Bimetallic phosphide and its preparation method and application

Through the preparation method of bimetallic phosphide, iron-cobalt Prussian blue is used as the precursor for phosphating treatment to prepare a bimetallic phosphide catalyst with a porous structure, which solves the problem of high cost of precious metal catalysts and improves electrocatalytic activity and stability. , suitable for electrolyzing water to produce hydrogen and electrode materials.

CN113772644BActive Publication Date: 2024-10-25DONGGUAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010518266.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-09
Publication Date
2024-10-25
Estimated Expiration
2040-06-09

AI Technical Summary

Technical Problem

In existing electrochemical water splitting methods for hydrogen production, the scarcity and high cost of precious metal catalysts limit their wide application in industrial production, resulting in high overpotential and high energy consumption for water splitting.

Method used

A bimetallic phosphide preparation method is used to prepare iron-cobalt Prussian blue through co-precipitation reaction of potassium ferricyanide and cobalt salt, and then phosphating is performed under a protective atmosphere to prepare a bimetallic phosphide with a porous structure. , as a low-cost catalyst.

Benefits of technology

This method reduces the charge transfer interface resistance and surface reaction kinetic energy barrier, improves the catalytic efficiency and stability of the catalyst, provides better conductivity and electron transport capabilities, and is suitable for the fields of electrolyzing water for hydrogen production and electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113772644B_ABST
    Figure CN113772644B_ABST
Patent Text Reader

Abstract

The present invention relates to a bimetallic phosphide and a preparation method and application thereof. The preparation method of the bimetallic phosphide comprises the following steps: coprecipitating potassium ferrocyanide and cobalt salt to prepare iron-cobalt Prussian blue; and phosphating the iron-cobalt Prussian blue under a protective atmosphere to prepare the bimetallic phosphide. The preparation method of the bimetallic phosphide is simple, and the raw materials used are low in cost and easy to obtain, and industrial-scale production can be achieved. The bimetallic phosphide prepared by the method has a rich porous structure, a regular cubic block morphology, and a relatively uniform particle size, and has broad application prospects in the field of catalysts or electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal phosphides, and in particular to a bimetallic phosphide and a preparation method and application thereof. Background Art

[0002] With the continuous consumption of fossil fuels, various new energy output plans have attracted wide attention in order to meet today's huge energy demand. Hydrogen energy, as a clean energy with less pollution, is expected to become the most effective substitute for fossil fuels.

[0003] The main method for preparing hydrogen energy is electrochemical water decomposition (hydrogen evolution reaction, HER). Electrochemical water decomposition is to pass direct current into an electrolyzer filled with electrolyte to make water molecules undergo electrochemical reactions on the electrodes and decompose into hydrogen and oxygen. This method has the advantages of high efficiency, environmental friendliness, high gas purity, and strong adaptability to energy fluctuations. In order to further reduce the overpotential of water decomposition and reduce the energy consumed by the reaction, catalysts are generally added. Precious metals such as Pt, Pd and their oxides have excellent catalytic activity for electrocatalytic water decomposition, but the scarcity and high cost of precious metal-based catalysts prevent them from being widely used in industrial production. Summary of the invention

[0004] Based on this, it is necessary to provide a low-cost bimetallic phosphide that can be used to prepare a catalyst for hydrogen production by electrolysis of water and a preparation method thereof.

[0005] A method for preparing a bimetallic phosphide comprises the following steps:

[0006] Co-precipitation of potassium ferrocyanide and cobalt salt to produce iron-cobalt Prussian blue; and

[0007] Under a protective atmosphere, the iron-cobalt Prussian blue is subjected to phosphating treatment to prepare a bimetallic phosphide.

[0008] The preparation method of the above-mentioned bimetallic phosphide is simple, and the raw materials used are low-cost and easy to obtain, and industrial-scale production can be achieved. The bimetallic phosphide prepared according to the method has a rich porous structure, a regular cubic block morphology, and a relatively uniform particle size, and has broad application prospects in the field of catalysts or electrode materials.

