Composition
By using a graft copolymer with a polyvinyl alcohol structure as the cathode binder of lithium-ion secondary batteries, the problem of poor cycle capacity maintenance rate of lithium-ion secondary batteries at high temperatures is solved, achieving high energy density and high durability. Excellent battery performance.
Patent Information
- Application Number
- CN202080027207.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-04-07
AI Technical Summary
Existing lithium-ion secondary batteries have poor cycle capacity maintenance at high temperatures, making it difficult to meet the requirements for high energy density, high voltage, and high durability.
A graft copolymer with a polyvinyl alcohol structure is used as a binder for the positive electrode, and the first monomer and the second monomer are graft-copolymerized with the backbone polymer to form a composition with a glass transition temperature of 260K to 365K Within the range, the cycle capacity maintenance rate at high temperatures is improved.
It achieves excellent cycle capacity maintenance rate at high temperatures, improves the durability and stability of lithium-ion secondary batteries, and is suitable for applications in high-temperature environments.
Smart Images

Figure BDA0003292764170000201 
Figure BDA0003292764170000211
Abstract
Description
Technical Field
[0001] The invention relates to a composition, a positive electrode slurry and a battery. Background Art
[0002] In recent years, secondary batteries have been used as power sources for electronic devices such as laptops and mobile phones, and hybrid vehicles or electric vehicles that use secondary batteries as power sources are being developed to reduce environmental load. These power sources require secondary batteries with high energy density, high voltage, and high durability. Lithium-ion secondary batteries have attracted much attention as secondary batteries that can achieve high voltage and high energy density.
[0003] A lithium-ion secondary battery is composed of components including a positive electrode, a negative electrode, an electrolyte, and a separator. The positive electrode is composed of a positive electrode active material, a conductive auxiliary agent, a metal foil, and a binder (Patent Documents 1 to 3).
[0004] As a positive electrode binder for lithium ion secondary batteries, a binder (graft copolymer) having high binding properties and oxidation resistance and containing polyvinyl alcohol and polyacrylonitrile as main components has been disclosed (Patent Document 4).
[0005] Prior art literature
[0006] Patent Literature
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2013-98123
[0008] [Patent Document 2] Japanese Patent Application Publication No. 2013-84351
[0009] [Patent Document 3] Japanese Patent Application Laid-Open No. 6-172452
[0010] [Patent Document 4] International Publication No. 2015 / 053224 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] However, there is a further demand for the development of a binder composition that is excellent in the cycle capacity retention rate at high temperatures, and a positive electrode slurry and a secondary battery using the composition.
[0013] The present invention has been made in view of the above circumstances, and provides a composition that serves as a binder having an excellent cycle capacity retention rate at high temperatures, and a positive electrode slurry and a secondary battery using the composition.
[0014] Means of solving the problem
[0015] According to the present invention, a composition is provided, comprising a graft copolymer, characterized in that the graft copolymer comprises a backbone polymer and a plurality of branch polymers, the backbone polymer has a polyvinyl alcohol structure, the first monomer unit and the second monomer unit are respectively contained in at least any one of the plurality of branch polymers, the second monomer unit is different from the first monomer unit, and has a glass transition temperature of 260K to 365K.
[0016] The inventors of the present invention have conducted intensive research and discovered that a composition can be used as a positive electrode composition to form a binder with excellent cycle capacity maintenance rate at high temperatures, thereby completing the present invention. In the composition, a backbone polymer having a polyvinyl alcohol structure contains a graft copolymer having a structure in which a first monomer unit and a second monomer unit (different from the first monomer unit) are grafted copolymerized, and the glass transition temperature is within a specified range.
[0017] Various embodiments of the present invention are described below. The embodiments described below can be combined with each other.
[0018] Preferably, the composition further comprises a free polymer, the free polymer is not covalently bonded to the graft copolymer, and the free polymer is at least one selected from a polymer having a polyvinyl alcohol structure and a polymer having the first monomer unit and / or the second monomer unit.
[0019] Preferably, the first monomer unit is a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer unit.
[0020] Preferably, in the above composition, if the content of the polyvinyl alcohol structure in the above composition is C PVA The total content of the first monomer unit and the second monomer unit in the composition is C M mass %, then the mass ratio of the content of the polyvinyl alcohol structure to the total content of the polyvinyl alcohol structure, the first monomer unit and the second monomer unit (C PVA / (C M +C PVA )) is 0.05~0.7.
[0021] Preferably, if the content of the above-mentioned first monomer unit is PM1 mol % and the content of the above-mentioned second monomer unit is PM2 mol %, then the molar ratio of the molar amount of the above-mentioned first monomer unit contained in the above-mentioned composition to the total molar amount of the above-mentioned first monomer unit and the above-mentioned second monomer unit (PM1 / (PM1+PM2)) is 0.1 to 0.9.
[0022] Preferably, at least one of the plurality of branched polymers has a copolymerization structure of the first monomer unit and the second monomer unit.
[0023] Preferably, the average degree of polymerization of the polyvinyl alcohol structure in the above composition is 300-4000.
[0024] Preferably, the saponification degree of the polyvinyl alcohol structure in the above composition is 60 to 100 mol%.
[0025] Preferably, the grafting rate of the graft copolymer is 40 to 3000%.
[0026] According to another aspect of the present invention, there is provided a positive electrode slurry containing the above composition, a positive electrode active material, and a conductive auxiliary agent.
[0027] Preferably, the solid content of the composition is 1 to 20% by mass relative to the total solid content in the positive electrode slurry.
[0028] Preferably, the positive electrode active material comprises a material selected from LiNi X Mn (2-X) O4 (where 0<X<2), Li(Co X Ni Y Mn Z )O2 (where 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1), Li(Ni X Co Y Al Z )O2 (wherein 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1) is one or more.
[0029] Preferably, the conductive additive is at least one selected from the group consisting of (i) fibrous carbon, (ii) carbon black, and (iii) a carbon composite in which fibrous carbon and carbon black are linked to each other.
