Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element

By using polyamic acid imidized polymers synthesized from specific aromatic tetracarboxylic dianhydrides and aliphatic tetracarboxylic dianhydrides and diamines, the problems of brush resistance and charge accumulation of the liquid crystal alignment film are solved, and the Liquid crystal indicates the display performance of the element and the recycling efficiency of the substrate.

CN113805386BActive Publication Date: 2024-10-22NISSAN CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111009465.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-09-29
Filing Date
2017-09-28
Publication Date
2024-10-22
Estimated Expiration
2037-09-28

AI Technical Summary

Technical Problem

The existing liquid crystal alignment film has insufficient brush resistance during the production process, resulting in scratches or peeling, and the charge accumulation problem leads to reduced display contrast and image sticking. The reprocessability is poor, making it difficult to achieve efficient recycling of the substrate.

Method used

Polyamic acid and polyamic acid imidized polymer synthesized from specific aromatic tetracarboxylic dianhydride and aliphatic tetracarboxylic dianhydride and diamine are used as liquid crystal aligning agents to form a liquid crystal aligning agent with excellent brush resistance and abrasion resistance. Liquid crystal alignment film with charge accumulation suppression capability.

Benefits of technology

It improves the brush resistance of the liquid crystal alignment film, suppresses charge accumulation caused by AC drive, improves the display contrast and reprocessability of liquid crystal display elements, and supports efficient recycling of substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113805386B_ABST
    Figure CN113805386B_ABST
Patent Text Reader

Abstract

The present application relates to a liquid crystal alignment agent, a liquid crystal alignment film and a liquid crystal display element, characterized in that the liquid crystal alignment agent contains: (A) at least one polymer selected from polyamic acid and an imidized polymer of the polyamic acid, wherein the polyamic acid is obtained using a tetracarboxylic dianhydride component containing a tetracarboxylic dianhydride represented by the following formula (1) and an aliphatic tetracarboxylic dianhydride in a ratio of 10:90 to 90:10, and a diamine component containing a diamine represented by the following formula (2); (B) at least one polymer selected from the group consisting of a polyimide precursor, an imidized polymer of the polyimide precursor, and a photosensitive side-chain acrylic polymer that exhibits liquid crystallinity within a specific temperature range; and an organic solvent. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the Chinese patent application with the application date of September 28, 2017, application number 201780060270.3, and invention name “Liquid Crystal Alignment Agent, Liquid Crystal Alignment Film and Liquid Crystal Display Element”. Technical Field

[0002] The present invention relates to a liquid crystal aligning agent for a liquid crystal display element, a liquid crystal aligning film, and a liquid crystal display element using the same. Background Art

[0003] Liquid crystal devices have been widely used as display units for personal computers, mobile phones, television receivers, etc. Liquid crystal devices include, for example, a liquid crystal layer sandwiched between an element substrate and a color filter substrate, pixel electrodes and common electrodes for applying an electric field to the liquid crystal layer, an orientation film for controlling the orientation of liquid crystal molecules in the liquid crystal layer, and a thin film transistor (TFT) for converting an electric signal supplied to the pixel electrode. As a driving method for liquid crystal molecules, longitudinal electric field methods such as the TN method and the VA method are known, and transverse electric field methods such as the IPS method and the boundary electric field switching (hereinafter referred to as FFS) method are known (for example, Patent Document 1).

[0004] In recent years, the economy of liquid crystal display elements and organic EL elements in the production process is also very important, so the recycling of element substrates is required. That is, after the liquid crystal alignment film is formed by the liquid crystal alignment agent, when the orientation is checked and defects occur, it is required to easily implement the reprocessing (rework) process of removing the liquid crystal alignment film from the substrate and recovering the substrate. However, the liquid crystal alignment film obtained by the liquid crystal alignment agent proposed in the past is to be insoluble in organic solvents after baking to reduce film loss as a goal. In addition, even if the structure of the liquid crystal alignment agent that has been studied for reprocessability so far is directly used in the structure of the liquid crystal alignment agent for the lateral electric field, it may not necessarily achieve the desired purpose. It is necessary to re-evaluate the reprocessability of the liquid crystal alignment agent and re-study the most suitable composition structure.

[0005] In addition, liquid crystal display elements are now widely used as display devices. The liquid crystal alignment film, which is a structural component of the liquid crystal display element, is a film for uniformly arranging the liquid crystal, but in addition to the orientation uniformity of the liquid crystal, various characteristics are also necessary. For example, in the production process of the liquid crystal alignment film, the orientation treatment of brushing the surface of the polymer film with a cloth is usually performed. However, when the brushing resistance of the liquid crystal alignment film is insufficient, the film is scraped and scratches or dust is generated, or the film itself is peeled off, causing the display quality of the liquid crystal display element to decrease. In addition, a voltage is applied to the liquid crystal to drive the liquid crystal display element. Therefore, when the voltage holding ratio (VHR) of the liquid crystal alignment film is low, it is impossible to apply a sufficient voltage to the liquid crystal, which will cause a decrease in display contrast. In addition, if the charge is accumulated in the liquid crystal alignment film due to the voltage driving the liquid crystal, or the escape of the accumulated charge takes time, phenomena such as afterimage or display afterimage will occur.

[0006] Various proposals have been made as products that simultaneously satisfy some of the above-mentioned required characteristics. For example, as a method for obtaining a liquid crystal alignment film with excellent brush abrasion resistance and less residual image and afterimage, a proposal such as Patent Document 2 has been made. In addition, as a method for obtaining a liquid crystal alignment film with excellent liquid crystal orientation, orientation control ability, and brush abrasion resistance, high voltage holding rate, and reduced charge accumulation, a proposal such as Patent Document 3 has been made.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-167782

[0010] Patent Document 2: International Publication No. WO02 / 33481 Pamphlet

[0011] Patent Document 3: International Publication No. WO2004 / 053583 Pamphlet Summary of the invention

[0012] Problem that the invention aims to solve

[0013] An object of the present invention is to provide a liquid crystal aligning agent that can obtain a liquid crystal aligning film that satisfies various characteristics required for the liquid crystal aligning film and is excellent in reworkability.

[0014] Solutions for solving problems

[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by using a polyamic acid and an imidized polymer of a polyamic acid obtained from a tetracarboxylic acid containing a specific aromatic tetracarboxylic dianhydride and an aliphatic tetracarboxylic dianhydride and a diamine having a specific structure, a liquid crystal alignment film that satisfies various properties required for a liquid crystal alignment film and has excellent reprocessability can be obtained, thereby completing the present invention.

[0016] Therefore, the present invention is based on the above findings and has the following gist.

[0017] 1. A liquid crystal alignment agent, characterized in that it contains:

[0018] (A) at least one polymer selected from the group consisting of polyamic acid and an imidized polymer of the polyamic acid, wherein the polyamic acid is obtained using a tetracarboxylic dianhydride component comprising a tetracarboxylic dianhydride represented by the following formula (1) and an aliphatic tetracarboxylic dianhydride in a ratio of 10:90 to 90:10, and a diamine component comprising a diamine represented by the following formula (2);

[0019] (B) at least one polymer selected from the group consisting of a polyimide precursor, an imidized polymer of the polyimide precursor, and a photosensitive side chain acrylic polymer that exhibits liquid crystallinity in a specific temperature range; and an organic solvent.

[0020]

[0021] (In formula (1), i is 0 or 1, and X is a single bond, an ether bond, a carbonyl group, an ester bond, a phenylene group, a straight-chain alkylene group having 1 to 20 carbon atoms, a branched-chain alkylene group having 2 to 20 carbon atoms, a cyclic alkylene group having 3 to 12 carbon atoms, a sulfonyl group, an amide bond, or a group composed of a combination thereof, wherein the alkylene group having 1 to 20 carbon atoms may be interrupted by a bond selected from an ester bond and an ether bond, and the carbon atoms of the phenylene group and the alkylene group may be substituted by one or more identical or different substituents selected from a halogen atom, a cyano group, an alkyl group, a haloalkyl group, an alkoxy group, and a haloalkoxy group.

[0022] In formula (2), Y1 is a divalent organic group having at least one structure selected from the group consisting of an amino group, an imino group and a nitrogen-containing heterocyclic ring, and B1 and B2 are each independently a hydrogen atom, or an alkyl group, alkenyl group or alkynyl group having 1 to 10 carbon atoms and optionally having a substituent.

[0023] 2. The liquid crystal aligning agent according to 1, wherein 10 to 100 mol % of the tetracarboxylic dianhydride component of the component (A) is tetracarboxylic dianhydride represented by the formula (1) and aliphatic tetracarboxylic dianhydride.

[0024] 3. The liquid crystal aligning agent according to 1 or 2, wherein 10 to 100 mol % of the diamine component of the component (A) is a diamine of formula (2).

[0025] 4. The liquid crystal aligning agent according to any one of 1 to 3, wherein Y1 in the formula (2) is at least one structure selected from the group consisting of the following formulae (YD-1) to (YD-5).

[0026]

[0027] (In formula (YD-1), A1 is a nitrogen-containing heterocyclic ring having 3 to 15 carbon atoms, Z1 is a hydrogen atom, or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. In formula (YD-2), W1 is a hydrocarbon group having 1 to 10 carbon atoms, A2 is a monovalent organic group having 3 to 15 carbon atoms which has a nitrogen-containing heterocyclic ring, or a disubstituted amino group substituted with an aliphatic group having 1 to 6 carbon atoms. In formula (YD-3), W2 is a divalent organic group having 6 to 15 carbon atoms and 1 to 2 benzene rings, W3 is an alkylene group having 2 to 5 carbon atoms or a biphenylene group, Z2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a benzene ring, and a is an integer of 0 to 1. In formula (YD-4), A3 is a nitrogen-containing heterocyclic ring having 3 to 15 carbon atoms. In formula (YD-5), A4 is a nitrogen-containing heterocyclic ring having 3 to 15 carbon atoms, and W5 is an alkylene group having 2 to 5 carbon atoms.)

[0028] 5. A liquid crystal alignment agent according to 4, wherein A1, A2, A3 and A4 described in formulas (YD-1), (YD-2), (YD-4) and (YD-5) are at least one selected from the group consisting of pyrrolidine, pyrrole, imidazole, pyrazole, oxazole, thiazole, piperidine, piperazine, pyridine, pyrazine, indole, benzimidazole, quinoline and isoquinoline.

[0029] 6. The liquid crystal aligning agent according to any one of 1 to 5, wherein Y1 in the formula (2) is at least one selected from the group consisting of divalent organic groups having structures of the following formulae (YD-6) to (YD-21).

[0030]

[0031] (In formula (YD-17), h is an integer of 1 to 3, and in formulas (YD-14) and (YD-21), j is an integer of 1 to 3.)

[0032] 7. The liquid crystal aligning agent according to 6, characterized in that Y1 in formula (2) is at least one selected from the group consisting of divalent organic groups having structures of the above formulas (YD-14) and (YD-18).

[0033] 8. The liquid crystal aligning agent as described in any one of 1 to 7, wherein the tetracarboxylic dianhydride represented by the above formula (1) is 3,3′,4,4′-biphenyltetracarboxylic dianhydride.

[0034] 9. The liquid crystal aligning agent according to any one of 1 to 8, wherein the aliphatic tetracarboxylic dianhydride is bicyclo[3.3.0]octane-2,4,6,8-tetracarboxylic acid-2,4:6,8-dianhydride.

[0035] 10. A liquid crystal aligning film obtained by applying the liquid crystal aligning agent according to any one of 1 to 9 and baking the coating.

[0036] 11. A liquid crystal display element comprising the liquid crystal alignment film according to 10.