[0009] In addition, the preparation method of the above-mentioned bimetallic phosphide uses a Prussian blue analog as a bimetallic precursor, and the unique bimetallic phosphide prepared by phosphating can exert the synergistic effect of two different metal ions, change the electronic structure of the catalyst, and provide more surface reaction active sites, thereby improving the catalytic efficiency and stability of the catalyst. Therefore, compared with single metal phosphides, bimetallic phosphides not only have better conductivity and are more conducive to electron transport, but also can further reduce the interface resistance of charge transfer and the surface reaction kinetic energy barrier, further improving the electrocatalytic activity.

[0010] In one embodiment, the chemical formula of the iron-cobalt Prussian blue is Fe 0.667 Co(CN)4(H2O)4.

[0011] In one embodiment, the step of co-precipitating potassium ferrocyanide and cobalt salt comprises: mixing a complexing agent, the potassium ferrocyanide, the cobalt salt and water for reaction.

[0012] In one embodiment, the step of mixing the complexing agent, the potassium ferrocyanide, the cobalt salt and water comprises:

[0013] Dissolve potassium ferrocyanide in water to form a potassium ferrocyanide solution;

[0014] dissolving a cobalt salt in water to form a cobalt salt solution; and

[0015] The potassium ferrocyanide solution, the cobalt salt solution and the complexing agent are mixed and reacted.

[0016] In one embodiment, the complexing agent is selected from at least one of sodium citrate and citric acid.

[0017] In one embodiment, the cobalt salt is selected from at least one of cobalt nitrate, cobalt sulfate, cobalt carbonate, cobalt chloride, cobalt bromide, cobalt iodide and cobalt fluoride.

[0018] In one embodiment, the phosphorus source in the phosphating treatment is selected from at least one of sodium hypophosphite, potassium hypophosphite and phosphine.

[0019] In one embodiment, the phosphating treatment temperature is 350°C to 650°C.

[0020] A bimetallic phosphide, the bimetallic phosphide is a porous cubic block of iron-cobalt phosphide, the particle size of the bimetallic phosphide is 300nm-350nm, and the pore volume of the bimetallic phosphide is 0.65cm 3 / g~0.75cm 3 / g, and the pore size of the bimetallic phosphide is 45nm-55nm.

[0021] The bimetallic phosphide prepared by the above-mentioned preparation method of the bimetallic phosphide or the use of the above-mentioned bimetallic phosphide in the preparation of catalysts or electrode materials.

[0022] A catalyst for producing hydrogen by electrolyzing water comprises the bimetallic phosphide prepared by the above-mentioned preparation method of the bimetallic phosphide or the above-mentioned bimetallic phosphide.

[0023] An electrode comprises an electrode active material, wherein the electrode active material comprises the bimetallic phosphide prepared by the above-mentioned preparation method of the bimetallic phosphide or the above-mentioned bimetallic phosphide. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a scanning electron microscope image of the iron-cobalt Prussian blue of Example 1;

[0025] Figure 2 is a transmission electron microscope image of the iron-cobalt Prussian blue of Example 1;

[0026] Figure 3 is a scanning electron microscope image of the bimetallic phosphide of Example 1;

[0027] Figure 4 is a transmission electron microscope image of the bimetallic phosphide of Example 1;

[0028] Figure 5 This is a scanning electron microscope image of the metal phosphide of Comparative Example 1. DETAILED DESCRIPTION

[0029] In order to facilitate understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0031] One embodiment of the present invention provides a method for preparing a bimetallic phosphide. The method for preparing the bimetallic phosphide is simple, and the raw materials used are low-cost and easy to obtain, and industrial-scale production can be achieved. The bimetallic phosphide prepared according to the method has a rich porous structure, a regular cubic block morphology, and a relatively uniform particle size. Compared with metal phosphides prepared by traditional methods, the precursor of the method can be prepared at room temperature, and the bimetallic phosphide prepared according to the method has a more regular morphology and a more prominent three-dimensional porous structure, and has broad application prospects in the field of catalysts or electrode materials.

[0032] Specifically, the preparation method of the bimetallic phosphide includes steps S110 to S120:

[0033] Step S110: coprecipitating potassium ferrocyanide and cobalt salt to produce iron-cobalt Prussian blue.

[0034] Specifically, potassium ferrocyanide and cobalt salt are dissolved in water to carry out a coprecipitation reaction to prepare iron-cobalt Prussian blue.