[0030] According to another aspect of the present invention, there is provided a positive electrode including a metal foil and a coating film of the positive electrode slurry formed on the metal foil.
[0031] According to another aspect of the present invention, there is provided a battery including the above-mentioned positive electrode.
[0032] According to another aspect of the present invention, there is provided an adhesive comprising the above composition.
[0033] Effects of the Invention
[0034] The present invention provides a composition having excellent cycle capacity retention rate at high temperature. DETAILED DESCRIPTION
[0035] The following describes the embodiments of the present invention. Various features described in the embodiments described below can be combined with each other. Furthermore, each feature independently establishes the invention.
[0036] 1. Composition
[0037] A composition according to one embodiment of the present invention is a composition containing a graft copolymer, and the graft copolymer is a composition having a main polymer and a plurality of branch polymers.
[0038] The graft copolymer involved in one embodiment of the present invention is synthesized by graft copolymerizing the first monomer and the second monomer with the backbone polymer. Here, the first monomer is a monomer different from the second monomer. The branched polymer generated by polymerization is grafted, i.e., covalently bonded to the backbone polymer. At this time, a polymer may be generated simultaneously as a free polymer, which is a polymer containing a backbone polymer that is not grafted or a polymer of the first monomer that is not grafted to the backbone polymer, i.e., not covalently bonded to the graft copolymer, and / or a polymer containing the second monomer. Therefore, the composition involved in one embodiment of the present invention is preferably substantially composed of branched copolymers and free polymers. In addition, monomers other than the first monomer and the second monomer may also be polymerized within the scope of not impairing the effect of the present invention.
[0039] The grafting rate of the graft copolymer is preferably 40 to 3000%, more preferably 300 to 1500%. From the viewpoint of solubility, the grafting rate is preferably within the above range. If the grafting rate is 40% or more, the solubility in NMP (N-methylpyrrolidone) will be improved, and if it is 3000% or less, the viscosity of the NMP solution will decrease, thereby improving the fluidity of the NMP solution.
[0040] 1-2. Backbone polymer
[0041] The backbone polymer has a polyvinyl alcohol structure. Here, the polyvinyl alcohol structure is, for example, a structure of polyvinyl alcohol synthesized by saponifying polyvinyl acetate obtained by polymerizing vinyl acetate monomers. Preferably, most of the backbone polymer is composed of the polyvinyl alcohol structure. More preferably, the backbone polymer is polyvinyl alcohol.
[0042] The average degree of polymerization of the polyvinyl alcohol structure in the composition is preferably 300 to 4000, more preferably 500 to 2000. If the average degree of polymerization is within the above range, the stability of the slurry is particularly high. In addition, from the viewpoint of solubility, adhesion and viscosity of the binder, the above range is also preferred. If the average degree of polymerization is above 300, the adhesion between the binder, the active material and the conductive aid is improved, and the durability is improved. In addition, if the average degree of polymerization is below 4000, the solubility is improved and the viscosity is reduced, so it is easy to manufacture the positive electrode slurry. The average degree of polymerization mentioned here is a value measured by the method of JIS K 6726.
[0043] The saponification degree of the polyvinyl alcohol structure in the composition is preferably 60 to 100 mol%, more preferably 80 to 100 mol%. When the saponification degree is within the above range, the stability of the slurry is particularly high. The saponification degree mentioned here is a value measured by the method of JIS K6726.
[0044] 1-3. Branched polymers
[0045] The first monomeric unit and the second monomeric unit are respectively at least contained in any one of the above-mentioned multiple branched polymers. That is, one of the multiple branched polymers only contains one of the first monomeric unit and the second monomeric unit, and may also contain both the first monomeric unit and the second monomeric unit. And, within the scope of not damaging the effect of the present invention, monomeric units other than the first monomeric unit and the second monomeric unit may also be included. Here, the first monomeric unit and the second monomeric unit are monomeric units derived from the first monomer and the second monomer for the synthesis of the graft copolymer, respectively. Preferably, at least one of the multiple branched polymers has a copolymerization structure of the first monomeric unit and the second monomeric unit. The branched polymer is preferably a copolymer substantially having the first monomeric unit and the second monomeric unit, and more preferably a copolymer consisting only of the first monomeric unit and the second monomeric unit.
[0046] 1-4. Free polymer
[0047] The composition involved in one embodiment of the present invention may also include free polymers. Free polymers are at least one selected from polymers having a polyvinyl alcohol structure and polymers having the first monomer unit and / or the second monomer unit. The polymer having a polyvinyl alcohol structure refers to a backbone polymer that is not primarily involved in graft copolymerization. Furthermore, the polymer having the first monomer unit and / or the second monomer unit refers to a homopolymer of the first monomer, a homopolymer of the second monomer, a copolymer comprising the first monomer and the second monomer, etc., which refers to not copolymerized with the graft copolymer (i.e., the backbone polymer).
[0048] Furthermore, within the scope of not impairing the effect of the present invention, a homopolymer of a monomer other than the first monomer unit and the second monomer unit and a copolymer of a monomer other than the first monomer unit and the second monomer unit may also be included. The free polymer is preferably a copolymer substantially containing the first monomer and the second monomer, and more preferably a copolymer consisting only of the first monomer and the second monomer.
[0049] In addition, the weight average molecular weight of the free polymer other than the backbone polymer in the free polymer, such as the homopolymer of the first monomer, the homopolymer of the second monomer, the copolymer containing the first monomer and the second monomer, is preferably 30,000 to 300,000, more preferably 40,000 to 200,000, and further preferably 50,000 to 150,000. From the viewpoint of suppressing the increase in viscosity and facilitating the manufacture of the positive electrode slurry, the weight average molecular weight of the free polymer other than the backbone polymer is preferably 300,000 or less, more preferably 200,000 or less, and further preferably 150,000 or less. The weight average molecular weight of the free polymer other than the backbone polymer can be obtained by GPC (gel permeation chromatography).