[0037] Effects of the Invention

[0038] The liquid crystal aligning film obtained from the liquid crystal aligning agent of this invention can suppress the charge accumulation by the asymmetry of AC drive, and is excellent in reworkability. DETAILED DESCRIPTION

[0039] The liquid crystal alignment agent of the present invention is characterized in that it contains: (A) at least one polymer selected from polyamic acid and an imidized polymer of the polyamic acid, wherein the polyamic acid is obtained using a tetracarboxylic dianhydride component containing a tetracarboxylic dianhydride represented by the following formula (1) and an aliphatic tetracarboxylic dianhydride in a ratio of 10:90 to 90:10, and a diamine component containing a diamine represented by the following formula (2); (B) at least one polymer selected from the group consisting of a polyimide precursor, an imidized polymer of the polyimide precursor, and a photosensitive side-chain acrylic polymer that exhibits liquid crystallinity within a specific temperature range; and an organic solvent.

[0040]

[0041] In formula (1), i is 0 or 1, and X is a single bond, an ether bond, a carbonyl group, an ester bond, a phenylene group, a straight-chain alkylene group having 1 to 20 carbon atoms, a branched-chain alkylene group having 2 to 20 carbon atoms, a cyclic alkylene group having 3 to 12 carbon atoms, a sulfonyl group, an amide bond, or a group composed of a combination thereof, wherein the alkylene group having 1 to 20 carbon atoms may be interrupted by a bond selected from an ester bond and an ether bond, and the carbon atoms of the phenylene group and the alkylene group may be substituted by one or more identical or different substituents selected from a halogen atom, a cyano group, an alkyl group, a haloalkyl group, an alkoxy group, and a haloalkoxy group.

[0042] In formula (2), Y1 is a divalent organic group having at least one structure selected from the group consisting of an amino group, an imino group and a nitrogen-containing heterocyclic ring, and B1 to B2 are each independently a hydrogen atom, or an alkyl group, alkenyl group or alkynyl group having 1 to 10 carbon atoms which may have a substituent.

[0043] Hereinafter, each structural feature will be described in detail.

[0044] <(A)Component>

[0045] The component (A) used in the liquid crystal aligning agent of the present invention is at least one polymer selected from the group consisting of polyamic acid and an imidized polymer of the polyamic acid, wherein the polyamic acid is obtained using a tetracarboxylic dianhydride component containing tetracarboxylic dianhydride represented by the above formula (1) and aliphatic tetracarboxylic dianhydride at a ratio of 10:90 to 90:10, and a diamine component containing a diamine represented by the above formula (2).

[0046] <Tetracarboxylic dianhydride component>

[0047] Examples of the tetracarboxylic dianhydride represented by the above formula (1) include the following compounds, but the present invention is not limited to these compounds.

[0048]

[0049] (In the formula, q represents an integer from 1 to 20.)

[0050] Among the tetracarboxylic dianhydrides represented by the formula (1), from the viewpoint of a good effect of improving reprocessability, the tetracarboxylic dianhydride in which i is 1 in the formula (1), i.e., the tetracarboxylic dianhydride having two or more benzene rings, is preferred. Among the above specific examples, (1-2) to (1-11) are preferred. From the viewpoint of containing a biphenyl structure and having a rigid structure, 3,3',4,4'-biphenyltetracarboxylic dianhydride represented by the formula (1-5) is particularly preferred.

[0051] As the specific aliphatic tetracarboxylic dianhydride used in the present invention, tetracarboxylic dianhydride represented by the following formula (3) can be mentioned.

[0052]

[0053] In the formula, X1 is any one of the following (X-1) to (X-28).

[0054]

[0055]

[0056] In formula (X-1), R3 to R6 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group, and more preferably a hydrogen atom or a methyl group.

[0057] Among the above, (X-1) to (X-20) are preferred from the viewpoint of not containing an aromatic part, and (X-10) is most preferred from the viewpoint of being particularly unlikely to undergo thermal imidization.

[0058] In the whole tetracarboxylic dianhydride component used to manufacture the (A) component of the present invention, if the total amount of the tetracarboxylic dianhydride represented by formula (1) and the aliphatic tetracarboxylic dianhydride is too small, the effect of the present invention cannot be obtained. Therefore, the total amount of the tetracarboxylic dianhydride represented by formula (1) and the aliphatic tetracarboxylic dianhydride is preferably 10 to 100 mol%, more preferably 50 to 100 mol%, and further preferably 80 to 100 mol%, relative to 1 mol of all tetracarboxylic dianhydrides.

[0059] The content ratio of the tetracarboxylic dianhydride represented by formula (1) and the aliphatic tetracarboxylic dianhydride is 10:90 to 90:10, preferably 20:80 to 80:20, more preferably 40:60 to 60:40, particularly preferably 46:54 to 54:46, and most preferably substantially equal amounts.

[0060] The tetracarboxylic dianhydride represented by formula (1) and the aliphatic tetracarboxylic dianhydride may be used alone or in combination of two or more. In this case, the tetracarboxylic dianhydride represented by formula (1) and the aliphatic tetracarboxylic dianhydride are preferably used in total in the above-mentioned preferred amount.

[0061] As the polyamic acid contained in the liquid crystal aligning agent of the present invention, tetracarboxylic dianhydride represented by the following formula (4) may be used in addition to the tetracarboxylic dianhydride represented by the formula (1) and the aliphatic tetracarboxylic dianhydride.

[0062]

[0063] In formula (4), X is a tetravalent organic group, and its structure is not particularly limited. Specific examples include the following structures of formulae (X-31) to (X-36).

[0064]

[0065] <Diamine component>

[0066] The diamine component used in the manufacture of the liquid crystal aligning agent of the present invention contains the diamine of the above formula (2). In formula (2), Y1 is a divalent organic group having at least one structure selected from the group consisting of an amino group, an imino group and a nitrogen-containing heterocyclic ring, and B1 to B2 are each independently a hydrogen atom, or an alkyl group, an alkenyl group or an alkynyl group having 1 to 10 carbon atoms and optionally having a substituent.

[0067] Specific examples of the above-mentioned alkyl groups include methyl, ethyl, propyl, butyl, tert-butyl, hexyl, octyl, decyl, cyclopentyl, cyclohexyl, etc. As alkenyl groups, groups obtained by replacing one or more CH-CH structures present in the above-mentioned alkyl groups with C=C structures can be mentioned, and more specifically, vinyl, allyl, 1-propenyl, isopropenyl, 2-butenyl, 1,3-butadienyl, 2-pentenyl, 2-hexenyl, cyclopropenyl, cyclopentenyl, cyclohexenyl, etc. can be mentioned. As alkynyl groups, groups obtained by replacing one or more CH2-CH2 structures present in the above-mentioned alkyl groups with C≡C structures can be mentioned, and more specifically, ethynyl, 1-propynyl, 2-propynyl, etc. can be mentioned.

[0068] The alkyl, alkenyl and alkynyl groups may have substituents as long as they have 1 to 10 carbon atoms, and may form a ring structure with the help of substituents. It should be noted that forming a ring structure with the help of substituents means that substituents are bonded to each other or to a part of the parent skeleton to form a ring structure.

[0069] Examples of the substituent include a halogen group, a hydroxyl group, a mercapto group, a nitro group, an aryl group, an organic oxy group, an organic thio group, an organic silyl group, an acyl group, an ester group, a thioester group, a phosphate group, an amide group, an alkyl group, an alkenyl group, and an alkynyl group.

[0070] Examples of the halogen group as a substituent include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom.

[0071] Examples of the aryl group as a substituent include a phenyl group. The aryl group may be further substituted with the other substituents described above.

[0072] As an organic oxy group belonging to a substituent, a structure represented by OR can be shown. The R can be the same or different, and the aforementioned alkyl, alkenyl, alkynyl, aryl, etc. can be exemplified. These R are optionally further substituted by the aforementioned substituent. As specific examples of alkoxy, methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, etc. can be cited.

[0073] As an organic thio group belonging to a substituent, a structure represented by -SR can be shown. As this R, the aforementioned alkyl, alkenyl, alkynyl, aryl, etc. can be exemplified. These Rs are optionally further substituted by the aforementioned substituent. As specific examples of alkylthio, methylthio, ethylthio, propylthio, butylthio, pentylthio, hexylthio, heptylthio, octylthio, etc. can be cited.

[0074] As an organosilyl group belonging to a substituent, a structure represented by -Si-(R)3 can be shown. The R can be the same or different, and the aforementioned alkyl, alkenyl, alkynyl, aryl, etc. can be exemplified. These R are optionally further substituted by the aforementioned substituent. As specific examples of alkylsilyl, trimethylsilyl, triethylsilyl, tripropylsilyl, tributylsilyl, tripentylsilyl, trihexylsilyl, amyldimethylsilyl, hexyldimethylsilyl, etc. can be cited.

[0075] As the acyl group belonging to the substituent, the structure represented by -C(O)-R can be shown. As the R, the above-mentioned alkyl, alkenyl, aryl, etc. can be exemplified. These Rs are optionally further substituted by the above-mentioned substituents. As specific examples of the acyl group, formyl, acetyl, propionyl, butyryl, isobutyryl, valeryl, isovaleryl, benzoyl, etc. can be cited.

[0076] As the ester group which is a substituent, a structure represented by -C(O)OR or -OC(O)-R can be shown. As this R, the above-mentioned alkyl group, alkenyl group, alkynyl group, aryl group, etc. can be exemplified. These R may be further substituted by the above-mentioned substituent.

[0077] As the thioester group which is a substituent, a structure represented by -C(S)OR or -OC(S)-R can be shown. As this R, the above-mentioned alkyl group, alkenyl group, alkynyl group, aryl group, etc. can be exemplified. These Rs may be further substituted by the above-mentioned substituents.

[0078] As a phosphate group belonging to a substituent, a structure represented by -OP(O)-(OR)2 can be shown. The R may be the same or different, and examples thereof include the aforementioned alkyl, alkenyl, alkynyl, aryl, etc. These R may be further substituted by the aforementioned substituent.

[0079] As the amide group belonging to the substituent, the structure represented by -C(O)NH2 or -C(O)NHR, -NHC(O)R, -C(O)N(R)2, -NRC(O)R can be shown. The R may be the same or different, and examples thereof include the above-mentioned alkyl, alkenyl, alkynyl, aryl, etc. These R may be further substituted by the above-mentioned substituent.

[0080] Examples of the aryl group as a substituent include the same groups as those mentioned above for the aryl group. The aryl group may be further substituted with the other substituent mentioned above.

[0081] Examples of the alkyl group as a substituent include the same groups as those mentioned above for the alkyl group. The alkyl group may be further substituted with the other substituent mentioned above.

[0082] Examples of the alkenyl group as a substituent include the same groups as those for the alkenyl group described above. The alkenyl group may be further substituted with the other substituent described above.

[0083] Examples of the alkynyl group as a substituent include the same groups as those mentioned above for the alkynyl group. The alkynyl group may be further substituted by the other substituent mentioned above.

[0084] Generally, when a bulky structure is introduced, the reactivity of the amino group and the liquid crystal orientation may be reduced. Therefore, B1 and B2 are more preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms which may have a substituent, and particularly preferably a hydrogen atom, a methyl group or an ethyl group.

[0085] The structure of Y1 in formula (2) is not particularly limited as long as it has at least one structure selected from the group consisting of an amino group, an imino group and a nitrogen-containing heterocyclic ring. If specific examples are given, divalent organic groups having at least one structure selected from the group consisting of an amino group, an imino group and a nitrogen-containing heterocyclic ring as shown in the following formulas (YD-1) to (YD-5) can be given.

[0086]

[0087] In the formula (YD-1), A1 is a nitrogen atom-containing heterocyclic ring having 3 to 15 carbon atoms, and Z1 is a hydrogen atom or an optionally substituted hydrocarbon group having 1 to 20 carbon atoms.

[0088] In formula (YD-2), W1 is a hydrocarbon group having 1 to 10 carbon atoms, and A2 is a monovalent organic group having 3 to 15 carbon atoms and having a nitrogen atom-containing heterocyclic ring, or a disubstituted amino group substituted with an aliphatic group having 1 to 6 carbon atoms.

