A topological stealth structure and preparation method thereof
Through topological stealth structure, the absorption form of electromagnetic waves is transformed from surface absorption to bulk absorption, and a composite material of graphene, ferrite and silicone resin is used to form a three-dimensional network structure, which solves the insufficient absorption rate in the prior art The problem of high-performance stealth is achieved and the implementation difficulty is reduced.
Patent Information
- Application Number
- CN202110931663.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-08-13
AI Technical Summary
Due to the limitation of the intrinsic characteristics of the existing stealth technology, the absorbance rate cannot reach 100%, resulting in the inability to achieve high-performance stealth under some conditions.
The topological stealth structure is adopted to transform the absorbing form of electromagnetic waves from surface absorption to bulk absorption. By mixing graphene and ferrite with silicone resin to form an absorbing slurry, penetrate into the permeable material and cure it to form a three-dimensional network structure. To improve the absorption rate of electromagnetic waves.
The absorption rate of electromagnetic waves is greatly increased, high-performance stealth is achieved, and particle precipitation and stratification problems are avoided through composite materials, reducing the difficulty of implementation.
Smart Images

Figure CN113777679B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerospace materials, and in particular relates to a topological stealth structure and a preparation method thereof. Background Art
[0002] Stealth technology is one of the important ways to improve the survivability of aircraft. Existing stealth technology mainly improves the wave absorption performance of materials, absorbs and loses electromagnetic radiation on the surface of aircraft, and reduces the reflection and scattering of electromagnetic waves, thereby achieving stealth performance.
[0003] Due to the intrinsic characteristics of the material, its absorption rate cannot reach 100%, that is, the existing stealth technology has a capacity limit and can only achieve stealth under certain conditions. In order to solve this problem, the present invention provides a topological stealth structure, which transforms the electromagnetic wave absorption form from surface absorption to volume absorption, greatly increases its electromagnetic wave absorption rate, and thus achieves high-performance stealth. Summary of the invention
[0004] In order to overcome the deficiencies in the prior art, the inventors have conducted intensive research and provided a topological stealth structure and a preparation method thereof, which transforms the absorption form from surface absorption to volume absorption, improves its electromagnetic wave absorption rate, and facilitates the realization of high-performance stealth of aircraft.
[0005] The technical solution provided by the present invention is as follows:
[0006] In the first aspect, a topological stealth structure is provided, which includes a topological unit A, an electric loss unit B, a magnetic loss unit C and a silicone resin D, wherein the topological unit A is a wave-transmitting material and presents a three-dimensional network structure; the electric loss unit B and the magnetic loss unit C are graphene and ferrite, respectively, which are mixed with the silicone resin D to obtain an absorbing slurry, and then the absorbing slurry is infiltrated into the topological unit A and solidified to obtain a topological stealth structure.
[0007] In the second aspect, a method for preparing a topological stealth structure comprises the following steps: mixing an electric loss unit B and a magnetic loss unit C with a silicone resin D to obtain an absorbing slurry, and then infiltrating the absorbing slurry into a topological unit A for curing to obtain a topological stealth structure.
[0008] A topological stealth structure and a preparation method thereof provided by the present invention have the following beneficial effects:
[0009] (1) The present invention provides a topological stealth structure that changes the electromagnetic wave absorption form from surface absorption to volume absorption, thereby increasing the electromagnetic wave absorption capacity;
[0010] (2) The present invention provides a topological stealth structure and a preparation method thereof. The electric loss unit and the magnetic loss unit are both nanoparticles with good compatibility with silicone. The electric loss unit and the magnetic loss unit are added in the form of a composite material, thereby avoiding problems such as particle precipitation and stratification, and reducing the difficulty of realizing the stealth structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 A schematic diagram of a topological stealth structure provided by the present invention;
[0012] Figure 2 This is the principle diagram of wave absorption of topological stealth structure;
[0013] Figure 3 AFM image of graphene oxide sheets;
[0014] Figure 4 SEM images of graphene oxide (a) and reduced graphene oxide (b);
[0015] Figure 5 Raman spectra of graphene oxide (a) and reduced graphene oxide (b);
[0016] Figure 6 is the SEM image of oxygen nickel ferrite / graphene nanocomposite;
[0017] Figure 7 is the XRD pattern of nickel ferrite;
[0018] Figure 8 is the XRD image of ferrite / graphene composite material;
[0019] Fig. 9 This is the simulation result of the topological stealth structure. DETAILED DESCRIPTION
[0020] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0021] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.
