Antistatic resin composition, method for producing antistatic resin composition, and electronic component packaging material
Patent Information
- Application Number
- CN202110621845.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-08
- Filing Date
- 2021-06-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-06-03
AI Technical Summary
[0006]现有技术提出的在苯乙烯系树脂中混配有导电性碳的苯乙烯系抗静电材料发挥出105Ω/□程度的表面电阻率,根据电子部件的种类而表现出必不可缺的极低的表面电阻率,但根据电子部件的不同,表面电阻率低至这种程度未必是必不可缺的,也存在许多即使表面电阻率为1010Ω/□的程度仍为充分的电子部件
[0088] According to the present invention, even when combined with styrene-based resins such as general-purpose polystyrene (GPPS), rubber-modified polystyrene (HIPS), methyl methacrylate/styrene copolymer resin (MS resin), etc. An antistatic resin composition that also exhibits excellent antistatic properties and has excellent transparency, a method for producing the antistatic resin composition, and an electronic component packaging material.
Smart Images

Figure BDA0003098883970000061 
Figure BDA0003098883970000271 
Figure BDA0003098883970000331
Abstract
Description
Technical Field
[0001] The present invention relates to an antistatic resin composition, a method for producing the antistatic resin composition, and an electronic component packaging material. Background Art
[0002] Generally, vinyl aromatic hydrocarbon resins (e.g., styrene resins) are excellent in molding processability, rigidity, transparency, etc., and are low in cost, low in specific gravity, and excellent in economy. Therefore, molded products obtained by molding vinyl aromatic hydrocarbon resins are widely used in various fields as injection molded products, sheet molded products extruded from T-dies, spherical or square tubular special-shaped extrusion molded products extruded from special-shaped dies, etc.
[0003] Among them, sheet-shaped molded products or tubular extruded molded products made of vinyl aromatic hydrocarbon resins such as high-impact polystyrene and transparent MBS resin (methyl methacrylate / butadiene / styrene copolymer resin) are widely used in various electronic component packaging materials such as carriers for mounting / packaging electronic components such as integrated circuits (ICs) or large-scale integrated circuits (LSIs) in electronic devices, loading tubes (also called strips) for mounting / packaging connectors and various semiconductor components, and transport trays for packaging liquid crystal panels, etc.
[0004] The above-mentioned electronic component packaging materials such as carrier tapes, loading tubes, and transport trays are required to have various properties, in addition to mechanical properties such as rigidity and impact resistance, such as molding processability to avoid burrs during slit processing or to obtain a uniform thickness without uneven thickness during vacuum forming, transparency (visibility), and antistatic properties to prevent damage or destruction of electronic components due to static electricity. In response to these situations, various improvement studies have been conducted to improve these properties and obtain a better balance of physical properties.
[0005] In particular, as an antistatic material based on a vinyl aromatic hydrocarbon resin, a composition in which a conductive carbon such as Ketjen Black is mixed with a styrene resin has been widely known.
[0006] The prior art proposes that the styrene-based antistatic material in which conductive carbon is mixed in a styrene-based resin can exert 10 5 Ω / □ surface resistivity, which is indispensable for the type of electronic component, but it is not necessarily necessary to have such a low surface resistivity depending on the electronic component. There are many electronic components that have a surface resistivity of 10 10 The degree of Ω / □ is still sufficient for electronic components.
[0007] On the other hand, as a disadvantage of antistatic materials mixed with conductive carbon, the molded product is black and opaque, so it has poor visibility and is difficult to confirm the contents in the packaged state. In addition, the following problem is pointed out: when the electronic components are installed in the molded electronic component packaging material and actually transported, the contact part between the electronic components and the packaging material is rubbed due to vibration during transportation, thereby causing the conductive carbon to fall off, and the fallen conductive carbon may adhere to the electronic components, etc., which may cause contamination.
[0008] On the other hand, conventionally, development of related technologies for resin compositions that exhibit antistatic properties without using conductive carbon has been conducted.
[0009] For example, there has been proposed a technique for producing a resin composition in which a high molecular weight conductive polymer having a polyoxyalkylene chain is blended with a thermoplastic resin such as a styrene resin (for example, see Patent Document 1).
[0010] However, the refractive index of a high molecular conductive polymer is generally lower than that of a styrene resin as a base resin, and the electronic component packaging material formed by a resin composition mixed with a high molecular conductive polymer has a problem of causing white turbidity and impaired visibility due to a large deviation in their refractive indices. In addition, in order to exhibit antistatic properties, a high molecular conductive polymer must be mixed in a large amount at a content of generally 10% or more, and there is also a problem that the mechanical properties of the resin composition are greatly changed due to the polymer structure, such as a decrease in elastic modulus and a decrease in rigidity of the resin composition.
[0011] In addition, as a method for obtaining an antistatic resin composition, there is also a known method of adding a surfactant as a general-purpose antistatic agent to a thermoplastic resin.
[0012] However, surfactant-type antistatic agents exhibit their performance by seeping out on the surface of molded products. Therefore, when the surface of the molded product is wiped with water, there are problems with the stability of the antistatic performance, such as a temporary decrease in antistatic performance and an increase in surface resistivity. In addition, since the antistatic agent itself seeps out on the surface of the molded product, there is a concern that it may adhere to the electronic components as the content and cause contamination, making it unsuitable for use as a packaging material for electronic components.
[0013] Therefore, in recent years, as a new type of antistatic agent, an antistatic resin composition using a donor-acceptor system molecular compound composed of an organic boron compound and a nitrogen-containing compound and adding the compound to a thermoplastic resin has been proposed (see, for example, Patent Document 2 and Non-Patent Document 1).
[0014] This is an antistatic agent that combines the concept of molecular compounds. Unlike the existing surfactant type that oozes out on the surface of molded products to exert antistatic effects, this antistatic resin composition combines electron donors and acceptors to instantly exchange charges, thereby causing the charged charges to decay instantly and exhibit antistatic effects.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Application Publication No. 2011-6604
[0018] Patent Document 2: Japanese Patent No. 5734491
[0019] Non-patent literature
[0020] Non-patent document 1: Plastic Age magazine, April 2018, pp. 47-52 Summary of the invention
[0021] Problems to be solved by the invention
[0022] However, the antistatic resin composition using the above-mentioned donor-acceptor system molecular compound formed of an organic boron compound and a nitrogen-containing compound still has problems.
[0023] Resins that exhibit antistatic properties are limited to so-called crystalline polyolefin resins such as PE, PP, and cyclic polyolefins, or so-called polar resins containing heteroatoms other than hydrocarbons in a certain concentration or more in the polymer skeleton such as polyamide, PET resin, ABS resin, polyvinyl chloride, and polyacetal. That is, general-purpose polystyrene (also known as GPPS), rubber-modified polystyrene (also known as HIPS), and methyl methacrylate / styrene copolymer resins having a methyl methacrylate content of about 20% by mass (also known as MS resin) have the following problem: even if the above-mentioned donor-acceptor system molecular compound is mixed in an amount of, for example, about 4% by mass, which is generally considered to be sufficient, the effect of reducing the surface resistivity cannot be obtained, and the antistatic property cannot be exhibited.
[0024] Therefore, in view of the above-mentioned problems of the prior art, the object of the present invention is to provide an antistatic resin composition and a method for preparing the same, which can induce the original properties of the donor-acceptor system molecular compound in the resin composition mixed with the above-mentioned donor-acceptor system molecular compound, and show excellent antistatic performance and excellent transparency even when a styrene-based resin such as general-purpose polystyrene (GPPS), rubber-modified polystyrene containing grafted rubber particles (HIPS) or styrene acrylic copolymer resin is used as the base resin.
[0025] Means for solving problems
[0026] The present inventors have conducted intensive studies and have found that an antistatic resin composition exhibiting excellent antistatic performance and transparency can be obtained by combining a donor-acceptor system molecular compound with a specific block copolymer and optimizing the composition, thereby completing the present invention.
[0027] That is, the present invention is as follows. [1]
[0029] An antistatic resin composition comprising:
[0030] block copolymer (b), and
[0031] Donor-acceptor system molecular compound (c), wherein
[0032] The block copolymer (b) is a block copolymer comprising a vinyl aromatic hydrocarbon monomer unit and a conjugated diene monomer unit, and has a polymer block mainly composed of a vinyl aromatic hydrocarbon monomer unit, wherein the vinyl aromatic hydrocarbon monomer unit is 30 to 90% by mass, and the conjugated diene monomer unit is 70 to 10% by mass.
[0033] When the total amount of the block copolymer (b) and the donor-acceptor molecular compound (c) is 100% by mass, the content of the donor-acceptor molecular compound (c) is 0.5% by mass or more and 5% by mass or less. [2]
[0035] The antistatic resin composition as described in [1] above, wherein the surface resistivity is 1×10 12 Ω / □ or less. [3]
[0037] An antistatic resin composition comprising:
[0038] Vinyl aromatic hydrocarbon resin (a),
[0039] block copolymer (b), and
[0040] Donor-acceptor system molecular compound (c), wherein
[0041] The block copolymer (b) is a block copolymer comprising a vinyl aromatic hydrocarbon monomer unit and a conjugated diene monomer unit, and has a polymer block mainly composed of a vinyl aromatic hydrocarbon monomer unit, wherein the vinyl aromatic hydrocarbon monomer unit is 30 to 90% by mass, the conjugated diene monomer unit is 70 to 10% by mass,
[0042] When the total amount of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100% by mass, the mass ratio of the vinyl aromatic hydrocarbon resin (a) is 81% by mass or less, and the mass ratio of the block copolymer (b) is 19% by mass or more and less than 100% by mass,
[0043] When the total amount of the vinyl aromatic hydrocarbon resin (a), the block copolymer (b) and the donor-acceptor molecular compound (c) is 100% by mass, the content of the donor-acceptor molecular compound (c) is 0.5% by mass or more and 5% by mass or less,
[0044] The surface resistivity is 1×10 12 Ω / □ or less. [4]
[0046] The antistatic resin composition as described in the above [3], wherein the above-mentioned vinyl aromatic hydrocarbon resin (a) is any one selected from the group consisting of a homopolymer (a1) of a vinyl aromatic hydrocarbon monomer, a graft copolymer (a2) of a vinyl aromatic hydrocarbon monomer, and a random copolymer (a3) of a vinyl aromatic hydrocarbon monomer unit and a (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer unit. [5]
[0048] The antistatic resin composition as described in [3] or [4] above, wherein, in the melt flow rate (MFR) under 200°C and 5 kg load conditions specified in ISO 1133, the relationship between the MFR (hereinafter referred to as MFRa) of the vinyl aromatic hydrocarbon resin (a) and the MFR (hereinafter referred to as MFRb) of the block copolymer (b) satisfies:
[0049] Any one of the following conditions (i) to (iv).
