Hydroisomerization catalyst and hydrocarbon oil hydroisomerization method

Through the combination of low silicon to aluminum ratio ZSM-48 molecular sieve carrier and active metal components, a catalyst for the hydroisomerization reaction of hydrocarbon oil is prepared, which solves the problems of elevated freezing point of feed oil and insufficient catalyst utilization, and achieves Efficient and environmentally friendly hydroisomerization treatment effect.

CN113751061BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010497323.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-04
Publication Date
2024-10-11
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively reduce the freezing point of the feed oil while maintaining a suitable viscosity in the paraffin hydroisomerization reaction, and the catalyst reusability and environmental performance are insufficient.

Method used

ZSM-48 molecular sieve with low silicon to aluminum ratio is used as a carrier, and the catalyst is prepared through hydrothermal crystallization and aluminum supplementation processes, and active metal components, such as Pt and Pd, are loaded on it to form a hydroisomerization catalyst for Hydroisomerization reaction of hydrocarbon oils.

Benefits of technology

The freezing point of the target product is significantly reduced, the product yield is increased, the catalyst can be reused, the environmental performance is good, and environmental pollution is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113751061B_ABST
    Figure CN113751061B_ABST
Patent Text Reader

Abstract

The present invention relates to a hydroisomerization catalyst, a preparation method and an application, wherein the catalyst comprises a carrier and an active metal component loaded on the carrier, wherein the carrier comprises a ZSM-48 molecular sieve having a low silicon-aluminum ratio, and the preparation method of the ZSM-48 molecular sieve having a low silicon-aluminum ratio comprises: (1) preparing a pure silicon ZSM-48 molecular sieve intermediate having a relative crystallinity of ≥90% in the presence of an inorganic base; (2) supplementing the pure silicon ZSM-48 molecular sieve intermediate with aluminum under inorganic base conditions and recovering the product. Compared with the prior art, when the catalyst provided by the present invention is subjected to hydroisomerization treatment on a feedstock oil rich in paraffins, the target product obtained has a lower pour point and a high yield of the target product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrocarbon oil refining, and more specifically, the invention relates to a hydroisomerization catalyst and application thereof in paraffin hydroisomerization reaction. Background Art

[0002] When using raw oil with a high content of paraffins to produce low-freezing diesel or lubricating oil base oil, dewaxing treatment is required to reduce the freezing point and improve the low-temperature fluidity of the product. Isomerization of paraffins in the presence of a hydroisomerization catalyst can significantly improve the low-temperature fluidity of the oil while maintaining a suitable viscosity. The carrier material of the hydroisomerization catalyst usually contains different types of molecular sieves. The molecular sieve material has high acidity and high specific surface area and is an excellent acid catalyst. At the same time, the molecular sieve material has strong chemical stability and hydrothermal stability, and it is difficult to be corroded and dissolved by the reactants and destroyed. Compared with the commonly used homogeneous catalysts, the molecular sieve material catalyst can be directly reused without separation, and will not cause pollution to the environment and products. Therefore, the preparation of new molecular sieve materials and the construction of new morphologies of known molecular sieves have always been a hot topic in this field.

[0003] CN104353484A discloses a method for preparing a cheap strongly acidic multi-level pore Beta zeolite, and relates to a method for preparing a multi-level pore Beta zeolite. The invention aims to solve the problem of weakened acidity of the existing multi-level pore Beta zeolite molecular sieve after desiliconization. The method comprises: (1) calcining Beta zeolite to obtain microporous hydrogen-type Beta zeolite; (2) adding the microporous hydrogen-type Beta zeolite to an alkaline solution, stirring, washing, and drying to obtain a sodium-type desiliconized multi-level pore Beta zeolite; (3) adding the sodium-type desiliconized multi-level pore Beta zeolite to an ammonium nitrate aqueous solution for exchange, and obtaining a hydrogen-type desiliconized multi-level pore Beta zeolite after calcination; (4) adding the hydrogen-type desiliconized multi-level pore Beta zeolite to an acid solution, stirring, washing, and drying, and then repeating step (3) to obtain a strongly acidic multi-level pore Beta zeolite.

[0004] CN104891526A discloses a method for preparing a mesoporous molecular sieve with high hydrothermal stability. The method comprises the following steps: (1) preparation of a first Y-type molecular sieve precursor: (2) crystallization: adding a seed to the first Y-type molecular sieve precursor, adjusting the pH value to 0.5-5, stirring at 20°C-50°C for 10h-24h, and then aging at 20°C-50°C for 2h-24h to obtain an assembled product, transferring the assembled product to a microreactor with a polytetrafluoroethylene liner, and then transferring it to a high pressure reaction jar together with the reactor, crystallizing at 100°C-200°C for 10h-48h, filtering, washing, and drying to obtain a high-stability mesoporous molecular sieve. First, a precursor of a microporous molecular sieve is prepared, and a meso-microporous molecular sieve is used as a seed for the preparation of a mesoporous molecular sieve, combining the molecular sieve precursor assembly and seeding methods, and obtaining a mesoporous molecular sieve with high stability without using an organic template. It not only greatly reduces the preparation cost of molecular sieves, but also eliminates the process of calcining templates and reduces energy consumption.