[0089] In formula (YD-3), W2 is a divalent organic group having 6 to 15 carbon atoms and 1 to 2 benzene rings, W3 is an alkylene group having 2 to 5 carbon atoms or a biphenylene group, Z2 is a hydrogen atom, an alkyl group having 1 to 5 carbon atoms or a benzene ring, and a is an integer of 0 to 1.

[0090] In the formula (YD-4), A3 is a nitrogen atom-containing heterocyclic ring having 3 to 15 carbon atoms.

[0091] In the formula (YD-5), A4 is a nitrogen atom-containing heterocyclic ring having 3 to 15 carbon atoms, and W5 is an alkylene group having 2 to 5 carbon atoms.

[0092] The nitrogen-containing heterocyclic ring having 3 to 15 carbon atoms as A1, A2, A3 and A4 of formula (YD-1), (YD-2), (YD-4) and (YD-5) is not particularly limited as long as it is a known structure. Among them, pyrrolidine, pyrrole, imidazole, pyrazole, oxazole, thiazole, piperidine, piperazine, pyridine, pyrazine, indole, benzimidazole, quinoline, isoquinoline and carbazole are mentioned, and piperazine, piperidine, indole, benzimidazole, imidazole, carbazole and pyridine are more preferred.

[0093] Furthermore, as specific examples of Y2 in formula (2), divalent organic groups having nitrogen atoms as shown in the following formulas (YD-6) to (YD-38) can be cited. In order to suppress charge accumulation caused by AC drive, formulas (YD-14) to (YD-21) are more preferred, and (YD-14) and (YD-18) are particularly preferred.

[0094]

[0095] In formula (YD-14) and (YD-21), j is an integer of 0 to 3. In formula (YD-17), h is an integer of 1 to 3.

[0096]

[0097] In the formulas (YD-24), (YD-25), (YD-28) and (YD-29), j is an integer of 0 to 3.

[0098]

[0099] The proportion of the diamine represented by formula (2) in the polyamic acid and the imidized polymer of the polyamic acid of the present invention is preferably 10 to 100 mol %, more preferably 30 to 100 mol %, and even more preferably 50 to 100 mol %, based on 1 mol of all diamines.

[0100] The diamine represented by formula (2) in the polyamic acid and the imidized polymer of the polyamic acid as the component (A) of the present invention may be used alone or in combination of two or more. In this case, the diamine represented by formula (2) is preferably used in the above-mentioned preferred amount in total.

[0101] In addition to using the diamine represented by the above formula (2), the polyamic acid contained in the liquid crystal aligning agent of the present invention can also use the diamine represented by the following formula (5). Y2 in the following formula (5) is a divalent organic group, and its structure is not particularly limited, and two or more types can also be mixed. If specific examples are specifically given, the following (Y-1) to (Y-49) and (Y-57) to (Y-75) can be given.

[0102] H2N-Y2-NH2 (5)

[0103]

[0104]

[0105]

[0106] In the polyamic acid and the imidized polymer of the polyamic acid as the component (A) contained in the liquid crystal aligning agent of the present invention, when the proportion of the diamine represented by formula (5) increases, it is possible to impair the effect of the present invention, and is therefore not preferred. Therefore, the proportion of the diamine represented by formula (5) is preferably 0 to 90 mol%, more preferably 0 to 50 mol%, and further preferably 0 to 20 mol% relative to 1 mol of all diamines.

[0107] <Production Method of Polyamic Acid>

[0108] The polyamic acid as a polyimide precursor used in the present invention can be synthesized by the method shown below.

[0109] Specifically, it can be synthesized by reacting tetracarboxylic dianhydride and diamine in the presence of an organic solvent at -20 to 150°C, preferably 0 to 70°C, for 30 minutes to 24 hours, preferably 1 to 12 hours.

[0110] From the viewpoint of solubility of monomers and polymers, the organic solvent used in the above reaction is preferably N,N-dimethylformamide, N-methyl-2-pyrrolidone, γ-butyrolactone, or the like, and these may be used alone or in combination of two or more.

[0111] The concentration of the polymer is preferably 1 to 30% by mass, more preferably 5 to 20% by mass, from the viewpoint of preventing the polymer from precipitating and easily obtaining a high molecular weight product.

[0112] The polyamic acid obtained by the above-mentioned operation is injected into a poor solvent by fully stirring the reaction solution, so that the polymer can be precipitated and recovered. In addition, after repeatedly precipitating and cleaning with a poor solvent, by normal temperature drying or heat drying, it is possible to obtain a refined polyamic acid powder. The poor solvent is not particularly limited, and water, methanol, ethanol, 2-propanol, hexane, butyl cellosolve, acetone, toluene, etc. can be cited, preferably water, methanol, ethanol, 2-propanol, etc.

[0113] <Production Method of Polyimide>

[0114] The polyimide used in the present invention can be produced by imidizing the above-mentioned polyamic acid.

[0115] When polyimide is produced from polyamic acid, chemical imidization, which is a simple process in which a catalyst is added to a solution of the polyamic acid obtained by reacting a diamine component with tetracarboxylic dianhydride, is performed. Chemical imidization is preferred because the imidization reaction is carried out at a relatively low temperature and the molecular weight of the polymer is not easily reduced during the imidization process.

[0116] Chemical imidization can be carried out by stirring the polymer to be imidized in an organic solvent in the presence of a basic catalyst and an acid anhydride. As an organic solvent, the solvent used in the above-mentioned polymerization reaction can be used. As a basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc. can be mentioned. Among them, pyridine has a moderate alkalinity for making the reaction proceed, so it is preferred. In addition, as an acid anhydride, acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc. can be mentioned, wherein, when acetic anhydride is used, it is easy to purify after the reaction is completed, so it is preferred.

[0117] The temperature during the imidization reaction is -20 to 140°C, preferably 0 to 100°C, and the reaction time can be 1 to 100 hours. The amount of the basic catalyst is 0.5 to 30 times the mole of the polyamic acid group, preferably 2 to 20 times the mole, and the amount of the acid anhydride is 1 to 50 times the mole of the polyamic acid group, preferably 3 to 30 times the mole. The imidization rate of the obtained polymer can be controlled by adjusting the amount of catalyst, temperature, and reaction time.

[0118] Since the added catalyst and the like remain in the solution after the imidization reaction of the polyamic acid, it is preferable to recover the obtained imidized polymer by the following means and redissolve it in an organic solvent to obtain the liquid crystal aligning agent of the present invention.

[0119] The polyimide solution obtained as described above can be poured into a poor solvent while being sufficiently stirred to precipitate a polymer. The precipitation is repeated several times and the solution is washed with a poor solvent, followed by drying at room temperature or by heating to obtain a purified polymer powder.

[0120] The poor solvent is not particularly limited, and examples thereof include methanol, 2-propanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, and the like. Preferred are methanol, ethanol, 2-propanol, acetone, and the like.

[0121] <(B) Component>

[0122] (B) Component contained in the liquid crystal aligning agent of this invention is at least 1 type of polymer selected from the group consisting of a polyimide precursor, an imidation polymer of the polyimide precursor, and a photosensitive side chain type acrylic polymer which shows liquid crystallinity in a specific temperature range.

[0123] <Polyimide Precursor>

[0124] The polyimide precursor is a polyimide precursor having a structural unit represented by the following formula (11).

[0125]

[0126] In formula (11), X 11 are independently a tetravalent organic group, Y 11 are each independently a divalent organic group. 11 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, A 11 ~A 12 Each independently represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms which may have a substituent.

[0127] As R 11 Specific examples of the above-mentioned alkyl group include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, etc. From the viewpoint of the ease of imidization by heating, R 11 Preferred is a hydrogen atom or a methyl group.

[0128] In formula (11), X 11 is a tetravalent organic group derived from a tetracarboxylic acid derivative, and its structure is not particularly limited. 11 Two or more types may be present in combination. 11 Specific examples include structures of the following formulae (X-1) to (X-44).

[0129]

[0130]

[0131] In the above formula (X-1), R8 to R 11 R8 to R1 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group, or a phenyl group. 11 In the case of a bulky structure, there is a possibility that the liquid crystal orientation may be reduced, and therefore a hydrogen atom, a methyl group, or an ethyl group is more preferred, and a hydrogen atom or a methyl group is particularly preferred.

[0132] In formula (11), from the viewpoint of the availability of monomers, X 11 It preferably contains a structure selected from (X-1) to (X-14).

[0133] The preferred ratio of the structures selected from the above (X-1) to (X-14) is 11 The content is 20 mol% or more of the total, more preferably 60 mol% or more, and even more preferably 80 mol% or more.

[0134] In formula (11), A 11 and A 12Each independently represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms which may have a substituent, an alkenyl group having 2 to 10 carbon atoms which may have a substituent, or an alkynyl group having 2 to 10 carbon atoms which may have a substituent.

[0135] These A 11 and A 12 Specific examples and preferred examples are the same as B1 and B2 in the sections of the above-mentioned components (A-1) and (A-2).

[0136] In formula (11), Y 11 It is a divalent organic group derived from diamine, and its structure is not particularly limited. 11 As specific examples of the structure of the present invention, the above-mentioned (Y-1) to (Y-49) and (Y-57) to (Y-75) and (YD-6) to (YD-38) described in the item of the aforementioned (A) component can be cited. In addition, on this basis, the following (Y-76) to (Y-97) and (YD-39) to (YD-52) can also be cited.

[0137]

[0138]

[0139]

[0140] (In formula (YD-50), m and n are each an integer of 1 to 11, and m+n is an integer of 2 to 12.)

[0141] As Y 11 The structure is more preferably at least one selected from the group consisting of the structures represented by the following formulae (15) and (16), from the viewpoint of the liquid crystal orientation and pretilt angle of the obtained liquid crystal alignment film.

[0142]

[0143] In formula (15), R 12 is a single bond or a divalent organic group having 1 to 30 carbon atoms, R 13 is a hydrogen atom, a halogen atom or a monovalent organic group having 1 to 30 carbon atoms, a is an integer of 1 to 4, and when a is 2 or more, R 12 , R 13 can be the same or different from each other. R in formula (16) 14 Single bond, -O-, -S-, -NR 15 -, an amide bond, an ester bond, a urea bond, or a divalent organic group having 1 to 40 carbon atoms, R 15 A hydrogen atom or a methyl group.

[0144] Specific examples of formula (15) and formula (16) include the following structures.

[0145] The highly linear structure can improve the orientation of the liquid crystal when it is made into a liquid crystal alignment film, so as a Y 11 , and the aforementioned Y-7, Y-21, Y-22, Y-23, Y-25, Y-43, Y-44, Y-45, Y-46, Y-48, Y-63, Y-71, Y-72, Y-73, Y-74, and Y-75 are further preferred. The ratio of the above structure that can improve the orientation of the liquid crystal is preferably Y 11 The content is 20 mol% or more of the total, more preferably 60 mol% or more, and even more preferably 80 mol% or more.

[0146] When it is desired to increase the pretilt angle of liquid crystal when forming a liquid crystal alignment film, it is preferred to 11 In the side chain, Y has a long chain alkyl group, an aromatic ring, an aliphatic ring, a steroid skeleton, or a structure obtained by combining these. 11 , preferably Y-76, Y-77, Y-78, Y-79, Y-80, Y-81, Y-82, Y-83, Y-84, Y-85, Y-86, Y-87, Y-88, Y-89, Y-90, Y-91, Y-92, Y-93, Y-94, Y-95, Y-96, and Y-97. When the ratio of the above structure is to be increased, Y- 11 The content is 1 to 30 mol %, more preferably 1 to 20 mol % of the total.

[0147] Moreover, when using the polyimide (precursor) which has a photo-alignable side chain as a polymer of (B) component, it is preferable to use the polyimide (precursor) which has the following photoreactive side chain.