[0050] <Condition(i)>
[0051] When the total of the above-mentioned (a) component and the above-mentioned (b) component is 100 mass%, when the above-mentioned (a) component is greater than 0 mass% and less than 30 mass%, and the above-mentioned (b) component is 70 mass% or more and less than 100 mass%, regardless of the numerical values of MFRa and MFRb, when the total of the above-mentioned (a) component, the above-mentioned (b) component and the above-mentioned (c) component is 100 mass%, the above-mentioned (c) component is 0.5 mass% or more and less than 5 mass%.
[0052] <Condition (ii)>
[0053] When the total of the above-mentioned component (a) and the above-mentioned component (b) is 100% by mass, when the above-mentioned component (a) is more than 30% by mass and 50% by mass or less, and the above-mentioned component (b) is less than 70% by mass and 50% by mass or more, when satisfying
[0054] MFRa < MFRb ··· (Formula 1)
[0055] the relationship, when the total of the above-mentioned component (a), the above-mentioned component (b) and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.5% by mass or more and 5% by mass or less; when satisfying
[0056] MFRa ≥ MFRb ··· (Formula 2)
[0057] the relationship, when the total of the above-mentioned component (a), the above-mentioned component (b) and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.9% by mass or more and 5% by mass or less.
[0058] <Condition (iii)>
[0059] When the total of the above-mentioned component (a) and the above-mentioned component (b) is 100% by mass, when the above-mentioned component (a) is more than 50% by mass and 70% by mass or less, and the above-mentioned component (b) is less than 50% by mass and 30% by mass or more, satisfying
[0060] MFRa < MFRb ··· (Formula 1)
[0061] the relationship, when the total of the above-mentioned component (a), the above-mentioned component (b) and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.9% by mass or more and 5% by mass or less.
[0062] <Condition (iv)>
[0063] When the total of the above-mentioned component (a) and the above-mentioned component (b) is 100% by mass, when the above-mentioned component (a) is more than 70% by mass and 81% by mass or less, and the above-mentioned component (b) is less than 30% by mass and 19% by mass or more, satisfying
[0064] MFRa < MFRb ··· (Formula 1)
[0065] the relationship, when the total of the above-mentioned component (a), the above-mentioned component (b) and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 3% by mass or more and 5% by mass or less. [6]
[0067] The antistatic resin composition as described in [4] above, wherein, in the melt flow rate (MFR) under the conditions of 200 °C and 5 kg load specified by ISO 1133, the relationship between the MFR of the vinyl aromatic hydrocarbon resin (a3) (hereinafter referred to as MFRa) and the MFR of the block copolymer (b) (hereinafter referred to as MFRb) satisfies the following condition (v) or (vi).
[0068] <Condition (v)>
[0069] When the total of the above (a3) component and the above (b) component is 100% by mass, the above (a3) component is more than 0% by mass and 20% by mass or less, and the above (b) component is 80% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the above (a3) component, the above (b) component and the above (c) component is 100% by mass, (c) is 0.5% by mass or more and 5% by mass or less.
[0070] <Condition (vi)>
[0071] When the total of the above (a3) component and the above (b) component is 100% by mass, the above (a3) component is more than 20% by mass and 50% by mass or less, and the above (b) component is less than 80% by mass and 50% by mass or more, satisfying
[0072] MFRa < MFRb ··· (Formula 1)
[0073] the relationship, when the total of the above (a3) component, the above (b) component and the above (c) component is 100% by mass, the above (c) component is 3% by mass or more and 5% by mass or less. [7]
[0075] The antistatic resin composition according to any one of [1] to [6] above, wherein the donor-acceptor type molecular compound (c) is represented by the following general formula (1).
[0076] [Chemical formula 1]
[0077]
[0078] (In formula (1), R1 and R2 are each independently CH3(CH2) n -CO-OCH2 (n is an integer from 12 to 22), or HOCH2, and at least one of them is CH3(CH2) n -CO-OCH3 (n is an integer from 12 to 22).
[0079] R3 and R4 are each independently any one selected from the group consisting of CH3, C2H5, HOCH2, HOC2H4, and HOCH2CH(CH3).
[0080] Here, "δ+" in the general formula (1) indicates the presence of polarity in the covalent bond within the molecule, (+) indicates that the oxygen atom has a strong electron-donating property, (-) indicates that the boron atom has a strong electron-withdrawing property, "→" indicates a path for electrons to be attracted, and "---" indicates a state in which the bonding force between atoms is weakened.) [8]
[0082] A method for producing an antistatic resin composition, which is the method for producing an antistatic resin composition according to any one of [1] to [7] above, comprising the following steps:
[0083] Step (I), using a block copolymer (b) and a donor-acceptor system molecular compound (c), when the total amount of the masterbatch is 100 mass%, melt-kneading with a composition ratio of the donor-acceptor system molecular compound (c) of 5 mass% to 20 mass%, thereby producing a masterbatch; and
[0084] In step (II), the masterbatch is diluted by kneading the masterbatch with the vinyl aromatic hydrocarbon resin (a) and / or the block copolymer (b). [9]
[0086] An electronic component packaging material, which is a molded product of the antistatic resin composition described in any one of [1] to [7].
[0087] Effects of the Invention
[0088] According to the present invention, an antistatic resin composition which exhibits excellent antistatic performance and excellent transparency even when combined with a styrene-based resin such as general-purpose polystyrene (GPPS), rubber-modified polystyrene (HIPS), or a methyl methacrylate / styrene copolymer resin (MS resin), a method for producing the antistatic resin composition, and an electronic component packaging material can be provided. DETAILED DESCRIPTION
[0089] A specific embodiment of the present invention (hereinafter referred to as “this embodiment”) will be described in detail below.
[0090] It should be noted that the following embodiments are examples for explaining the present invention and are not intended to limit the present invention to the following contents. The present invention can be implemented with various modifications within the scope of the gist.
[0091] [Antistatic resin composition]
[0092] (First antistatic resin composition)
[0093] The first antistatic resin composition of the present embodiment is an antistatic resin composition comprising a block copolymer (b) and a donor-acceptor system molecular compound (c).
[0094] The block copolymer (b) is a block copolymer containing vinyl aromatic hydrocarbon monomer units and conjugated diene monomer units, and has a polymer block mainly composed of vinyl aromatic hydrocarbon monomer units, wherein the vinyl aromatic hydrocarbon monomer units account for 30 to 90% by mass and the conjugated diene monomer units account for 70 to 10% by mass.
[0095] When the total amount of the block copolymer (b) and the donor-acceptor type molecular compound (c) is 100% by mass, the content of the donor-acceptor type molecular compound (c) is 0.5% by mass or more and 5% by mass or less.
[0096] By having the above-mentioned structure, even when combined with a styrene resin such as general-purpose polystyrene (GPPS), rubber-modified polystyrene (HIPS), or methyl methacrylate / styrene copolymer resin (MS resin), an antistatic resin composition having excellent antistatic performance and excellent transparency can be obtained.
[0097] The surface resistivity of the first antistatic resin composition of this embodiment is preferably 1×10 12 Ω / □ or less.
[0098] This can bring out excellent antistatic properties.
[0099] The surface resistivity of the first antistatic resin composition is preferably 5×10 11 Ω / □ or less, more preferably 5×10 10 Ω / □ or less.
[0100] The surface resistivity of the antistatic resin composition can be measured by the method described in Examples below.
[0101] The surface resistivity of the first antistatic resin composition can be controlled within the above numerical range by blending an appropriate amount of the donor-acceptor system molecular compound (c) in addition to optimizing the polymer structure of the block copolymer (b).
[0102] There is no lower limit to the surface resistivity, and the lower the value, the better the performance. However, since the reduction of surface resistivity is proportional to the cost, it is actually preferred to increase the surface resistivity to 1×10 8 Ω / □~1×10 9 Ω / □ is designed as the lower limit.
[0103] (Second antistatic resin composition)
[0104] The second antistatic resin composition of this embodiment comprises
[0105] Vinyl aromatic hydrocarbon resin (a),
[0106] block copolymer (b), and
[0107] An antistatic resin composition containing a donor-acceptor system molecular compound (c).
[0108] The block copolymer (b) is a block copolymer containing vinyl aromatic hydrocarbon monomer units and conjugated diene monomer units, and has a polymer block mainly composed of vinyl aromatic hydrocarbon monomer units, wherein the vinyl aromatic hydrocarbon monomer units account for 30 to 90% by mass and the conjugated diene monomer units account for 70 to 10% by mass.
[0109] When the total amount of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100 mass %, the mass ratio of the vinyl aromatic hydrocarbon resin (a) is 81 mass % or less, and the mass ratio of the block copolymer (b) is 19 mass % or more and less than 100 mass %.
