Lithium secondary battery
By using lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide with a particle size of 3 μm or more, and adjusting the ratio of negative electrode capacity to positive electrode capacity, the cycle characteristics and expansion problems of lithium secondary batteries at high voltage and high temperature are solved. Excellent battery performance and energy density are achieved.
Patent Information
- Application Number
- CN202080006640.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-07
- Filing Date
- 2020-03-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-06
AI Technical Summary
Existing lithium secondary batteries have problems with rapid decline in cycle characteristics and expansion under high voltage and high temperature conditions. Especially when using a mixture of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide, side reactions are aggravated, leading to battery performance degradation. .
Use lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide with an average particle size of more than 3 μm as the positive electrode active material, and design the ratio of negative electrode capacity to positive electrode capacity in the range of 1.06 to 1.15 to reduce contact with the electrolyte solution area and side reactions to improve structural stability.
It achieves the excellent cycle characteristics and expansion characteristics of lithium secondary batteries under high voltage, extends the service life of the battery and increases the energy density, and significantly improves the battery performance under high temperature and high voltage.
Smart Images

Figure CN113678286B_ABST
Abstract
Description
[0001] Cross - reference to related applications
[0002] This application claims the priority of Korean Patent Application No. 10 - 2019 - 0026395, filed on March 7, 2019, the disclosure of which is incorporated herein by reference. Technical field
[0003] The present invention relates to a lithium secondary battery having excellent life characteristics and swelling characteristics at high voltages. Background art
[0004] With the development of technology and the increasing demand for mobile devices, the demand for secondary batteries as an energy source has increased significantly. Among these secondary batteries, lithium secondary batteries having high energy density, high voltage, long cycle life, and low self - discharge rate have been commercialized and widely used.
[0005] Recently, the demand for high - capacity batteries has tended to increase more and more. Therefore, lithium secondary batteries operating at high voltages (e.g., above 4.3 V) capable of increasing battery capacity have been actively researched and developed.
[0006] Various lithium transition metal oxides such as LiCoO2 and LiNi 1-n-m Co n Mn m O2 (0 < n < 1, 0 < m < 1) are used as the positive electrode active material of the lithium secondary battery.
[0007] LiNi 1-n-m Co n Mn m The advantage of LiNiCoMnO2 is that it can achieve relatively high capacity characteristics. However, since side reactions occur at high voltages above 4.2 V, there are limitations in that the battery performance rapidly deteriorates and swelling occurs.
[0008] The advantage of LiCoO2 is that it exhibits excellent cycle characteristics even at high voltages. However, since the remaining amount of charge and discharge is low, there are limitations in that the capacity characteristics are poor.
[0009] To solve the above limitations, attempts have been made to use a mixture of two or more different lithium transition metal oxides as the positive electrode material. However, in the case of mixing lithium transition metal oxides having different compositions, new problems that do not occur when using one type of lithium transition metal oxide may occur. For example, for a secondary battery using a mixed positive electrode material of LiNiCoMnO2 and LiCoO2, the following phenomenon occurs: during the charge - discharge process, the positive electrode potential is higher than that when only using LiNi 1-n-m Co n Mn m O2 and LiCoO2 mixed positive electrode material, the following phenomena will occur: during the charge - discharge process, the positive electrode potential is higher than that when only using LiNi1-n-m Co n Mn m The secondary battery of O2 or LiCoO2 is degraded more, and as a result, the following problems occur: the battery performance is rapidly degraded while a side reaction occurs under high temperature and / or high voltage conditions. Summary of the invention
[0010] [Technical issues]
[0011] One aspect of the present invention provides a lithium secondary battery having excellent cycle characteristics and expansion characteristics even during high temperature and / or high voltage operation.
[0012] [Technical solution]
[0013] According to one aspect of the present invention, a lithium secondary battery is provided, comprising: a positive electrode, the positive electrode comprising a positive electrode active material layer containing a lithium nickel cobalt manganese-based oxide and a lithium cobalt-based oxide; a negative electrode, the negative electrode comprising a negative electrode active material layer containing a negative electrode active material; and an electrolyte, wherein the average particle size of the primary particles of the lithium nickel cobalt manganese-based oxide is greater than 3 μm, and the ratio of the negative electrode capacity to the positive electrode capacity is 1.06 to 1.15.
[0014] [Beneficial Effects]
[0015] By using a mixture of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide as a positive electrode active material, the lithium secondary battery of the present invention has a wide operating voltage range, and as a result, high energy density and high capacity characteristics can be achieved.
[0016] In addition, in the lithium secondary battery of the present invention, since large particles with a primary particle diameter of 3 μm or more are used as lithium nickel cobalt manganese-based oxide, the contact area with the electrolyte solution is smaller than that of the conventional lithium nickel cobalt manganese-based oxide commonly used, thereby minimizing the side reaction with the electrolyte solution, thereby effectively suppressing the capacity drop and expansion during high voltage operation.
[0017] In addition, since the lithium secondary battery of the present invention is designed so that the capacity ratio of the negative electrode to the positive electrode satisfies a specific range, the problem occurring in secondary batteries using conventional mixed positive electrode materials of lithium nickel cobalt manganese-based oxides and lithium cobalt-based oxides, namely, the rapid deterioration of battery characteristics under high temperature and / or high voltage conditions, can be effectively suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a scanning electron microscope (SEM) image of the lithium nickel cobalt manganese-based oxide powder prepared in Preparation Example 1;
[0019] Figure 2 is a SEM image of the lithium nickel cobalt manganese-based oxide powder prepared in Preparation Example 2;
[0020] Figure 3 is a SEM image of the lithium nickel cobalt manganese-based oxide powder prepared in Preparation Example 3;
[0021] Figure 4 are graphs showing high voltage life characteristics and expansion characteristics of lithium secondary batteries of Examples 1 to 5 and Comparative Examples 3, 4, and 6; and
[0022] Figure 5 Graphs showing high voltage life characteristics and expansion characteristics of the lithium secondary batteries of Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0023] It will be understood that the words or terms used in the specification and claims should not be interpreted as the meanings defined in commonly used dictionaries, and it will also be understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best explain the present invention, the words or terms should be understood to have meanings consistent with their meanings in the context of the relevant technology and the technical idea of the present invention.