[0035] Prussian Blue (PB), also known as ferric ferrocyanide, Berlin Blue, Gong Blue, Iron Blue, Milori Blue, Milori Blue, Chinese Blue, Hualan, Mineral Blue, has a chemical formula of Fe4[Fe(CN)6]3. It is a metal organic framework compound (MOF) with a simple structure, easy preparation, low price and a long history. A large number of Prussian blue analogs can be prepared by selecting appropriate transition metal ions (Co, Fe, Ni, Mn, Pt, Cr, etc.) to replace the divalent iron ions and trivalent iron ions in Prussian blue.

[0036] Prussian blue analogs have the advantages of adjustable morphology, good molecular-level tuning ability, high porosity and high specific surface area. Using Prussian blue analogs as bimetallic precursors, the unique bimetallic phosphide prepared by phosphating can play the synergistic effect of two different metal ions, change the electronic structure of the catalyst, and provide more surface reaction active sites, thereby improving the catalytic efficiency and stability of the catalyst. Therefore, compared with single metal phosphides, bimetallic phosphides not only have better conductivity and are more conducive to electron transport, but also can further reduce the interfacial resistance of charge transfer and the surface reaction kinetic energy barrier, further improving the electrocatalytic activity.

[0037] Specifically, the cobalt salt is a water-soluble divalent cobalt salt. Further, the cobalt salt is selected from at least one of cobalt nitrate, cobalt sulfate, cobalt carbonate, cobalt chloride, cobalt bromide, cobalt iodide and cobalt fluoride. It should be noted that the acid cobalt can be anhydrous cobalt nitrate or hexahydrate cobalt nitrate. Further, the cobalt salt is selected from one of cobalt nitrate, cobalt sulfate, cobalt carbonate, cobalt chloride, cobalt bromide, cobalt iodide and cobalt fluoride.

[0038] More specifically, a complexing agent, potassium ferrocyanide and a cobalt salt are mixed and reacted to produce iron-cobalt Prussian blue. The complexing agent complexes with metal ions and slowly releases the metal ions, thereby avoiding crystal structure defects of the produced iron-cobalt Prussian blue caused by an extremely fast reaction speed.

[0039] In one embodiment, the complexing agent is selected from at least one of sodium citrate and citric acid. Preferably, the complexing agent is selected from one of citric acid and sodium citrate.

[0040] In one embodiment, the step of mixing the complexing agent, potassium ferrocyanide and cobalt salt for reaction comprises: dissolving potassium ferrocyanide in water to form a potassium ferrocyanide solution; dissolving cobalt salt in water to form a cobalt salt solution; and mixing the potassium ferrocyanide solution, the cobalt salt solution and the complexing agent for reaction. Dissolving potassium ferrocyanide and cobalt salt in water respectively and then mixing with the complexing agent for reaction facilitates the uniform reaction of potassium ferrocyanide and cobalt salt, and the formed iron-cobalt Prussian blue has a uniform morphology. Of course, in some other embodiments, it is not necessary to separately prepare potassium ferrocyanide and cobalt salt into solutions and then mix them for reaction. Potassium ferrocyanide, cobalt salt and complexing agent can also be dissolved in water together.

[0041] Specifically, the temperature of the mixed reaction of the complexing agent, potassium ferrocyanide and cobalt salt is 15° C. to 50° C. In one embodiment, the temperature of the mixed reaction of the complexing agent, potassium ferrocyanide and cobalt salt is 15° C. to 30° C. Carrying out the reaction at a lower temperature is conducive to improving the morphological uniformity of the formed iron-cobalt Prussian blue.

[0042] Specifically, the mixing method of the complexing agent, potassium ferrocyanide and cobalt salt is stirring mixing. Of course, in some other embodiments, the mixing method of the complexing agent, potassium ferrocyanide and cobalt salt is not limited to stirring mixing, and can also be other mixing methods commonly used in the art.

[0043] Specifically, the reaction time of the mixed reaction of the complexing agent, potassium ferrocyanide and cobalt salt is 5 hours to 30 hours. In one embodiment, the reaction time of the mixed reaction of the complexing agent, potassium ferrocyanide and cobalt salt is 24 hours to 30 hours.