[0050] 1-5. The first monomer unit
[0051] The first monomer unit is a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer unit. The first monomer unit is more preferably a (meth)acrylonitrile monomer unit, and further preferably an acrylonitrile monomer unit.
[0052] That is, the first monomer used in synthesizing the graft copolymer is preferably (meth)acrylonitrile and / or (meth)acrylic acid, more preferably (meth)acrylonitrile, and further preferably acrylonitrile. Therefore, the first monomer unit has a structure derived from these monomer units.
[0053] 1-6. Second monomer unit
[0054] The second monomer unit is not particularly limited as long as it is a unit different from the first monomer unit, and examples thereof include alkoxy polyethylene glycol (meth)acrylates such as (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate, methoxy polyethylene glycol (meth)acrylate (poly: 23), methoxydipropylene glycol (meth)acrylate, and 3,6,9,12,15-pentaoxa-1-heptadecene; alkyl (meth)acrylates such as dodecyl (meth)acrylate and 2,2,3,3,3-pentafluoropropylene (meth)acrylate; and polyethylene glycol monovinyl ether (poly: 3). Among them, alkoxy polyethylene glycol (meth)acrylates are preferred.
[0055] 1-7. Content and characteristics
[0056] The content and properties of each component preferably satisfy the following requirements. When the content and properties of each component are within the following ranges, a positive electrode composition that serves as a binder having an excellent cycle capacity retention rate at high temperatures can be provided.
[0057] The glass transition temperature of the composition is 260K to 365K, preferably 280K to 350K, and more preferably 300K to 340K. By being within such a range, the cycle capacity maintenance rate at high temperature is excellent. The glass transition temperature is specifically, for example, 260, 265, 270, 275, 280, 285, 290, 295, 300, 305, 310, 315, 320, 325, 330, 335, 340, 345, 350, 355, 360, 365K, and can also be exemplified here in the range between any two numerical values. The glass transition mentioned here refers to the change that due to the temperature drop of a substance having fluidity at high temperature, its viscosity increases sharply within a certain temperature range, and loses fluidity to become an amorphous solid. The method for measuring the glass transition temperature is not particularly limited, and refers to the glass transition temperature calculated by thermogravimetry, differential scanning calorimetry, differential thermal analysis, and dynamic viscoelasticity determination. Among them, differential scanning calorimetry is preferred.
[0058] If the polyvinyl alcohol structure is included and the content of the polyvinyl alcohol structure in the composition is C PVA The total content of the first monomer unit and the second monomer unit in the composition is C M mass %, then the mass ratio of the content of the polyvinyl alcohol structure to the total content of the polyvinyl alcohol structure, the first monomer unit and the second monomer unit (C PVA / (C M +C PVA )) is preferably 0.05 to 0.7, more preferably 0.10 to 0.55. From the viewpoint of solubility, adhesion and viscosity of the binder, it is preferably within the above range. If it is 0.05 or more, the adhesion between the binder and the active material and the conductive aid will be improved, and the durability will be improved. If it is 0.7 or less, the solubility will be improved, and it is easy to become a uniform resin solution, so the manufacture of the positive electrode slurry becomes easy.
[0059] The ratio (C PVA / (C M +C PVA )) Specifically, it is 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, and 0.70, and the range between any two numerical values can also be exemplified here.
[0060] If the content of the first monomer unit in the composition is PM1 mol%, and the content of the second monomer unit is PM2 mol%, the molar ratio of the molar amount of the first monomer unit contained in the composition to the total molar amount of the first monomer unit and the second monomer unit (PM1 / (PM1+PM2)) is preferably 0.1 to 0.9, and more preferably 0.2 to 0.9. Within such a range, the cycle capacity maintenance rate at high temperature is excellent. Specifically, the ratio is, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, and 0.9, and may also be exemplified here in the range between any two values.
[0061] 1-8. Various measurement / calculation methods
[0062] (Total content of the first monomer unit and the second monomer unit)
[0063] The composition includes a PVA component, a first monomer component, and a second monomer component. The composition ratio (PVA / PM1 / PM2) in the composition can be obtained from the amount (g) of polymerization input, the polymerization rate of the first monomer and the second monomer. The polymerization rate (%) can be obtained by NMR.
[0064] If
[0065] A: The mass of the first monomer used for copolymerization (input amount)
[0066] B: Polymerization rate of the first monomer after reaction (%)
[0067] C: Mass of the second monomer used for copolymerization (input amount)
[0068] D: The polymerization rate of the second monomer after the reaction (%)
[0069] E: The mass of PVA used for polymerization (input amount)
[0070] The mass % of the total content of the first monomer unit and the second monomer unit in the composition can be calculated by the following formula (2): The amount of PVA added is calculated based on the "total content of the first monomer unit and the second monomer unit", which is regarded as the "content of the polyvinyl alcohol structure".
[0071] ((A×B / 100+C×D / 100) / (A×B / 100+C×D / 100+E))×100(%)···(2)
[0072] The mass % of the total content of the first monomer unit and the second monomer unit can be calculated from the integral ratio of NMR. Assuming that the integral value of each proton of polyvinyl alcohol is S PVAThe integral values of the protons of each of the first monomer and the second monomer are S1 and S2 respectively, and the total content of the first monomer unit and the second monomer unit can be calculated by the following formula (2-2).
[0073] ((S1+S2)×100) / (S PVA +S1+S2)···(2-2)
[0074] (Ratio of the first monomer unit to the second monomer unit)
[0075] The mass % of the first monomer in the total amount of the first monomer unit and the second monomer unit in the composition can be calculated from the following formula (3).
[0076] ((A×B / 100) / (A×B / 100+C×D / 100))×100(%)···(3)
[0077] Furthermore, the mass % of the first monomer in the total amount of the first monomer unit and the second monomer unit in the composition can be calculated from the following formula (3-2).