[0148] -R 16 -R 17 -R 18 -R 19 (b)

[0149] (R 16 represents any one of -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)-, and -N(CH3)CO-, and R 17 Represents a cyclic, unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, wherein any -CH2- of the alkylene group is optionally replaced by -CF2- or -C=C-, and when any of the following groups are not adjacent to each other, they are optionally replaced by these groups: -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, carbocyclic ring, heterocyclic ring. R 18represents any one of -CH2-, -O-, -COO-, -OCO-, -NHCO-, -NH-, -N(CH3)-, -CON(CH3)-, -N(CH3)CO-, a carbocyclic ring or a heterocyclic ring, and R 19 Vinylphenyl, -CR 20 =CH2 group, -CR 20 (OH)-CH3 group, carbocyclic ring, heterocyclic ring or a structure represented by a formula selected from the following group, R 20 represents a hydrogen atom or a methyl group which may be substituted by a fluorine atom. )

[0150]

[0151]

[0152] When producing such a polyimide precursor, it is convenient to use a diamine substituted with a side chain represented by the above formula (b) as the diamine.

[0153] In addition, a polyimide precursor having a photo-alignment group in the main chain may be used. In this case, it is convenient to use a diamine having a bond containing a photo-alignment group between amines as represented by the following formula (21).

[0154]

[0155] (In formula (21), X 21 is a single bond or an alkylene group with 1 to 5 carbon atoms, X 22 is -OCO-CH=CH- or -CH=CH-COO-, X 23 is a single bond, an alkylene group having 1 to 10 carbon atoms, or a divalent benzene ring, X 24 is a single bond, -OCO-CH=CH- or -CH=CH-COO-, X 25 is a single bond or an alkylene group having 1 to 5 carbon atoms. Among them, it has one or more cinnamoyl groups.

[0156] Examples of the diamine represented by formula (21) include the following diamines.

[0157]

[0158] (In the formula, X is independently a single bond or a bonding group selected from ether (-O-), ester (-COO- or -OCO-) and amide (-CONH- or -NHCO-), Y is independently a single bond or an alkylene group having 1 to 5 carbon atoms, and Z is independently an alkylene group having 1 to 10 carbon atoms or a phenylene group. There are no particular limitations on the bonding position of the amino group on the benzene ring and the position of the bonding group relative to the central benzene ring.)

[0159] Specific examples of the diamine represented by formula (21) include the following diamines.

[0160]

[0161]

[0162] The liquid crystal orientation film formed by using the liquid crystal orientation agent containing polyimide precursors such as polyamic acid, polyamic acid ester, polyimide, and polyamide with the diamine shown in the above formula (21) as raw materials is a film that reduces the changes in liquid crystal orientation performance caused by AC (alternating current) drive, such as changes in the orientation direction of the liquid crystal. Therefore, for the liquid crystal display element having the liquid crystal orientation film, since the liquid crystal orientation performance of the liquid crystal orientation film under AC drive is stable, it is not easy to produce residual images due to AC drive, that is, the residual image characteristics based on AC drive are very good. In addition, the liquid crystal orientation film formed using the diamine shown in the above formula (21) can be made into a film having excellent liquid crystal orientation performance itself and substantially no orientation defects.

[0163] The polyimide precursor used in the present invention is obtained by reacting a diamine component with a tetracarboxylic acid derivative, and examples thereof include polyamic acid and polyamic acid ester.

[0164] <Production of polyimide precursor-polyamic acid>

[0165] The method for producing the polyamic acid described in the sections of the components (A-1) and (A-2) is followed.

[0166] <Production of polyimide precursor-polyamic acid ester>

[0167] The polyamic acid ester which is a polyimide precursor used in the present invention can be produced by the production method of (1), (2) or (3) shown below.

[0168] (1) When produced from polyamic acid

[0169] Polyamic acid ester can be produced by esterifying the polyamic acid produced as described above. Specifically, it can be produced by reacting a polyamic acid with an esterifying agent in the presence of an organic solvent at -20°C to 150°C, preferably 0°C to 50°C for 30 minutes to 24 hours, preferably 1 to 4 hours.

[0170] As the esterifying agent, a substance that can be easily removed by purification is preferred, and examples thereof include N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, N,N-dimethylformamide dipropyl acetal, N,N-dimethylformamide dineopentyl butyl acetal, N,N-dimethylformamide di-tert-butyl acetal, 1-methyl-3-p-tolyl triazene, 1-ethyl-3-p-tolyl triazene, 1-propyl-3-p-tolyl triazene, 4-(4,6-dimethoxy-1,3,5-triazine-2-yl)-4-methylmorpholine hydrochloride, etc. The amount of the esterifying agent added is preferably 2 to 6 molar equivalents relative to 1 mole of the repeating unit of the polyamic acid.

[0171] Examples of the organic solvent include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and 1,3-dimethyl-imidazolidinone. In addition, when the polyimide precursor has high solvent solubility, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or solvents represented by formulas [D-1] to [D-3] described later can be used.

[0172] These solvents can be used alone or in combination. Furthermore, even if the solvent cannot dissolve the polyimide precursor, it can be mixed in the above-mentioned solvent for use as long as the generated polyimide precursor is not precipitated. In addition, the moisture in the solvent can hinder the polymerization reaction and even hydrolyze the generated polyimide precursor, so the solvent is preferably used after dehydration and drying.

[0173] From the viewpoint of polymer solubility, the solvent used in the above reaction is preferably N,N-dimethylformamide, N-methyl-2-pyrrolidone or γ-butyrolactone, and one or more of them can be used in combination. From the viewpoint of polymer precipitation being less likely to occur and high molecular weight bodies being easily obtained, the concentration during production is preferably 1 to 30% by mass, more preferably 5 to 20% by mass.

[0174] (2) When produced by reaction of tetracarboxylic acid diester dichloride and diamine

[0175] Polyamic acid ester can be produced from tetracarboxylic acid diester dichloride and diamine.

[0176] Specifically, it can be produced by reacting a tetracarboxylic acid diester dichloride with a diamine in the presence of a base and an organic solvent at -20°C to 150°C, preferably 0°C to 50°C, for 30 minutes to 24 hours, preferably 1 to 4 hours.

[0177] The base may be pyridine, triethylamine, 4-dimethylaminopyridine, etc., and pyridine is preferred for smooth reaction. The amount of base added is preferably 2 to 4 times the molar amount of the tetracarboxylic acid diester dichloride from the viewpoint of being easily removed and easily obtaining a high molecular weight product.

[0178] From the viewpoint of solubility of monomer and polymer, the solvent used in the above reaction is preferably N-methyl-2-pyrrolidone or γ-butyrolactone, and they can be used as one or as a mixture of two or more. From the viewpoint that precipitation of polymer is not easy to occur and high molecular weight body is easily obtained, the polymer concentration during manufacture is preferably 1 to 30% by mass, more preferably 5 to 20% by mass. In addition, in order to prevent the hydrolysis of tetracarboxylic acid diester dichloride, the solvent used in the manufacture of polyamic acid ester is preferably dehydrated as much as possible, preferably in a nitrogen atmosphere to prevent the mixing of external air.

[0179] (3) When produced from tetracarboxylic acid diester and diamine

[0180] Polyamic acid ester can be produced by polycondensing a tetracarboxylic-acid diester and a diamine.

[0181] Specifically, it can be produced by reacting a tetracarboxylic acid diester with a diamine at 0° C. to 150° C., preferably 0° C. to 100° C., in the presence of a condensing agent, a base, and an organic solvent for 30 minutes to 24 hours, preferably 3 to 15 hours.

[0182] The condensing agent may be triphenyl phosphite, dicyclohexylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N,N'-carbonyldiimidazole, dimethoxy-1,3,5-triazinylmethylmorpholinium, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium tetrafluoroborate, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate, (2,3-dihydro-2-thioxo-3-benzoxazolyl)phosphonic acid diphenyl ester, etc. The amount of the condensing agent added is preferably 2 to 3 times the molar amount of the tetracarboxylic acid diester.

[0183] The base may be a tertiary amine such as pyridine or triethylamine. The amount of the base added is preferably 2 to 4 times the mole of the diamine component from the viewpoint of being an amount that is easily removed and easily obtaining a high molecular weight product.

[0184] In the above reaction, the reaction can be efficiently advanced by adding a Lewis acid as an additive. The Lewis acid is preferably a lithium halide such as lithium chloride or lithium bromide. The amount of the Lewis acid added is preferably 0 to 1.0 times the mole of the diamine component.

[0185] In order to obtain high molecular weight polyamic acid ester among the manufacturing methods of said 3 kinds of polyamic acid ester, the manufacturing method of said (1) or said (2) is particularly preferable.

[0186] The solution of polyamic acid ester obtained by the above operation is injected into a poor solvent while being fully stirred, so that the polymer can be precipitated. It is precipitated several times and washed with a poor solvent, and then dried at room temperature or heated to obtain a refined polyamic acid ester powder. There is no particular limitation on the poor solvent, and water, methanol, ethanol, hexane, butyl cellosolve, acetone, toluene, etc. can be cited.

[0187] <Polyimide>

[0188] The polyimide used in the present invention can be produced by imidizing the polyamic acid ester or the polyamic acid described above. The method for producing the polyimide described in the sections of the (A-1) component and the (A-2) component can be followed.

[0189] <Photosensitive side chain acrylic polymer showing liquid crystallinity in a specific temperature range>

[0190] One form of the component (B) is a photosensitive side chain acrylic polymer that exhibits liquid crystallinity within a specific temperature range.

[0191] The side chain acrylic polymer may react under light having a wavelength of 250 nm to 400 nm and exhibit liquid crystallinity within a temperature range of 100° C. to 300° C.

[0192] The side chain type acrylic polymer preferably has a photosensitive side chain that reacts under light in a wavelength range of 250 nm to 400 nm.

[0193] The side chain type acrylic polymer preferably has a mesogen group that exhibits liquid crystallinity in a temperature range of 100°C to 300°C.

[0194] The side chain type acrylic polymer has a photosensitive side chain bonded to the main chain, which can sense light and undergo a cross-linking reaction, an isomerization reaction or a photo-Fries rearrangement. There is no particular limitation on the photosensitive side chain structure, and it is ideal to sense light and undergo a cross-linking reaction or a photo-Fries rearrangement, and it is more ideal to undergo a cross-linking reaction. In this case, even if exposed to external stresses such as heat, the achieved orientation control ability can be maintained stably for a long time. The structure of the photosensitive side chain type acrylic polymer film that can show liquid crystal properties is not particularly limited as long as it meets this characteristic, and it is preferred to have a rigid mesogen component in the side chain structure. In this case, when the side chain type acrylic polymer is made into a liquid crystal alignment film, a stable liquid crystal orientation can be obtained.

[0195] The structure of the acrylic polymer can be, for example, the following structure: a main chain and side chains bonded thereto, wherein the side chains have liquid crystal components such as biphenyl, terphenyl, phenylcyclohexyl, phenyl benzoate, and azophenyl, and a photosensitive group bonded to the front end that reacts to light to undergo cross-linking reactions and isomerization reactions; a main chain and side chains bonded thereto, wherein the side chains have a phenyl benzoate group that serves as a liquid crystal component and also undergoes a photo-Fries rearrangement reaction.

[0196] As a more specific example of the structure of a photosensitive side-chain acrylic polymer that exhibits liquid crystallinity within a specific temperature range, a structure having the following main chain and the following side chain is preferred, wherein the main chain is composed of at least one selected from the group consisting of free radical polymerizable groups such as hydrocarbons, (meth)acrylates, itaconates, fumarates, maleates, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, and norbornene, and the side chain is formed by at least one of the following formulae (31) to (35).