[0024] The expression "average particle size (D 50 The average particle size (D) can be defined as the particle size at which the cumulative volume is 50% in the particle size distribution curve, and the average particle size (D 50 ) can be measured using a laser diffraction method. Specifically, after the target particles are dispersed in a dispersion medium, the dispersion medium is introduced into a commercially available laser diffraction particle size measuring instrument (e.g., Microtrac MT3000), irradiated with ultrasonic waves having a frequency of about 28 kHz and an output of 60 W, and then the average particle size (D ) at a cumulative volume of 50% is calculated by the measuring instrument. 50 ).
[0025] In this specification, the expression "ratio of the negative electrode capacity to the positive electrode capacity" means a value obtained by dividing the theoretical discharge capacity per unit area of the negative electrode by the theoretical discharge capacity per unit area of the positive electrode.
[0026] Furthermore, in this specification, unless otherwise specified, the expression "%" means weight %. DETAILED DESCRIPTION
[0028] Hereinafter, the present invention will be described in more detail.
[0029] The lithium secondary battery of the present invention comprises: a positive electrode including a positive electrode active material layer, a negative electrode including a negative electrode active material layer, and an electrolyte, wherein the positive electrode active material layer contains primary particles having an average particle size D 50 Lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide with a particle size of 3 μm or more are used as positive electrode active materials, and the ratio of negative electrode capacity to positive electrode capacity is 1.06 to 1.15.
[0030] For secondary batteries that usually use only lithium nickel cobalt manganese-based oxide as a positive electrode active material, there is a limitation that the battery characteristics cannot be operated at a high voltage because side reactions occur at voltages above 4.20V, which rapidly reduce the battery characteristics. For secondary batteries that use only lithium cobalt-based oxide as a positive electrode active material, high voltage operation is feasible, but there is a limitation of poor capacity characteristics. In order to solve the above limitations, secondary batteries using a mixture of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide have been proposed, but these conventional secondary batteries use powders in the form of secondary particles (in which a plurality of primary particles with a particle size of about 0.1 μm to about 1 μm are agglomerated) as lithium nickel cobalt manganese-based oxide. In the case of using lithium nickel cobalt manganese-based oxide secondary particles formed by the agglomeration of primary particles with a small average particle size as described above, due to the side reactions with the electrolyte solution due to the high specific surface area and the cracking phenomenon (the pores between the primary particles are opened during charging and discharging), even if lithium nickel cobalt manganese-based oxide is used together with lithium cobalt-based oxide, the cycle characteristics will rapidly decrease at high voltage, and it is difficult to obtain satisfactory performance at high voltage.
[0031] In addition, in the case of using two types of positive electrode active materials having different compositions, the electrochemical behavior that occurs is different from that when each positive electrode active material is used alone. For example, with respect to a secondary battery using a mixture of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide, the following phenomenon occurs: during charge and discharge, the positive electrode potential decreases more than a secondary battery using each positive electrode active material alone, wherein, in the case of the positive electrode potential decrease as described above, there is a problem of aggravation of the side reaction with the electrolyte solution under high temperature and / or high voltage conditions.
[0032] In order to solve the above-mentioned problems and develop a lithium secondary battery with excellent characteristics at high voltage, a lot of research has been conducted. As a result, the inventors found that when aluminum-nickel-cobalt-manganese-based oxides with an average particle size of primary particles of more than 3 μm are mixed with lithium-cobalt-based oxides as positive electrode active materials and the secondary battery is designed so that the capacity ratio of the negative electrode to the positive electrode meets a specific range, cycle characteristics, capacity characteristics and expansion characteristics that are significantly better than those of conventional secondary batteries can be achieved at a high voltage of 4.35 V or higher, thereby completing the present invention.
[0033] Hereinafter, each component of the lithium secondary battery of the present invention will be described in more detail.
[0034] positive electrode
[0035] The positive electrode of the present invention comprises a positive electrode active material layer comprising a mixed positive electrode material composed of two positive electrode active materials having different compositions. Specifically, the positive electrode active material layer of the present invention comprises lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide having an average primary particle diameter of 3 μm or more.
[0036] The lithium nickel cobalt manganese-based oxide is a lithium composite transition metal oxide containing nickel, cobalt, and manganese as transition metal elements, wherein the lithium nickel cobalt manganese-based oxide can be represented by the following Formula 1, for example.
[0037] [Formula 1]
[0038] Li x [Ni y Co z Mn w M 1 v ]O 2-p A p
[0039] In [Formula 1], M 1 It is a doping element that replaces the transition metal site, and may include at least one element selected from the group consisting of tungsten (W), copper (Cu), iron (Fe), vanadium (V), chromium (Cr), titanium (Ti), zirconium (Zr), zinc (Zn), aluminum (Al), indium (In), tantalum (Ta), yttrium (Y), lanthanum (La), strontium (Sr), gallium (Ga), scandium (Sc), gadolinium (Gd), samarium (Sm), calcium (Ca), cerium (Ce), niobium (Nb), magnesium (Mg), boron (B) and molybdenum (Mo).
[0040] A is an element substituting for an oxygen site, and may include at least one element selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I), astatine (At), and sulfur (S).
[0041] x represents the atomic ratio of lithium to the total transition metal in the lithium nickel cobalt manganese-based oxide, wherein x may be from 1 to 1.30, preferably greater than 1 and less than 1.30, more preferably from 1.005 to 1.30, for example, from 1.01 to 1.20. When the atomic ratio of lithium satisfies the above range, a lithium nickel cobalt manganese-based oxide having high crystallinity, an average particle size of primary particles of 3 μm or more, and low cation mixing can be obtained.
[0042] y represents the atomic ratio of nickel in the transition metal in the lithium nickel cobalt manganese-based oxide, wherein y is greater than 0.3 and less than 1, for example, 0.5 to 0.95. Since increasing the content of nickel in the transition metal can achieve a higher capacity, an atomic ratio of nickel of greater than 0.5 is more advantageous for achieving a high capacity.
[0043] z represents the atomic ratio of cobalt in the transition metal in the lithium nickel cobalt manganese-based oxide, wherein z is greater than 0 and is 0.6 or less, for example, 0.01 to 0.4.
[0044] w represents the atomic ratio of manganese in the transition metal in the lithium nickel cobalt manganese-based oxide, wherein w is greater than 0 and is 0.6 or less, for example, 0.01 to 0.4.
[0045] v represents the doping element M doped into the transition metal site in the lithium nickel cobalt manganese-based oxide 1 The atomic ratio of wherein v can be 0 to 0.2, for example 0 to 0.1. 1 In the case of , there is an effect of improving the structural stability of the lithium nickel cobalt manganese-based oxide, but since the capacity may decrease when the amount of the doping element is increased, it is desirable to contain the doping element at an atomic ratio of 0.2 or less.