[0078] (S1×100) / (S1+S2)···(3-2)
[0079] (Grafting rate)
[0080] When a graft copolymer is generated (graft copolymerization), a homopolymer of the first monomer and the second monomer may be generated. Therefore, when a graft copolymer is generated, a process of separating the homopolymer from the graft copolymer is required. The homopolymer is soluble in dimethylformamide (hereinafter sometimes abbreviated as DMF), but PVA and the graft copolymer are not soluble in DMF. By utilizing this difference in solubility, the homopolymer can be separated by centrifugal separation or the like.
[0081] Here, if
[0082] F: mass of the component dissolved in DMF (g)
[0083] G: Mass of the composition used for the test (g)
[0084] H: the total content of the first monomer unit and the second monomer unit in the composition (mass %),
[0085] The grafting rate can be obtained by the following formula (4).
[0086] ((G-F) / (G×(100-H) / 100))×100···(4)
[0087] (Glass transition temperature)
[0088] In the specification, the glass transition point (Tg) is measured as follows.
[0089] The differential scanning calorimetry (DSC) measurement was performed in accordance with JIS K 7121: 1987. The intersection of the tangent line of the base line in the DSC curve and the tangent line at the position of the sharp drop in the endothermic region due to the glass transition was defined as Tg.
[0090] 1-9. Method for producing graft copolymer
[0091] The method for producing the graft copolymer according to one embodiment of the present invention is not particularly limited, but preferably comprises polymerizing polyvinyl acetate, saponifying polyvinyl alcohol, and then graft-copolymerizing the first monomer, the second monomer, and other monomers to the polyvinyl alcohol.
[0092] As a method for polymerizing polyvinyl acetate, any known method such as bulk polymerization and solution polymerization can be used.
[0093] Examples of the initiator used for the polymerization of polyvinyl acetate include azo initiators such as azobisisobutyronitrile and the like, and organic peroxides such as benzoyl peroxide and bis(4-tert-butylcyclohexyl)peroxydicarbonate.
[0094] The saponification reaction of polyvinyl acetate can be carried out, for example, by a method of carrying out saponification in an organic solvent in the presence of a saponification catalyst.
[0095] Examples of the organic solvent include methanol, ethanol, propanol, ethylene glycol, methyl acetate, ethyl acetate, acetone, methyl ethyl ketone, benzene, and toluene. One or more of these may be used. Among them, methanol is preferred.
[0096] Examples of the saponification catalyst include alkaline catalysts such as sodium hydroxide, potassium hydroxide, and sodium alkoxide; and acidic catalysts such as sulfuric acid and hydrochloric acid. Among them, sodium hydroxide is preferred from the viewpoint of the saponification rate.
[0097] As a method for graft-copolymerizing a monomer to polyvinyl alcohol, for example, a solution polymerization method is mentioned. As a solvent used for the solution polymerization method, dimethyl sulfoxide, N-methylpyrrolidone, etc. are mentioned.
[0098] As an initiator used for graft copolymerization, organic peroxides such as benzoyl peroxide, azo compounds such as azobisisobutyronitrile, potassium persulfate, ammonium persulfate, etc. can be used.
[0099] The graft copolymer according to one embodiment of the present invention may be dissolved in a solvent for use. Examples of the solvent include dimethyl sulfoxide and N-methylpyrrolidone. The composition and the positive electrode slurry described below may contain these solvents.
[0100] 1-10. Others
[0101] In the range that does not damage the effect of the present invention, the composition involved in one embodiment of the present invention may also include other components, such as resins, etc. As such resins, fluorine-based resins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, styrene-butadiene copolymers (styrene butadiene rubber, etc.) and (methyl) acrylic copolymers, etc., can be cited. Wherein, from the viewpoint of stability, fluorine-based resins are preferred. In fluorine-based resins, polyvinylidene fluoride is preferred.
[0102] 2. Cathode slurry
[0103] The positive electrode slurry according to one embodiment of the present invention contains the above-mentioned composition and has excellent stability. The positive electrode slurry according to one embodiment of the present invention contains the above-mentioned composition and has low viscosity. The positive electrode slurry according to one embodiment of the present invention contains the above-mentioned composition and can produce a positive electrode with excellent rate characteristics. The positive electrode slurry may contain the composition and a conductive additive, and may contain the composition, a positive electrode active material and a conductive additive.
[0104] The viscosity of the positive electrode slurry according to one embodiment of the present invention is preferably 350 mPa·s or less, and more preferably 300 mPa·s or less. The viscosity of the slurry was measured using a cone-plate type rotational viscometer according to the method of JIS Z 8803:2011 (measurement machine: MCR302 manufactured by Kitahama Seisakusho Co., Ltd., measurement temperature: 25°C, rotation speed: 1 s -1 ).
[0105] The solid content of the (binder) composition for a positive electrode in the slurry for a positive electrode according to one embodiment of the present invention is preferably 0.1 to 20% by mass, and more preferably 1 to 10% by mass.
[0106] 3. Lithium-ion secondary battery
[0107] As a battery involved in one embodiment of the present invention, a battery having a positive electrode is preferred. As a battery having a positive electrode, a secondary battery is preferred. As a secondary battery, it is preferred to be selected from one or more of a lithium ion secondary battery, a sodium ion secondary battery, a magnesium ion secondary battery, and a potassium ion secondary battery, and a lithium ion secondary battery is more preferred.
[0108] The positive electrode and the lithium ion secondary battery having the positive electrode according to one embodiment of the present invention can be prepared using the positive electrode slurry containing the above composition, and preferably contain the above positive electrode, negative electrode, separator and electrolyte solution (hereinafter sometimes referred to as electrolyte or electrolytic solution).
[0109] [positive electrode]
[0110] The positive electrode according to one embodiment of the present invention can be prepared by applying a positive electrode slurry containing a composition, a conductive aid, and a positive electrode active material as needed on a current collector such as aluminum foil, removing the solvent contained in the slurry by heating, and further pressing the current collector and the electrode mixture layer by rolling to make them close. That is, a positive electrode having a metal foil and a positive electrode slurry coating film formed on the metal foil is obtained.