[0197]

[0198] In the formula, Ar1 represents a divalent substituent obtained by removing two hydrogen atoms from a benzene ring, a naphthalene ring, a pyrrole ring, a furan ring, a thiophene ring, or a pyridine ring, Ar2 and Ar3 each independently represent a divalent substituent obtained by removing two hydrogen atoms from a benzene ring, a naphthalene ring, a pyrrole ring, a furan ring, a thiophene ring, or a pyridine ring, and q 1 and q 2 one of them is 1 and the other is 0, Ar4 and Ar5 each independently represent a divalent substituent obtained by removing two hydrogen atoms from a benzene ring, a naphthalene ring, a pyrrole ring, a furan ring, a thiophene ring, or a pyridine ring, Y1-Y2 represent CH=CH, CH=N, N=CH, or C≡C, S1-S3 each independently represent a single bond, a linear or branched alkylene group having 1 to 18 carbon atoms, a cycloalkylene group having 5 to 8 carbon atoms, a phenylene group, or a biphenylene group; or represent a single bond, one or more bonds selected from ether bonds, ester bonds, amide bonds, urea bonds, carbamate bonds, amino bonds, carbonyl groups, or combinations thereof; or a structure in which two or more and ten sites selected from a linear or branched alkylene group having 1 to 18 carbon atoms, a cycloalkylene group having 5 to 8 carbon atoms, a phenylene group, a biphenylene group, or combinations thereof are bonded via the one or more bonds, or a structure in which a plurality of the above substituents are connected via the above bonds,

[0199] R 31represents a hydrogen atom, a hydroxyl group, a mercapto group, an amino group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylamino group having 1 to 8 carbon atoms, or a dialkylamino group having 2 to 16 carbon atoms, and the benzene ring and / or the naphthalene ring may be substituted by one or more substituents which are the same or different and are selected from a halogen atom, a cyano group, a nitro group, a carboxyl group, and an alkoxycarbonyl group having 2 to 11 carbon atoms. In this case, the alkyl group having 1 to 10 carbon atoms may be linear, branched, or cyclic, or may be a combination thereof, and may be optionally substituted by a halogen atom.

[0200] The photosensitive side chain type acrylic polymer which is the component (B) of the present application and which exhibits liquid crystallinity in a specific temperature range may contain a liquid crystal side chain.

[0201] The mesogen group of the liquid crystal side chain may be a group that is a mesogen structure alone, such as biphenyl or phenyl benzoate, or a group that is a mesogen structure by forming hydrogen bonds between side chains, such as benzoic acid. The following structure is preferred as the mesogen group of the side chain.

[0202]

[0203] <<Method for producing photosensitive side chain polymer>>

[0204] The photosensitive side chain acrylic polymer that exhibits liquid crystallinity in a specific temperature range can be obtained by polymerizing a photoreactive side chain monomer having the photosensitive side chain and a liquid crystal side chain monomer.

[0205] [Photoreactive side chain monomer]

[0206] The photoreactive side chain monomer refers to a monomer that can form a polymer having a photosensitive side chain at a polymer side chain site when forming the polymer.

[0207] As the photoreactive group contained in the side chain, structures represented by the above formulae (31) to (35) are preferred.

[0208] As a more specific example of a photoreactive side chain monomer, it is preferred to have a structure having the following polymerizable group and a photosensitive side chain, wherein the polymerizable group is composed of at least one selected from the group consisting of free radical polymerizable groups such as hydrocarbons, (meth)acrylates, itaconates, fumarates, maleates, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, norbornene, etc., and the photosensitive side chain is formed by at least one of the above-mentioned formulas (31) to (35).

[0209] [Photoreactive side chain monomer]

[0210] The photoreactive side chain monomer refers to a monomer in which a polymer derived from the monomer exhibits liquid crystallinity and the polymer can form a mesogen group at the side chain site.

[0211] As a more specific example of a liquid crystalline side chain monomer, it is preferred to have a structure having the following polymerizable group and side chain, wherein the polymerizable group is composed of at least one selected from the group consisting of free radical polymerizable groups such as hydrocarbons, (meth)acrylates, itaconates, fumarates, maleates, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, norbornene, etc., and the side chain has at least one of the aforementioned “mesogen groups possessed by the liquid crystalline side chain”.

[0212] The side chain acrylic polymer as one form of component (B) can be obtained by polymerization of the above-mentioned photoreactive side chain monomer showing liquid crystallinity. Alternatively, it can be obtained by copolymerization of a photoreactive side chain monomer not showing liquid crystallinity with a liquid crystal side chain monomer, or copolymerization of a photoreactive side chain monomer showing liquid crystallinity with a liquid crystal side chain monomer. Furthermore, it can be copolymerized with other monomers within the range that does not impair the ability to show liquid crystallinity.

[0213] Examples of other monomers include industrially available monomers capable of undergoing radical polymerization.

[0214] Specific examples of other monomers include unsaturated carboxylic acids, acrylate compounds, methacrylate compounds, maleimide compounds, acrylonitrile, maleic anhydride, styrene compounds, and vinyl compounds.

[0215] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, maleic acid, and fumaric acid.

[0216] Examples of the acrylate compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, benzyl acrylate, naphthyl acrylate, anthracene acrylate, anthracenyl methyl acrylate, phenyl acrylate, 2,2,2-trifluoroethyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, 2-propyl-2-adamantyl acrylate, 8-methyl-8-tricyclodecanyl acrylate, and 8-ethyl-8-tricyclodecanyl acrylate.

[0217] Examples of the methacrylate compound include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthracene methacrylate, anthracenyl methyl methacrylate, phenyl methacrylate, 2,2,2-trifluoroethyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, 2-methoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 3-methoxybutyl methacrylate, 2-methyl-2-adamantyl methacrylate, 2-propyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecanyl methacrylate, and 8-ethyl-8-tricyclodecanyl methacrylate. (Meth)acrylate compounds having a cyclic ether group such as glycidyl (meth)acrylate, (3-methyl-3-oxetanyl)methyl (meth)acrylate, and (3-ethyl-3-oxetanyl)methyl (meth)acrylate may also be used.

[0218] Examples of the vinyl compound include vinyl ether, methyl vinyl ether, benzyl vinyl ether, 2-hydroxyethyl vinyl ether, phenyl vinyl ether, and propyl vinyl ether.

[0219] Examples of the styrene compound include styrene, methylstyrene, chlorostyrene, and bromostyrene.

[0220] Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide.

[0221] The method for producing the side chain polymer of the present embodiment is not particularly limited, and a general method used in industry can be used. Specifically, it can be produced by cationic polymerization, free radical polymerization, and anionic polymerization using vinyl groups of liquid crystal side chain monomers and photoreactive side chain monomers. Among these, free radical polymerization is particularly preferred from the viewpoints of the difficulty of reaction control, etc.

[0222] As the polymerization initiator for radical polymerization, known radical polymerization initiators such as AIBN (azobisisobutyronitrile) and known compounds such as a reversible addition-fragmentation chain transfer (RAFT) polymerization agent can be used.

[0223] The radical polymerization method is not particularly limited, and emulsion polymerization, suspension polymerization, dispersion polymerization, precipitation polymerization, bulk polymerization, solution polymerization, etc. can be used.

[0224] The organic solvent used in the polymerization reaction of the photosensitive side chain acrylic polymer that exhibits liquid crystallinity within a specific temperature range is not particularly limited as long as it is an organic solvent that dissolves the produced polymer. Specific examples thereof are given below.

[0225] Examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-methylcaprolactam, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentyl alcohol, dipentene, ethyl amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, methyl cellosolve, ethyl cellosolve, and methyl cellosolve acetate. , ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol tert-butyl ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol mono Acetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, dioxane, n-hexane, n-pentane, n-octane, diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl ether Acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diethylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, etc.

[0226] These organic solvents may be used alone or in combination. Furthermore, even a solvent that cannot dissolve the generated polymer may be used as long as the generated polymer does not precipitate.

[0227] In radical polymerization, oxygen in the organic solvent may inhibit the polymerization reaction, and therefore, the organic solvent is preferably degassed as much as possible before use.

[0228] The polymerization temperature during free radical polymerization can be selected from any temperature of 30°C to 150°C, preferably in the range of 50°C to 100°C. In addition, the reaction can be carried out at any concentration. When the concentration is too low, it is difficult to obtain a high molecular weight polymer. When the concentration is too high, the viscosity of the reaction solution becomes too high and it is difficult to stir uniformly. Therefore, the monomer concentration is preferably 1% to 50% by mass, more preferably 5% to 30% by mass. The reaction can be carried out at a high concentration in the initial stage, and then an organic solvent can be added.

[0229] In the above-mentioned free radical polymerization reaction, when the ratio of the free radical polymerization initiator is large relative to the monomer, the molecular weight of the obtained polymer becomes small, and when it is small, the molecular weight of the obtained polymer becomes large, so the ratio of the free radical initiator is preferably 0.1 mol% to 10 mol% relative to the polymerized monomer. In addition, various monomer components, solvents, initiators, etc. can also be added during polymerization.

[0230] [Recovery of photosensitive side-chain acrylic polymers that exhibit liquid crystallinity within a specific temperature range]

[0231] When the polymer generated is recovered from the reaction solution of the photosensitive side chain polymer obtained by the above reaction and capable of showing liquid crystallinity, the reaction solution is put into a poor solvent to precipitate these polymers. As the poor solvent used for precipitation, methanol, acetone, hexane, heptane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, diethyl ether, methyl ethyl ether, water, etc. can be mentioned. The polymer precipitated by being put into the poor solvent can be dried at room temperature or heated under normal pressure or reduced pressure after being filtered and recovered. In addition, when the operation of re-dissolving the precipitated polymer in an organic solvent and re-precipitating and recovering it is repeated 2 to 10 times, the impurities in the polymer can be reduced. As the poor solvent at this time, for example, alcohols, ketones, hydrocarbons, etc. can be mentioned. When 3 or more poor solvents selected from them are used, the refining efficiency is further improved, so it is preferred.

[0232] The molecular weight of the photosensitive side chain acrylic polymer which is one form of the component (B) and which exhibits liquid crystallinity in a specific temperature range is preferably 2,000 to 1,000,000, more preferably 5,000 to 100,000, as measured by GPC (Gel Permeation Chromatography) method, in consideration of the strength of the resulting coating film, workability during coating film formation, and uniformity of the coating film.

[0233] About content of (A) component and (B) component in the liquid crystal aligning agent of this invention, the mass ratio of the total amount of (A) component and (B) component is 5:95-95:5, More preferably, it is 10:90-90:10.

[0234] The imidization rate of the component (A) and the component (B) in the liquid crystal aligning agent of the present invention when the component (B) is a polyimide (precursor) can be arbitrarily adjusted according to the use or purpose. From the viewpoint of solubility and charge storage characteristics, the imidization rate of the specific polymer (A) component is preferably 0 to 55%, more preferably 0 to 20%. In addition, from the viewpoint of the orientation of the liquid crystal, the orientation control ability, and the voltage holding rate, the imidization rate of the specific polymer (B) is preferably high, preferably 40% to 95%, more preferably 55 to 90%.

[0235] <Liquid Crystal Alignment Agent>

[0236] The liquid crystal aligning agent used in the present invention has a solution form in which a polymer component is dissolved in an organic solvent. The molecular weight of the polymer is preferably 2,000 to 500,000, more preferably 5,000 to 300,000, and further preferably 10,000 to 100,000 in terms of weight average molecular weight. In addition, the number average molecular weight is preferably 1,000 to 250,000, more preferably 2,500 to 150,000, and further preferably 5,000 to 50,000.

[0237] The polymer concentration of the liquid crystal aligning agent used in the present invention can be appropriately changed according to the setting of the thickness of the coating film to be formed. From the viewpoint of forming a uniform and defect-free coating film, it is preferably 1% by mass or more, and from the viewpoint of the storage stability of the solution, it is preferably set to 10% by mass or less. The particularly preferred polymer concentration is 2 to 8% by mass.

[0238] For the organic solvent contained in the liquid crystal alignment agent used in the present invention, as long as it is a solvent that makes the polymer component uniformly dissolved, there is no particular limitation. If its specific example is given, N, N-dimethylformamide, N, N-diethylformamide, N, N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-methylcaprolactam, 2-pyrrolidone, N-vinyl-2-pyrrolidone, dimethyl sulfoxide, dimethyl sulfone, γ-butyrolactone, 1,3-dimethylimidazolidinone, 3-methoxy-N, N-dimethylpropionamide, etc. can be given. They can use one or more than two kinds in a mixed manner. In addition, even if it is a solvent that cannot uniformly dissolve the polymer component in a single case, it can also be mixed in the above-mentioned organic solvent as long as the polymer does not precipitate.