[0046] p represents the atomic ratio of the element A replacing the oxygen site, wherein p may be from 0 to 0.2, for example, from 0 to 0.1.
[0047] In Formula 1, y+z+w+v=1.
[0048] The average particle size of the primary particles of the lithium nickel cobalt manganese-based oxide used in the present invention is 3 μm or more, for example, 3 μm to 10 μm. In the case where the average particle size of the primary particles of the lithium nickel cobalt manganese-based oxide is less than 3 μm, the contact area with the electrolyte solution is increased due to the increase in specific surface area, which leads to the following limitations: metal ions are dissolved from the lithium nickel cobalt manganese-based oxide, or the side reaction with the electrolyte solution is aggravated, and this phenomenon is more obvious when the operating voltage is high. As a result, under high voltage conditions, the cycle characteristics decrease rapidly and expansion occurs. In contrast, if particles with an average particle size of 3 μm or more of the primary particles are used as lithium nickel cobalt manganese-based oxides, due to the reduced contact area with the electrolyte solution, not only can the side reaction with the electrolyte solution that causes expansion and battery performance degradation be minimized, but also the compression density can be improved during the preparation of the positive electrode, thereby achieving high energy density.
[0049] The average particle size D of the lithium nickel cobalt manganese-based oxide in the form of single particles or secondary particles 50 The average particle size D of the lithium nickel cobalt manganese-based oxide may be 3 μm to 30 μm, preferably 3 μm to 15 μm, and more preferably 3 μm to 10 μm. 50 In the case where the above range is satisfied, when a lithium cobalt-based oxide to be described below is mixed, a high compression density can be obtained, and thus an effect of improving energy density can be obtained.
[0050] In addition, in the lithium nickel cobalt manganese-based oxide used in the present invention, Ni 2+ The amount of ions may be 5.0 atm% or less, for example, 0.1 atm% to 4.0 atm%. 2+ When the amount of ions satisfies the above range, better electrochemical performance can be achieved.
[0051] When lithium ions (Li +) similar transition metal cations, the transition metal will be incorporated into the lithium layer, which is called cation mixing. For lithium nickel cobalt manganese-based oxides, due to Li + With Co 3+ , Mn 4+ or Ni 3+ The size difference between the ions is large, so cation mixing is less likely to occur. However, since the nickel ion has an oxidation number of +2, 2+ ions are similar in size to lithium ions, so cation mixing may occur. 2+ When the ions are mixed in the lithium layer, they cannot form a layered crystal structure properly, so the structural stability of the active material is reduced, and the Ni 2+ The ions prevent the movement of lithium ions, so the battery performance is reduced. Therefore, in the present invention, Ni ions occupying lithium sites are used. 2+ The lithium nickel cobalt manganese-based oxide having an ion amount of 5.0 atm % or less can achieve excellent electrochemical performance.
[0052] The lithium nickel cobalt manganese-based oxide may have a monolithic structure composed of primary particles, or may be in the form of secondary particles formed by agglomeration of 30 or less, preferably 10 or less primary particles. When using a lithium nickel cobalt manganese-based oxide having a monolithic structure or a structure in which a relatively small amount of primary particles are agglomerated as described above, the specific surface area can be reduced, thereby minimizing side reactions with the electrolyte solution, and the compression density can be increased to achieve high energy density.
[0053] The lithium nickel cobalt manganese-based oxide of the present invention as described above can be prepared by mixing a lithium raw material with a transition metal precursor so that the ratio of the number of lithium atoms to the total number of transition metal atoms is 1 or more, for example, 1.005 to 1.30, and then heat-treating at a relatively high temperature.
[0054] Lithium raw materials may include, for example, lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide monohydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide, etc.), nitrates (e.g., lithium nitrate (LiNO3)), etc.), or chlorides (e.g., lithium chloride (LiCl)), etc., but the lithium raw materials are not limited thereto.
[0055] The transition metal precursor may include, for example, a hydroxide, an oxyhydroxide, a carbonate, or an organic complex of nickel, manganese, and cobalt, or may include a doping element M 1 A nickel-manganese-cobalt hydroxide, an oxyhydroxide, a carbonate or an organic complex. For example, a nickel-cobalt-manganese-based precursor may be [Ni y Co z Mn w ](OH)2,[Ni yCo z Mn w Al v ](OH)2,[Ni y Co z Mn w ]O·OH or [Ni y Co z Mn w Al v ]O·OH (wherein y, z, w and v are the same as defined in Formula 1), but the nickel-manganese-cobalt-based precursor is not limited thereto.
[0056] Desirably, the heat treatment temperature may be a temperature higher than the sintering temperature generally used when preparing a conventional lithium nickel cobalt manganese-based oxide having the same transition metal ratio, for example, a temperature higher than the commonly used sintering temperature by more than 100° C. For example, the heat treatment temperature may be 850° C. to 1,100° C., for example, 950° C. to 1,050° C.
[0057] Generally speaking, lithium nickel cobalt manganese-based oxides have an appropriate sintering temperature depending on the transition metal composition. For example, in the case where the atomic ratio of nickel:cobalt:manganese is 5:3:2, the appropriate sintering temperature is known to be 750°C to 850°C, and in the case where the atomic ratio of nickel:cobalt:manganese is 8:1:1, the appropriate sintering temperature is known to be 700°C to 800°C.
[0058] In the case of sintering at a temperature lower than the appropriate sintering temperature, the electrochemical performance may be reduced due to insufficient crystal growth, and if the sintering temperature is excessively higher than the appropriate sintering temperature, cation mixing or oxygen desorption may occur, thereby reducing the structural stability.
[0059] When a conventional appropriate sintering temperature is used, the particle size of the primary particles of the lithium nickel cobalt manganese-based oxide is formed to be less than 3 μm (usually at the level of 0.1 μm to 1 μm). When the sintering temperature is increased, the particle size of the primary particles can be formed to be larger, but when the sintering temperature is increased without changing other conditions, oxygen desorption occurs, and when oxygen desorption occurs, a large amount of Ni 3+ Ni ions are relatively more stable 2+ ions to maintain electrical equilibrium, resulting in an intensified cation mixing phenomenon and reduced crystallinity, which significantly reduces the electrochemical performance.