[0110] In addition, when the total amount of the above-mentioned vinyl aromatic hydrocarbon resin (a), the above-mentioned block copolymer (b) and the above-mentioned donor-acceptor system molecular compound (c) is 100 mass%, the content of the above-mentioned donor-acceptor system molecular compound is greater than 0.5 mass% and less than 5 mass%.
[0111] In addition, the surface resistivity of the second antistatic resin composition is 1×10 12 Ω / □ or less.
[0112] By having the above-mentioned configuration, it is possible to obtain an antistatic resin composition as various styrene resin compositions which exhibits excellent antistatic performance and also has excellent transparency.
[0113] The surface resistivity of the second antistatic resin composition of this embodiment is 1×10 12 Ω / □ or less.
[0114] This can bring out excellent antistatic properties.
[0115] The surface resistivity of the second antistatic resin composition is more preferably 5×10 11 Ω / □ or less, more preferably 5×10 10 Ω / □ or less.
[0116] The surface resistivity of the antistatic resin composition can be measured by the method described in Examples below.
[0117] By appropriately blending the donor-acceptor molecular compound (c) in addition to optimizing the composition ratio and polymer structure of the above-mentioned block copolymer (b), the surface resistivity of the second antistatic resin composition can be controlled within the above numerical range.
[0118] The preferred mode of the above-mentioned second antistatic resin composition is as follows.
[0119] In the above-mentioned second antistatic resin composition, in the melt flow rate (MFR) under the conditions of 200 °C and 5 kg load specified by ISO1133, the relationship between the MFR of the above-mentioned vinyl aromatic hydrocarbon resin (a) (hereinafter referred to as MFRa) and the MFR of the block copolymer (b) (hereinafter referred to as MFRb) preferably satisfies any one of the following (i) to (iv).
[0120] <Condition (i)>
[0121] When the total of the above-mentioned vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100% by mass, when the component (a) is more than 0% by mass and 30% by mass or less, and the component (b) is 70% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the component (a), the component (b), and the component (c) is 100% by mass, the above-mentioned donor-acceptor molecular compound (c) is 0.5% by mass or more and 5% by mass or less.
[0122] By satisfying the above condition (i), an antistatic resin composition having excellent antistatic performance and excellent transparency can be obtained. In addition, since the composition ratio of the block copolymer (b) is high, an effect of being rich in flexibility and having excellent impact strength can be obtained.
[0123] In condition (i), the content of the above-mentioned donor-acceptor molecular compound (c) is preferably 1 to 5% by mass, more preferably 2 to 4% by mass.
[0124] <Condition (ii)>
[0125] When the total of the above-mentioned vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100% by mass, when the component (a) is more than 30% by mass and 50% by mass or less, and the component (b) is less than 70% by mass and 50% by mass or more, when satisfying
[0126] MFRa < MFRb ··· (Formula 1)
[0127] the relationship, when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 0.5% by mass or more and 5% by mass or less; when satisfying
[0128] MFRa ≧ MFRb ··· (Formula 2)
[0129] When in the relationship of, when the total of the above-mentioned component (a), the above-mentioned component (b), and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.9% by mass or more and 5% by mass or less.
[0130] By satisfying the above condition (ii), an antistatic resin composition showing excellent antistatic performance and also excellent transparency can be obtained. And an effect of further improving the rigidity of the resin composition derived from the vinyl aromatic hydrocarbon resin (a) can be obtained.
[0131] In condition (ii), regarding the content of the above-mentioned donor-acceptor system molecular compound (c), when satisfying the above (Formula 1), it is preferably 1 to 5% by mass, more preferably 2 to 4% by mass.
[0132] In addition, when satisfying the above (Formula 2), the content is preferably 2 to 5% by mass, more preferably 2 to 4% by mass.
[0133] <Condition (iii)>
[0134] When the total of the above-mentioned vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100% by mass, when the above-mentioned component (a) is more than 50% by mass and 70% by mass or less, and the above-mentioned component (b) is less than 50% by mass and 30% by mass or more, satisfy
[0135] MFRa < MFRb ··· (Formula 1)
[0136] the relationship, and when the total of the above-mentioned component (a), the above-mentioned component (b), and the above-mentioned component (c) is 100% by mass, the above-mentioned donor-acceptor system molecular compound (c) is 0.9% by mass or more and 5% by mass or less.
[0137] By satisfying the above condition (iii), an antistatic resin composition showing excellent antistatic performance and also excellent transparency can be obtained. And an effect of further improving the rigidity of the resin composition derived from the vinyl aromatic hydrocarbon resin (a) can be obtained.
[0138] In condition (iii), the content of the above-mentioned donor-acceptor system molecular compound (c) is preferably 2 to 5% by mass, more preferably 3 to 5% by mass.
[0139] <Condition (iv)>
[0140] When the total of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100% by mass, when the component (a) is more than 70% by mass and 81% by mass or less, and the component (b) is less than 30% by mass and 19% by mass or more, the following is satisfied
[0141] MFRa < MFRb ··· (Equation 1)
[0142] Regarding the relationship, when the total of the component (a), the component (b), and the component (c) is 100% by mass, the content of the donor-acceptor molecular compound (c) is 3% by mass or more and 5% by mass or less.
[0143] By satisfying the above condition (iv), an antistatic resin composition that exhibits excellent antistatic properties and also excellent transparency can be obtained. In addition, an effect of increasing the rigidity to a value close to the original rigidity of the vinyl aromatic hydrocarbon resin (a) can be obtained.
[0144] In condition (iv), the content of the donor-acceptor molecular compound (c) is preferably 3.5 to 5% by mass, more preferably 4 to 5% by mass.
[0145] In this specification, the naming of each monomer unit constituting the polymer follows the naming of the monomer from which the monomer unit is derived. For example, a "vinyl aromatic hydrocarbon monomer unit" refers to a structural unit of a polymer produced by polymerizing a vinyl aromatic hydrocarbon monomer as a monomer, and its structure is a molecular structure in which two carbons of a substituted ethylidene derived from a substituted vinyl form the polymer main chain.
[0146] In addition, a "conjugated diene monomer unit" refers to a structural unit of a polymer produced by polymerizing a conjugated diene as a monomer, and its structure is a molecular structure in which two carbons of an olefin of the conjugated diene monomer form the polymer main chain.
[0147] It should be noted that in this specification, "being the main component" means that the content of a specific monomer unit is 90% by mass or more.
[0148] For example, in the block copolymer (b), a "polymer block mainly composed of vinyl aromatic hydrocarbon monomer units" refers to a block in which the vinyl aromatic hydrocarbon monomer units are 90% by mass or more.
[0149] A polymer block in which the vinyl aromatic hydrocarbon monomer units are less than 90% by mass and the conjugated diene monomer units are more than 10% by mass is defined as a random copolymer block.
[0150] The random copolymer block can have a completely random structure or a gradient structure (the copolymer composition ratio changes stepwise along the chain).
[0151] (Mass ratio of block copolymer (b) and donor-acceptor system molecular compound (c))
[0152] The first antistatic resin composition of the present embodiment includes a block copolymer (b) of a vinyl aromatic hydrocarbon monomer unit and a conjugated diene monomer unit and a donor-acceptor system molecular compound (c).
[0153] In the block copolymer (b), the vinyl aromatic hydrocarbon monomer unit accounts for 30 to 90% by mass, and the conjugated diene monomer unit accounts for 70 to 10% by mass.
[0154] When the total of the block copolymer (b) and the donor-acceptor type molecular compound (c) is 100% by mass, the content of the donor-acceptor type molecular compound (c) is 0.5% by mass or more and 5% by mass or less.
[0155] (Mass ratio of vinyl aromatic hydrocarbon resin (a), block copolymer (b), and donor-acceptor molecular compound (c))
[0156] In the second antistatic resin composition of the present embodiment, the mass ratio of the vinyl aromatic hydrocarbon resin (a) to the block copolymer (b) is vinyl aromatic hydrocarbon resin (a) / block copolymer (b)=amount greater than 0 / less than 100 to 81 / 19 or more.
[0157] Within the above-mentioned mass ratio, the minimum required amount of the donor-acceptor system molecular compound (c) that exhibits the performance is determined according to the size of each MFR value (MFRa and MFRb) in accordance with the change in the mass ratio of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b).
[0158] Based on the conditions of the respective MFR values of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) corresponding to the mass ratio, the ratio of the vinyl aromatic hydrocarbon resin (a) / block copolymer (b) and / or the content of the donor-acceptor system molecular compound (c) are set in a manner that can exhibit sufficient antistatic performance.
[0159] In the antistatic resin composition of the present embodiment, the mass ratio of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) for achieving excellent antistatic performance, i.e., the relative comparison value of MFR, is closely related to the minimum necessary compounding amount of the donor-acceptor system molecular compound (c) that leads to the exhibiting of antistatic performance.
[0160] For example, when block copolymer (b) is not used, even if about 4% by mass of donor-acceptor system molecular compound (c) is mixed with vinyl aromatic hydrocarbon resin (a), antistatic performance is not exhibited. In order to exhibit antistatic performance, when the total amount of vinyl aromatic hydrocarbon resin (a) and block copolymer (b) is 100 parts by mass, a composition in which the content of block copolymer (b) is at least 19% by mass is required.
[0161] In addition, when the total amount of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100 mass%, if the block copolymer (b) is 70 mass% or more, the minimum mixing amount of the donor-acceptor system molecular compound (c) that leads to the exhibiting antistatic performance is 0.5 mass%. In addition, since it does not depend on the MFR value of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b), the composition range in which the performance is exhibited is significantly expanded.