[0022] The present invention provides a topological stealth structure, such as Figure 1As shown, the topological stealth structure includes a topological unit A, an electric loss unit B, a magnetic loss unit C and a silicone resin D, wherein the topological unit A is a wave-transmitting material, presenting a three-dimensional network structure, and can play a structural support role; the electric loss unit B and the magnetic loss unit C are graphene and ferrite, respectively, which are mixed with the silicone resin D to obtain an absorbing slurry, and then the absorbing slurry is infiltrated into the topological unit A and solidified to obtain a topological stealth structure.
[0023] Furthermore, the topological unit A is at least one of silicon dioxide, silicon carbide or polyurethane, and is prepared by 3D printing or injection molding. The topological structure includes but is not limited to a honeycomb structure.
[0024] Furthermore, the electric loss unit B and the magnetic loss unit C are used in a topological stealth structure in the form of a composite material, which improves the dispersion of the electric loss unit B and the magnetic loss unit C and avoids the electric loss unit B and the magnetic loss unit C from agglomerating due to their small size, thereby affecting the wave absorbing performance.
[0025] The electric loss unit B is graphene, and the number of layers of graphene is 1-20;
[0026] The magnetic loss unit C is nickel ferrite, and its average particle size is 50-500 nanometers.
[0027] Furthermore, the organic silicone resin D is at least one of KH550 and KH570.
[0028] Furthermore, the volume of the topological unit A in the topological stealth structure is greater than 30%, the content of graphene in the absorbing slurry is 10-30wt.%, the content of ferrite is 20-70wt.%, and the rest is silicone resin D.
[0029] Working principle: When electromagnetic waves are incident on the surface of the topological stealth structure, a small amount is absorbed by the electric loss unit B and the magnetic loss unit C, and most of the electromagnetic waves enter the stealth structure along the topological unit A (wave-transmitting material). The electromagnetic waves entering the stealth structure are reflected and scattered multiple times along the topological unit A and the electric loss unit B and the magnetic loss unit C, and are finally all absorbed, and the electromagnetic energy is converted into heat energy, such as Figure 2 shown.
[0030] The present invention also provides a method for preparing a topological stealth structure, comprising the following steps: mixing an electric loss unit B and a magnetic loss unit C with a silicone resin D to obtain an absorbing slurry, and then infiltrating the absorbing slurry into a topological unit A for curing to obtain a topological stealth structure.
[0031] In a preferred embodiment, when the electric loss unit B and the magnetic loss unit C are used in a topological stealth structure in the form of a composite material, the ferrite graphene composite material is prepared by a preparation method comprising the following steps:
[0032] S1, dispersing potassium permanganate and graphite powder in concentrated sulfuric acid to obtain graphite oxide flakes after reaction;
[0033] S2, washing the graphite oxide flakes, stirring during the washing process, exfoliating the graphite oxide flakes into graphene oxide by centrifugation, and forming a stable few-layer or single-layer graphene oxide suspension in water;
[0034] S3, adding soluble ferrous salt and nickel salt to the graphene oxide suspension;
[0035] S4, heating the mixed solution in step S3 to 160-200° C. in a reaction kettle and keeping the temperature for 8-12 hours;
[0036] S5, adding a reducing agent to the mixed solution of step S4 after cooling, treating in an oven at 70-80° C. for at least 72 h, cooling to room temperature, and reducing the graphene oxide to reduced graphene oxide (RGO);
[0037] S6, separating and washing the sample after the reaction in step S5, and fully drying it to obtain a ferrite graphene composite material.
[0038] In a preferred embodiment, in step S1, the potassium permanganate and graphite powder are dispersed in concentrated sulfuric acid to react to obtain graphite oxide flakes, which specifically includes the following steps: stirring and suspending natural flake graphite and KNO3 in concentrated sulfuric acid, adding KMnO4 to react under ice water cooling, and then returning the mixture to room temperature and continuing stirring for at least 3 days.