[0005] CN102050459A discloses a method for preparing a high-silicon molecular sieve, wherein the method includes allowing the molecular sieve to flow with the inert carrier gas under the carrying of the inert carrier gas flow, and contacting with gas-phase SiCl4 in a flowing state, and the contact time between the molecular sieve and the gas-phase SiCl4 is 10 seconds to 100 minutes. The method for preparing a high-silicon molecular sieve provided by the invention can realize the continuous contact reaction between the molecular sieve and SiCl4, and by controlling the flow rate of the carrier gas and the length of the tubular reactor, the contact time between the molecular sieve and SiCl4 can be controlled, so that the contact reaction between the molecular sieve and SiCl4 can be fully carried out in the tubular reactor. Summary of the invention

[0006] The purpose of the present invention is to provide a hydroisomerization catalyst and to provide the application of the catalyst in the hydroisomerization reaction of hydrocarbon oil feedstock. Specifically, the present invention mainly includes the following contents:

[0007] First, the present invention provides a hydroisomerization catalyst, which comprises a carrier and an active metal component supported on the carrier, wherein the carrier contains a ZSM-48 molecular sieve with a low silicon-to-aluminum ratio, and the preparation method of the ZSM-48 molecular sieve with a low silicon-to-aluminum ratio comprises:

[0008] (1) hydrothermally crystallizing a first mixture of a silicon source, an inorganic base and a first organic template to obtain a pure silicon ZSM-48 molecular sieve intermediate having a relative crystallinity of ≥90%, wherein the molar ratio of the first mixture is: M+ / SiO2=0.01-0.30, R1 / SiO2=0.01-0.50, H2O / SiO2=5-100, M is an alkali metal, and R1 is a first organic template;

[0009] (2) mixing the pure silicon ZSM-48 molecular sieve intermediate obtained in step (1) with an aluminum source, an inorganic base and an optional second organic template to obtain a second mixture, supplementing aluminum and recovering the product, wherein the molar ratio of the second mixture is: SiO2 / Al2O3=5-500, M + / SiO2=0.01~0.30, R2 / SiO2=0~0.50, H2O / SiO2=5~30, R2 is the second organic template.

[0010] Secondly, the present invention also provides a hydrocarbon oil hydroisomerization method, comprising contacting and reacting a raw material oil with any one of the catalysts provided by the present invention under hydroisomerization conditions; the raw material oil is preferably at least one of cracking tail oil, bio-jet fuel production raw materials, C5C6 isomerization raw materials, and Fischer-Tropsch synthesis wax.

[0011] Compared with the catalyst prepared by ZSM-48 molecular sieve obtained by the prior art, when the hydroisomerization catalyst of the present invention is used to carry out hydroisomerization treatment on the raw oil rich in paraffins, the target product obtained has a lower pour point and a high yield of the target product. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The XRD spectrum of the molecular sieve sample synthesized in Preparation Example 1;

[0013] Figure 2 This is the 27Al MAS NMR spectrum of the molecular sieve sample synthesized in Preparation Example 1. DETAILED DESCRIPTION

[0014] First of all, it should be noted that the endpoints and any values ​​of the ranges disclosed in this specification are not limited to the exact ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.

[0015] According to the catalyst provided by the present invention, the silicon-aluminum ratio of the low silicon-aluminum ratio ZSM-48 molecular sieve in the carrier can be adjusted according to actual needs. For example, the molar ratio of silicon oxide to aluminum oxide SiO2 / Al2O3 can be 20 to 500, preferably, SiO2 / Al2O3≤200.

[0016] According to the catalyst provided by the present invention, the aluminum in the ZSM-48 molecular sieve with a low silicon-to-aluminum ratio in the carrier is preferably present in the form of skeleton aluminum.

[0017] The catalyst provided by the present invention further contains an active metal component, the type and content of which are conventionally selected in the art, for example, the active metal component is preferably at least one of the metal components of Group VIII, and further preferably at least one of the noble metal components of Group VIII, such as Pt and / or Pd. The content of the active metal component based on the total amount of the catalyst and in reduced state can be 0.1 to 1.0 wt%.

[0018] In addition, the catalyst may also contain other types of additives that can improve the performance of the catalyst. The types and contents of the additives are conventionally selected in the art, such as commonly used phosphorus additives.