[0162] For example, in the case of not using the vinyl aromatic hydrocarbon resin (a), antistatic performance can be exhibited by mixing 0.5% by mass of the donor-acceptor system molecular compound (c) with 99.5% by mass of the block copolymer (b). That is, in order to exhibit antistatic performance, the block copolymer (b) must be present in a certain proportion or more in the vinyl aromatic hydrocarbon resin, and it is believed that there is a certain interaction that leads to the exhibiting of antistatic performance.
[0163] The vinyl aromatic hydrocarbon resin (a), the block copolymer (b), and the donor-acceptor system molecular compound (c), which are the constituent components of the antistatic resin composition of the present embodiment, are described in detail below.
[0164] (Vinyl aromatic hydrocarbon resin (a))
[0165] The vinyl aromatic hydrocarbon resin (a) is preferably any one selected from the group consisting of the following substances: a homopolymer (a1) of a vinyl aromatic hydrocarbon monomer represented by general-purpose polystyrene (GPPS); a graft copolymer (a2) obtained by dissolving a synthetic rubber such as polybutadiene or styrene-butadiene rubber in a styrene monomer and graft-polymerizing the mixture under stirring, represented by rubber-modified polystyrene (HIPS); and a random copolymer (a3) of a vinyl aromatic hydrocarbon monomer unit and a (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer unit, represented by an MS resin.
[0166] Since (a3) has a different polarity from (a1) and (a2), the dispersion form after mixing with the block copolymer (b) is different, and therefore the composition range in which the antistatic performance is exhibited in the antistatic resin composition is different.
[0167] In the above-mentioned second antistatic resin composition, in the melt flow rate (MFR) under the conditions of 200 °C and 5 kg load specified by ISO1133, the relationship between the MFR of the above vinyl aromatic hydrocarbon resin (a3) (hereinafter referred to as MFRa) and the MFR of the block copolymer (b) (hereinafter referred to as MFRb) preferably satisfies the following condition (v) or (vi).
[0168] <Condition (v)>
[0169] When the total of the above vinyl aromatic hydrocarbon resin (a3) and the block copolymer (b) is 100% by mass, when the (a3) component is more than 0% by mass and 20% by mass or less, and the (b) component is 80% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the (a3) component, the (b) component, and the (c) component is 100% by mass, the content of the donor-acceptor molecular compound (c) is 0.5% by mass or more and 5% by mass or less.
[0170] By satisfying the above condition (v), an antistatic resin composition exhibiting excellent antistatic performance and excellent transparency can be obtained. Also, compared with the composition using (a1) or (a2), a resin composition with a low haze value and excellent transparency can be obtained.
[0171] In condition (v), the content of the donor-acceptor molecular compound (c) is preferably 1 to 5% by mass, more preferably 2 to 4% by mass.
[0172] <Condition (vi)>
[0173] When the total of the above vinyl aromatic hydrocarbon resin (a3) and the block copolymer (b) is 100% by mass, when the (a3) component is more than 20% by mass and 50% by mass or less, and the (b) component is less than 80% by mass and 50% by mass or more, it satisfies
[0174] MFRa < MFRb ··· (Formula 1)
[0175] the relationship, and when the total of the (a3) component, the (b) component, and the (c) component is 100% by mass, the (c) component is 3% by mass or more and 5% by mass or less.
[0176] By satisfying the above condition (vi), an antistatic resin composition exhibiting excellent antistatic performance and excellent transparency can be obtained. In addition, compared with the composition using (a1) or (a2), a resin composition with a low haze value and excellent transparency can be obtained.
[0177] In the condition (vi), the content of the donor-acceptor system molecular compound (c) is preferably 3.5 to 5% by mass, more preferably 4 to 5% by mass.
[0178] In the MS resin (a3), the copolymerization ratio of the vinyl aromatic hydrocarbon monomer unit (S) and the (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer unit (M) is preferably S / M = 83 / 17 to 60 / 40 (mass %), more preferably S / M = 82 / 18 to 68 / 32 (mass %), and further preferably S / M = 82 / 18 to 78 / 22 (mass %).
[0179] By using the MS resin of this composition ratio, an antistatic resin composition can be obtained which has a refractive index similar to that of the block copolymer (b), is uniformly dispersed on the micrometer scale although the dispersion form is not completely compatible, and has excellent transparency and mechanical properties.
[0180] On the other hand, when the content of the vinyl aromatic hydrocarbon monomer unit of component (a3) is less than 60% by mass, the deviation of the refractive index from the block copolymer (b) increases, the antistatic resin composition tends to become turbid, and the deviation of polarity also increases, so the compatibility also deteriorates, and the mechanical properties of the antistatic resin composition are significantly reduced, which is not preferred.
[0181] The MS resin (a3) may contain other copolymerizable monomer units as required, as long as the antistatic performance is not impaired.
[0182] The vinyl aromatic hydrocarbon monomer constituting the vinyl aromatic hydrocarbon resin (a) is not particularly limited as long as it has an aromatic ring and a vinyl group in the molecule, and examples thereof include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, p-ethylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, 1,3-dimethylstyrene, α-methylstyrene, α-methyl-p-methylstyrene, vinylnaphthalene, vinylanthracene, 1,1-diphenylethylene, and the like.
[0183] These vinyl aromatic hydrocarbon monomers may be used alone or in combination of two or more.
[0184] Among these, styrene is preferred from the viewpoint of ease of industrial availability and economic efficiency.
[0185] In the above-mentioned vinyl aromatic hydrocarbon resin, in particular, the (meth)acrylic acid and / or (meth)acrylic acid ester monomer constituting the random copolymer (a3) of the vinyl aromatic hydrocarbon monomer unit and the (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer unit means one or more monomers selected from the group consisting of acrylic acid, methacrylic acid, alkyl acrylates and alkyl methacrylates.
[0186] The alkyl ester may be one or more ester compounds of an alkyl alcohol having 1 to 8 carbon atoms (C1 to C8) and acrylic acid and / or methacrylic acid.
[0187] Examples of the (meth)acrylic acid and / or (meth)acrylic acid ester monomer include, but are not limited to, acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate (butyl acrylate), n-pentyl acrylate, n-hexyl acrylate and other C1-6 alkyl acrylates, cycloalkyl acrylates such as cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate and other C1-6 alkyl methacrylates, and cyclohexyl methacrylates such as cyclohexyl methacrylate. Among these, C1-6 alkyl acrylates and C1-6 alkyl methacrylates are preferred, and C1-4 alkyl acrylates and C1-4 alkyl methacrylates are more preferred, and methyl acrylate and / or methyl methacrylate are further preferred, and methyl methacrylate is still more preferred, as they can further increase the softening temperature of the vinyl aromatic hydrocarbon resin (a) and, as a result, can further improve the moldability and heat deformation resistance of the obtained molded article.
[0188] In the present specification, the "random copolymer of vinyl aromatic hydrocarbon monomer units and (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer units" (a3) also includes a polymer containing a small amount of other monomer units other than the vinyl aromatic hydrocarbon monomer units and (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer units that are polymerizable with these monomer units.
[0189] The amount of other monomer units in the vinyl aromatic hydrocarbon resin (a) is preferably 2% by mass or less.
[0190] When "a random copolymer of a vinyl aromatic hydrocarbon monomer unit and methyl methacrylate" is exemplified as a particularly preferred copolymer, an embodiment containing 2% by mass or less of other monomer units is also included.
[0191] The vinyl aromatic hydrocarbon resin (a) can be produced by a known polymerization method.
[0192] Examples of known polymerization methods include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization.
[0193] When the vinyl aromatic hydrocarbon resin (a) is a homopolymer (a1) of a vinyl aromatic hydrocarbon monomer represented by GPPS, for example, if styrene monomer is taken as an example, free radical polymerization can be carried out in the coexistence of ethylbenzene, in the presence of an organic peroxide, or only under the action of heat without using an organic peroxide, and the solvent ethylbenzene and unreacted styrene monomer can be removed to obtain a styrene homopolymer (GPPS).
[0194] In addition, when the vinyl aromatic hydrocarbon resin (a) is a graft copolymer (a2) of a rubber-modified polystyrene represented by HIPS, for example, polybutadiene can be dissolved in a mixed solution of ethylbenzene and styrene monomers, free radical polymerization can be carried out while stirring at an appropriate temperature in the presence of an organic peroxide, and the solvent ethylbenzene and unreacted styrene monomers can be removed to obtain a rubber-modified polystyrene (HIPS).
[0195] The size of the grafted rubber particles, the embedding shape or the density thereof can be controlled by the molecular weight (Mooney viscosity or solution viscosity) of polybutadiene, by using styrene-butadiene rubber instead of polybutadiene, or by controlling the stirring speed.
[0196] In addition, when the vinyl aromatic hydrocarbon resin (a) is a random copolymer (a3) containing (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer units represented by MS resin, it is generally industrially carried out by a production method based on free radical polymerization in the coexistence of a vinyl aromatic hydrocarbon monomer and (meth)acrylic acid and / or (meth)acrylic acid ester in the same manner as in the above example.
[0197] The MFR of the vinyl aromatic hydrocarbon resin (a) varies according to factors such as the degree of polymerization and grafting rate of the monomer unit, and in addition to these factors, it also significantly changes by adding additives such as mineral oil. The MFR of the vinyl aromatic hydrocarbon resin (a) affects the dispersion state of the above-mentioned components (a) and (b), which is an important factor for the antistatic resin composition of the present embodiment to exhibit antistatic performance.
[0198] The above conditions (i) to (vi) define the MFR value of the component (a) in a state containing additives such as mineral oil, and the MFR value directly affects the performance of the antistatic resin composition of the present embodiment.
[0199] In the method for producing the vinyl aromatic hydrocarbon resin (a), a polymerization solvent such as ethylbenzene, a radical initiator such as an organic peroxide, and a chain transfer agent such as an aliphatic mercaptan can be used appropriately. Specific examples are described below.