[0060] However, in the case of the present invention, after mixing the lithium raw material and the transition metal precursor so that the ratio of the number of lithium atoms to the total number of transition metals is 1 or more (e.g., 1.005 to 1.30), sintering is performed at a relatively high temperature to obtain a lithium nickel cobalt manganese-based oxide with low cation mixing, an average particle size of primary particles of 3 μm or more, and excellent crystallinity. When there are many lithium ions in the reactants, the proportion of lithium ions occupying the lithium site increases randomly, and the oxidation number of the transition metal increases to convert Ni 2+ Ions converted to Ni 3+ ions. In addition, when the oxidation number of the transition metal element increases, the binding energy between the transition metal ions and the oxygen ions increases, thereby reducing the transition metal interlayer spacing, thereby increasing the interlayer spacing between the lithium layer and the transition metal layer to inhibit the incorporation of the transition metal into the lithium layer. Therefore, the above method can prepare a lithium nickel cobalt manganese-based oxide with low cation mixing, an average primary particle size of 3 μm or more, and excellent crystallinity.
[0061] Next, the lithium cobalt-based oxide is a lithium transition metal oxide containing cobalt as a transition metal element, wherein the lithium cobalt-based oxide can be represented by the following Formula 2, for example.
[0062] [Formula 2]
[0063] LiCo 1-a M 2 a O 2-b B b
[0064] In formula 2, M 2 It is a doping element that replaces the cobalt site and may include at least one element selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo.
[0065] B is an element substituting for an oxygen site, and may include at least one element selected from the group consisting of F, Cl, Br, I, At, and S.
[0066] a represents the doping element M replacing the cobalt site 2 An atomic ratio of , wherein a may be from 0 to 0.2, such as from 0 to 0.1.
[0067] b represents the atomic ratio of the element B substituting the oxygen site, wherein b may be from 0 to 0.2, for example, from 0 to 0.1.
[0068] Generally speaking, lithium cobalt-based oxides have better life characteristics and expansion characteristics at high voltages than lithium nickel cobalt manganese-based oxides. In the case where lithium cobalt-based oxides are mixed with lithium nickel cobalt manganese-based oxides, the mixture can operate stably even at high voltages, similar to lithium cobalt-based oxides.
[0069] The average particle size D of lithium cobalt-based oxide 50 The average particle size D of the lithium cobalt-based oxide may be 10 μm to 20 μm, for example 12 μm to 20 μm, but the lithium cobalt-based oxide used in the present invention is not limited thereto. 50 When the above range is satisfied, the lithium cobalt-based oxide may be mixed with lithium nickel cobalt manganese-based oxide particles having a relatively small size to achieve high compression density, thereby obtaining an effect of improving energy density.
[0070] The lithium nickel cobalt manganese-based oxide and the lithium cobalt-based oxide may be included in the positive electrode active material layer in a weight ratio of 50:50 to 80:20, for example, 60:40 to 80:20. Since the content of the lithium nickel cobalt manganese-based oxide having relatively good capacity characteristics is 50% or more, high capacity characteristics can be achieved.
[0071] In addition, based on the total weight of the positive electrode active material layer, the total weight of the lithium nickel cobalt manganese-based oxide and the lithium cobalt-based oxide may be 80 wt % to 98 wt %, for example 85 wt % to 98 wt %. When the content of the positive electrode active material is within the above range, excellent capacity characteristics may be exhibited.
[0072] The positive electrode active material layer may further contain a conductive agent and a binder as necessary.
[0073] The conductive agent is used to provide conductivity to the electrode, wherein any conductive agent may be used without particular limitation as long as it has suitable electron conductivity and does not cause adverse chemical changes in the battery.
[0074] Specific examples of the conductive agent may be graphite, such as natural graphite and artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and carbon fiber; powders or fibers of metals such as copper, nickel, aluminum and silver; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium dioxide; or conductive polymers, such as polyphenylene derivatives, and any one of them or a mixture of two or more thereof may be used.
[0075] The content of the conductive agent may be 1.5 wt% or more, preferably 1.5 wt% to 5 wt%, and more preferably 1.5 wt% to 3 wt%, based on the total weight of the positive electrode active material layer. If the amount of the conductive agent in the positive electrode using a mixture of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide as in the present invention is less than 1.5 wt%, the output may be reduced.
[0076] Next, the binder improves adhesion between positive electrode active material particles and between the positive electrode active material and the current collector.
[0077] Specific examples of binders may be polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or various copolymers thereof, and any one thereof or a mixture of two or more thereof may be used. Based on the total weight of the positive electrode active material layer, the content of the binder may be 0.1 wt % to 15 wt %.
[0078] The positive electrode of the present invention can be prepared according to a typical method for preparing a positive electrode, except that the above-mentioned positive electrode active material is used. Specifically, a positive electrode material mixture prepared by dissolving or dispersing a positive electrode active material, a binder and / or a conductive agent in a solvent is coated on a positive electrode current collector, and then the positive electrode is prepared by drying and rolling the coated positive electrode current collector.
[0079] There is no specific limitation on the positive electrode current collector, as long as it has conductivity and does not cause adverse chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, fired carbon, or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium or silver, etc., can be used. In addition, the thickness of the positive electrode current collector can generally be 3 μm to 500 μm, and small irregularities can be formed on the surface of the current collector to improve the adhesion of the positive electrode material. For example, various shapes of positive electrode current collectors can be used, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0080] The solvent may be a commonly used solvent in the art, may include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, and any one thereof or a mixture of two or more thereof may be used. Considering the coating thickness, manufacturing yield and processability of the positive electrode material mixture, if the positive electrode material mixture can be adjusted to have an appropriate viscosity, the amount of the solvent used may be sufficient, and there is no specific restriction.
[0081] In addition, as another method, the positive electrode may be prepared by casting the positive electrode material mixture on a separate support and then laminating a film separated from the support on a positive electrode current collector.
[0082] negative electrode
[0083] Next, the negative electrode will be described.
[0084] The negative electrode of the present invention includes a negative electrode active material layer containing a negative electrode active material.
[0085] The negative electrode active material may include at least one of a carbon-based negative electrode active material or a silicon-based negative electrode active material.
[0086] As the carbon-based negative electrode active material, various carbon-based negative electrode active materials used in the art can be used, such as amorphous, plate-shaped, flaky, spherical or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesophase carbon microbead, mesophase pitch, high-temperature sintered carbon (such as coke derived from petroleum or coal tar pitch), soft carbon, and hard carbon.
[0087] Preferably, the carbon-based negative electrode active material may include at least one of natural graphite or artificial graphite. More preferably, the carbon-based negative electrode active material may include natural graphite and artificial graphite. When natural graphite and artificial graphite are used together, the binding with the current collector can be improved, thereby suppressing the peeling of the active material.