[0239] In addition, the organic solvent contained in the liquid crystal alignment agent is usually a mixed solvent, and the mixed solvent is combined with a solvent that improves the coating property when the liquid crystal alignment agent is applied or the surface smoothness of the coating film in addition to the above-mentioned solvents, and the liquid crystal alignment agent of the present invention is also preferably used in this mixed solvent. Specific examples of organic solvents used in combination are given below, but are not limited to these examples.

[0240] For example, ethanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, isopentanol, tert-pentanol, 3-methyl-2-butanol, neopentyl alcohol, 1-hexanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 2-ethyl-1-hexanol, cyclohexanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 2,6-dimethyl-4-heptanol, 1,2-ethanediol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4 -Butanediol, 2,3-butanediol, 1,5-pentanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, diisopropyl ether, dipropyl ether, dibutyl ether, dihexyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-butoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 2-pentanone, 3-pentanone, 2-hexanone, 2-heptanone, 4-heptanone, 2,6-dimethyl-4-heptanone, 4,6-dimethyl-2-heptanone, 3-ethoxybutyl acetate, 1-methylpentyl acetate, 2-ethylbutyl acetate, 2-ethyl Hexyl acetate, ethylene glycol monoacetate, ethylene glycol diacetate, propylene carbonate, ethylene carbonate, 2-(methoxymethoxy)ethanol, ethylene glycol monobutyl ether, ethylene glycol monoisoamyl ether, ethylene glycol monohexyl ether, 2-(hexyloxy)ethanol, furfuryl alcohol, diethylene glycol, propylene glycol, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monobutyl ether, 1-(butoxyethoxy)propanol, propylene glycol monomethyl ether acetate, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, ethylene glycol monoacetate, ethylene glycol diacetate, diethylene glycol monoethyl ether acetate, di Ethylene glycol monobutyl ether acetate, 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl ether acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isoamyl lactate, and solvents represented by the following formulas [D-1] to [D-3].

[0241]

[0242] In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms, wherein in the formula [D-2], D 2 represents an alkyl group having 1 to 3 carbon atoms, wherein D 3 It represents an alkyl group having 1 to 4 carbon atoms.

[0243] Among them, as a preferred combination of solvents, there can be mentioned: N-methyl-2-pyrrolidone, γ-butyrolactone and ethylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone and propylene glycol monobutyl ether; N-ethyl-2-pyrrolidone and propylene glycol monobutyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, 4-hydroxy-4-methyl-2-pentanone and diethylene glycol diethyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and 2,6-dimethyl-4-heptanone; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and diisopropyl ether; N-methyl-2-pyrrolidone, γ-butyrolactone, propylene glycol monobutyl ether and 2,6-dimethyl-4-heptanol; N-methyl-2-pyrrolidone, γ-butyrolactone and dipropylene glycol dimethyl ether, etc. The kind and content of such a solvent are appropriately selected depending on a coating device, coating conditions, coating environment, and the like of the liquid crystal aligning agent.

[0244] Moreover, in order to improve the mechanical strength of a film, the following additives can be added to the liquid crystal aligning agent of this invention.

[0245]

[0246]

[0247] These additives are preferably used in an amount of 0.1 to 30 parts by mass based on 100 parts by mass of the polymer component contained in the liquid crystal aligning agent. If the amount is less than 0.1 parts by mass, no effect can be expected, and if the amount exceeds 30 parts by mass, the orientation of the liquid crystal decreases, so 0.5 to 20 parts by mass is more preferred.

[0248] In addition to the above, the liquid crystal alignment agent of the present invention may also be added within the scope that does not impair the effects of the present invention: polymers other than polymers; dielectrics or conductive substances for changing the electrical properties of the liquid crystal alignment film, such as the dielectric constant and conductivity; silane coupling agents for improving the adhesion between the liquid crystal alignment film and the substrate; cross-linking compounds for improving the film hardness and density when the liquid crystal alignment film is made; and further, imidization promoters for efficiently promoting the imidization of polyamic acid when the coating film is fired.

[0249] <Liquid crystal alignment film>

[0250] <Method for producing liquid crystal alignment film>

[0251] The liquid crystal alignment film of the present invention is a film obtained by coating the above-mentioned liquid crystal alignment agent on a substrate and drying and firing. As a substrate for coating the liquid crystal alignment agent of the present invention, there is no particular limitation as long as it is a substrate with high transparency, and a glass substrate, a silicon nitride substrate, an acrylic substrate, a plastic substrate such as a polycarbonate substrate, etc. can be used. From the viewpoint of simplifying the process, it is preferred to use a substrate formed with an ITO electrode for liquid crystal driving. In addition, in a reflective liquid crystal display element, if it is only a single-sided substrate, an opaque substance such as a silicon wafer can also be used, and the electrode at this time can also use a material that reflects light such as aluminum.

[0252] As the coating method of the liquid crystal alignment agent of the present invention, spin coating, printing, inkjet and the like can be cited. The drying and firing steps after coating the liquid crystal alignment agent of the present invention can select any temperature and time. In order to fully remove the organic solvent contained, it is usually dried at 50°C to 120°C for 1 minute to 10 minutes, and then fired at 150°C to 300°C for 5 minutes to 120 minutes. There is no particular limitation on the thickness of the coating after firing. When it is too thin, the reliability of the liquid crystal display element is sometimes reduced, so it is 5 to 300nm, preferably 10 to 200nm.

[0253] As a method of performing an alignment treatment on the obtained liquid crystal alignment film, a brushing method, a photo-alignment treatment method, etc. are mentioned.

[0254] The brushing treatment can be performed using an existing brushing device. The material of the brushing cloth at this time includes cotton, nylon, rayon, etc. The conditions for the brushing treatment are usually a rotation speed of 300 to 2000 rpm, a feed speed of 5 to 100 mm / s, and a press depth of 0.1 to 1.0 mm. Subsequently, the residue generated by brushing is removed by ultrasonic cleaning using pure water, alcohol, etc.

[0255] As a specific example of the photo-orientation treatment method, the following method can be cited: the surface of the aforementioned coating film is irradiated with radiation polarized in a certain direction, and further heated at a temperature of 150 to 250°C according to the situation, thereby imparting liquid crystal orientation ability. As radiation, ultraviolet rays and visible light with a wavelength of 100nm to 800nm ​​can be used. Among them, ultraviolet rays with a wavelength of 100nm to 400nm are preferred, and ultraviolet rays with a wavelength of 200nm to 400nm are particularly preferred. In addition, in order to improve the orientation of the liquid crystal, the coating substrate can be irradiated with radiation while being heated at 50 to 250°C. The irradiation amount of the aforementioned radiation is preferably 1 to 10,000mJ / cm 2 , particularly preferably 100 to 5,000 mJ / cm 2 The liquid crystal alignment film prepared as described above can stably align liquid crystal molecules in a certain direction.

[0256] The higher the extinction ratio of polarized ultraviolet light is, the higher anisotropy can be imparted, which is preferred. Specifically, the extinction ratio of linearly polarized ultraviolet light is preferably 10:1 or more, and more preferably 20:1 or more.

[0257] The film irradiated with the polarized radiation as described above may then be subjected to a contact treatment with a solvent containing at least one selected from water and an organic solvent.

[0258] The solvent used in the contact treatment is not particularly limited as long as it is a solvent that dissolves the decomposition product generated by light irradiation. As specific examples, water, methanol, ethanol, 2-propanol, acetone, methyl ethyl ketone, 1-methoxy-2-propanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, methyl lactate, diacetone alcohol, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, propyl acetate, butyl acetate, and cyclohexyl acetate can be cited. These solvents can be used in combination of two or more.

[0259] From the viewpoint of versatility and safety, at least one selected from the group consisting of water, 2-propanol, 1-methoxy-2-propanol and ethyl lactate is more preferred. Water, 2-propanol and a mixed solvent of water and 2-propanol are particularly preferred.

[0260] In the present invention, the contact treatment between the film irradiated with polarized radiation and the solution containing an organic solvent is carried out by a treatment such as immersion treatment, spray treatment, etc. that allows the film and the liquid to preferably be fully contacted. Among them, a method of immersing the film in a solution containing an organic solvent for preferably 10 seconds to 1 hour, more preferably 1 to 30 minutes is preferred. The contact treatment can be carried out at room temperature or heating, preferably at 10 to 80°C, more preferably at 20 to 50°C. In addition, a means of improving contact such as ultrasound can be implemented as needed.

[0261] After the contact treatment, in order to remove the organic solvent in the solution used, either or both of rinsing (washing) with a low boiling point solvent such as water, methanol, ethanol, 2-propanol, acetone, methyl ethyl ketone, or drying may be performed.

[0262] Furthermore, the film subjected to the above-mentioned contact treatment with the solvent may be heated at 150° C. or higher in order to dry the solvent and reorient the molecular chains in the film.

[0263] The heating temperature is preferably 150 to 300° C. The higher the temperature, the more the molecular chain reorientation is promoted, but if the temperature is too high, the molecular chain may be decomposed. Therefore, the heating temperature is more preferably 180 to 250° C., and particularly preferably 200 to 230° C.

[0264] If the heating time is too short, the effect of reorientation of the molecular chains may not be obtained, and if it is too long, the molecular chains may be decomposed. Therefore, the heating time is preferably 10 seconds to 30 minutes, more preferably 1 minute to 10 minutes.

[0265] Moreover, the obtained liquid crystal aligning film is a film which is easily dissolved in a reprocessing material and is excellent in reprocessability.

[0266] Examples of the solvent used in the reprocessing include glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and propylene glycol monomethyl ether; glycol esters such as methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, and propylene glycol propyl ether acetate; glycols such as diethylene glycol, propylene glycol, butylene glycol, and hexylene glycol; alcohols such as methanol, ethanol, 2-propanol, and butanol; and ketones such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and γ-butyrolactone. Esters such as methyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, etc.; amides such as N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone.

[0267] As the reprocessing material, it is preferred that the solvent contains an alkaline component such as ethanolamine, and contains a rust inhibitor so that the alkalinity does not damage other parts such as electrodes. Manufacturers that provide such reprocessing materials include Hoemyung Industrial Co., Ltd. and KPX Chemial in South Korea.

[0268] The reprocessing is carried out by the following steps: the substrate with the liquid crystal alignment film is immersed in the above-mentioned reprocessing material at room temperature or heated to 30°C to 100°C for 1 second to 1000 seconds, preferably 30 seconds to 500 seconds; or the reprocessing material is sprayed in a spraying manner, and then the liquid is removed and washed with an alcohol solvent or pure water. It should be noted that from the perspective of work efficiency, the temperature of the reprocessing liquid during reprocessing is preferably low temperature, usually room temperature to 60°C, more preferably room temperature to 40°C.

[0269] <Liquid Crystal Display Element>

[0270] The liquid crystal display element of the present invention is obtained by obtaining a substrate with a liquid crystal alignment film from the liquid crystal aligning agent of the present invention by the above-mentioned method for producing a liquid crystal alignment film, preparing a liquid crystal cell by a known method, and using the liquid crystal cell to produce a liquid crystal display element.

[0271] As an example of a method for manufacturing a liquid crystal unit, a liquid crystal display element with a passive matrix structure is used as an example for explanation. It should be noted that a liquid crystal display element with an active matrix structure in which a switching element such as a TFT (Thin Film Transistor) is provided in each pixel portion constituting an image display may also be used.

[0272] First, a transparent glass substrate is prepared, a common electrode is provided on one substrate, and a segment electrode is provided on the other substrate. These electrodes can be formed into ITO electrodes, for example, and patterned in a manner that allows a desired image display. Next, an insulating film is provided on each substrate in a manner that covers the common electrode and the segment electrode. The insulating film can be made into a film formed of SiO2-TiO2 formed by a sol-gel method, for example.

[0273] Next, the liquid crystal alignment film of the present invention is formed on each substrate by the above-mentioned method.

