and R4 is hydrogen, In formula 3, R 5a and R 5b is hydrogen, and R6 is C3 to C6 alkyl, Among the benzene rings contained in the alkoxylated resol-type phenolic resin, a ratio of benzene rings not directly bonded to a C1 to C8 alkyl group to benzene rings directly bonded to a C1 to C8 alkyl group is in a range of 1:2 to 1:5, and The total amount of alkoxy groups contained in the alkoxylated resol-type phenolic resin is 50% to 100% of the total amount of alkoxy groups and hydroxyalkyl groups contained in the alkoxylated resol-type phenolic resin.

17. A resin composition comprising the alkoxylated resol-type phenolic resin according to any one of claims 13 to 16.

18. A varnish comprising the resin composition according to claim 17.

Citation Information

Cited By

  • Preparation method of phenolic resin with high curing speed

    CN120329499A