[0044] In one embodiment, the cobalt salt is cobalt nitrate hexahydrate, and the mass ratio of potassium ferrocyanide to the cobalt salt is 1:0.8-1.2. Preferably, the cobalt salt is cobalt nitrate hexahydrate, and the mass ratio of potassium ferrocyanide to the cobalt salt is 1:1.

[0045] In one embodiment, the chemical formula of the iron-cobalt Prussian blue prepared by coprecipitation reaction of potassium ferrocyanide and cobalt salt is Fe 0.667 Co(CN)4(H2O)4.

[0046] Of course, after the coprecipitation reaction of potassium ferrocyanide and cobalt salt is completed, the process also includes washing and drying the product of the coprecipitation reaction.

[0047] Step S120: Under a protective atmosphere, the iron-cobalt Prussian blue is subjected to phosphating treatment to prepare a bimetallic phosphide.

[0048] Specifically, the phosphorus source in the phosphating treatment is selected from at least one of sodium hypophosphite, potassium hypophosphite and phosphine. In one embodiment, the phosphorus source in the phosphating treatment is selected from one of sodium phosphate, potassium hypophosphite and phosphine. Preferably, the phosphorus source in the phosphating treatment is selected from one of sodium phosphate and potassium hypophosphite.

[0049] Specifically, the temperature of the phosphating treatment is 350° C. to 650° C. In one embodiment, the temperature of the phosphating treatment is 580° C. to 650° C.

[0050] Specifically, the gas of the protective atmosphere is an inert gas. In one embodiment, the gas of the protective atmosphere is nitrogen or argon.

[0051] In one embodiment, the mass ratio of the iron-cobalt Prussian blue to the phosphorus source is 1: 10. Further, the mass ratio of the iron-cobalt Prussian blue to the phosphorus source is 1: 4-10.

[0052] In one embodiment, the phosphorus source is sodium hypophosphite, and the mass ratio of iron cobalt Prussian blue to the phosphorus source is 1:2 to 10. Preferably, the phosphorus source is sodium hypophosphite, and the mass ratio of iron cobalt Prussian blue to the phosphorus source is 1:4 to 10.

[0053] In one embodiment, iron-cobalt Prussian blue and sodium hypophosphite are placed in two porcelain boats at a mass ratio of 1:5, respectively. The porcelain boat containing sodium hypophosphite is placed above the air flow, and then argon gas is introduced and reacted at 600° C. for two hours to prepare a bimetallic phosphide.

[0054] The present invention also provides a bimetallic phosphide, which is prepared by the above-mentioned preparation method of bimetallic phosphide. Specifically, the bimetallic phosphide is a porous cubic block of iron-cobalt phosphide, the particle size of the bimetallic phosphide is 300nm-350nm, and the pore volume of the bimetallic phosphide is 0.65cm 3 / g~0.75cm 3 / g, and the pore size of the bimetallic phosphide is 45nm-55nm.

[0055] The above-mentioned bimetallic phosphide has a rich porous structure, a regular cubic block morphology, and a relatively uniform particle size, and can be applied in the field of catalysts or electrode materials.

[0056] One embodiment of the present invention also provides an application of the above-mentioned bimetallic phosphide in hydrogen production by water electrolysis.

[0057] One embodiment of the present invention also provides a use of the above-mentioned bimetallic phosphide in the preparation of catalysts or electrode materials.

[0058] Specifically, the bimetallic phosphide is used in preparing a catalyst for producing hydrogen by electrolysis of water or in preparing an electrode material for a lithium battery.

[0059] One embodiment of the present invention further provides a catalyst for producing hydrogen by electrolyzing water, the catalyst comprising the above-mentioned bimetallic phosphide.

[0060] An embodiment of the present invention further provides an electrode, wherein the electrode material includes an electrode active material, and the electrode active material includes the above-mentioned bimetallic phosphide.

[0061] Specifically, the electrode further includes at least one of a conductive agent, a dispersant and a binder.

[0062] In one embodiment, the binder is selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene and sodium carboxymethyl cellulose. Of course, it is understood that in the embodiment, the binder is not limited to the above, and can also be other binders commonly used in the art.

[0063] In one embodiment, the dispersant is selected from at least one of N-methylpyrrolidone, N-methyl-2-pyrrolidone and deionized water. Of course, it can be understood that in the embodiment, the dispersant is not limited to the above, and can also be other dispersants commonly used in the art.