[0088] The silicon-based negative electrode active material may include those selected from the group consisting of metallic silicon (Si), silicon oxide (SiO x , where 0 < x ≤ 2), silicon carbide (SiC), and Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si). The element Y may be selected from the group consisting of Mg, Ca, Sr, barium (Ba), radium (Ra), Sc, Y, Ti, Zr, hafnium (Hf), (Rf), V, Nb, Ta, (Db), Cr, Mo, W, (Sg), technetium (Tc), rhenium (Re), (Bh), Fe, lead (Pb), ruthenium (Ru), osmium (Os), (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), Cu, silver (Ag), gold (Au), Zn, cadmium (Cd), B, Al, Ga, tin (Sn), In, germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), S, selenium (Se), tellurium (Te), polonium (Po), and combinations thereof.
[0089] Since the silicon-based negative electrode active material has higher capacity characteristics than the carbon-based negative electrode active material, better capacity characteristics can be obtained when the silicon-based negative electrode active material is included.
[0090] According to one embodiment, the negative electrode active material may be a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material, in which case, as a weight ratio, the mixing ratio of the silicon-based negative electrode active material: the carbon-based negative electrode active material may be 1:99 to 50:50, for example, 5:95 to 30:70. When the mixing ratio of the silicon-based negative electrode active material to the carbon-based negative electrode active material satisfies the above range, since the volume expansion of the silicon-based negative electrode active material is suppressed while improving the capacity characteristics, excellent cycle performance can be ensured.
[0091] The negative electrode active material may be contained in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode active material layer. When the amount of the negative electrode active material satisfies the above range, excellent capacity characteristics and electrochemical properties may be obtained.
[0092] The negative electrode active material layer may further include a binder and a conductive agent in addition to the negative electrode active material.
[0093] The binder is a component that helps the bonding between the conductive agent, the active material and the current collector, wherein the binder is generally added in an amount of 0.1 wt % to 10 wt % based on the total weight of the negative electrode active material layer. Examples of binders may be polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber and various copolymers thereof.
[0094] The conductive agent is a component for further improving the conductivity of the negative electrode active material, wherein the amount of the conductive agent added may be 10% by weight or less, for example, 5% by weight or less, based on the total weight of the negative electrode active material layer. Any conductive agent may be used without specific limitation, as long as it has conductivity and does not cause adverse chemical changes in the battery, for example, conductive materials such as the following may be used: graphite, such as natural graphite or artificial graphite; carbon black, such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as fluorocarbon powders, aluminum powders, and nickel powders; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium dioxide; or polyphenylene derivatives.
[0095] The negative electrode active material layer can be manufactured as follows: a negative electrode material mixture prepared by dissolving or dispersing the negative electrode active material and optional binder and conductive agent in a solvent is coated on a negative electrode collector, and the coated negative electrode collector is dried; or it can be manufactured as follows: the negative electrode material mixture is cast on a separate support, and a film layer separated from the support is then stacked on the negative electrode collector.
[0096] There is no specific limitation on the negative electrode current collector, as long as it has high conductivity and does not cause adverse chemical changes in the battery, for example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, or copper or stainless steel surface-treated with one of carbon, nickel, titanium or silver, and aluminum-cadmium alloys can be used. In addition, the thickness of the negative electrode current collector can generally be 3 μm to 500 μm, and similar to the positive electrode current collector, tiny irregularities can be formed on the surface of the current collector to improve the adhesion of the negative electrode active material. For example, various shapes of negative electrode current collectors can be used, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0097] The solvent may be a commonly used solvent in the art, may include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, and any one thereof or a mixture of two or more thereof may be used. Considering the coating thickness, manufacturing yield and processability of the negative electrode material mixture, if the negative electrode material mixture can be adjusted to have an appropriate viscosity, the amount of the solvent used may be sufficient and is not specifically limited.
[0098] The ratio of the negative electrode capacity to the positive electrode capacity of the lithium secondary battery of the present invention is 1.06 to 1.15, for example, 1.06 to 1.12.
[0099] According to the research of the present inventors, for lithium secondary batteries using mixed positive electrode materials of lithium nickel cobalt manganese-based oxides and lithium cobalt-based oxides, it has been found that when the ratio of the negative electrode capacity to the positive electrode capacity meets a specific range, i.e., 1.06 to 1.15, significantly better cycle characteristics and expansion characteristics can be obtained at high voltages. Specifically, it has been found that when the ratio of the negative electrode capacity to the positive electrode capacity is less than 1.06 or greater than 1.15, the capacity characteristics and expansion characteristics deteriorate rapidly in long-term cycles, and the expansion increases rapidly during high-temperature storage.
[0100] These characteristics are completely different from those observed in lithium secondary batteries using lithium nickel cobalt manganese-based oxides or lithium cobalt-based oxides alone. Figure 4 and Figure 5 Be confirmed.
[0101] Figure 5 , a comparison chart of the cycle characteristics and expansion characteristics of a lithium secondary battery (Comparative Example 1) using lithium cobalt-based oxide alone and having a negative electrode capacity to positive electrode capacity ratio of 1.01 and a lithium secondary battery (Comparative Example 2) using lithium cobalt-based oxide alone and having a negative electrode capacity to positive electrode capacity ratio of 1.07 is shown. Figure 5As shown, for the lithium secondary battery using lithium cobalt-based oxide alone, it can be confirmed that the cycle characteristics and expansion characteristics of Comparative Example 2 in which the ratio of the negative electrode capacity to the positive electrode capacity is 1.07 are significantly deteriorated compared to Comparative Example 1 in which the ratio of the negative electrode capacity to the positive electrode capacity is 1.01. That is, for the lithium secondary battery using lithium cobalt-based oxide alone, when the ratio of the negative electrode capacity to the positive electrode capacity is less than 1.06, the cycle characteristics and expansion characteristics are better.
[0102] In contrast, for a lithium secondary battery using a mixed positive electrode material as in the present invention, unlike a lithium secondary battery using a lithium cobalt-based oxide, when the ratio of the negative electrode capacity to the positive electrode capacity is 1.06 or more, the cycle characteristics and the expansion characteristics are better. Figure 4 A comparison chart showing the cycle characteristics and expansion characteristics of a lithium secondary battery (Example 1) using a mixed positive electrode material of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide and having a negative electrode capacity to positive electrode capacity ratio of 1.07 and a lithium secondary battery (Comparative Example 3) using the same mixed positive electrode material but having a negative electrode capacity to positive electrode capacity ratio of 1.04. Figure 4 In the lithium secondary battery using the mixed positive electrode material as in the present invention, it can be confirmed that when the ratio of the negative electrode capacity to the positive electrode capacity is 1.06 or more, the cycle characteristics and the expansion characteristics are better.