[0039] Among them, the volume ratio of the mass (in grams) of the natural flake graphite, KNO3, and KMnO4 to concentrated sulfuric acid (in milliliters) is 5:4.2-4.8:20-25:160-180, preferably 5:4.4-4.6:22-23:165-175, and more preferably 5:4.5:22.5:169.
[0040] In a preferred embodiment, in step S2, the cleaning of the graphite oxide flakes specifically comprises the following steps:
[0041] S2.1, slowly dispersing the mixture in step S1 in a 5-10wt% H2SO4 aqueous solution, and continuing to stir; then adding an aqueous hydrogen peroxide solution, and continuing to stir for at least 1 hour; wherein the mass ratio of the natural flake graphite to the aqueous hydrogen peroxide solution is 5:12-18, preferably 5:14-16, more preferably 5:15, and the concentration of the aqueous hydrogen peroxide solution is 30vol%;
[0042] S2.2, dilute with 3-4wt% H2SO4 / 0.5-0.6wt% H2O2, and stir overnight;
[0043] S2.3, the mixture is centrifuged at 8000-90000 rpm for 15-25 minutes to separate a viscous dark yellow liquid;
[0044] S2.4, after vigorously shaking the viscous liquid for at least 5 minutes, repeat steps S2.2 to S2.3 at least three times, and during the cleaning process, the gloss of the viscous component gradually decreases and the color gradually darkens until no gloss is seen during cleaning;
[0045] S2.5, continue washing the mixture with pure water and centrifuge to separate the viscous liquid until the supernatant is neutral. This produces a dark brown viscous liquid graphene oxide (GO), which can be used directly as a water suspension of GO (such as a concentration of 3 mg / ml) or can be removed by high-speed centrifugation (such as 20,000 rpm, 30 minutes) and vacuum drying to remove the remaining water.
[0046] In a preferred embodiment, in step S3, the soluble ferrous salt includes at least one of ferrous chloride, ferrous bromide, ferrous iodide, ferrous sulfate, ferrous nitrate, or soluble ferrous carboxylate, etc.; and the nickel salt is nickel chloride hexahydrate.
[0047] In a preferred embodiment, in step S3, the soluble ferrous salt and nickel salt are used in a ratio of (1.9-2.1):1 based on the amount of positively charged metal ions.
[0048] In a preferred embodiment, in step S3, soluble ferrous salt and nickel salt are added to the graphene oxide suspension according to the mass ratio of graphene oxide to nickel ferrite of 1:(1.9-2.1), and the nickel ferrite is nickel ferrite (NiFe2O4).
[0049] In a preferred embodiment, in step S5, the reducing agent is selected from at least one of ascorbic acid, hydrazine hydrate or sodium borohydride, preferably ascorbic acid.
[0050] In a preferred embodiment, in step S5, the mass ratio of the reducing agent to graphene oxide is (6-8):1, preferably 7:1.
[0051] Example
[0052] Example 1
[0053] Using polyamide as the wave-transmitting material, the topological unit A was obtained by 3D printing. Using ferrite graphene composite material and KH550 as raw materials, the absorbing slurry was mixed in a mass ratio of 6:4. The absorbing slurry was then infiltrated into the topological unit A and solidified to obtain a topological stealth structure.
[0054] Wherein, the ferrite graphene composite material is prepared by the following steps:
[0055] Natural flake graphite (5 g) and KNO3 (4.5 g) were stirred and suspended in concentrated sulfuric acid (169 ml), the mixture was cooled in ice, KMnO4 (22.5 g) was added over 70 minutes, and then the mixture was allowed to return to room temperature by stirring and stirred for 7 days.