[0019] In order to obtain the catalyst of the present invention, a ZSM-48 molecular sieve with a low silicon-aluminum ratio can be prepared first, and then a carrier is prepared and an active metal component is loaded on the carrier. Under the premise that the active metal component is loaded on the carrier, the present invention has no particular restrictions on the loading method. The preferred method is an impregnation method, including preparing an impregnation solution containing a compound of the metal, and then impregnating the carrier with the solution. The impregnation method is a conventional method, for example, it can be an excess liquid impregnation method or a pore saturation impregnation method. The compound containing the active metal component is selected from one or more of the soluble compounds therein, such as dichlorotetraammineplatinum, chloroplatinic acid, platinum acetate, platinum nitrate, tetrachlorodiamminepalladium, chloropalladic acid, palladium acetate, and palladium nitrate.

[0020] According to the catalyst provided by the present invention, the carrier containing the low silicon-aluminum ratio ZSM-48 molecular sieve may also contain molecular sieves of other configurations and\or heat-resistant inorganic oxides other than molecular sieves, the molecular sieves of other configurations are selected from one or more of ZSM-22 molecular sieves, ZSM-23 molecular sieves, SAPO-11 molecular sieves, ZSM-5 molecular sieves, SSZ-32 molecular sieves and Eu-1 molecular sieves, and the heat-resistant inorganic oxides other than molecular sieves are selected from one or more of alumina, alumina-magnesia, silica-alumina, silica-alumina-titania, silica-alumina-magnesia, and silica-alumina-zirconium oxide; based on the carrier, the content of the ZSM-48 molecular sieve is 10-100wt%, the content of the molecular sieves of other configurations is 0-90wt%, and the content of the heat-resistant inorganic oxides other than molecular sieves is 0-60wt%. The method of forming a carrier by combining ZSM-48 molecular sieve with other molecular sieves and / or heat-resistant inorganic oxides is a conventional method in the art. Generally, the carrier raw materials can be mixed with appropriate additives for extrusion molding, and then dried and optionally calcined to obtain the corresponding carrier.

[0021] When the catalyst also contains an auxiliary agent, the method for introducing the auxiliary agent component can be any method, such as preparing a compound containing the auxiliary agent component and a compound containing the active metal component into a mixed solution and then impregnating the carrier; or preparing a solution of the compound containing the auxiliary agent component separately and then impregnating the carrier and roasting it. When the auxiliary agent component and the active metal are introduced into the carrier separately, it is preferred that the carrier is first impregnated with a solution containing the auxiliary agent component compound and roasted, and then impregnated with a solution containing the active metal component compound. Wherein, the roasting temperature is 400-600°C, preferably 420-500°C, and the roasting time is 2-6 hours, preferably 3-6 hours.

[0022] According to the catalyst provided by the present invention, the silicon source, aluminum source and template in the step of preparing the low silicon-aluminum ratio ZSM-48 molecular sieve are all conventionally selected in the art. For example, the silicon source is a silicon-containing compound that can be stably dispersed in an aqueous phase and form a uniform colloidal solution, preferably at least one of silica sol, white carbon black or tetraethyl orthosilicate; the aluminum source is selected from one or more of aluminum chloride, aluminum sulfate, aluminum hydroxide, sodium aluminate and aluminum sol, preferably sodium aluminate and / or aluminum sol; the first organic template and the second organic template are independently selected from ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, and a mixture of one or more of the above diamines with substituents; the preferred organic template is selected from ethylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, and at least one of the above diamines with substituents, preferably 1,6-hexanediamine. When a template is added in step (2), the second template is preferably the same as the first template, and more preferably, the first template and the second template are both 1,6-hexanediamine. The inorganic base is preferably NaOH and / or KOH.

[0023] According to the catalyst of the present invention, the raw material ratio can be adjusted according to the requirements of the silicon-aluminum ratio in the final low silicon-aluminum ratio ZSM-48 molecular sieve. Preferably, in the hydrothermal crystallization step, the molar ratio of the first mixture is: + / SiO2=0.01~0.20、R1 / SiO2=0.03~0.30、H2O / SiO2=20~50;In the aluminum supplementation step, the molar ratio of the second mixture is: SiO2 / Al2O3=20~200、M + / SiO2=0.01~0.20, R2 / SiO2=0~0.20, H2O / SiO2=5~20.

[0024] According to the catalyst provided by the present invention, the purpose of the hydrothermal crystallization in step (1) is to obtain a pure silicon ZSM-48 molecular sieve intermediate with a crystallinity of ≥90%, preferably ≥95%, the temperature of the hydrothermal crystallization is preferably 100-180°C, more preferably 140-180°C, and the time of the hydrothermal crystallization is preferably 4-240h, more preferably 12-96h. In the present invention, the pure silicon molecular sieve refers to a molecular sieve with a silicon-aluminum molecular ratio greater than 500 as determined by the XRF method, which does not contain aluminum or contains a very small amount of aluminum introduced by the silicon source itself. Therefore, in order to obtain a pure silicon molecular sieve with a higher purity, no aluminum source is added in step (1), and the silicon source can be controlled. Preferably, SiO2 / Al2O3 in the silicon source is not less than 300.