[0111] As the current collector for the positive electrode, a metal foil is preferably used. As the metal foil for the positive electrode, aluminum foil is preferably used, and its thickness is preferably 5 to 30 μm from the viewpoint of processability.
[0112] [Conductive additive]
[0113] The conductive aid is preferably selected from at least one of (i) fibrous carbon, (ii) carbon black, and (iii) a carbon composite formed by interconnecting fibrous carbon and carbon black. Examples of fibrous carbon include vapor-grown carbon fibers, carbon nanotubes, and carbon nanofibers. Examples of carbon black include acetylene black, furnace black, and Ketjen black (registered trademark). These conductive aids may be used singly or in combination. Among them, from the viewpoint of improving the dispersibility of the conductive aid, it is preferably selected from at least one of acetylene black, carbon nanotubes, and carbon nanofibers.
[0114] In the positive electrode slurry according to one embodiment of the present invention, the solid content of the conductive auxiliary agent is preferably 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, relative to the total solid content in the positive electrode slurry.
[0115] [Positive electrode active material]
[0116] [Positive electrode active material]
[0117] Positive electrode active materials can be used as needed. Positive electrode active materials are preferably those that can reversibly absorb and release cations. Positive electrode active materials preferably contain a volume resistivity of 1×10 4 Ω·cm or more Mn lithium-containing composite oxide or lithium-containing polyanion compound. Examples include LiCoO2, LiMn2O4, LiNiO2, LiMPO4, Li2MSiO4, LiNi X Mn (2-X) O4、Li(Co X Ni Y Mn Z )O2、Li(Ni X Co Y Al Z )O2 or xLi2MnO3-(1-X)LiMO2, etc. Among them, LiNi X Mn(2-X) X in O4 satisfies the relation of 0 < X < 2, and Li(Co X Ni Y Mn Z )O2 or Li(Ni X Co Y Al Z )O2, X, Y, and Z in which satisfy the relation of X + Y + Z = 1, and also satisfy the relations of 0 < X < 1, 0 < Y < 1, 0 < Z < 1. x in xLi2MnO3-(1-x)LiMO2 satisfies the relation of 0 < x < 1. In addition, M in LiMPO4, Li2MSiO4, or xLi2MnO3-(1-x)LiMO2 is preferably at least one element selected from Fe, Co, Ni, and Mn.
[0118] Among the positive electrode active materials, those preferably selected from LiNi X Mn (2-X) O4 (where 0 < X < 2), Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1 and X + Y + Z = 1), Li(Ni X Co Y Al Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1 and X + Y + Z = 1) are one or more, and more preferably one or more selected from LiNi X Mn (2-X) O4 (where 0 < X < 2) and Li(Co X Ni Y Mn Z )O2 (where 0 < X < 1, 0 < Y < 1, 0 < Z < 1 and X + Y + Z = 1).
[0119] The slurry for positive electrode according to one embodiment of the present invention preferably has a solid content of the positive electrode active material of 50 to 99.8% by mass, more preferably 80 to 99.5% by mass, and most preferably 95 to 99.0% by mass, relative to the total solid content in the slurry for positive electrode.
[0120] [Negative electrode]
[0121] The negative electrode used in the lithium-ion secondary battery involved in one embodiment of the present invention is not particularly limited, and can be manufactured using a negative electrode slurry containing a negative electrode active material. The negative electrode can be manufactured, for example, using a negative electrode metal foil and a negative electrode slurry arranged on the metal foil. The negative electrode slurry preferably contains a negative electrode binder (negative electrode composition), a negative electrode active material, and the above-mentioned conductive aid. As a negative electrode binder, there is no particular limitation, for example, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene copolymers (styrene butadiene rubber, etc.) and acrylic copolymers can be used. As a negative electrode binder, a fluorine-based resin is preferred. As a fluorine-based resin, it is more preferred to be selected from one or more of polyvinylidene fluoride and polytetrafluoroethylene, and more preferably polyvinylidene fluoride.
[0122] Examples of negative electrode active materials used for the negative electrode include carbon materials such as graphite, polyacene, carbon nanotubes, and carbon nanofibers; alloy materials such as tin and silicon; or oxide materials such as tin oxide, silicon oxide, and lithium titanate. One or more of these materials may be used.
[0123] As the metal foil for the negative electrode, copper foil is preferably used, and its thickness is preferably 5 to 30 μm from the viewpoint of processability. The negative electrode can be produced using the negative electrode slurry and the negative electrode metal foil according to the above-mentioned method for producing the positive electrode.
[0124] [Diaphragm]
[0125] As for the separator, any material with sufficient strength such as an electrically insulating porous film, a net, a nonwoven fabric, or a fiber can be used. It is particularly suitable to use a separator that has low resistance to ion migration of the electrolyte and excellent solution retention. The material is not particularly limited, and examples include inorganic fibers such as glass fibers or organic fibers; synthetic resins such as polyethylene, polypropylene, polyester, polytetrafluoroethylene, polytetrafluoroethylene (Polyflon), or layered composites thereof. From the viewpoint of adhesion and stability, polyethylene, polypropylene, or layered composites thereof are preferred.
[0126] [Electrolytes]
[0127] As the electrolyte, any known lithium salt can be used, for example, LiClO4, LiBF4, LiBF6, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiB 10 Cl 10 , LiAlCl4, LiCl, LiBr, LiI, LiB(C2H5)4, LiCF3SO3, LiCH3SO3, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiC(CF3SO2)3, lithium lower fatty acid carboxylates, etc.