[0274] Next, another substrate is overlapped on one substrate in such a manner that the orientation film surfaces face each other, and the periphery is bonded with a sealant. In order to control the gap between the substrates, a spacer is usually pre-mixed in the sealant. In addition, spacers for controlling the gap between the substrates are preferably pre-spread in the in-plane portion where the sealant is not provided. An opening portion that can be filled with liquid crystal from the outside is pre-set in a portion of the sealant.

[0275] Next, a liquid crystal material is injected into the space surrounded by the two substrates and the sealant through the opening provided in the sealant. Then, the opening is sealed with an adhesive. The injection can be performed by a vacuum injection method or by a method utilizing a capillary phenomenon in the atmosphere. Next, a polarizing plate is provided. Specifically, a pair of polarizing plates are attached to the surfaces of the two substrates on the opposite side to the liquid crystal layer. After the above steps, the liquid crystal display element of the present invention is obtained.

[0276] In the present invention, as the sealant, for example, a resin that is cured by ultraviolet irradiation or heating and has reactive groups such as epoxy, acryloyl, methacryloyl, hydroxyl, allyl, and acetyl can be used. It is particularly preferred to use a curing resin system having reactive groups of both epoxy and (meth)acryloyl.

[0277] In order to improve adhesion and moisture resistance, inorganic fillers can be mixed in the sealant of the present invention. As the inorganic filler that can be used, it is not particularly limited. Specifically, spherical silica, fused silica, crystalline silica, titanium oxide, titanium black, silicon carbide, silicon nitride, boron nitride, calcium carbonate, magnesium carbonate, barium sulfate, calcium sulfate, mica, talc, clay, aluminum oxide, magnesium oxide, zirconium oxide, aluminum hydroxide, calcium silicate, aluminum silicate, lithium aluminum silicate, zirconium silicate, barium titanate, glass fiber, carbon fiber, molybdenum disulfide, asbestos, etc. are preferably spherical silica, fused silica, crystalline silica, titanium oxide, titanium black, silicon nitride, boron nitride, calcium carbonate, barium sulfate, calcium sulfate, mica, talc, clay, aluminum oxide, aluminum hydroxide, calcium silicate, aluminum silicate. The above-mentioned inorganic filler can be mixed and used in two or more kinds.

[0278] Since this liquid crystal display element uses the liquid crystal aligning film obtained by the manufacturing method of the liquid crystal aligning film of this invention as a liquid crystal aligning film, it is excellent in reworkability, and can be used suitably for large-screen and high-definition liquid crystal television etc.

[0279] Example

[0280] The details of the production method of the present invention are described below by citing experimental methods and results of studying the raw material composition and mixing ratio, and examples of typical production methods, etc. It should be noted that the present invention is not limited to these examples.

[0281] Description of Abbreviations Used in This Example

[0282] (Organic Solvent)

[0283] NMP: N-methyl-2-pyrrolidone

[0284] GBL: gamma-butyrolactone

[0285] BCS: Butyl Cellosolve

[0286] Acid dianhydride (A): the following formula (A)

[0287] Acid dianhydride (B): the following formula (B)

[0288] Acid dianhydride (C): the following formula (C)

[0289] Acid dianhydride (D): the following formula (D)

[0290] Acid dianhydride (E): the following formula (E)

[0291] DA-1: The following formula (DA-1)

[0292] DA-2: The following formula (DA-2)

[0293] DA-3: The following formula (DA-3)

[0294] DA-4: The following formula (DA-4)

[0295] DA-5: The following formula (DA-5)

[0296] DA-6: The following formula (DA-6)

[0297] DA-7: The following formula (DA-7)

[0298] DA-8: The following formula (DA-8)

[0299] DA-9: The following formula (DA-9)

[0300] DA-10: The following formula (DA-10)

[0301] AD-1: The following formula (AD-1)

[0302] AD-2: The following formula (AD-2)

[0303]

[0304]

[0305] The following describes methods for measuring viscosity, measuring imidization ratio, evaluating reprocessability, preparing a liquid crystal cell, and evaluating charge relaxation characteristics.

[0306] [Viscosity measurement]

[0307] In the synthesis example, the viscosity of the polyamic acid ester and the polyamic acid solution was measured under the conditions of a sample amount of 1.1 mL, CORD-1 (1°34′, R24), and a temperature of 25°C using an E-type viscometer TV-25H (manufactured by Toki Sangyo Co., Ltd.).

[0308] [Determination of Imidization Ratio]

[0309] 20 mg of polyimide powder was added to an NMR sample tube (standard φ5 NMR sample tube manufactured by Kusano Scientific Co., Ltd.), 0.53 ml of deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS (tetramethylsilane) mixture) was added, and ultrasonic waves were applied to completely dissolve it. The solution was measured by 500 MHz proton NMR using an NMR measuring instrument (JNW-ECA500) manufactured by JEOL DATUM Co., Ltd. The imidization rate was determined by using a proton derived from a structure that did not change before and after imidization as a reference proton, and the peak integral value of the proton derived from the NH group of the amic acid appearing near 9.5 ppm to 10.0 ppm was used to determine the peak integral value of the proton, and the peak integral value of the proton derived from the NH group of the amic acid appearing near 9.5 ppm to 10.0 ppm was used to determine it by the following formula.

[0310] Imidization rate (%) = (1-α·x / y) × 100

[0311] In the above formula, x is the peak integral value of protons derived from NH groups of amic acid, y is the peak integral value of reference protons, and α is the number ratio of reference protons to one NH proton of amic acid in the case of polyamic acid (imidation ratio 0%).

[0312] [Evaluation of reprocessability]

[0313] The liquid crystal alignment agent of the present invention is applied to the Cr substrate by spin coating. After drying on a hot plate at 60°C for 1 minute and 30 seconds, it is sintered in a hot air circulation oven at 230°C for 20 minutes to form a coating with a film thickness of 100 nm. Then, the prepared substrate is immersed in a reprocessing material heated to 55°C for 300 seconds and developed, and then washed with ultrapure water for 20 seconds. Then, air is blown, and the liquid crystal alignment film that completely disappears is set as ○, and the one that remains is set as ×. The results are shown in Table 3.

[0314] [Fabrication of Liquid Crystal Cell]

[0315] A liquid crystal cell having a Fringe Field Switching (FFS) mode liquid crystal display element structure was prepared.

[0316] First, prepare a substrate with electrodes. The substrate is a glass substrate with a size of 30 mm × 35 mm and a thickness of 0.7 mm. On the substrate, as the first layer, an ITO electrode having a solid pattern for constituting a counter electrode is formed. On the counter electrode of the first layer, as the second layer, a SiN (silicon nitride) film formed by a CVD method is formed. The film thickness of the SiN film of the second layer is 500 nm, and it functions as an interlayer insulating film. On the SiN film of the second layer, as the third layer, a comb-shaped pixel electrode formed by patterning the ITO film is arranged to form two pixels, the first pixel and the second pixel. The size of each pixel is 10 mm in length and about 5 mm in width. At this time, the counter electrode of the first layer and the pixel electrode of the third layer are electrically insulated due to the action of the SiN film of the second layer.

[0317] The pixel electrode of the third layer has a comb-like shape formed by arranging a plurality of "く"-shaped electrode elements with a bent central portion. The width of each electrode element in the width direction is 3μm, and the interval between the electrode elements is 6μm. The pixel electrode forming each pixel is composed of an arrangement of a plurality of "く"-shaped electrode elements with a bent central portion, so the shape of each pixel is not a rectangle, but a shape similar to a bold "く" character that is bent in the central portion like the electrode elements. In addition, each pixel is divided into upper and lower parts with the central bent portion as the boundary, and has a first area on the upper side of the bent portion and a second area on the lower side.

[0318] When comparing the first area and the second area of ​​each pixel, the electrode elements constituting the pixel electrodes are formed in different directions. That is, when the brushing direction of the liquid crystal alignment film described later is used as a reference, in the first area of ​​the pixel, the electrode elements of the pixel electrode are formed at an angle of +10° (clockwise), and in the second area of ​​the pixel, the electrode elements of the pixel electrode are formed at an angle of -10° (clockwise). That is, the first area and the second area of ​​each pixel are constructed as follows: the directions of the rotation action (plane switching) of the liquid crystal in the substrate surface induced by applying a voltage between the pixel electrode and the counter electrode are opposite to each other.

[0319] Next, the obtained liquid crystal alignment agent was filtered with a 1.0 μm filter, and then applied to the prepared substrate with electrodes and a glass substrate with an ITO film formed on the back and a columnar spacer with a height of 4 μm by spin coating. After drying on a hot plate at 80°C for 5 minutes, it was sintered in a hot air circulation oven at 230°C for 20 minutes to form a coating with a film thickness of 100 nm. The coating surface was subjected to orientation treatments such as brushing and polarized ultraviolet irradiation to obtain a substrate with a liquid crystal alignment film. The above two substrates were taken as a group, and a sealant was printed on the substrate. After the other substrate was laminated in a manner where the liquid crystal alignment film was face to face and the orientation direction was 0°, the sealant was cured to make an empty unit. Liquid crystal MLC-2041 (manufactured by MERCK Co., Ltd.) was injected into the empty unit by a reduced pressure injection method, and the injection port was sealed to obtain an FFS driven liquid crystal unit. Subsequently, the obtained liquid crystal unit was heated at 110°C for 1 hour, left overnight, and used for each evaluation.

[0320] [Charge relaxation characteristics evaluation]

[0321] The above-mentioned liquid crystal unit is placed on a light source, and after measuring the VT characteristics (voltage-transmittance characteristics) at room temperature, the transmittance (Ta) of the liquid crystal unit under the state of applying a rectangular wave of ±1.5V / 60Hz is measured. Subsequently, the transmittance (Tb) of the liquid crystal unit is measured while superimposing a direct current of 1V and driving for 30 minutes, the direct current voltage is cut off, and the transmittance (Tc) of the liquid crystal unit when it is driven again for 20 minutes with only a rectangular wave of ±1.5V / 60Hz is measured. The difference (ΔT) between the transmittance (Tb, Tc) at each time and the initial transmittance (Ta) is calculated. The difference in transmittance caused by the voltage remaining in the liquid crystal display element is calculated. It can be considered that the earlier the residual voltage is relaxed, the less likely it is to produce afterimages. (Tb-Ta) is set to ○ when it is less than 2% 5 minutes after the start of applying the direct current voltage, and it is set to × when it is above, and (Tc-Ta) is set to ○ when it is less than 2% 5 minutes after the direct current voltage is cut off, and it is set to × when it is above. The results are shown in Table 3.

[0322] (Comparative Polymerization Example 1)

[0323] A 50 mL four-necked flask with a stirring device was placed in a nitrogen atmosphere, 2.55 g of (DA-1) and 0.96 g of (DA-3) were taken, and 25.7 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 3.00 g of acid dianhydride (C) was added while stirring the diamine solution, and 11.2 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere, and then 0.77 g of acid dianhydride (D) was added, and 4.4 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, the mixture was stirred at 50° C. for 16 hours to obtain a polyamic acid solution (PAA-1). The viscosity of the polyamic acid solution at a temperature of 25° C. was 358 cps.

[0324] (Comparative Polymerization Example 2)

[0325] A 50 mL four-necked flask with a stirring device was placed in a nitrogen atmosphere, 2.55 g of (DA-1) and 0.46 g of (DA-2) were taken, and 22.3 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 2.00 g of acid dianhydride (C) was added while stirring the diamine solution, and 6.3 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere, and then 1.51 g of acid dianhydride (D) was added, and 8.5 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, the mixture was stirred at 50° C. for 16 hours to obtain a polyamic acid solution (PAA-2). The viscosity of the polyamic acid solution at a temperature of 25° C. was 333 cps.