[0025] According to the catalyst of the present invention, the pure silicon ZSM-48 molecular sieve obtained in step (1) is used as an intermediate product, and its form is selected from one of the following: (a) molecular sieve slurry; (b) molecular sieve filter cake after filtering and washing the molecular sieve slurry; (c) molecular sieve raw powder filtered, washed and dried; (d) molecular sieve filtered, washed, dried and calcined to remove the organic template. Then the intermediates in various forms are subjected to the reaction of step (2). In order to better obtain a pure silicon ZSM-48 molecular sieve intermediate that meets the requirements, a small amount of pure silicon ZSM-48 seeds can be added to the first mixture. The small amount is relative to the total amount of pure silicon ZSM-48 molecular sieve prepared in step (1), for example, the added pure silicon ZSM-48 seeds are within 1 weight %, or within 0.5 weight %, or within 0.1 weight % of the total pure silicon ZSM-48 molecular sieve.

[0026] In addition, the hydrocarbon oil hydroisomerization method provided by the present invention comprises contacting the feedstock oil with the catalyst provided by the present invention under hydroisomerization conditions. The hydroisomerization conditions are conventional conditions. For example, in the method of the present invention, the hydroisomerization conditions are not particularly limited, as long as they are sufficient to cause the feedstock oil to undergo a hydroisomerization reaction. Generally, the reaction conditions may include: a temperature of 200-500°C, preferably 250-400°C, and more preferably 300-350°C; a pressure of 1-30MPa, preferably 2-20MPa, and more preferably 5-20MPa, and the pressure described herein refers to absolute pressure; a space velocity of 0.1-5h-1, preferably 0.1-3h-1, and more preferably 0.5-2h-1; a hydrogen-to-oil volume ratio of 50-3000, preferably 300-3000, and more preferably 400-600.

[0027] The present invention will be described in detail below through examples.

[0028] In the embodiment, the chemical composition of the molecular sieve is determined by X-ray fluorescence. The relative crystallinity is expressed as a percentage of the sum of the peak heights of two characteristic diffraction peaks at 2θ between 20 and 24° in the X-ray diffraction (XRD) spectra of the obtained product and the ZSM-48 molecular sieve standard. The ZSM-48 molecular sieve synthesized by the method of Example 5 in US4423021 is used as the standard sample, and its crystallinity is set to 100%. XRD is measured on a SIMENS D5005 X-ray diffractometer, CuKα radiation, 44 kV, 40 mA, and a scanning speed of 2 / min.

[0029] The 27Al MAS NMR spectrum was obtained by a Bruker AVANCE Ⅲ 600WB nuclear magnetic resonance spectrometer. The test conditions were: resonance frequency 78.155 MHz, magic angle speed 5 kHz, pulse width 1.6 μs, cycle delay time 1 s, and scan times 8000 times.

[0030] Preparation Example 1

[0031] 400 g of silica sol (Shandong Yiming Industry and Trade Co., Ltd., 30% SiO2), 7 g of NaOH, 48 g of 1,6-hexanediamine (analytical grade, Sinopharm Chemical Reagent Co., Ltd.) and 260 g of water were fully mixed, and the reaction mixture had the following composition (mole / mole, expressed in the form of oxide): M + / SiO2=0.1;R / SiO2=0.2;H2O / SiO2=15. The mixture was placed in a crystallization kettle and heated to 160℃, and hydrothermally crystallized for 48h. After the crystallization was completed, it was filtered, washed and dried to obtain pure silicon ZSM-48 molecular sieve raw powder with a crystallinity of 90%.

[0032] The molecular sieve was aluminum-supplemented. 20 g of the above pure silicon molecular sieve was mixed evenly with 2.26 g of sodium aluminate, 0.8 g of NaOH, and 53 g of water. The mixture had the following composition (mol / mol, expressed in the form of oxides): SiO2 / Al2O3=110, M + / SiO2=0.1,H2O / SiO2=9. The mixture was mixed evenly and then put into a crystallization kettle and heated to 150℃ for hydrothermal crystallization for 23h. After the crystallization, the silicon-alumina molecular sieve S1 was obtained by filtration, washing and drying.

[0033] XRD test ( Figure 1 ), sample S1 is ZSM-48, with a relative crystallinity of 99% and a silicon-aluminum ratio of 100. From the 27Al MAS NMR spectrum ( Figure 2 ) It can be seen that all the aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum.