[0200] The polymerization solvent is used to maintain low viscosity in the reaction system during the continuous polymerization process. Examples of the organic solvent include, but are not limited to, alkylbenzenes such as benzene, toluene, ethylbenzene and xylene, ketones such as acetone and methyl ethyl ketone, and aliphatic hydrocarbons such as hexane and cyclohexane.
[0201] In particular, when a polyfunctional vinyl aromatic hydrocarbon monomer or the like is used as a polymerization monomer, it is preferred to use a polymerization solvent from the viewpoint of suppressing gelation.
[0202] By using a polymerization solvent, gel is less likely to be generated, and the polymerization process can be more finely controlled, so that a vinyl aromatic hydrocarbon resin (a) having a desired composition and physical properties can be obtained more easily.
[0203] The amount of the polymerization solvent used is not particularly limited, but is usually preferably within a range of 1 to 50% by mass, more preferably 5 to 25% by mass, based on the entire composition in the polymerization reactor from the viewpoint of controlling gelation.
[0204] By using 1 to 50% by mass of the polymerization solvent, gelation can be suppressed and the polymerization process can be highly controlled, thereby obtaining a vinyl aromatic hydrocarbon resin (a) excellent in industrial productivity and economic efficiency.
[0205] In the polymerization step of the vinyl aromatic hydrocarbon resin (a), a radical initiator such as an organic peroxide can be preferably used.
[0206] As free radical initiators, there can be mentioned, but are not limited to, peroxyketals such as 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(tert-butylperoxy)butane, 2,2-di(4,4-di-tert-butylperoxycyclohexyl)propane, and 1,1-di(tert-amylperoxy)cyclohexane; hydroperoxides such as cumene hydroperoxide and tert-butyl hydroperoxide; alkyl peroxides such as tert-butyl peroxyacetate and tert-amyl peroxyisononanoate; tert-butyl cumyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, and the like. Oxides, dialkyl peroxides such as di-tert-hexyl peroxide; peroxyesters such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate, and tert-butyl peroxyisopropyl monocarbonate; peroxycarbonates such as tert-butyl peroxyisopropyl carbonate and polyether tetrakis (tert-butyl peroxycarbonate); N,N'-azobis(cyclohexane-1-carbonitrile), N,N'-azobis(2-methylbutyronitrile), N,N'-azobis(2,4-dimethylvaleronitrile), N,N'-azobis[2-(hydroxymethyl)propionitrile], etc.
[0207] These radical initiators may be used alone or in combination of two or more.
[0208] Furthermore, in the polymerization step of the vinyl aromatic hydrocarbon resin (a), a chain transfer agent may be used for the purpose of adjusting the molecular weight of the vinyl aromatic hydrocarbon resin (a).
[0209] Examples of the chain transfer agent include, but are not limited to, aliphatic mercaptans, aromatic mercaptans, pentaphenylethane, α-methylstyrene dimer, terpinolene, and the like.
[0210] The molecular weight of the vinyl aromatic hydrocarbon resin (a) can be controlled by adjusting the monomer concentration, the amount of a radical initiator such as an organic peroxide, the presence or absence and amount of a chain transfer agent, and the like.
[0211] Generally, if the amount of free radical generation is reduced and a chain transfer agent is not used, the molecular weight will be increased; if the amount of free radical generation is increased, a chain transfer agent is added or the amount of the chain transfer agent is increased, the molecular weight will be decreased.
[0212] As the vinyl aromatic hydrocarbon resin (a), commercial products can be used. For example, GPPS and HIPS can be cited as "PSJ-Polystyrene" manufactured by PS Japan. GPPS is transparent and HIPS is milky white. Either brand can be used appropriately, but it should be noted that the performance tendency varies depending on the MFR.
[0213] In addition, among the MS resins, preferred brands include "PSJ-Polystyrene SC004" and "PSJ-Polystyrene MM290" manufactured by PS Japan Co., Ltd. and "TOYO MS MS200", "TOYO MS MS300" and "TOYO MS KS10" manufactured by TOYO Styrene Co., Ltd.
[0214] These substances have a refractive index similar to that of the block copolymer (b), and are easy to obtain a transparent composition. Although the dispersion form is not completely compatible, they are uniformly dispersed at the micron level and can obtain an antistatic resin composition with excellent transparency and mechanical properties. Therefore, they can be preferably used.
[0215] (Block copolymer (b))
[0216] The block copolymer (b) is a block copolymer comprising vinyl aromatic hydrocarbon monomer units and conjugated diene monomer units, wherein the vinyl aromatic hydrocarbon monomer units account for 30 to 90% by mass, the conjugated diene monomer units account for 70 to 10% by mass, and the block copolymer has at least one polymer block mainly composed of the vinyl aromatic hydrocarbon monomer units.
[0217] The polymer block mainly composed of vinyl aromatic hydrocarbon monomer units constituting the block copolymer (b) refers to a polymer block in which the vinyl aromatic hydrocarbon monomer units account for 90% by mass or more.
[0218] In addition, the conjugated diene monomer units constituting the block copolymer (b) may contain, in addition to the conjugated diene polymer blocks formed by the conjugated diene monomer units alone, copolymer blocks of conjugated diene monomer units and vinyl aromatic hydrocarbon monomer units. In the case of copolymer blocks, various copolymer block structures may be provided, such as a uniform random structure and a tapered structure (the composition ratio of the monomers changes along the chain).
[0219] In the block copolymer (b), two or more block copolymers having different average molecular weights may be combined, or two or more block copolymers having different copolymerization ratios of the vinyl aromatic hydrocarbon monomer unit and the conjugated diene monomer unit may be combined.
[0220] Furthermore, the block copolymer (b) may contain other polymerizable monomer units other than the vinyl aromatic hydrocarbon monomer unit and the conjugated diene monomer unit, as required.
[0221] The vinyl aromatic hydrocarbon monomer only needs to have an aromatic ring and a vinyl group in the molecule, and examples thereof include, but are not limited to, styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, p-ethylstyrene, p-tert-butylstyrene, 2,4-dimethylstyrene, 1,3-dimethylstyrene, α-methylstyrene, α-methyl-p-methylstyrene, vinylnaphthalene, vinylanthracene, and 1,1-diphenylethylene.
[0222] These vinyl aromatic hydrocarbon monomers may be used alone or in combination of two or more.
[0223] Among these, styrene is preferred from the viewpoint of industrial and economic efficiency.
[0224] The conjugated diene monomer may be any diene having a pair of conjugated double bonds, and examples thereof include, but are not limited to, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene.
[0225] These conjugated diene monomers are used alone or in combination of two or more.
[0226] Among these, 1,3-butadiene and isoprene are preferred from the viewpoint of industrial availability and economic efficiency, and 1,3-butadiene is more preferred from the viewpoint of further improving industrial availability and economic efficiency.
[0227] The mass ratio of the vinyl aromatic hydrocarbon monomer unit to the conjugated diene monomer unit in the block copolymer (b) is vinyl aromatic hydrocarbon monomer unit / conjugated diene monomer unit=30 / 70 to 90 / 10.
[0228] When the ratio of each monomer unit is within the above range, good antistatic properties can be expressed in the antistatic resin composition of the present embodiment in combination with the donor-acceptor system molecular compound (c) described later.
[0229] In the block copolymer (b), as described above, the mass % ratio of the vinyl aromatic hydrocarbon monomer unit / the conjugated diene monomer unit is in the range of 30 / 70 to 90 / 10.
[0230] When the proportion of the vinyl aromatic hydrocarbon monomer units constituting the block copolymer (b) is less than 30% by mass, the elastic modulus of the monomer is very low. Therefore, in order to use the antistatic resin composition using the block copolymer (b) as an electronic component packaging material, it is necessary to prepare a composition mainly composed of the vinyl aromatic hydrocarbon resin as component (a). However, since the proportion of the vinyl aromatic hydrocarbon monomer units in the block copolymer (b) itself is low, the compatibility with the vinyl aromatic hydrocarbon resin as component (a) deteriorates, and under this influence, the dispersibility of the donor-acceptor system molecular compound (c) also tends to deteriorate.
[0231] In the block copolymer (b), when the content of the vinyl aromatic hydrocarbon monomer unit is 30% by mass or more, an antistatic resin composition can be obtained which can ensure a practically sufficient elastic modulus, has good compatibility with the component (a), and has good dispersibility in the component (c) described later.
[0232] On the other hand, when the proportion of the vinyl aromatic hydrocarbon monomer units constituting the block copolymer (b) is greater than 90% by mass, even if the block copolymer (b) is 100% by mass as the base resin of the antistatic resin composition, the vinyl aromatic hydrocarbon resin (a) is blended in an arbitrary proportion, or 4% by mass of the donor-acceptor system molecular compound (c) is mixed, there is still a tendency that the surface resistivity is not easily reduced.
[0233] The contents of the vinyl aromatic hydrocarbon monomer unit and the conjugated diene monomer unit in the block copolymer (b) can be quantitatively determined by the method described in the examples below.
[0234] The content of these monomer units can be controlled by adjusting the amount and ratio of each monomer added in the polymerization step of the block copolymer (b).
[0235] The block copolymer (b) is not particularly limited, and examples thereof include block copolymers having block structures represented by the following general formulae (1) to (7).