[0103] Electrolytes
[0104] Next, the electrolyte will be described.
[0105] As the electrolyte used in the present invention, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte or a molten inorganic electrolyte that can be used in a lithium secondary battery can be used, but the electrolyte is not particularly limited.
[0106] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0107] Any organic solvent can be used as an organic solvent without particular limitation, as long as it can serve as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, as the organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone can be used; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; or carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol solvents such as ethanol and isopropanol; nitriles such as Ra-CN (wherein Ra is a linear, branched or cyclic C2-C20 hydrocarbon group, which may include a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or cyclopentane sulfones.
[0108] Among these solvents, carbonate solvents are preferred, and more preferably a mixture of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant (which can improve the charge and discharge performance of the battery) and low-viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate).
[0109] Any lithium salt commonly used in an electrolyte solution for a lithium secondary battery may be used as the lithium salt without limitation. For example, the lithium salt may include Li + as a cation, and may include as an anion at least one selected from the group consisting of: F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - 、AlO4 - 、AlCl4 - PF6 - 、SbF6 - 、AsF6 - 、BF2C2O4 - , BC4O8 - PF4C2O4 - PF2C4O8 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 -、C4F9SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - Specifically, the lithium salt may include a salt selected from the group consisting of LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiAlO4 and LiCH3SO3, or a mixture of two or more thereof.
[0110] The lithium salt may be appropriately changed within a normal use range, but may be specifically contained in the electrolyte solution at a concentration of 0.8M to 3M, for example, 0.1M to 2.5M.
[0111] In order to improve the life characteristics of the battery, suppress the reduction of the battery capacity and increase the discharge capacity of the battery, in addition to the above-mentioned components, various additives may also be included in the electrolyte. For example, the additive may include halogenated alkylene carbonate compounds (such as difluoroethylene carbonate), pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glycol dimethyl ether, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N, N-substituted imidazolidinones, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol or aluminum chloride, and these additives may be used alone or in their mixtures. In this case, based on the gross weight of the electrolyte, the content of the additive may be 0.1 wt % to 5 wt %.
[0112] Diaphragm
[0113] The lithium secondary battery of the present invention may include a separator as necessary.
[0114] The separator separates the negative electrode and the positive electrode and provides a movement channel for lithium ions. Any separator can be used as the separator without specific limitation as long as it is commonly used in lithium secondary batteries. Specifically, a separator having high moisture retention capacity for electrolytes and low resistance to the transfer of electrolyte ions can be used.
[0115] Specifically, a porous polymer film can be used, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer or an ethylene / methacrylate copolymer, or a laminated structure having two or more layers thereof. In addition, a typical porous nonwoven fabric can be used, for example, a nonwoven fabric formed by a high melting point glass fiber or a polyethylene terephthalate fiber. In addition, a coated diaphragm comprising a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a diaphragm with a monolayer or multilayer structure can be selectively used.
[0116] Since the lithium secondary battery of the present invention as described above has excellent stability and electrochemical performance even at high voltage, the operating voltage can be above 4.35V, and when the lithium secondary battery operates at such a high voltage, excellent high capacity characteristics can be achieved compared with conventional lithium secondary batteries.
[0117] The lithium secondary battery of the present invention as described above can be applied to portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0118] Therefore, according to another embodiment of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit cell and a battery pack including the battery module are provided.
[0119] The battery module or battery pack can be used as a power source for at least one of the following large and medium-sized devices: power tools; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or energy storage systems.
[0120] The shape of the lithium secondary battery of the present invention is not particularly limited, but a cylindrical type using a can, a prismatic type, a pouch type, or a coin type may be used.
[0121] The lithium secondary battery of the present invention can be used not only in a battery cell used as a power source for small-sized devices but also as a unit cell in a large or medium-sized battery module including a plurality of battery cells.
[0122] Hereinafter, the present invention will be described in detail according to specific embodiments. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these exemplary embodiments are provided so that the description will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.
[0123] Preparation Example 1
[0124] Mixed lithium raw material LiOH and nickel-cobalt-manganese precursor Ni 0.5 Co 0.3 Mn 0.2 (OH)2 so that the atomic ratio of lithium to transition metal is 1.05:1.00, and then heat-treated at 1,000°C for 10 hours to prepare primary particles with an average particle size of D 50 5μm Li[Ni 0.5 Co 0.3 Mn 0.2 ]O2 powder.
[0125] Figure 1 The Li[Ni 0.5 Co 0.3 Mn 0.2 ]Scanning electron microscope (SEM) image of O2 powder. Figure 1 As shown, it shows that in Li[Ni 0.5 Co 0.3 Mn 0.2 ]O2 powder contains a mixture of single primary particles and secondary particles formed by agglomeration of less than 10 primary particles. 0.5 Co 0.3 Mn 0.2 ] The average particle size of O2 powder is D 50 7μm.
[0126] Preparation Example 2
[0127] The average particle size D of primary particles was prepared in the same manner as in Preparation Example 1. 50 The Li[Ni 0.5 Co 0.3 Mn 0.2 ]O2 powder, except that it is heat treated at 950℃.
[0128] Figure 2 The Li[Ni 0.5 Co 0.3 Mn 0.2 ]SEM image of O2 powder. Figure 2 As shown, the prepared Li[Ni 0.5 Co0.3 Mn 0.2 ]O2 powder is in the form of secondary particles, wherein the number of agglomerated primary particles is 30 or less, and the Li[Ni 0.5 Co 0.3 Mn 0.2 ] The average particle size of O2 powder is D 50 8μm.
[0129] Preparation Example 3
[0130] Li[Ni 0.5 Co 0.3 Mn 0.2 ]O2 powder, the difference being that the heat treatment is carried out at 800°C.
[0131] Figure 3 The Li[Ni 0.5 Co 0.3 Mn 0.2 ]SEM image of O2 powder. Figure 3 As shown, the prepared Li[Ni 0.5 Co 0.3 Mn 0.2 The O2 powder is in the form of secondary particles (in which several tens of primary particles with a particle size of 1 μm or less are aggregated), and the average particle size of the secondary particles is D 50 is 6μm.