[0056] The dark mixture was then slowly dispersed into 550 ml of a 5 wt% H2SO4 aqueous solution over 1 hour and stirred for an additional 3 hours. Hydrogen peroxide (15 g, 30 vol%) was added over 5 minutes, with considerable foaming after the addition of hydrogen peroxide, and the mixture became a yellow / golden suspension and stirred for an additional 2 hours. The mixture was diluted with 500 ml of 3 wt% H2SO4 / 0.5 wt% H2O2 and stirred overnight. Thereafter, the resulting mixture was subjected to a washing process to obtain a graphene oxide suspension. The resulting mixture was centrifuged at 8000 rpm for 20 minutes, resulting in the separation of the mixture into two approximately equal portions, with a small amount of very dark spheres (discarded), one of which was a clear supernatant (decanted and discarded) and the other a viscous dark yellow liquid. The viscous liquid was then dispersed into 500 ml of 3 wt% H2SO4 / 0.5 wt% H2O2 by vigorous shaking (5-10 minutes). The washing process of the resulting mixture was repeated 4 times. During this process, the gloss of the viscous component gradually decreased and the color gradually darkened, so that no glitter was seen by the fourth washing. The mixture was then washed with pure water (500 ml) and concentrated by centrifugation (discarding the colorless supernatant) until the supernatant was neutral (pH 7). Figure 3 As shown, the AFM results of graphene oxide indicate that the thickness of the material is 1.2 nm, which is consistent with the thickness of single-layer graphene in the literature.
[0057] In order to synthesize nickel ferrite (NiFe2O4), first prepare 0.1M ferric chloride hexahydrate in 50ml deionized water and stir evenly. Then, under the same conditions, prepare 0.1M nickel chloride hexahydrate solution in 25ml deionized water and stir evenly. The two solutions are mixed and stirred in a magnetic stirrer to form a precursor (color: light yellow); the graphene oxide solution (matched according to the mass ratio of graphene oxide to nickel ferrite of 1:2) is mixed with the precursor and placed in a reactor at 180°C for 10h.
[0058] Add ascorbic acid as a reducing agent to the cooled mixed solution, the amount of ascorbic acid added is 7 times the mass of graphene oxide, heat the mixed solution to 80° C. in an oven, and fully react for 72 hours. After the reaction is completed, the graphene oxide is reduced to reduced graphene oxide; Figure 4 As shown, the SEM images of graphene oxide (Figure a) and reduced graphene oxide (Figure b) indicate that the prepared graphene oxide and reduced graphene oxide have a good lamellar structure. Figure 5 Figure 3 is the Raman spectra of graphene oxide and reduced graphene oxide. The ratio of the D-band peak to the G-band peak increases, indicating that the graphene oxide undergoes a chemical reaction and is reduced to reduced graphene oxide.
[0059] The sample after the reaction is separated, washed, and fully dried to obtain a ferrite graphene composite material. Figure 6 As shown in the SEM image of nickel ferrite / graphene nanocomposite, the nickel ferrite nanoparticles are covered by graphene sheets, and the mass ratio of nickel ferrite to graphene is calculated to be 67:33. Figure 7 and Figure 8 As shown, they are the XRD images of nickel ferrite and ferrite / graphene composite materials, respectively. The particle size of nickel ferrite on the graphene composite material is about 200-500nm. From the XRD image of the ferrite / graphene composite material, 7 obvious peaks can be observed at 18.4°, 30.3°, 35.6°, 43.3°, 53.8°, 57.2° and 62.8°, which are consistent with the peak positions of nickel ferrite and conform to the reflection characteristics of spinel ferrite. At the same time, there is no characteristic diffraction peak of graphene oxide, indicating that the graphene oxide is reduced and there is no stacking of reduced graphene oxide sheets. In addition, there is no other crystal peak, indicating that the purity of the ferrite / graphene composite material is very high, and the preparation process of ferrite / graphene nanocomposite materials is feasible. Through determination,
[0060] The simulation results of the topological stealth structure are as follows: Fig. 9 As shown, the effective bandwidth (frequency band with reflection loss less than -10dB) is 7.27-18GHz, which can achieve broadband stealth performance compared to the effective narrowband frequency band of the absorbing composite material.
[0061] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
[0062] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.
Claims
1. A topological stealth structure, characterized in that: The topological stealth structure comprises a topological unit A, an electric loss unit B, a magnetic loss unit C and an organic silicone resin D, wherein the topological unit A is a wave-transmitting material and presents a three-dimensional mesh structure; the electric loss unit B and the magnetic loss unit C are graphene and ferrite respectively, and the two are mixed with the organic silicone resin D to obtain a wave-absorbing slurry, and then the wave-absorbing slurry is infiltrated into the topological unit A and solidified to obtain a topological stealth structure; The volume of the topological unit A in the topological stealth structure is greater than 30%, the content of graphene in the absorbing slurry is 10-30wt.%, the content of ferrite is 20-70wt.%, and the rest is silicone resin D.