[0034] Preparation Example 2

[0035] 281 g of tetraethyl orthosilicate (containing 28% SiO2, Beijing Chemical Reagent Company), 10.5 g of NaOH, 16.5 g of 1,6-hexanediamine and 378 g of water were fully mixed, and the reaction mixture had the following composition (mol / mol, expressed in the form of oxide): M + / SiO2=0.2;R / SiO2=0.1;H2O / SiO2=16. The mixture was placed in a crystallization kettle and heated to 160℃, and hydrothermal dynamic crystallization was performed for 48h. After the crystallization was completed, the molecular sieve slurry (the molecular sieve slurry was filtered, washed, and dried, and the crystallinity of the obtained pure silicon molecular sieve was measured to be 91%) was directly used for aluminum supplementation.

[0036] The above pure silicon molecular sieve slurry containing 20g of dry basis was mixed with 4.9g of sodium aluminate, 1g of NaOH, 0.5g of 1,6-hexanediamine and an appropriate amount of water to obtain a mixture having the following composition (mol / mol, expressed in the form of oxide): SiO2 / Al2O3=51, M + / SiO2=0.17,R / SiO2=0.01,H2O / SiO2=20. The mixture was mixed evenly and then put into a crystallization kettle and heated to 160℃ for hydrothermal crystallization for 24h. After the crystallization, the silicon-alumina molecular sieve S2 was obtained by filtration, washing and drying.

[0037] XRD testing showed that sample B2 was ZSM-48 with a relative crystallinity of 98% and a silicon-aluminum ratio of 50. The 27Al MAS NMR spectrum showed that all aluminum was inserted into the framework to produce framework aluminum, with no obvious non-framework aluminum.

[0038] Preparation Example 3

[0039] 200 g of silica sol, 6.7 g of NaOH, 18 g of 1,6-hexanediamine and 220 g of water were fully mixed, and the reaction mixture had the following composition (mol / mol, expressed in the form of oxide): M + / SiO2=0.167;R / SiO2=0.15;H2O / SiO2=20. The mixture was placed in a crystallization kettle and heated to 140℃, and hydrothermally crystallized for 48h. After the crystallization was completed, the mixture was filtered, washed and dried to obtain pure silicon ZSM-48 molecular sieve raw powder with a crystallinity of 93%.

[0040] 31 g of pure silicon molecular sieve was mixed with 4.8 g of sodium aluminate, 2 g of NaOH, 14 g of 1,6-hexanediamine (analytical grade, Sinopharm Chemical Reagent Co., Ltd.), and 137 g of water. The mixture had the following composition (mol / mol, expressed in oxide form): SiO2 / Al2O3=80, M + / SiO2=0.15,R / SiO2=0.23,H2O / SiO2=15. The mixture was mixed evenly and then put into a crystallization kettle and heated to 160℃ for hydrothermal crystallization for 20h. After the crystallization, the molecular sieve S3 was obtained by filtration, washing and drying.

[0041] XRD test shows that sample S3 is ZSM-48, with a relative crystallinity of 105% and a silicon-aluminum ratio of 78. The 27Al MAS NMR spectrum shows that all aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum. The relative crystallinity of S3 is 105%, and the silicon-aluminum ratio is 78.

[0042] Preparation Example 4

[0043] 200 g of silica sol, 10 g of NaOH, 12 g of 1,6-hexanediamine and 400 g of water were mixed thoroughly, and the reaction mixture had the following composition (mol / mol, expressed in the form of oxide): M + / SiO2=0.25;R / SiO2=0.1;H2O / SiO2=30. The mixture was placed in a crystallization kettle and heated to 160℃, and hydrothermal dynamic crystallization was performed for 48h. After the crystallization was completed, it was filtered, washed, dried, and calcined at 580℃ for 3h to obtain pure silicon ZSM-48 molecular sieve (crystallinity 95%).

[0044] The molecular sieve was aluminum-supplemented. 20 g of the above pure silicon molecular sieve was mixed evenly with 5 g of sodium aluminate, 1.4 g of NaOH, and 120 g of water. The mixture had the following composition (mol / mol, expressed in the form of oxides): SiO2 / Al2O3=50, M + / SiO2=0.2,H2O / SiO2=20. The mixture was mixed evenly and then put into a crystallization kettle and heated to 160℃ for hydrothermal crystallization for 23h. After the crystallization, the silicon-alumina molecular sieve S4 was obtained by filtration, washing and drying.

[0045] According to XRD test, sample S4 is ZSM-48, with a relative crystallinity of 102% and a silicon-aluminum ratio of 48. The 27Al MAS NMR spectrum shows that all aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum.