[0132] Example 1
[0133] The positive electrode active material, the conductive agent, and the binder were mixed in an N-methylpyrrolidone solvent at a weight ratio of 96.9:1.7:1.4 to prepare a positive electrode material mixture.
[0134] In this case, the lithium nickel cobalt manganese-based oxide prepared in Preparation Example 1 is mixed with an average particle size D 50 LiCoO2 with a size of 16 μm was mixed at a weight ratio of 70:30 and used as a positive electrode active material.
[0135] Li435 from Denka Company Limited was used as a conductive agent, and KF9700 from Zeon Corporation was used as a binder.
[0136] An aluminum current collector (Sam-AAluminum) having a thickness of 10 μm was coated with the prepared positive electrode material mixture, dried at 100° C., and then roll-pressed to prepare a positive electrode.
[0137] Next, the negative electrode active material, binder / thickener and conductive agent were mixed in N-methylpyrrolidone solvent at a weight ratio of 95.8:3.7:0.5 to prepare a negative electrode material mixture. In this case, artificial graphite (Shanshan Technology, QCGX) was used as the negative electrode active material, Li435 from Denka Company Limited was used as the conductive agent, and BML302 from Zeon Corporation was used as the binder.
[0138] A copper current collector (LS Mtron Ltd.) having a thickness of 8 μm was coated with the prepared negative electrode material mixture, dried at 130° C., and then roll-pressed to prepare a negative electrode.
[0139] During the preparation of the negative electrode and the positive electrode, the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.07.
[0140] A separator was disposed between the positive electrode and the negative electrode prepared as described above, and an electrolyte solution was injected to prepare a lithium secondary battery.
[0141] Example 2
[0142] A lithium secondary battery was prepared in the same manner as in Example 1, except that the lithium nickel cobalt manganese-based oxide prepared in Preparation Example 2 was mixed with a particle size D 50 LiCoO2 with a size of 16 μm was mixed at a weight ratio of 70:30 and used as a positive electrode active material.
[0143] Example 3
[0144] A lithium secondary battery was prepared in the same manner as in Example 1, except that the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.09.
[0145] Example 4
[0146] A lithium secondary battery was prepared in the same manner as in Example 1, except that the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.10.
[0147] Example 5
[0148] A lithium secondary battery was prepared in the same manner as in Example 1, except that the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.12.
[0149] Comparative Example 1
[0150] A lithium secondary battery was prepared in the same manner as in Example 1, except that only the average particle size D 50 LiCoO2 with a particle size of 16 μm was used as the positive electrode active material, and the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.01.
[0151] Comparative Example 2
[0152] A lithium secondary battery was prepared in the same manner as in Example 1, except that only the average particle size D 50 LiCoO2 with a particle size of 16 μm was used as the positive electrode active material, and the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.07.
[0153] Comparative Example 3
[0154] A lithium secondary battery was prepared in the same manner as in Example 1, except that the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.04.
[0155] Comparative Example 4
[0156] A lithium secondary battery was prepared in the same manner as in Example 1, except that the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.17.
[0157] Comparative Example 5
[0158] A lithium secondary battery was prepared in the same manner as in Example 1, except that the lithium nickel cobalt manganese-based oxide prepared in Preparation Example 3 was mixed with a particle size of D 50 LiCoO2 with a size of 16 μm was mixed at a weight ratio of 70:30 and used as a positive electrode active material.
[0159] Comparative Example 6
[0160] A lithium secondary battery was prepared in the same manner as in Example 1, except that the loading amount of the positive electrode and the loading amount of the negative electrode were adjusted so that the ratio of the negative electrode capacity to the positive electrode capacity was 1.05.
[0161] Experimental Example 1
[0162] The high voltage life characteristics and swelling characteristics of the lithium secondary batteries prepared in Examples 1 to 5 and Comparative Examples 1 to 6 were evaluated.
[0163] Specifically, each lithium secondary battery prepared in Examples 1 to 5 and Comparative Examples 1 to 6 was charged to 4.35 V (0.05 C cut-off) at 1.0 C under constant current / constant voltage (CC / CV) conditions at 23° C. Subsequently, each lithium secondary battery was discharged to 3.0 V at a constant current (CC) of 0.5 C.
[0164] The above charge and discharge behavior was set as one cycle, and after the cycle was repeated 300 times, the discharge capacity after 300 cycles and the initial discharge capacity (discharge capacity after 1 cycle) were compared to measure the capacity retention ratio defined by the following equation (1).
[0165] Equation (1): Capacity retention rate (%) = [(discharge capacity after 300 cycles - initial discharge capacity) / initial discharge capacity] × 100
[0166] In addition, the battery thickness after 300 cycles and the initial battery thickness (battery thickness after 1 cycle) were measured to measure the expansion characteristics defined by the following equation (2).
[0167] Equation (2): Expansion (%) = [(battery thickness after 300 cycles - initial battery thickness) / initial battery thickness] × 100
[0168] The measurement results are listed in Table 1 below.
[0169] [Table 1]
[0170] Capacity retention rate (%) Expansion characteristics (%) Example 1 97 5 Example 2 96 6 Example 3 96 6 Example 4 96 5 Example 5 96 6 Comparative Example 1 92 8 Comparative Example 2 78 21 Comparative Example 3 0 30 Comparative Example 4 93 12.5 Comparative Example 5 80 12 Comparative Example 6 92.5 7.5
[0171] With reference to Table 1, it can be understood that during high voltage operation, the lithium secondary batteries of Examples 1 to 5 that meet the conditions of the present invention have better cycle characteristics and expansion characteristics than the lithium secondary batteries of Comparative Examples 1 to 6. In particular, for the lithium secondary battery of Comparative Example 3 (wherein the ratio of the negative electrode capacity to the positive electrode capacity is 1.04) and the lithium secondary battery of Comparative Example 5 (wherein the particle size of the primary particles of the lithium nickel cobalt manganese-based oxide is outside the scope of the present invention), it can be confirmed that the cycle characteristics and expansion characteristics during high voltage operation are significantly deteriorated compared to the case of the present invention. These results show that in order to achieve stable battery performance at high voltage for a lithium secondary battery using a mixed positive electrode material of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide, the particle size of the primary particles of the lithium nickel cobalt manganese-based oxide and the ratio of the negative electrode capacity to the positive electrode capacity must meet the scope of the present invention.