[0064] In one embodiment, the conductive agent is selected from at least one of carbon black, activated carbon and mesoporous carbon. Of course, it can be understood that in the embodiment, the conductive agent is not limited to the above, and can also be other conductive agents commonly used in the art.

[0065] The electrode includes the bimetallic phosphide. Since the bimetallic phosphide has a rich porous structure, a regular cubic block morphology, and a relatively uniform particle size, the electrode has a larger specific capacitance and better stability. Specific embodiments

[0067] The following is a detailed description with reference to specific examples. The drugs and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods without specific conditions in the examples are carried out according to conventional conditions, such as those described in literature or books or methods recommended by manufacturers.

[0068] Example 1

[0069] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0070] Dissolve 0.65 g of potassium ferrocyanide in 100 mL of water, then pour into 100 mL of 0.65 g of cobalt nitrate hexahydrate and 1.3 g of sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0071] (2) The iron-cobalt Prussian blue obtained in step (1) was photographed using a scanning electron microscope and a transmission electron microscope. The results are as follows: Figure 1 and Figure 2 shown. Figure 1 is a scanning electron microscope image of the iron-cobalt Prussian blue obtained in step (1), Figure 2 This is a transmission electron micrograph of the iron-cobalt Prussian blue prepared in step (1).

[0072] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then argon gas is introduced, and the reaction is carried out at 600°C for two hours to obtain bimetallic phosphide.

[0073] (4) The bimetallic phosphide obtained in step (3) was photographed by scanning electron microscopy and transmission electron microscopy. Figure 3 and Figure 4 shown. Figure 3 is a scanning electron microscope image of the bimetallic phosphide obtained in step (3), Figure 4 This is a transmission electron micrograph of the bimetallic phosphide obtained in step (3).

[0074] Depend on Figure 1 and Figure 2 It can be seen that the iron-cobalt Prussian blue prepared in step (1) has a uniform particle size of about 200 nm and a smooth surface.

[0075] Depend on Figure 3 and Figure 4 It can be seen that the bimetallic phosphide prepared in step (3) maintains the cubic structure of Prussian blue and generates a rich pore structure during the phosphating process.

[0076] Example 2

[0077] Compared with Example 1, the amount of reactants for preparing iron-cobalt Prussian blue in Example 2 is twice that of Example 1, specifically as follows:

[0078] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0079] Dissolve 1.3 g of potassium ferrocyanide in 100 mL of water, then pour into 100 mL of a solution containing 1.3 g of cobalt nitrate hexahydrate and 2.6 g of sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0080] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0081] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then argon gas is introduced, and the reaction is carried out at 600°C for two hours to obtain bimetallic phosphide.

[0082] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0083] The iron-cobalt Prussian blue and bimetallic phosphide prepared in Example 2 were compared with the iron-cobalt Prussian blue and bimetallic phosphide prepared in Example 1. It was found that the iron-cobalt Prussian blue prepared in Example 2 had no significant difference from the iron-cobalt Prussian blue prepared in Example 1, and the bimetallic phosphide prepared in Example 2 had no significant difference from the bimetallic phosphide prepared in Example 1. It can be seen that the raw materials for preparing bimetallic phosphides according to the above method can be multiplied, and the preparation method is stable and can be used for large-scale production.

[0084] Example 3

[0085] Compared with Example 1, the cobalt salt in Example 3 is cobalt nitrate, specifically as follows:

[0086] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0087] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.41 g cobalt nitrate and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0088] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0089] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then argon gas is introduced, and the reaction is carried out at 600°C for two hours to obtain bimetallic phosphide.

[0090] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0091] When the iron-cobalt Prussian blue and bimetallic phosphide prepared in Example 3 were compared with the iron-cobalt Prussian blue and bimetallic phosphide prepared in Example 1, it was found that there was no significant difference between the iron-cobalt Prussian blue prepared in Example 3 and the iron-cobalt Prussian blue prepared in Example 1, and there was no significant difference between the bimetallic phosphide prepared in Example 3 and the bimetallic phosphide prepared in Example 1.