[0046] Preparation Example 5

[0047] 140 g of tetraethyl orthosilicate (containing 28% SiO2, Beijing Chemical Reagent Company), 2.2 g of NaOH, 16 g of 1,6-hexanediamine and 360 g of water were fully mixed, and the reaction mixture had the following composition (mol / mol, expressed in the form of oxide): M + / SiO2=0.08;R / SiO2=0.2;H2O / SiO2=30. The mixture was placed in a crystallization kettle and heated to 160℃, and hydrothermal dynamic crystallization was performed for 48h. After the crystallization was completed, the molecular sieve slurry (the molecular sieve slurry was filtered, washed and dried, and the crystallinity of the obtained pure silicon molecular sieve was measured to be 96%) was directly used for aluminum supplementation.

[0048] The above pure silicon molecular sieve slurry containing 40g of dry basis was mixed with 4.9g of sodium aluminate, 0.08g of NaOH, 8g of 1,6-hexanediamine and an appropriate amount of water to obtain a mixture having the following composition (mol / mol, expressed in the form of oxide): SiO2 / Al2O3=102, M + / SiO2=0.05,R / SiO2=0.1,H2O / SiO2=20. The mixture was mixed evenly and then put into a crystallization kettle and heated to 160℃ for hydrothermal crystallization for 24h. After the crystallization, the silicon-alumina molecular sieve S5 was obtained by filtration, washing and drying.

[0049] According to XRD testing, sample B5 is ZSM-48, with a relative crystallinity of 105% and a silicon-aluminum ratio of 99. The 27Al MAS NMR spectrum shows that all aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum.

[0050] Preparation Example 6

[0051] 200 g of silica sol, 4 g of NaOH, 30 g of 1,6-hexanediamine and 220 g of water were fully mixed, and the reaction mixture had the following composition (mol / mol, expressed in the form of oxide): M + / SiO2=0.1;R / SiO2=0.25;H2O / SiO2=20. The mixture was placed in a crystallization kettle and heated to 140℃, and hydrothermal dynamic crystallization was performed for 48h. After the crystallization was completed, the ZSM-48 filter cake was used as an intermediate product for the next step of aluminum supplementation, and the molecular sieve crystallinity was measured to be 95%.

[0052] 58 g of pure silicon molecular sieve was mixed with 4.8 g of sodium aluminate, 4.5 g of NaOH, 23 g of 1,6-hexanediamine (analytical grade, Sinopharm Chemical Reagent Co., Ltd.), and 310 g of water. The mixture had the following composition (mole / mole, expressed in the form of oxide): SiO2 / Al2O3=151, M + / SiO2=0.15,R / SiO2=0.2,H2O / SiO2=18. The mixture was mixed evenly and then put into a crystallization kettle and heated to 160℃ for hydrothermal crystallization for 20h. After the crystallization, the silicon-alumina molecular sieve S6 was obtained by filtration, washing and drying.

[0053] According to XRD test, sample S6 is ZSM-48, with a relative crystallinity of 105% and a silicon-aluminum ratio of 140. The 27Al MAS NMR spectrum shows that all aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum.

[0054] Preparation Example 7

[0055] 200 g of silica sol, 4 g of NaOH, 16 g of 1,5-pentanediamine and 185 g of water were mixed thoroughly, and the reaction mixture had the following molar composition: M + / SiO2=0.1、R / SiO2=0.15、H2O / SiO2=18. The mixture was placed in a crystallization kettle and heated to 150℃, and hydrothermal dynamic crystallization was performed for 50h. After the crystallization was completed, the molecular sieve raw powder obtained after filtration, washing and drying was used as an intermediate product for the next step of aluminum supplementation, and the crystallinity was 95%.

[0056] The intermediate product was hydrothermally aluminum-filled. 40 g of pure silicon molecular sieve was evenly mixed with 4.8 g of sodium aluminate, 4.5 g of NaOH, 6 g of 1,5-pentanediamine, and 250 g of water. The mixture had the following molar composition: SiO2 / Al2O3=104, M + / SiO2=0.21、R / SiO2=0.08、H2O / SiO2=21. The mixture was mixed evenly and then put into a crystallization kettle and heated to 100℃ and aluminum was added for 24h. After the crystallization was completed, the molecular sieve sample S7 was obtained by filtration, washing and drying.

[0057] According to XRD test, sample S7 is ZSM-48, with a relative crystallinity of 101% and a silicon-aluminum ratio of 98. The 27Al MAS NMR spectrum shows that all aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum.

[0058] Preparation Example 8

[0059] 195 g of silica sol, 4 g of NaOH, 20 g of 1,7-heptanediamine and 145 g of water were mixed thoroughly to obtain a reaction mixture having the following molar composition: + / SiO2=0.1、R / SiO2=0.15、H2O / SiO2=16. The mixture was placed in a crystallization kettle and heated to 140℃ for hydrothermal dynamic crystallization for 48h. After the crystallization was completed, the molecular sieve raw powder obtained after filtration, washing and drying was used as an intermediate product for the next step of aluminum supplementation, with a crystallinity of 92%.