[0236] S1-B1-S2···(1)
[0237] S1-B / S1-S2···(2)
[0238] S1-B1-S2-B2···(3)
[0239] S1-B / S1-S2-B / S2···(4)
[0240] S1-B / S1-B / S2-S2···(5)
[0241] S1-B1-B / S1-S2···(6)
[0242] S1-B1-S2-B2-S3···(7)
[0243] In the above general formulas (1) to (7), S1, S2 and S3 respectively represent polymer blocks mainly composed of vinyl aromatic hydrocarbon monomer units, B1 and B2 respectively represent polymer blocks (B) mainly composed of conjugated diene monomer units, and B / S1 and B / S2 represent random copolymer blocks (B / S) in which the contents of vinyl aromatic hydrocarbon monomer units and conjugated diene copolymer units are less than 90% by weight, respectively.
[0244] It should be noted that the numbers of S, B, and B / S in the above general formulas (1) to (7) are numbers for identifying polymer block (S), polymer block (B), and random copolymer block (B / S), respectively. When the numbers are different, the molecular weight (polymerization degree) or copolymerization ratio of each block may be the same or different. In addition, the chain structure of the random copolymer block (B / S) may be a uniform random block or a tapered block (the composition ratio changes slowly along the chain).
[0245] In addition, the block copolymer (b) may be any of a linear polymer and a branched polymer.
[0246] Examples of methods for obtaining a branched polymer include a method of subjecting a polymerization terminal to a coupling reaction and a method of causing branching from the initial stage of polymerization using a polyfunctional initiator.
[0247] In addition, as a suitable use of the antistatic resin composition of this embodiment, electronic component packaging materials can be cited. In view of this use, from the perspective of various required mechanical properties, the block copolymer (b) has at least one polymer block S mainly composed of vinyl aromatic hydrocarbon monomer units, and preferably has at least two polymer blocks S.
[0248] In addition, in this specification, a "polymer block mainly composed of a vinyl aromatic hydrocarbon monomer unit" may be described as a "polymer block S".
[0249] <Peak Molecular Weight and Molecular Weight Distribution of Block Copolymer (b)>
[0250] Regarding the antistatic resin composition of the present embodiment, in the molecular weight distribution curve measured by gel permeation chromatography (GPC), preferably there is at least one peak molecular weight from the block copolymer (b) in the range of molecular weight from 30,000 to 300,000. Thus, the balance between the mechanical properties and molding processability of the antistatic resin composition of the present invention is better.
[0251] From the same viewpoint, the peak molecular weight derived from the block copolymer (b) is more preferably in the range of 40,000 to 250,000, and further preferably in the range of 50,000 to 210,000.
[0252] In addition, the peak molecular weight of the block copolymer (b) can be measured by the method described in Examples below.
[0253] <Molecular Weight Distribution (Mw / Mn) of Block Copolymer (b)>
[0254] The molecular weight distribution (Mw / Mn) of the block copolymer (b) is not particularly limited. By associating the polymerization active ends of some polymers using a coupling agent described later, different molecular weight combinations can be obtained, thereby obtaining a block copolymer (b) with a large molecular weight distribution (Mw / Mn).
[0255] In addition, by adding an appropriate amount of alcohol such as ethanol during the polymerization, the polymerization of part of the polymer can be stopped, thereby obtaining a block copolymer (b) as a mixture of different molecular weights. For example, by adding an alcohol such as ethanol in a molar equivalent amount less than the molar number of the polymerization initiator in the polymerization system to the polymerization system, the polymerization of the polymer can be partially stopped, thereby obtaining a block copolymer (b) having a large molecular weight distribution (Mw / Mn) with multiple peak molecular weights.
[0256] <Number Average Molecular Weight (Mn) of Polymer Block S>
[0257] The number average molecular weight (Mn) of the polymer block S mainly composed of vinyl aromatic hydrocarbon monomer units in the block copolymer (b) is preferably 10,000 to 60,000, more preferably 15,000 to 50,000, and even more preferably 20,000 to 40,000.
[0258] When the number average molecular weight (Mn) of the polymer block S is within the above range, a molded product (for example, a styrene-based resin sheet) having better mechanical properties and a good molded appearance in a well-balanced manner can be obtained.
[0259] The number average molecular weight (Mn) of the polymer block S in the block copolymer (b) can be controlled by adjusting the supply amount (charge amount) of the vinyl aromatic hydrocarbon monomer relative to the polymerization initiator.
[0260] The block copolymer (b) comprises at least one polymer block S mainly composed of a vinyl aromatic hydrocarbon monomer unit. Preferably, two or more polymer blocks S are included, and more preferably, at least one polymer block S is present at the end of the polymer chain. Regarding the molecular weight of the polymer block S, even when the block copolymer (b) comprises two or more polymer blocks S, the structure can be controlled independently.
[0261] It should be noted that the number average molecular weight (Mn) of the above polymer block S is expressed as the number average molecular weight of all polymer blocks S in the block copolymer (b) combined. For example, in the case of a block copolymer (b) having a S1-B / S1-S2 structure, the number average molecular weight of the polymer block S is the number average molecular weight of S1 and S2 combined.
[0262] The number average molecular weight of the polymer block S in the block copolymer (b) can be obtained by measuring the polymer block S component (but excluding the vinyl aromatic hydrocarbon monomer polymer component having an average degree of polymerization of about 30 or less) by using gel permeation chromatography (GPC) using a method (IMKOLTHOFF, et al., J. Polym. Sci. 1, 429 (1946)) in which the block copolymer is subjected to oxidative decomposition using osmium tetroxide as a catalyst by tert-butyl hydroperoxide. Specifically, the number average molecular weight can be obtained by the method described in the Examples.
[0263] <Molecular Weight Distribution (Mw / Mn) of Polymer Block S>
[0264] The molecular weight distribution (Mw / Mn) of the polymer block S mainly composed of vinyl aromatic hydrocarbon monomer units in the block copolymer (b) is preferably 1.5 to 4.0, more preferably 1.6 to 3.6, and even more preferably 1.7 to 3.2.
[0265] By making the molecular weight distribution (Mw / Mn) of the polymer block S within the above range, the molding processability of the antistatic resin composition of this embodiment and the balance of the dispersibility of the block copolymer (b) and the vinyl aromatic hydrocarbon resin (a) become better, and a molded product with good molding appearance and not prone to poor molding appearance such as material flow pattern during molding is obtained.
[0266] The molecular weight distribution (Mw / Mn) of the polymer block S in the block copolymer (b) is the overall average molecular weight distribution of all the polymer blocks S in the block copolymer (b). For example, in the case of a block copolymer (b) having a structure of S1-B / S1-S2, the average molecular weight of the polymer block S is the average molecular weight distribution of S1 and S2. The supply amount (feed amount) of the vinyl aromatic hydrocarbon monomer relative to the polymerization initiator is adjusted by making the chain lengths of the two or more polymer blocks S close or far away, thereby controlling.
[0267] As another method for controlling the molecular weight distribution (Mw / Mn) of the polymer block S in the block copolymer (b), for example, a method of stopping the polymerization of part of the polymer by adding an alcohol such as ethanol in a molar amount less than the polymerization initiator in the polymerization process of the polymer block S. Thus, the polymer block S becomes a mixture of two different molecular weights. The block copolymer (b) prepared in this way having two or more different chain length distributions of the polymer block S can also control the molecular weight distribution of the polymer block S.
[0268] The molecular weight distribution (Mw / Mn) of the polymer block S in the block copolymer (b) can be specifically determined by the method described in Examples below.
[0269] <Method for producing block copolymer (b)>
[0270] The manufacture method of the block copolymer (b) constituting the antistatic resin composition of the present embodiment can utilize known technology.If representative prior art is illustrated, then anionic polymerization initiators such as organic lithium compounds can be cited in hydrocarbon solvents, and a method for block copolymerization of conjugated diene monomers and vinyl aromatic hydrocarbon monomers can be carried out.For example, it can be manufactured by the method described in Japanese Patent Publication No. 36-19286, Japanese Patent Publication No. 43-17979, Japanese Patent Publication No. 48-2423, Japanese Patent Publication No. 49-36957, Japanese Patent Publication No. 57-49567, and Japanese Patent Publication No. 58-11446.
[0271] The block copolymer (b) is obtained by copolymerizing a vinyl aromatic hydrocarbon monomer and a conjugated diene monomer in a hydrocarbon solvent.
[0272] As the hydrocarbon solvent used in the production of the block copolymer (b), any known hydrocarbon solvent can be used, including, but not limited to, aliphatic hydrocarbons such as n-butane, isobutane, n-pentane, n-hexane, n-heptane, and n-octane; alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane, cycloheptane, and methylcycloheptane; and aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene.
[0273] These hydrocarbon solvents may be used alone or in combination of two or more. Among these, when an organic lithium initiator is used, the hydrocarbon solvent is usually n-hexane or cyclohexane, among which cyclohexane is the most commonly used in industry and can be used appropriately.
[0274] The polymerization initiator is not particularly limited, and for example, a polymerization initiator that exhibits anionic polymerization activity with respect to a conjugated diene monomer or a vinyl aromatic hydrocarbon monomer can be suitably used. Specifically, alkali metal compounds such as aliphatic hydrocarbon alkali metal compounds, aromatic monomer alkali metal compounds, and organic amino alkali metal compounds can be cited.
[0275] The alkali metal used for the alkali metal compound is not particularly limited, and examples thereof include lithium, sodium, and potassium.
[0276] Suitable alkali metal compounds include, but are not limited to, aliphatic and aromatic hydrocarbon lithium compounds having 1 to 20 carbon atoms and containing one lithium in one molecule, or dilithium compounds, trilithium compounds, and tetralithium compounds containing two or more lithiums in one molecule.
[0277] Specific examples of such alkali metal compounds include, but are not limited to, n-propyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexamethylene dilithium, butadienyl dilithium, isoprenyl dilithium, the reaction product of diisopropenylbenzene and sec-butyl lithium, and the reaction product of divinylbenzene, sec-butyl lithium and a small amount of 1,3-butadiene.