[0092] Example 4

[0093] Compared with Example 1, the amount of sodium hypophosphite was increased to 200 mg, as follows:

[0094] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0095] Dissolve 0.65 g of potassium ferrocyanide in 100 mL of water, then pour into 100 mL of 0.65 g of cobalt nitrate hexahydrate and 1.3 g of sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0096] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0097] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 200 mg of sodium hypophosphite prepared in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then argon gas is introduced, and the reaction is carried out at 600°C for two hours to obtain bimetallic phosphide.

[0098] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0099] Comparing the bimetallic phosphide prepared in Example 4 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 4 and the bimetallic phosphide prepared in Example 1.

[0100] Example 5

[0101] Compared with Example 1, the protective atmosphere was changed from argon to nitrogen, as follows:

[0102] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0103] Dissolve 0.65 g of potassium ferrocyanide in 100 mL of water, then pour into 100 mL of 0.65 g of cobalt nitrate hexahydrate and 1.3 g of sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0104] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0105] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0106] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0107] Comparing the bimetallic phosphide prepared in Example 5 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 5 and the bimetallic phosphide prepared in Example 1.

[0108] Example 6

[0109] Compared with Example 1, the cobalt salt is changed from cobalt nitrate hexahydrate to cobalt sulfate, as follows:

[0110] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0111] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.63 g cobalt sulfate and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0112] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0113] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0114] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0115] Comparing the bimetallic phosphide prepared in Example 6 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 6 and the bimetallic phosphide prepared in Example 1.

[0116] Example 7

[0117] Compared with Example 1, the cobalt salt is changed from cobalt nitrate hexahydrate to cobalt carbonate, as follows:

[0118] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0119] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.27 g cobalt carbonate and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0120] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0121] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0122] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0123] Comparing the bimetallic phosphide prepared in Example 7 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 7 and the bimetallic phosphide prepared in Example 1.

[0124] Example 8

[0125] Compared with Example 1, the cobalt salt is changed from cobalt nitrate hexahydrate to cobalt chloride, as follows:

[0126] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0127] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.29 g cobalt chloride and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0128] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0129] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0130] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0131] Comparing the bimetallic phosphide prepared in Example 8 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 8 and the bimetallic phosphide prepared in Example 1.

[0132] Example 9

[0133] Compared with Example 1, the cobalt salt is changed from cobalt nitrate hexahydrate to cobalt bromide, as follows:

[0134] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0135] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.53 g cobalt bromide and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0136] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0137] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0138] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0139] Comparing the bimetallic phosphide prepared in Example 9 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 9 and the bimetallic phosphide prepared in Example 1.

[0140] Example 10

[0141] Compared with Example 1, the cobalt salt is changed from cobalt nitrate hexahydrate to cobalt iodide, as follows:

[0142] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0143] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.70 g cobalt iodide and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0144] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0145] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0146] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0147] Comparing the bimetallic phosphide prepared in Example 10 with the bimetallic phosphide prepared in Example 1, it is found that there is no obvious difference between the bimetallic phosphide prepared in Example 10 and the bimetallic phosphide prepared in Example 1.

[0148] Embodiment 11

[0149] Compared with Example 1, the cobalt salt is changed from cobalt nitrate hexahydrate to cobalt fluoride, as follows:

[0150] (1) Preparation of cubic iron-cobalt Prussian blue, the specific steps are as follows:

[0151] Dissolve 0.65 g potassium ferrocyanide in 100 mL water, then pour into 100 mL of 0.22 g cobalt fluoride and 1.3 g sodium citrate under stirring, and then stir at room temperature for 24 h to obtain a solution with the chemical formula Fe 0.667 Iron-cobalt Prussian blue of Co(CN)4(H2O)4.

[0152] (2) The iron-cobalt Prussian blue obtained in step (1) is photographed using a scanning electron microscope and a transmission electron microscope.

[0153] (3) Preparation of bimetallic phosphide, the specific steps are as follows: 20 mg of Prussian blue and 100 mg of sodium hypophosphite obtained in step (1) are placed in two porcelain boats respectively, and the porcelain boat containing sodium hypophosphite is placed above the air flow, and then nitrogen is introduced, and the reaction is carried out at 600° C. for two hours to obtain bimetallic phosphide.