[0060] The intermediate product was hydrothermally aluminum-filled. 42 g of pure silicon molecular sieve was evenly mixed with 4.8 g of sodium aluminate, 4.5 g of NaOH, 7 g of 1,7-heptanediamine, and 230 g of water. The mixture had the following molar composition: SiO2 / Al2O3=109, M + / SiO2=0.20、R / SiO2=0.07、H2O / SiO2=18. The mixture was mixed evenly and then put into a crystallization kettle and heated to 100℃ and aluminum was added for 24h. After the crystallization was completed, the molecular sieve sample S8 was obtained by filtration, washing and drying.

[0061] XRD testing showed that sample S8 was ZSM-48 with a relative crystallinity of 96% and a silicon-aluminum ratio of 101. The 27Al MAS NMR spectrum showed that all aluminum was inserted into the framework to produce framework aluminum, with no obvious non-framework aluminum.

[0062] Preparation Example 9

[0063] Take 45g of white carbon black, 1.25g of analytically pure Al2(SO4)3·18H2O, 1.88g of analytically pure NaOH and 39.3g of hexamethylenediamine for standby use. Mix hexamethylenediamine with white carbon black and 200g of deionized water, mix NaOH with Al2(SO4)3·18H2O and 272g of deionized water, then mix the two solutions, stir for 1h and transfer to a reactor, crystallize at 160°C for 72h. After the crystallization is completed, filter, wash and dry to obtain silicon-aluminum structure molecular sieve S9.

[0064] According to XRD test, sample S9 is ZSM-48, with a relative crystallinity of 99% and a silicon-aluminum ratio of 190. The 27Al MAS NMR spectrum shows that all aluminum is inserted into the framework to produce framework aluminum, and there is no obvious non-framework aluminum.

[0065] Preparation Example 10

[0066] 400 g of silica sol, 13.56 g of sodium aluminate, 48 g of 1,6-hexanediamine, 4.8 g of NaOH and 315 g of water were mixed evenly, and the mixture had the following molar composition: SiO2 / Al2O3=110, M + / SiO2=0.1, R / SiO2=0.2, H2O / SiO2=9, the mixture was mixed evenly and then put into a crystallization kettle and heated to 160℃ for hydrothermal crystallization for 50h. After the crystallization, the molecular sieve sample S10 was obtained by filtration, washing and drying. The XRD test showed that the sample was ZSM-22 molecular sieve with a silicon-aluminum ratio of 98.

[0067] Preparation Example 11

[0068] The same as Example 1, except that the hydrothermal dynamic crystallization was changed to 12h, 24h and 36h respectively, and the corresponding ZSM-48 molecular sieve intermediate product crystallinity was 0%, 26% and 78% respectively. The above three ZSM-48 molecular sieves that were not completely crystallized were hydrothermally aluminum-filled to obtain three molecular sieve samples S11-13 respectively. According to XRD test, all three samples were ZSM-5 molecular sieves with a silicon-aluminum ratio of 98.

[0069] Evaluation Examples and Comparative Examples

[0070] Catalysts C1-C8 were prepared using molecular sieves S1-S8 obtained in the above-mentioned Preparation Examples 1-8, and catalysts DC1 and DC2 were prepared using molecular sieves S9 and S14 obtained in the above-mentioned Preparation Examples 9 and 12, respectively, as follows: 60 grams of molecular sieve and 20 grams of alumina were weighed, mixed with 80 grams of a 2 wt% nitric acid solution, formed on an extruder, and calcined at 600°C for 4 hours to obtain a carrier.

[0071] A 2wt% tetraammine dichloroplatinum impregnation solution was prepared, and the carrier was impregnated with the impregnation solution to load 0.5% Pt on the carrier, and then calcined in air at 400°C for 4h and reduced in hydrogen at 400°C for 4h to obtain a catalyst.

[0072] Evaluation Example

[0073] The following evaluation methods are used to evaluate C1-C8 and DC1:

[0074] 50g of catalyst was loaded into a high-pressure hydrogenation reactor. The hydrocracking tail oil raw material was injected into the reactor from top to bottom for reaction, and the reaction conditions were shown in Table 1. After the reaction, the product was distilled to remove the light components less than 370 degrees, and the components greater than 370 degrees were analyzed and the yield was calculated. The properties of the hydrocracking tail oil raw material are shown in Table 2, and the catalyst evaluation results are shown in Table 3.

[0075] Table 1 Reaction conditions

[0076] Reaction conditions Condition 1 Condition 2 Pressure, MPa 15.0 15.0 <![CDATA[Air speed, h -1 > 0.8 0.8 Reaction temperature, °C 330 340 Hydrogen to oil ratio, v / v 500 500

[0077] Table 2

[0078] Analyze Project Analyze the data Analytical methods 20℃ density / (kg / m3) 837.6 SH / T0604-2000 Kinematic viscosity / (mm2 / s) 80℃ 7.214 GB / T 265-88 100℃ 4.744 GB / T 265-88 Pour point / ℃ +37 Nitrogen mass fraction / (μg / g) <1 Sulfur mass fraction / (μg / g) 10 SH / T 0842-2010

[0079] Table 3

[0080]

[0081] It can be seen from the data in Table 3 above that the target product obtained by hydrotreating the oil rich in paraffins using the hydroisomerization catalyst of the present invention has a high yield and a low pour point.