2. The topological stealth structure according to claim 1, characterized in that: The topological unit A is at least one of silicon dioxide, silicon carbide or polyurethane.
3. The topological stealth structure according to claim 1, characterized in that: The electric loss unit B and the magnetic loss unit C are used in a topological stealth structure in the form of composite materials.
4. The topological stealth structure according to claim 1, characterized in that: The organic silicone resin D is at least one of KH550 and KH570.
5. The topological stealth structure according to claim 3, characterized in that: The ferrite graphene composite material composed of the electric loss unit B and the magnetic loss unit C is prepared by a preparation method comprising the following steps: S1, dispersing potassium permanganate and graphite powder in concentrated sulfuric acid to obtain graphite oxide flakes after reaction; S2, washing the graphite oxide flakes, stirring during the washing process, exfoliating the graphite oxide flakes into graphene oxide by centrifugation, and forming a stable few-layer or single-layer graphene oxide suspension in water; S3, adding soluble ferrous salt and nickel salt to the graphene oxide suspension; S4, heating the mixed solution in step S3 to 160-200° C. in a reaction kettle and keeping the temperature for 8-12 hours; S5, adding a reducing agent to the mixed solution of step S4 after cooling, treating in an oven at 70-80° C. for at least 72 h, cooling to room temperature, and reducing the graphene oxide to reduced graphene oxide; S6, separating and washing the sample after the reaction in step S5, and fully drying it to obtain a ferrite graphene composite material.
6. The topological stealth structure according to claim 5, characterized in that: In step S1, potassium permanganate and graphite powder are dispersed in concentrated sulfuric acid to react to obtain graphite oxide flakes, which specifically includes the following steps: natural flake graphite and KNO3 are stirred and suspended in concentrated sulfuric acid, KMnO4 is added under ice water cooling to react, and the mixture is then restored to room temperature and stirred for at least 3 days.
7. The topological stealth structure according to claim 5, characterized in that: In step S2, the graphite oxide flakes are cleaned, specifically comprising the following steps: S2.1, slowly dispersing the mixture in step S1 in a 5-10 wt% H2SO4 aqueous solution, and continuing to stir; then adding a hydrogen peroxide aqueous solution, and continuing to stir for at least 1 hour; S2.2, dilute with 3-4wt% H2SO4 / 0.5-0.6wt% H2O2, and stir overnight; S2.3, the mixture is centrifuged at 8000-90000 rpm for 15-25 minutes to separate a viscous dark yellow liquid; S2.4, after vigorously shaking the viscous liquid, repeat steps S2.2 to S2.3 at least three times, and during the cleaning process, the gloss of the viscous component gradually decreases and the color gradually darkens until no gloss is seen during cleaning; S2.5, continue washing the mixture with pure water and centrifuge to separate the viscous liquid until the supernatant is neutral.
8. The topological stealth structure according to claim 5, characterized in that: In step S3, the soluble ferrous salt and nickel salt are used in a ratio of (1.9-2.1):1 based on the amount of the positively charged metal ions. The soluble ferrous salt and nickel salt are mixed with graphene oxide in an amount such that the mass ratio of graphene oxide to nickel ferrite is 1:(1.9-2.1), and the nickel ferrite is nickel ferrite.
9. A method for preparing a topological stealth structure according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: mixing an electric loss unit B and a magnetic loss unit C with an organic silicone resin D to obtain a wave-absorbing slurry, and then infiltrating the wave-absorbing slurry into a topological unit A for curing to obtain a topological stealth structure.
Citation Information
Patent Citations
Graphene-ferrite-polymer ternary nano-composite wave absorption material and preparation method thereof
CN108251053A
Passive frequency control material based on graphene / ferrite and preparation method of passive frequency control material
CN108298973A
Wave-absorbing polyurethane sponge / rigid foam composite material and preparation method thereof
CN112126116A