[0128] [Electrolyte]
[0129] The electrolyte solution for dissolving the above electrolyte is not particularly limited. Examples of the electrolyte solution include carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; lactones such as γ-butyrolactone; ethers such as trimethoxymethane, 1,2-dimethoxyethane, diethyl ether, 2-ethoxyethane, tetrahydrofuran, and 2-methyltetrahydrofuran; sulfoxides such as dimethyl sulfoxide; oxolanes such as 1,3-dioxolane and 4-methyl-1,3-dioxolane; nitrogen-containing compounds such as acetonitrile, nitromethane, and N-methyl-2-pyrrolidone; methyl formate, acetic acid, Esters such as methyl ester, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate and triester phosphate; inorganic acid esters such as sulfate, nitrate and hydrochloride; amides such as dimethylformamide and dimethylacetamide; glycol dimethyl ethers such as diethylene glycol dimethyl ether, triethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether; ketones such as acetone, diethyl ketone, methyl ethyl ketone and methyl isobutyl ketone; cyclopentane sulfones such as cyclopentane; oxazolidinones such as 3-methyl-2-oxazolidinone; and sultones such as 1,3-propane sultone, 4-butane sultone and naphthalene sultone. At least one selected from these electrolytes can be used.
[0130] Among the above-mentioned electrolytes and electrolyte solutions, LiPF6 is preferably dissolved in a carbonate electrolyte solution. The concentration of the electrolyte in the solution preferably varies depending on the electrode and electrolyte used, and is preferably 0.5 to 3 mol / L.
[0131] The use of the lithium ion secondary battery of the embodiment of the present invention is not particularly limited, and examples thereof include various fields such as digital cameras, video cameras, portable audio players, portable LCD TVs and other portable AV devices, notebook computers, smart phones, mobile computers and other mobile information terminals, portable game consoles, power tools, electric bicycles, hybrid vehicles, electric vehicles, and power storage systems.
[0132] The present embodiment can provide a composition that serves as a binder having an excellent cycle capacity retention rate at high temperatures, a positive electrode slurry using the composition, and a battery.
[0133] Example
[0134] The present invention will be further described in detail below by way of examples. In addition, these examples are all for illustration only and do not limit the content of the present invention.
[0135] [Example 1]
[0136] <Preparation of polyvinyl alcohol (PVA)>
[0137] 600 parts by mass of vinyl acetate and 400 parts by mass of methanol were added, and nitrogen was bubbled to deoxygenate. Then, 0.3 parts by mass of di(4-tert-butylcyclohexyl)peroxydicarbonate was added as a polymerization initiator, and polymerization was carried out at 60° C. for 4 hours. The solid content concentration of the polymerization solution at the time of polymerization termination was 48% by mass, and the polymerization rate of vinyl acetate determined from the solid content was 80%. Methanol vapor was blown into the obtained polymerization solution to remove unreacted vinyl acetate, and then the solution was diluted with methanol to a polyvinyl acetate concentration of 40% by mass.
[0138] To 1200 parts by mass of the diluted polyvinyl acetate solution, 20 parts by mass of a methanol solution of sodium hydroxide having a concentration of 10% by mass was added, and a saponification reaction was performed at 30° C. for 2 hours.
[0139] The saponified solution was neutralized with acetic acid, filtered, and dried at 100° C. for 2 hours to obtain PVA. Table 1 shows the average degree of polymerization and degree of saponification of the obtained PVA.
[0140] The average degree of polymerization and saponification degree of PVA were measured according to the method of JIS K6726.
[0141] <Preparation of Composition>
[0142] 1.65 parts by mass of the obtained PVA was added to 8.63 parts by mass of dimethyl sulfoxide, and dissolved by stirring at 60° C. for 2 hours. Separately, 2.72 parts by mass of acrylonitrile, 0.47 parts by mass of ethyl 2-(2-ethoxyethoxy)acrylate, and 0.45 parts by mass of ammonium persulfate dissolved in 1.51 parts by mass of dimethyl sulfoxide were added at 60° C., and graft copolymerization was performed while stirring at 60° C. Four hours after the start of polymerization, the polymerization was stopped by cooling to room temperature.
[0143] 100 parts by mass of the obtained reaction solution was dropped into 300 parts by mass of methanol to precipitate the composition. The polymer was separated by filtration and vacuum dried at room temperature for 2 hours and then at 80°C for 2 hours to obtain a composition (adhesive). The solid content was 9.76% by mass. 1 The polymerization ratio of acrylonitrile (first monomer) and (2-(2-ethoxy)ethoxy)ethyl acrylate (second monomer) was calculated by H-NMR and found to be 95%.
[0144] In the obtained composition, the mass % of the polyvinyl alcohol structure was 30 mass %, the mass % of the total content of the first monomer unit and the second monomer unit was 70 mass %, the grafting rate was 222%, and the weight average molecular weight of the free polymer other than the main polymer in the free polymer was 76200. These measurement methods will be described in the (total content of the first monomer unit and the second monomer unit), (grafting rate) and (weight average molecular weight) described later.
[0145] Table 1 shows the composition of the composition containing the obtained graft copolymer.
[0146] (Total content of the first monomer unit and the second monomer unit)
[0147] A: The mass of the first monomer used for copolymerization (input amount)
[0148] B: Polymerization rate of the first monomer after reaction (%)
[0149] C: Mass of the second monomer used for copolymerization (input amount)
[0150] D: The polymerization rate of the second monomer after the reaction (%)
[0151] E: the mass of PVA used for polymerization (input amount),
[0152] The mass % of the total content of the first monomer unit and the second monomer unit in the composition was calculated using the following formula (2).
[0153] ((A×B / 100+C×D / 100) / (A×B / 100+C×D / 100+E))×100(%)···(2)
[0154] Furthermore, the total content of the first monomer unit and the second monomer unit can be calculated based on the integral ratio of NMR. PVA The integrated values of each proton of the first monomer and the second monomer are S1 and S2 respectively, and the total content of the first monomer unit and the second monomer unit can be calculated by the following formula (2-2).