[0326] (Polymerization Example 1)

[0327] A 100 mL four-necked flask equipped with a stirring device was placed in a nitrogen atmosphere, 0.58 g of (DA-6), 1.32 g of (DA-4), 0.93 g of (DA-5), and 3.01 g of (DA-7) were taken, and 42.8 g of NMP was added, and the mixture was dissolved at 23° C. while stirring while nitrogen was supplied. 3.91 g of acid dianhydride (E) was added while stirring the diamine solution, and 12.4 g of NMP was further added, and the mixture was stirred at 40° C. for 16 hours under a nitrogen atmosphere to obtain a polyamic acid solution (PAA-3). The viscosity of the polyamic acid solution at a temperature of 25° C. was 450 cps.

[0328] (Polymerization Example 2)

[0329] A 100 mL four-necked flask equipped with a stirrer was placed in a nitrogen atmosphere, 6.19 g of (DA-9) and 2.14 g of (DA-8) were taken, and 61.1 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 5.71 g of acid dianhydride (B) was added while stirring the diamine solution, and 18.5 g of NMP was further added, and the mixture was stirred at 50° C. for 16 hours under a nitrogen atmosphere to obtain a polyamic acid solution (PAA-4). The viscosity of the polyamic acid solution at a temperature of 25° C. was 351 cps.

[0330] (Polymerization Example 3)

[0331] A 1L four-necked flask equipped with a stirring device was placed in a nitrogen atmosphere, and 86.0 g of (DA-4), 53.4 g of (DA-7), and 76.5 g of (DA-10) were taken, and 1580 g of NMP was added, and the mixture was dissolved at 23° C. while stirring while nitrogen was supplied. 93.2 g of acid dianhydride (E) was added while stirring the diamine solution, and 168 g of NMP was further added, and the mixture was stirred at 40° C. for 3 hours under a nitrogen atmosphere. Furthermore, 28.2 g of acid dianhydride (D) was added, and 160 g of NMP was further added, and the mixture was stirred at 23° C. for 4 hours under a nitrogen atmosphere to obtain a polyamic acid solution (PAA-5). The viscosity of the polyamic acid solution at a temperature of 25° C. was 200 mPa·s.

[0332] (Polymerization Example 4)

[0333] A 50 mL four-necked flask with a stirring device was placed in a nitrogen atmosphere, 2.55 g of (DA-1) and 0.78 g of (DA-4) were taken, and 24.4 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 1.75 g of acid dianhydride (B) was added while stirring the diamine solution, and 4.3 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere, and then 1.41 g of acid dianhydride (D) was added, and 8.0 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, the mixture was stirred at 50° C. for 16 hours to obtain a polyamic acid solution (PAA-6). The viscosity of the polyamic acid solution at a temperature of 25° C. was 240 cps.

[0334] (Polymerization Example 5)

[0335] A 50 mL four-necked flask with a stirring device was placed in a nitrogen atmosphere, 2.55 g of (DA-1) and 0.49 g of (DA-2) were taken, and 22.3 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 2.35 g of acid dianhydride (A) was added while stirring the diamine solution, and 8.3 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere, and then 1.80 g of acid dianhydride (C) was added, and 10.2 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, the mixture was stirred at 70° C. for 16 hours to obtain a polyamic acid solution (PAA-7). The viscosity of the polyamic acid solution at a temperature of 25° C. was 380 cps.

[0336] (Polymerization Example 6)

[0337] A 50 mL four-necked flask with a stirring device was placed in a nitrogen atmosphere, 2.55 g of (DA-1) and 0.49 g of (DA-2) were taken, and 22.3 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 2.35 g of acid dianhydride (A) was added while stirring the diamine solution, and 8.3 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere, and then 1.41 g of acid dianhydride (D) was added, and 8.0 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, the mixture was stirred at 70° C. for 16 hours to obtain a polyamic acid solution (PAA-8). The viscosity of the polyamic acid solution at a temperature of 25° C. was 321 cps.

[0338] (Polymerization Example 7)

[0339] A 50 mL four-necked flask with a stirring device was placed in a nitrogen atmosphere, 2.55 g of (DA-1) and 0.49 g of (DA-2) were taken, and 22.3 g of NMP was added, and the mixture was dissolved at 23° C. while stirring the mixture while nitrogen was supplied. 1.41 g of acid dianhydride (A) was added while stirring the diamine solution, and 2.9 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere, and then 1.41 g of acid dianhydride (B) was added, and 7.9 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, 1.00 g of acid dianhydride (C) was added, and 5.7 g of NMP was further added, and the mixture was stirred at 23° C. for 2 hours under a nitrogen atmosphere. Then, the mixture was stirred at 70° C. for 16 hours to obtain a polyamic acid solution (PAA-9). The viscosity of the polyamic acid solution at a temperature of 25° C. was 365 cps.

[0340] (Comparative Example 1)

[0341] Into a 50 mL conical flask containing a stirrer, 6.73 g of the polyamic acid solution (PAA-3) obtained in the comparative synthesis example, 15.27 g of (PAA-1), 2.40 g of an NMP solution containing 1 wt% of (AD-1), and 0.72 g of an NMP solution containing 10 wt% of (AD-2) were taken out, 2.88 g of NMP and 12.00 g of BCS were added, and the mixture was stirred with a magnetic stirrer for 2 hours to obtain a liquid crystal alignment agent (A-1).

[0342] (Comparative Example 2)

[0343] Into a 50 mL conical flask containing a stirrer, 4.00 g of the polyamic acid solution (PAA-4) obtained in the comparative synthesis example, 12.80 g of (PAA-2), and 2.40 g of an NMP solution containing 1 wt % of (AD-1) were taken out, 8.80 g of NMP and 12.00 g of BCS were added, and stirred for 2 hours with a magnetic stirrer to obtain a liquid crystal alignment agent (A-2).

[0344] (Comparative Example 3)

[0345] 800 g of the polyamic acid solution (PAA-5) obtained in (Polymerization Example 3) was taken out of a 3L conical flask with a stirrer, and 700 g of NMP, 69.7 g of acetic anhydride, and 18.0 g of pyridine were added. After stirring at room temperature for 30 minutes, the mixture was reacted at 55° C. for 3 hours. The reaction solution was put into 5600 g of methanol, and the resulting precipitate was filtered out. After washing the precipitate with methanol, it was dried under reduced pressure at a temperature of 60° C. to obtain a polyimide powder. The imidization rate of the polyimide powder was 75%.

[0346] 20.4 g of the polyamide powder was taken out from a 300 mL conical flask containing a stirrer, 150 g of NMP was added, and the mixture was stirred at 50° C. for 20 hours to dissolve the mixture, thereby obtaining a polyimide solution (SPI-1).

[0347] Into a 50 mL conical flask with a stirrer, 7.00 g of the polyimide solution (SPI-1), 10.40 g of (PAA-6), 2.40 g of an NMP solution containing 1 wt% of (AD-1), and 0.72 g of an NMP solution containing 10 wt% of (AD-2) were taken out, 7.48 g of NMP and 12.00 g of BCS were added, and the mixture was stirred with a magnetic stirrer for 2 hours to obtain a liquid crystal alignment agent (A-3).

[0348] (Examples 1 to 3)

[0349] Into a 50 mL conical flask containing a stirrer, 7.00 g of the polyimide solution (SPI-1) obtained in (Comparative Example 3) and 10.40 g of the polyamic acid solution (PAA-7 to 9) obtained in (Polymerization Examples 5 to 7) were taken out separately, 2.40 g of an NMP solution containing 1 wt% (AD-1) and 0.72 g of an NMP solution containing 10 wt% (AD-2) were taken out separately, 7.48 g of NMP and 12.00 g of BCS were added, and the mixture was stirred for 2 hours with a magnetic stirrer to obtain liquid crystal aligning agents (B-1 to 3) as shown in Table 1.

[0350] [Table 1]

[0351]

[0352] (Examples 4 to 6)

[0353] Into a 50 mL conical flask containing a stirrer, 4.00 g of the polyamic acid solution (PAA-4) obtained in (Polymerization Example 2), 12.80 g of the polyamic acid solution (PAA-7 to 9) obtained in (Polymerization Examples 5 to 7), and 2.40 g of an NMP solution containing 1 wt% of (AD-1) were taken out, 4.80 g of NMP and 12.00 g of BCS were added, and the mixture was stirred for 2 hours with a magnetic stirrer to obtain liquid crystal aligning agents (B-4 to 6) as shown in Table 2.

[0354] [Table 2]

[0355]

[0356] (Example 7)

[0357] Into a 50 mL conical flask containing a stirrer, 6.00 g of the polyamic acid solution (PAA-7) obtained in the comparative synthesis example, 11.20 g of (PAA-1), 2.40 g of an NMP solution containing 1 wt% of (AD-1), and 0.72 g of an NMP solution containing 10 wt% of (AD-2) were taken out, 7.68 g of NMP and 12.00 g of BCS were added, and the mixture was stirred for 2 hours with a magnetic stirrer to obtain a liquid crystal alignment agent (B-7).

[0358] [Table 3]

[0359]

[0360] Industrial Applicability

[0361] The liquid crystal alignment film obtained by the liquid crystal alignment agent of the present invention can reduce the charge accumulation caused by the asymmetry of the AC drive in the liquid crystal display element of the IPS drive mode and the FFS drive mode, and quickly relax the residual charge accumulated by the DC voltage, so that the IPS drive mode and the FFS drive mode liquid crystal display element with excellent afterimage characteristics can be obtained. Therefore, it is particularly useful as a liquid crystal display element of the IPS drive mode and the FFS drive mode, and a liquid crystal alignment film of a liquid crystal television.

Claims

1. A liquid crystal alignment agent, characterized in that: The invention comprises: (A) at least one polymer selected from the group consisting of a polyamic acid and an imidized polymer of the polyamic acid, wherein the polyamic acid is obtained using a tetracarboxylic dianhydride component comprising a tetracarboxylic dianhydride represented by the following formula (1) and an aliphatic tetracarboxylic dianhydride in a ratio of 10:90 to 90:10, and a diamine component comprising a diamine represented by the following formula (2); (B) at least one polymer selected from the group consisting of a polyimide precursor, an imidized polymer of the polyimide precursor, and a photosensitive side chain acrylic polymer that exhibits liquid crystallinity within a specific temperature range; and an organic solvent, In formula (1), i is 0 or 1, X is a single bond, an ether bond, a carbonyl group, an ester bond, a phenylene group, a linear alkylene group having 1 to 20 carbon atoms, a branched alkylene group having 2 to 20 carbon atoms, a cyclic alkylene group having 3 to 12 carbon atoms, a sulfonyl group, an amide bond, or a group composed of a combination thereof, wherein the alkylene group having 1 to 20 carbon atoms may be interrupted by a bond selected from an ester bond and an ether bond, and the carbon atoms of the phenylene group and the alkylene group may be substituted by one or more identical or different substituents selected from a halogen atom, a cyano group, an alkyl group, a haloalkyl group, an alkoxy group, and a haloalkoxy group, In formula (2), Y1 is at least one selected from the group consisting of divalent organic groups having structures of the following formulae (YD-14) and (YD-18), B1 and B2 are each independently a hydrogen atom, or an alkyl, alkenyl, or alkynyl group having 1 to 10 carbon atoms and optionally having a substituent; in formula (YD-14), j is an integer of 1 to 3; 10 to 100 mol % of the tetracarboxylic dianhydride component of the component (A) is tetracarboxylic dianhydride represented by the formula (1) and aliphatic tetracarboxylic dianhydride. The tetracarboxylic dianhydride represented by the formula (1) is 3,3',4,4'-biphenyltetracarboxylic dianhydride.

2. The liquid crystal alignment agent according to claim 1, characterized in that: 10 to 100 mol % of the diamine component of the component (A) is a diamine of formula (2).

3. The liquid crystal alignment agent according to claim 1, wherein The aliphatic tetracarboxylic dianhydride is bicyclo[3.3.0]octane 2,4,6,8-tetracarboxylic dianhydride 2,4:6,8. 4 . A liquid crystal aligning film obtained by applying the liquid crystal aligning agent according to claim 1 and baking the film. A liquid crystal display element comprising the liquid crystal aligning film according to claim 4 .