[0082] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A hydroisomerization catalyst comprising a carrier and an active metal component supported on the carrier, characterized in that: The carrier contains a ZSM-48 molecular sieve with a low silicon-to-aluminum ratio, and the aluminum in the ZSM-48 molecular sieve with a low silicon-to-aluminum ratio exists in the form of skeleton aluminum; the preparation method of the ZSM-48 molecular sieve with a low silicon-to-aluminum ratio comprises: (1) hydrothermally crystallizing a first mixture of a silicon source, an inorganic base and a first organic template to obtain a pure silicon ZSM-48 molecular sieve intermediate having a relative crystallinity of ≥90%, wherein the molar ratio of the first mixture is: + / SiO2=0.01~0.30, R1 / SiO2=0.01~0.50, H2O / SiO2=5~100, M is an alkali metal, R1 is a first organic template; the conditions of the hydrothermal crystallization include: a temperature of 140~180℃, and a time of 48~96h; (2) mixing the pure silicon ZSM-48 molecular sieve intermediate obtained in step (1) with an aluminum source, an inorganic base, and a second organic template to obtain a second mixture, supplementing aluminum and recovering the product, wherein the molar ratio of the second mixture is: SiO2 / Al2O3=5-500, M + / SiO2=0.01~0.30, R2 / SiO2=0~0.50, H2O / SiO2=5~30, R2 is the second organic template; Wherein, the silicon source is a silicon-containing compound that can be stably dispersed in an aqueous phase and form a uniform colloidal solution; the aluminum source is selected from one or more of aluminum chloride, aluminum sulfate, aluminum hydroxide, sodium metaaluminate and aluminum sol; The first template and the second template are both 1,6-hexanediamine.

2. The catalyst according to claim 1, characterized in that The active metal component is selected from at least one of the noble metal components of Group VIII, and the content of the active metal component is 0.1-1.0 wt % based on the catalyst and in reduced state.

3. The catalyst according to claim 1, characterized in that The carrier may also contain molecular sieves of other configurations and / or heat-resistant inorganic oxides other than molecular sieves, wherein the molecular sieves of other configurations are one or more selected from ZSM-22 molecular sieve, ZSM-23 molecular sieve, SAPO-11 molecular sieve, ZSM-5 molecular sieve, SSZ-32 molecular sieve and Eu-1 molecular sieve, and the heat-resistant inorganic oxides other than molecular sieves are one or more selected from alumina, alumina-magnesia, silica-alumina, silica-alumina-titania, silica-alumina-magnesia, silica-alumina-zirconium oxide; based on the carrier, the content of the ZSM-48 molecular sieve with a low silicon-aluminum ratio is 10-100wt%, the content of the molecular sieves of other configurations is 0-90wt%, and the content of the heat-resistant inorganic oxides other than molecular sieves is 0-60wt%.

4. The catalyst according to claim 1, characterized in that The molar ratio of silicon oxide to aluminum oxide in the low silicon-aluminum ratio ZSM-48 molecular sieve is SiO2 / Al2O3≤200.

5. The catalyst according to claim 1, characterized in that The silicon source is at least one of silica sol, white carbon black or ethyl orthosilicate; the aluminum source is selected from sodium aluminate and / or aluminum sol.

6. The catalyst according to claim 1, characterized in that The molar ratio of the first mixture is: + / SiO2=0.01~0.20、R1 / SiO2=0.03~0.30、H2O / SiO2=20~50;The molar ratio of the second mixture is:SiO2 / Al2O3=20~200、M + / SiO 2 =0.01~0.20, R2 / SiO2=0~0.20, H2O / SiO2=5~20.

7. The catalyst according to claim 1, characterized in that The inorganic base is NaOH and / or KOH.

8. The catalyst according to claim 1, characterized in that The crystallinity of the pure silicon ZSM-48 molecular sieve intermediate in step (1) is ≥95%.

9. The catalyst according to claim 1, characterized in that A small amount of pure silicon ZSM-48 seed crystals is added to the first mixture.

10. A method for hydroisomerization of hydrocarbon oil, comprising contacting and reacting a raw oil with the catalyst according to any one of claims 1 to 9.

11. The method according to claim 10, characterized in that The raw oil is selected from at least one of cracking tail oil, bio-jet fuel production raw materials, C5C6 isomerization raw materials, and Fischer-Tropsch synthesis wax.