[0155] ((S1+S2)×100) / (S PVA +S1+S2)···(2-2)
[0156] (Ratio of the first monomer unit to the second monomer unit)
[0157] Furthermore, the mass % of the first monomer in the total amount of the first monomer unit and the second monomer unit in the composition can be calculated from the following formula (3).
[0158] ((A×B / 100) / (A×B / 100+C×D / 100))×100(%)···(3)
[0159] Furthermore, the mass % of the first monomer in the total amount of the first monomer unit and the second monomer unit in the composition can be calculated from the following formula (3-2).
[0160] S1*100 / (S1+S2)···(3-2)
[0161] (Grafting rate)
[0162] 1.00 g of the binder was weighed and added to 50 cc of special grade DMF (manufactured by Kokushin Kagaku Co., Ltd.), and stirred at 1000 rpm for 24 hours at 80°C. Then, the mixture was centrifuged at 10000 rpm for 30 minutes using a centrifuge manufactured by Kokusan Co., Ltd. (model: H2000B, rotor: H). After the filtrate (DMF soluble component) was carefully separated, the DMF insoluble component was vacuum dried at 100°C for 24 hours, and the grafting rate was calculated using the above formula (4).
[0163] (Weight average molecular weight of free polymer other than backbone polymer)
[0164] The filtrate (DMF soluble component) obtained during centrifugation was added to 1000 ml of methanol to obtain a precipitate. The precipitate was vacuum dried at 80° C. for 24 hours, and the weight average molecular weight in terms of standard polystyrene was measured by GPC. It should be noted that the GPC measurement was performed under the following conditions.
[0165] Column: 2 GPC LF-804, (Showa Denko K.K.) Used in series.
[0166] Column temperature: 40°C
[0167] Solvent: 20mM-LiBr / DMF
[0168] (Glass transition temperature)
[0169] About 5 mg of the obtained sample was used as a sample and DSC was measured (SEIKO Electronics EXSTAR 6000DSC-6200) according to JIS K 7121: 1987. The intersection of the tangent line of the base line and the tangent line of the steep drop position of the endothermic region due to the glass transition in the DSC curve was read as Tg.
[0170] <Preparation of slurry>
[0171] 5 parts by mass of the obtained binder was dissolved in 95 parts by mass of N-methylpyrrolidone (hereinafter referred to as NMP) to prepare a binder solution. In addition, 1 part by mass of acetylene black (Denka Black (registered trademark) "HS-100" manufactured by DENKA Corporation) and 1 part by mass of the binder solution in terms of solid content were stirred and mixed. After mixing, LiNi 0.5 Mn 1.5 O4: 98 parts by mass were stirred and mixed to obtain a slurry for a positive electrode.
[0172] <Production of positive electrode>
[0173] Use an automatic coating machine to coat aluminum foil with a thickness of 20 μm at a rate of 140 g / m 2 The prepared positive electrode slurry was applied and pre-dried at 105°C for 30 minutes. Then, a roller press was used to press at a linear pressure of 0.1 to 3.0 ton / cm to prepare a positive electrode plate with a thickness of 75 μm. The positive electrode plate was then cut into a width of 54 mm to produce a strip-shaped positive electrode plate. At the end of the positive electrode plate, an aluminum collector was ultrasonically welded, and then the positive electrode was dried at 105°C for 1 hour to completely remove volatile components such as residual solvents or adsorbed moisture.
[0174] <Production of negative electrode>
[0175] 96.6 parts by mass of graphite (Carbotron (registered trademark) P manufactured by KUREHA Co., Ltd.) as the negative electrode active material and 3.4 parts by mass of polyvinylidene fluoride (KF polymer (registered trademark) #1120 manufactured by KUREHA Co., Ltd.) as the binder were added in a solid content conversion, and an appropriate amount of NMP was added and stirred and mixed so that the total solid content was 50% by mass to obtain a negative electrode slurry.
[0176] On both sides of a 10 μm thick copper foil, an automatic coating machine was used to coat the copper foil at a temperature of 70 g / m 2 The prepared negative electrode slurry was applied to one side of the plate one by one in a manner and pre-dried at 105°C for 30 minutes. Next, a roller press was used to press the negative electrode plate at a linear pressure of 0.1 to 3.0 ton / cm to prepare a negative electrode plate with a thickness of 90 μm on both sides. The negative electrode plate was then cut into a width of 54 mm to produce a strip-shaped negative electrode plate. At the end of the negative electrode plate, a nickel collector was ultrasonically welded, and then dried at 105°C for 1 hour to completely remove volatile components such as residual solvents or adsorbed moisture to obtain a negative electrode.
[0177] <Manufacturing of lithium-ion secondary batteries>
[0178] The obtained positive electrode and negative electrode were combined, wound through a polyethylene microporous membrane diaphragm with a thickness of 25μm and a width of 60mm, and a spiral winding group was made, which was then inserted into the battery can. Next, 5ml of a non-aqueous electrolyte (ethylene carbonate / ethyl methyl carbonate = 30 / 70 (mass ratio) mixed solution) in which LiPF6 was dissolved at a concentration of 1mol / L was injected into the battery container, and the injection port was closed to make a cylindrical lithium secondary battery with a diameter of 18mm and a height of 65mm. For the produced lithium-ion secondary battery, the battery performance was evaluated by the following method.
[0179] (Cycle capacity maintenance rate after 50 cycles at 25°C)
[0180] At an ambient temperature of 25°C, constant current and constant voltage charging with a charging voltage of 5.00±0.02V and 1ItA, and constant current discharge with a discharge end voltage of 3.00±0.02V and 1ItA were performed. The charge and discharge cycles were repeated, and the ratio of the discharge capacity of the 50th cycle to the discharge capacity of the 1st cycle was calculated as the cycle capacity maintenance rate after 50 cycles at 25°C.