[0172] Experimental Example 2
[0173] In order to evaluate the battery characteristics according to the ratio of the negative electrode capacity to the positive electrode capacity in the lithium secondary battery using the mixed positive electrode material of lithium nickel cobalt manganese-based oxide and lithium cobalt-based oxide as the positive electrode active material, the lithium secondary batteries prepared in Examples 1 to 5 and Comparative Examples 3, 4 and 6 were charged and discharged under the same conditions as in Experimental Example 1, and the capacity retention rate and expansion characteristics were measured. The measurement results are shown in Figure 4 middle.
[0174] refer to Figure 4 , for the lithium secondary batteries in Comparative Examples 3, 4 and 6 (wherein a mixed positive electrode material is used and the ratio of the negative electrode capacity to the positive electrode capacity is outside the scope of the present invention), it can be confirmed that the capacity characteristics and expansion characteristics deteriorate rapidly compared with the lithium secondary batteries of the embodiments. Specifically, for the lithium secondary battery of Comparative Example 3, the capacity characteristics begin to deteriorate rapidly after 50 cycles, and the expansion increases significantly after 100 cycles; for the lithium secondary battery of Comparative Example 6, the capacity characteristics also begin to deteriorate after 50 cycles, the capacity decreases rapidly after 150 cycles, and the expansion increases significantly after 250 cycles. In addition, for the lithium secondary battery of Comparative Example 4 (wherein the ratio of the negative electrode capacity to the positive electrode capacity is 1.17), it can be confirmed that the capacity decreases rapidly after 200 cycles and the expansion increases significantly.
[0175] On the contrary, for the lithium secondary batteries of Examples 1 to 5 (in which a mixed positive electrode material is used and the ratio of the negative electrode capacity to the positive electrode capacity is in the range of 1.06 to 1.12), since the capacity retention rate and expansion characteristics are maintained well within 500 cycles, it can be understood that the life characteristics are significantly better than those of Comparative Examples 3, 4 and 6.
[0176] Experimental Example 3
[0177] In order to evaluate the battery characteristics based on the ratio of the negative electrode capacity to the positive electrode capacity in the lithium secondary battery using only the lithium cobalt-based oxide as the positive electrode active material, the lithium secondary batteries prepared in Comparative Examples 1 and 2 were charged and discharged under the same conditions as in Experimental Example 1, while measuring the capacity retention rate and expansion characteristics. The measurement results are shown in Figure 5 middle.
[0178] refer to Figure 5 For lithium secondary batteries using only lithium cobalt-based oxides, it was found that Comparative Example 1 (wherein the ratio of the negative electrode capacity to the positive electrode capacity was 1.01) had better cycle characteristics and expansion characteristics than Comparative Example 2 (wherein the ratio of the negative electrode capacity to the positive electrode capacity was 1.07), which is consistent with Figure 4 The trend shown is the opposite.
[0179] In addition, for the lithium secondary battery of Comparative Example 1, the capacity retention rate decreased to about 90% at the 400th cycle, the expansion characteristics were about 8% at the 300th cycle, and for the lithium secondary battery of Comparative Example 2, it was found that the capacity retention rate and expansion characteristics were significantly deteriorated after 150 cycles.
Claims
1. A lithium secondary battery, the lithium secondary battery comprising: a positive electrode including a positive electrode active material layer containing a lithium nickel cobalt manganese-based oxide and a lithium cobalt-based oxide; a negative electrode including a negative electrode active material layer containing a negative electrode active material; and an electrolyte, The average particle size of the primary particles of the lithium nickel cobalt manganese-based oxide is 3 μm to 10 μm, and the average particle size D of the lithium cobalt-based oxide is 50 10μm to 20μm; the lithium nickel cobalt manganese-based oxide has a monolithic structure composed of primary particles or is in the form of secondary particles formed by coalescence of 30 or fewer primary particles; the ratio of the negative electrode capacity to the positive electrode capacity is 1.06 to 1.09; and the positive electrode active material layer contains the lithium nickel cobalt manganese-based oxide and the lithium cobalt-based oxide in a weight ratio of 50:50 to 80:
20.
2. The lithium secondary battery according to claim 1, wherein The lithium nickel cobalt manganese-based oxide is represented by [Formula 1]: [Formula 1] Li x [Ni y Co z Mr w M 1 v ]O 2-p A p wherein, in [Formula 1], M 1 including at least one element selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, A includes at least one element selected from the group consisting of F, Cl, Br, I, At, and S, and 1.0 ≤ x ≤ 1.30, 0.3 ≤ y < 1, 0 < z ≤ 0.6, 0 < w ≤ 0.6, 0 ≤ v ≤ 0.2, and 0 ≤ p ≤ 0.
2.
3. The lithium secondary battery according to claim 2, wherein: The Ni occupying the lithium site in the lithium nickel cobalt manganese-based oxide 2+ The amount of ions is 5.0 atom % or less.
4. The lithium secondary battery according to claim 1, wherein The lithium cobalt-based oxide is represented by [Formula 2]: [Formula 2] LiCo 1-a M 2 a O 2-b B’ b wherein, in Formula 2, M 2 including at least one element selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo, B' includes at least one element selected from the group consisting of F, Cl, Br, I, At, and S, and 0 ≤ a ≤ 0.2 and 0 ≤ b ≤ 0.
1.
5. The lithium secondary battery according to claim 1, wherein The positive electrode active material layer contains the lithium nickel cobalt manganese-based oxide and the lithium cobalt-based oxide in a weight ratio of 60:40 to 80:
20.
6. The lithium secondary battery according to claim 1, wherein The average particle size D of the lithium cobalt-based oxide 50 12μm to 20μm.
7. The lithium secondary battery according to claim 1, wherein The positive electrode active material layer further contains a conductive agent and a binder.
8. The lithium secondary battery according to claim 7, wherein: Based on the total weight of the positive electrode active material layer, the content of the conductive agent is 1.5 wt% or more.
9. The lithium secondary battery according to claim 1, wherein: The negative electrode active material contains at least one of a carbon-based negative electrode active material or a silicon-based negative electrode active material.
10. The lithium secondary battery according to claim 9, wherein: The carbon-based negative electrode active material includes natural graphite and artificial graphite.
11. The lithium secondary battery according to claim 1, wherein The operating voltage of the lithium secondary battery is 4.35 V or more.
Citation Information
Patent Citations
Automotive Thin Display System using HTML5, In Car Server and Method thereof
KR1020190026395A
Nonaqueous electrolyte secondary battery
CN101154755A
Polymer compound, electrode binder composition, electrode and lithium secondary battery
CN103724523A
Lithium secondary battery
CN103907235A
Anode active material for secondary battery and lithium secondary battery comprising same
CN104471759A