[0154] (4) The bimetallic phosphide obtained in step (3) is photographed using a scanning electron microscope and a transmission electron microscope.

[0155] Comparing the bimetallic phosphide prepared in Example 11 with the bimetallic phosphide prepared in Example 1, it was found that there was no significant difference between the bimetallic phosphide prepared in Example 11 and the bimetallic phosphide prepared in Example 1.

[0156] Comparative Example 1

[0157] (1) Synthesis of cobalt tetroxide precursor: 0.5 M cobalt nitrate hexahydrate was dissolved in 100 mL of deionized water, and then stirred at 80° C. for 15 minutes. Subsequently, 5 mL of acetylacetone and 4.75 mL of 85% hydrazine hydrate were added to the above solution, and then stirred for 10 minutes. After that, the obtained precipitate was filtered and washed with deionized water, and finally dried at 60° C. for 24 hours to obtain cobalt tetroxide precursor.

[0158] (2) Synthesis of metal phosphide: The cobalt trioxide precursor and sodium hypophosphite are heated at 350° C. for 2 hours to obtain a metal phosphide, wherein the mass ratio of the cobalt trioxide precursor to the sodium hypophosphite is 1:4.

[0159] (3) The metal phosphide obtained in step (2) is photographed by scanning electron microscopy and transmission electron microscopy, wherein the scanning electron microscopy image is as follows: Figure 5 Comparing the metal phosphide prepared in Comparative Example 1 with the bimetallic phosphide prepared in Example 1, it is found that the metal phosphide prepared in Comparative Example 1 is significantly different from the bimetallic phosphide prepared in Example 1, and the metal phosphide in Example 1 has a more regular morphology and a more uniform particle size.

[0160] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0161] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a bimetallic phosphide, characterized in that: The following steps are involved: The complexing agent, potassium ferrocyanide, cobalt salt and water are mixed and reacted to prepare iron-cobalt Prussian blue, wherein the chemical formula of the iron-cobalt Prussian blue is Fe 0.667 Co(CN)4(H2O)4, the complexing agent is selected from at least one of sodium citrate and citric acid, and the mass ratio of the complexing agent, potassium ferrocyanide and cobalt salt is 2:1:0.8-1.2; and Under a protective atmosphere, the iron-cobalt Prussian blue is phosphated with sodium hypophosphite to prepare a bimetallic phosphide, and the phosphating temperature is 600°C.

2. The method for preparing bimetallic phosphide according to claim 1, characterized in that: The step of mixing the complexing agent, the potassium ferrocyanide, the cobalt salt and water for reaction comprises: Dissolve potassium ferrocyanide in water to form a potassium ferrocyanide solution; dissolving a cobalt salt in water to form a cobalt salt solution; and The potassium ferrocyanide solution, the cobalt salt solution and the complexing agent are mixed and reacted.

3. The method for preparing bimetallic phosphide according to claim 1, characterized in that: The cobalt salt is selected from at least one of cobalt nitrate, cobalt sulfate, cobalt carbonate, cobalt chloride, cobalt bromide, cobalt iodide and cobalt fluoride.

4. A bimetallic phosphide, characterized in that: The bimetallic phosphide is a porous cubic block of iron-cobalt phosphide, the particle size of the bimetallic phosphide is 300nm-350nm, and the pore volume of the bimetallic phosphide is 0.65cm 3 / g~0.75cm 3 / g, the pore size of the bimetallic phosphide is 45nm-55nm; the bimetallic phosphide is a phosphating product of iron-cobalt Prussian blue by phosphating with sodium hypophosphite under a protective atmosphere, and the chemical formula of the iron-cobalt Prussian blue is Fe 0.667 Co(CN)4(H2O)4, the temperature of the phosphating treatment is 600℃.

5. A catalyst for producing hydrogen by electrolysis of water, characterized in that: The invention comprises the bimetallic phosphide prepared by the preparation method of the bimetallic phosphide according to any one of claims 1 to 3 or the bimetallic phosphide according to claim 4.

6. An electrode, characterized in that: The invention comprises an electrode active material, wherein the electrode active material comprises the bimetallic phosphide prepared by the preparation method of the bimetallic phosphide according to any one of claims 1 to 3 or the bimetallic phosphide according to claim 4.