[0181] (Cycle capacity maintenance rate after 50 cycles at 45°C)
[0182] As a test at high temperature, constant current and constant voltage charging with a charging voltage of 5.00±0.02V and 1ItA, and constant current discharge with a discharge end voltage of 3.00±0.02V and 1ItA were performed at an ambient temperature of 45°C. The charging and discharging cycles were repeated, and the ratio of the discharge capacity of the 50th cycle to the discharge capacity of the 1st cycle was calculated as the cycle capacity maintenance rate after 50 cycles at 45°C.
[0183] (Decrease rate of cycle capacity maintenance rate due to temperature rise)
[0184] As an index of the cycle capacity maintenance rate at high temperature, the change of the "cycle capacity maintenance rate after 50 cycles at 45°C" relative to the "cycle capacity maintenance rate after 50 cycles at 25°C" is measured as the decrease rate of the cycle capacity maintenance rate due to the temperature rise. The decrease rate is calculated by the following formula (5).
[0185] Decrease rate of cycle capacity maintenance rate due to temperature rise (%)
[0186] =((cycle capacity maintenance rate after 50 cycles at 45°C) / (cycle capacity maintenance rate after 50 cycles at 25°C))×100···(5)
[0187] [Examples 2 to 12 & Comparative Examples 1 to 6]
[0188] Using the average degree of polymerization, saponification degree, and content of PVA shown in Tables 1 to 2; the type and content of the first monomer unit; and the type and content of the second monomer unit, a composition having the composition and physical properties shown in Tables 1 to 2 was obtained by the same method as in Example 1.
[0189] In addition, the abbreviations used in the following tables and the like represent the following compounds. The monomer unit represents a monomer from which the monomer unit is derived.
[0190] AN: Acrylonitrile
[0191] AA: Acrylic acid
[0192] EEA: 2-(2-ethoxyethoxy)ethyl acrylate
[0193] PPA: 2,2,3,3,3-pentafluoropropyl acrylate
[0194] DA: Dodecyl acrylate
[0195] MMA: Methyl Methacrylate
[0196] VA: Vinyl acetate
[0197] ST: Styrene
[0198] PVA: Polyvinyl alcohol
[0199] [Table 1]
[0200]
[0201] [Table 2]
[0202]
Claims
1. A composition comprising a graft copolymer, characterized in that: The graft copolymer has a main polymer and a plurality of branch polymers. The backbone polymer has a polyvinyl alcohol structure, The first monomer unit and the second monomer unit each contain at least one of the plurality of branched polymers. The second monomer unit is different from the first monomer unit, The glass transition temperature of the composition is 260K to 365K, The first monomer unit is a (meth)acrylonitrile monomer unit and / or a (meth)acrylic acid monomer unit, The second monomer unit is one or more selected from the group consisting of (2-(2-ethoxy)ethoxy)ethyl (meth)acrylate and 2,2,3,3,3-pentafluoropropyl (meth)acrylate, In the composition, if the content of the polyvinyl alcohol structure in the composition is C PVA % by mass, and the total content of the first monomer unit and the second monomer unit in the composition is C M quality%, The mass ratio of the content of the polyvinyl alcohol structure to the total content of the polyvinyl alcohol structure, the first monomer unit and the second monomer unit, i.e., C PVA / (C M +C PVA ) is 0.10~0.30, In the composition, if the content of the first monomer unit in the composition is PM1 mol%, and the content of the second monomer unit is PM2 mol%, The molar ratio of the molar amount of the first monomer unit contained in the composition to the total molar amount of the first monomer unit and the second monomer unit, ie, PM1 / (PM1+PM2), is 0.3 to 0.
8.
2. The composition according to claim 1, characterized in that The composition further comprises free polymer, The free polymer has no covalent bond with the graft copolymer, The free polymer is at least one selected from a polymer having a polyvinyl alcohol structure and a polymer having a first monomer unit and / or a second monomer unit.
3. The composition according to claim 1 or 2, characterized in that At least one of the plurality of branched polymers has a copolymerization structure of the first monomer unit and the second monomer unit.
4. The composition according to claim 1 or 2, characterized in that The average polymerization degree of the polyvinyl alcohol structure in the composition is 300 to 4000.
5. The composition according to claim 1 or 2, characterized in that The saponification degree of the polyvinyl alcohol structure in the composition is 60 to 100 mol %.
6. The composition according to claim 1 or 2, characterized in that The grafting rate of the graft copolymer is 40 to 3000%.
7. A positive electrode slurry, characterized in that: The invention comprises the composition according to any one of claims 1 to 6, a positive electrode active material and a conductive auxiliary agent.
8. The positive electrode slurry according to claim 7, characterized in that: The solid content of the composition is 1 to 20% by mass relative to the total solid content in the positive electrode slurry.
9. The positive electrode slurry according to claim 7 or 8, characterized in that: The positive electrode active material comprises one or more selected from the following compounds: LiNi X Mn (2-X) O4, where 0<X<2; Li(Co X Ni Y Mn Z )O2, where 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1; Li(Ni X Co Y Al Z )O2, where 0<X<1, 0<Y<1, 0<Z<1, and X+Y+Z=1.
10. The positive electrode slurry according to claim 7 or 8, characterized in that: The conductive additive is at least one selected from the group consisting of (i) fibrous carbon, (ii) carbon black, and (iii) a carbon composite in which fibrous carbon and carbon black are linked to each other.
11. A positive electrode, characterized in that: A positive electrode slurry according to any one of claims 7 to 10 formed on a metal foil.
12. A battery, characterized in that: A positive electrode according to claim 11 is provided.
13. An adhesive, characterized in that: A composition comprising the composition according to any one of claims 1 to 6.
Citation Information
Patent Citations
Vinylidene fluoride-based copolymer
JP1994172452A
Composite particle for electrochemical device electrode, electrochemical device electrode material, and electrochemical device electrode
JP2013084351A
Binder composition for electrode, slurry for electrode, electrode, and energy storage device
JP2013098123A
Cathode binder composition, cathode slurry, cathode, and lithium ion secondary battery
WO2015053224A1
Composition and positive-electrode binder composition
WO2018230599A1