[0278] In addition, organic alkali metal compounds disclosed in foreign patents shown in U.S. Patent No. 5708092, British Patent No. 2241239, and U.S. Patent No. 5527753 can also be used. These compounds can be used alone or in combination of two or more. Among these, n-butyl lithium is preferred.
[0279] In the process for producing the block copolymer (b), the content of the vinyl aromatic hydrocarbon monomer unit and the content of the conjugated diene monomer unit in the finally obtained block copolymer (b) can be controlled by adjusting the charging ratio of the vinyl aromatic hydrocarbon monomer and the conjugated diene monomer as polymerization raw materials.
[0280] In addition, as an option for the production process of the block copolymer (b), for example, the following steps can be appropriately adopted: a process of adding a polymerization initiator during polymerization; a process of partially performing a coupling reaction by adding a small amount of a multifunctional monomer having two or more reactive sites; or a process of adding alcohol, water, etc. lower than the polymerization active point during polymerization, and then supplying the monomer again to continue polymerization; etc. By appropriately selecting such a process, a block copolymer (b) having a plurality of components with different molecular weights can be produced.
[0281] As methods for preparing copolymer blocks composed of vinyl aromatic hydrocarbon monomer units and conjugated diene monomer units, there can be cited: a method of continuously supplying a mixture of vinyl aromatic hydrocarbon monomers and conjugated diene monomers to a polymerization system for polymerization; a method of copolymerizing vinyl aromatic hydrocarbon monomers and conjugated diene monomers using a polar compound or a randomizer; and the like.
[0282] Examples of polar compounds and randomizers include, but are not limited to, ethers such as tetrahydrofuran, diethylene glycol dimethyl ether, and diethylene glycol dibutyl ether; amines such as triethylamine and tetramethylethylenediamine; sulfides; phosphines; phosphoramides; alkylbenzene sulfonates; potassium or sodium alcohol salts; and the like.
[0283] The optimal polymerization temperature in the polymerization step of the block copolymer (b) varies depending on the polymer structure, but is generally in the range of -10°C to 150°C, preferably 40°C to 120°C in the case of anionic polymerization using a polymerization initiator.
[0284] In addition, the time required for polymerization is usually within 48 hours, preferably in the range of 1 hour to 10 hours. In addition, the atmosphere of the polymerization system is preferably replaced with an inert gas such as nitrogen. The polymerization pressure is not particularly limited as long as it is a pressure range sufficient to maintain the monomer and the polymerization solvent in the liquid phase within the above-mentioned polymerization temperature range. In addition, it is preferred to pay attention to not accidentally mixing impurities (such as water, oxygen, carbon dioxide, etc.) that deactivate the polymerization initiator and the active polymer into the polymerization system.
[0285] When the block copolymer (b) contains a random copolymer block, a mixture of a vinyl aromatic hydrocarbon monomer and a conjugated diene monomer may be continuously supplied to a polymerization system for polymerization and / or a vinyl aromatic hydrocarbon monomer and a conjugated diene monomer may be copolymerized using a polar compound or a randomizer.
[0286] In the manufacture of block copolymer (b), when using organic alkali metal as polymerization initiator, the coupling reaction that makes more than 2 molecules combine to stop when stopping polymerization reaction can be appropriately utilized. In the coupling reaction, the coupling agent shown in the following example can be added to the polymerization system. In addition, it is also possible to couple only the partial polymer in the polymerization system by adjusting the addition amount of the coupling agent, so that uncoupled polymer and coupled polymer coexist, thereby producing a block copolymer (b) with more than 2 peaks in molecular weight distribution.
[0287] The coupling agent that can be suitably used in the production of the block copolymer (b) is not particularly limited, and examples thereof include any coupling agent having two or more functional groups.
[0288] Specifically, there can be mentioned amino group-containing silane compounds such as tetraglycidyl-m-phenylenediamine, tetraglycidyl-1,3-bisaminomethylcyclohexane, tetraglycidyl-p-phenylenediamine, tetraglycidyldiaminodiphenylmethane, diglycidylaniline, diglycidyl-o-toluidine, γ-glycidyloxyethyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxybutyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, γ-glycidyloxypropyltripropoxysilane, and γ-glycidyloxypropyltributoxysilane.
[0289] In addition, as other coupling agents, for example, 1-[3-(triethoxysilyl)-propyl]-4-methylpiperazine, 1-[3-(diethoxyethylsilyl)-propyl]-4-methylpiperazine, 1-[3-(trimethoxysilyl)-propyl]-3-methylimidazolidine, 1-[3-(diethoxyethylsilyl)-propyl]-3-ethylimidazolidine, 1-[3-(triethoxysilyl)-propyl]-3-methylhexahydropyrimidine, 1-[3-(dimethoxymethylsilyl)-propyl]-4-methylpiperazine, Silane compounds containing a silyl group include silane compounds such as 1-{3-[3-(trimethoxysilyl)-propyl]-tetrahydropyrimidine, 3-[3-(tributoxysilyl)-propyl]-1-methyl-1,2,3,4-tetrahydropyrimidine, 3-[3-(dimethoxymethylsilyl)-propyl]-1-ethyl-1,2,3,4-tetrahydropyrimidine, 1-(2-ethoxyethyl)-3-[3-(trimethoxysilyl)-propyl]-imidazolidine, and (2-{3-[3-(trimethoxysilyl)-propyl]-tetrahydropyrimidin-1-yl}-ethyl)dimethylamine.
[0290] In addition, as other coupling agents, for example, γ-glycidoxypropyl triphenoxysilane, γ-glycidoxypropyl methyl dimethoxysilane, γ-glycidoxypropyl ethyl dimethoxysilane, γ-glycidoxypropyl ethyl diethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-glycidoxypropyl methyl dipropoxysilane, γ-glycidoxypropyl methyl dibutoxysilane, γ-glycidoxypropyl methyl diphenoxysilane, γ-glycidoxypropyl dimethyl methoxysilane, γ-glycidoxypropyl diethyl ethoxysilane, γ-glycidoxypropyl dimethyl ethoxysilane, γ-glycidoxypropyl dimethyl phenoxysilane, γ-glycidoxypropyl diethyl methoxysilane Silane compounds containing glycidoxy groups include γ-glycidoxypropylmethyldiisopropenoxysilane, bis(γ-glycidoxypropyl)dimethoxysilane, bis(γ-glycidoxypropyl)diethoxysilane, bis(γ-glycidoxypropyl)dipropoxysilane, bis(γ-glycidoxypropyl)dibutoxysilane, bis(γ-glycidoxypropyl)diphenoxysilane, bis(γ-glycidoxypropyl)methylmethoxysilane, bis(γ-glycidoxypropyl)methylethoxysilane, bis(γ-glycidoxypropyl)methylpropoxysilane, bis(γ-glycidoxypropyl)methylbutoxysilane, bis(γ-glycidoxypropyl)methylphenoxysilane, and tris(γ-glycidoxypropyl)methoxysilane.
[0291] In addition, as other coupling agents, for example, silane compounds containing methacryloxy groups such as γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxymethyltrimethoxysilane, γ-methacryloxyethyltriethoxysilane, bis(γ-methacryloxypropyl)dimethoxysilane, and tris(γ-methacryloxypropyl)methoxysilane can be mentioned.
[0292] In addition, examples of other coupling agents include β-(3,4-epoxycyclohexyl)ethyl-trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-triethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-tripropoxysilane, β-(3,4-epoxycyclohexyl)ethyl-tributoxysilane, β-(3,4-epoxycyclohexyl)ethyl-triphenoxysilane, β-(3,4-epoxycyclohexyl)ethyl-trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-ethyl-trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-ethyl-diethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-methyl-diethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-methyl- Silane compounds containing epoxycyclohexyl groups, such as dipropoxysilane, β-(3,4-epoxycyclohexyl)ethyl-methyldibutoxysilane, β-(3,4-epoxycyclohexyl)ethyl-methyldiphenoxysilane, β-(3,4-epoxycyclohexyl)ethyl-dimethylmethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-diethylethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-dimethylethoxysilane, β-(3,4-epoxycyclohexyl)ethyl-dimethylpropoxysilane, β-(3,4-epoxycyclohexyl)ethyl-dimethylbutoxysilane, β-(3,4-epoxycyclohexyl)ethyl-dimethylphenoxysilane, β-(3,4-epoxycyclohexyl)ethyl-diethylmethoxysilane, and β-(3,4-epoxycyclohexyl)ethyl-methyldiisopropenoxysilane. Examples of other coupling agents include 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, N,N′-dimethylpropyleneurea, and N-methylpyrrolidone.
[0293] It should be noted that when the coupling agent is subjected to addition reaction at the active end of the block copolymer (b), there is no limitation on the structure of the active end of the block copolymer (b). From the perspective of the mechanical strength of the antistatic resin composition of the present embodiment, the active end of the block mainly composed of a vinyl aromatic hydrocarbon monomer is preferred.
[0294] The amount of the coupling agent used is preferably 0.1 to 10 equivalents, more preferably 0.5 to 4 equivalents, per 1 equivalent of the active terminal of the block copolymer (b). The coupling agent may be used alone or in combination of any two or more.
[0295] (Donor-acceptor system molecular compound (c))
[0296] The antistatic resin composition of the present embodiment contains a donor-acceptor system compound (c).
[0297] The donor-acceptor system molecular compound (c) is a molecular compound having both donor and acceptor functions. The donor referred to here is an electron-donating group, and the acceptor is an electron-withdrawing group.
[0298] Specifically, the donor-acceptor system molecular compound (c) is preferably a compound obtained by mixing an organic boron compound represented by the upper side of the following general formula (1) as a donor component and an organic nitrogen compound represented by the lower side of the following general formula (1) as an acceptor component.
