Concrete surface hardening agent and preparation method thereof

A technology of concrete surface and hardener, which is applied in the field of concrete surface hardener, which can solve the problems of decreased protective ability of steel bars, ash and sand on the base surface, and reduced effect, so as to improve surface compactness, concrete hardness, and surface strength. Effect

CN113735622APending Publication Date: 2021-12-03SUZHOU GUARDEX NEW MATERIAL TECH CO LTD
2 Cites 0 Cited by

Patent Information

Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Publication Date
2021-12-03

Smart Images

  • Figure 1
    Figure 1
  • Figure 2
    Figure 2
  • Figure 3
    Figure 3
Patent Text Reader

Abstract

The invention discloses a concrete surface hardening agent and a preparation method thereof, the concrete surface hardening agent comprises the following components: 60-70 parts of a modified lithium silicate solution, 0.2-0.5 part of a liquid surface tension modifier, 0.2-0.5 part of an ion stabilizer and 30-40 parts of water, the modified lithium silicate solution comprises 40-60 parts of a potassium silicate solution, wherein the potassium silicate solution comprises 40-60 parts of a sodium silicate solution, 8-12 parts of sodium methyl silicate and 8-12 parts of magnesium fluosilicate. According to the concrete surface hardening agent, the surface compactness and surface strength of concrete can be improved, a shell-shaped structure can be generated in a concrete crack, and the effect of improving the hardness of the concrete is achieved; meanwhile, the concrete surface hardening agent has relatively strong permeability, and the surface strength can be improved by more than 5 Mpa within 3 days.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to a concrete surface hardener, which belongs to the technical field of building material additives. Background technique

[0002] One of the problems of the current common concrete structure is that the surface strength of the concrete is insufficient. The quality of the concrete is poor due to the humid environment during the storage and transportation of the cement, more impurities in the cement or the ratio of the admixture in the process of concrete mixing. , The poured concrete is maintained in a harsh environment, resulting in ash and sand on the base surface, and the strength cannot meet the design requirements. For some buildings that are exposed to the environment of harmful substances such as acid, alkali and salt all year round, harmful substances will enter the interior of the concrete structure from the tiny cracks on the concrete surface, and chemical reactions will occur, which will reduce the alkalinity of the con...

Examples

Embodiment 1

[0042] S1. Preparation of modified lithium silicate solution: Weigh 12 parts of sodium methyl silicate and 12 parts of magnesium fluorosilicate at room temperature, add 60 parts of potassium silicate solution, heat to 40-50°C, stir for 5-30 minutes until the solution is complete Mix and set aside.

[0043] S2. Weigh 40 parts of deionized water, 0.2 part of liquid surface tension modifier and 0.2 part of ion stabilizer;

[0044] S3, adding liquid surface tension modifier and ion stabilizer to deionized water, stirring at room temperature at low speed;

[0045] S4. Add 60 parts of the modified lithium silicate solution prepared in S1 to the liquid in S3, and stir for 10 minutes to prepare a concrete surface hardener.

Embodiment 2

[0047] S1. Preparation of modified lithium silicate solution: Weigh 10 parts of sodium methyl silicate and 10 parts of magnesium fluorosilicate at room temperature, add 50 parts of potassium silicate solution, heat to 50-60 ° C, stir for 5-30 minutes until the solution is complete Mix and set aside.

[0048] S2. Weigh 30 parts of deionized water, 0.2 part of liquid surface tension modifier and 0.2 part of ion stabilizer;

[0049] S3, adding liquid surface tension modifier and ion stabilizer to deionized water, stirring at room temperature at low speed;

[0050] S4. Add 70 parts of the modified lithium silicate solution prepared in S1 to the liquid in S3, and stir for 10 minutes to prepare a concrete surface hardener.

Embodiment 3

[0052] S1. Preparation of modified lithium silicate solution: weigh 9 parts of sodium methyl silicate and 9 parts of magnesium fluorosilicate at room temperature, add 45 parts of potassium silicate solution, heat to 60-70°C, stir for 5-30min until the solution is complete Mix and set aside.

[0053] S2. Weigh 40 parts of deionized water, 0.5 part of liquid surface tension modifier and 0.5 part of ion stabilizer;

[0054] S3, adding liquid surface tension modifier and ion stabilizer to deionized water, stirring at room temperature at low speed;

[0055] S4. Add 60 parts of the modified lithium silicate solution prepared in S1 to the liquid in S3, and stir for 20 minutes to prepare a concrete surface hardener.