[0299] [Chemistry 2]
[0300]
[0301] In the above general formula (1), R1 and R2 are each independently CH3(CH2) n -CO-OCH2 (n is an integer of 12 to 22), or HOCH2, and at least one of them is CH3(CH2) n -CO-OCH3 (n is an integer of 12 to 22).
[0302] R3 and R4 are each independently any one selected from the group consisting of CH3, C2H5, HOCH2, HOC2H4, and HOCH2CH(CH3).
[0303] Here, "δ+" in the general formula (1) indicates the presence of polarity in the covalent bond within the molecule, (+) indicates that the oxygen atom has a strong electron-donating property, (-) indicates that the boron atom has a strong electron-withdrawing property, "→" indicates a path through which electrons are attracted, and "---" indicates a state in which the bonding force between atoms is weakened.
[0304] The donor component formed by the organic boron compound portion represented by the upper side of the general formula (1) has at least one straight-chain hydrocarbon group having 12 to 22 carbon atoms. In addition, the acceptor component formed by the organic nitrogen compound portion represented by the lower side of the general formula (1) is a tertiary amine in which one N-substituent is a group having a straight-chain hydrocarbon group having 12 to 22 carbon atoms bonded to the end via an amide bond, and the remaining two N-substituents are hydrocarbon groups having 1 to 3 carbon atoms or hydroxyl hydrocarbon groups.
[0305] Many brands of donor-acceptor system molecular compounds are manufactured and sold by Boron Laboratory Co., Ltd., and the trade name "Biomicelle BN-105" is a representative example.
[0306] By adding the donor-acceptor system molecular compound (c) used in the antistatic resin composition of the present embodiment to a resin to prepare a composition, an antistatic effect can be obtained and antistatic properties can be exhibited.
[0307] Regarding the antistatic property exhibited by the donor-acceptor molecular compound (c), its performance is affected by the polymer species, composition ratio, melt viscosity of each component, etc. of the resin composition to be blended.
[0308] From the aspect of exhibiting antistatic performance, the composition range of the appropriate donor-acceptor molecular compound (c), especially its lower limit value, varies depending on the mass ratio of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) and the MFR values of each component.
[0309] That is, the antistatic resin composition of the present embodiment satisfies any one of the following (i) to (iv).
[0310] <Condition (i)>
[0311] When the total of the above-mentioned component (a) and the above-mentioned component (b) is 100% by mass, when the above-mentioned component (a) is more than 0% by mass and 30% by mass or less, and the above-mentioned component (b) is 70% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the above-mentioned component (a), the above-mentioned component (b), and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.5% by mass or more and 5% by mass or less.
[0312] <Condition (ii)>
[0313] When the total of the above-mentioned component (a) and the above-mentioned component (b) is 100% by mass, when the above-mentioned component (a) is more than 30% by mass and 50% by mass or less, and the above-mentioned component (b) is less than 70% by mass and 50% by mass or more, when satisfying
[0314] MFRa < MFRb ··· (Equation 1)
[0315] When the relationship is satisfied, when the total of the above-mentioned component (a), the above-mentioned component (b), and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.5% by mass or more and 5% by mass or less; when satisfying
[0316] MFRa ≧ MFRb ··· (Equation 2)
[0317] When the relationship is satisfied, when the total of the above-mentioned component (a), the above-mentioned component (b), and the above-mentioned component (c) is 100% by mass, the above-mentioned component (c) is 0.9% by mass or more and 5% by mass or less.
[0318] <Condition (iii)>
[0319] When the total of the above component (a) and the above component (b) is 100% by mass, when the above component (a) is more than 50% by mass and 70% by mass or less, and the above component (b) is less than 50% by mass and 30% by mass or more, the following is satisfied
[0320] MFRa < MFRb ··· (Formula 1)
[0321] Regarding the relationship, when the total of the above component (a), the above component (b), and the above component (c) is 100% by mass, the above component (c) is 0.9% by mass or more and 5% by mass or less.
[0322] <Condition (iv)>
[0323] When the total of the above component (a) and the above component (b) is 100% by mass, when the above component (a) is more than 70% by mass and 81% by mass or less, and the above component (b) is less than 30% by mass and 19% by mass or more, the following is satisfied
[0324] MFRa < MFRb ··· (Formula 1)
[0325] Regarding the relationship, when the total of the above component (a), the above component (b), and the above component (c) is 100% by mass, the above component (c) is 4% by mass or more and 5% by mass or less.
[0326] In this way, as the composition ratio of the block copolymer (b) increases and the MFR value (MFRb) of the block copolymer (b) is higher than the MFR value (MFRa) of the vinyl aromatic hydrocarbon resin (a), a reduction in surface resistivity is confirmed with a smaller addition amount of the donor-acceptor type molecular compound (c), and there is a tendency to easily exhibit antistatic performance.
[0327] (Other additives that can be blended in the antistatic resin composition)
[0328] The antistatic resin composition of the present embodiment may contain arbitrary additives within a range that does not impair the effects of the present embodiment.
[0329] As additives, there may be mentioned additives commonly used in the compounding of resins or rubber-like polymers, such as, but not limited to, inorganic fillers such as calcium carbonate, magnesium carbonate, silicon dioxide, zinc oxide, and carbon black; higher alcohols such as stearyl alcohol, fatty acids such as palmitic acid, stearic acid, and behenic acid, fatty acid metal salts such as zinc stearate, calcium stearate, magnesium stearate, magnesium behenate, and magnesium hydrogenated ricinoleate; lubricants and release agents such as fatty acid amides such as erucamide and ethylene bisstearamide; softeners and plasticizers such as paraffin oil, process oil, organopolysiloxane, and mineral oil; hindered phenol-based and phosphorus-based heat stabilizers and antioxidants; hindered amine-based light stabilizers; benzotriazole-based ultraviolet absorbers; flame retardants; reinforcing agents such as organic fibers, glass fibers, carbon fibers, and metal whiskers; colorants such as organic pigments, inorganic pigments, and organic dyes; and the like.
[0330] [Method for producing antistatic resin composition]
[0331] There is no particular limitation on the method for producing the antistatic resin composition of the present embodiment. For example, the following method can be cited: dry-mixing the block copolymer (b) and the donor-acceptor system molecular compound (c) (or adding a vinyl aromatic hydrocarbon resin (a) thereto) at room temperature, heating and melt-kneading them using a twin-screw extruder, extruding the heated and melted antistatic resin composition from a die in the form of strands, and granulating it again through a cooling bath to obtain a granular composition.
[0332] When heating and melt kneading is performed, there is no particular limitation as long as it is a kneading machine for thermoplastic resins that can be heated and melted. For example, a kneading machine such as a kneader, a Banbury mixer, a roll, a ribbon mixer, a single-screw extruder, or a twin-screw extruder can be appropriately used.
[0333] In addition, not only the wire cutting method using a cooling bath but also a heat cutting method, an underwater cutting method, or the like can be preferably used depending on the purpose.
[0334] In order to fully exert the antistatic performance of the donor-acceptor system molecular compound (c), it is preferred to produce the antistatic resin composition by the following production method.
[0335] That is, the antistatic resin composition of the present embodiment is obtained through the following steps: step (I), melt-kneading the block copolymer (b) and the donor-acceptor system molecular compound (c) in a manner such that the composition ratio of the donor-acceptor system molecular compound (c) is 5 mass % to 20 mass %, to produce a masterbatch with a high concentration of component (c); and step (II), kneading the above-mentioned masterbatch with a vinyl aromatic hydrocarbon resin (a) and / or a block copolymer (b) to dilute the masterbatch.
[0336] By adopting the above-mentioned manufacturing method via masterbatch, the dispersibility of the donor-acceptor system molecular compound (c) in the antistatic resin composition is exceptionally improved, and the desired reduced surface resistivity can be efficiently exhibited with a smaller addition amount, and the balance between the mechanical properties and antistatic performance of the obtained antistatic resin composition is optimal.
[0337] In the antistatic resin composition of this embodiment, the donor-acceptor system molecular compound (c) is fully dispersed in the resin matrix formed by component (b), or the resin matrix formed by component (a) and component (b) using a resin mixer. This is very important for the performance. The following manufacturing method is recommended: temporarily prepare a high-concentration masterbatch and then dilute it to obtain the desired antistatic resin composition.
[0338] [Electronic parts packaging materials]
[0339] The molded product of the antistatic resin composition of the present embodiment is suitable as an electronic component packaging material.
[0340] Examples of electronic component packaging materials include carrier tapes, transport trays, and packaging tubes.
[0341] The electronic component packaging material of this embodiment may have a single layer or multiple layers in thickness direction. From the perspective of economic efficiency, the electronic component packaging material of this embodiment usually uses the antistatic resin composition of this embodiment as the surface layer or the surface layer and the back layer of the electronic component packaging material.
[0342] A multilayer sheet having a layer of several tens of microns formed by the antistatic resin composition of the present embodiment is formed on the surface layer of the side in contact with the electronic component product, and then a concave portion (also referred to as a bag or embossing) for storing the electronic component product is formed by vacuum forming, compression molding, etc. In the electronic component packaging material used by stacking a conveying pallet, etc., since the back side thereof is also in contact with the electronic component product, it is generally preferred to use an electronic component packaging material having the antistatic resin composition of the present embodiment not only on the surface layer but also on the back layer.
[0343] Even when the donor-acceptor system molecular compound (c) is added to the antistatic resin composition of the present embodiment, the transparency of the base resin formed by the component (a) and the component (b) is not so impaired.
[0344] By selecting the combination of the component (a) and the component (b) to be used, an electronic component packaging material having excellent transparency can be obtained.
[0345] In the electronic component packaging material of the present embodiment, the thickness thereof or the thickness of each constituent layer is not particularly limited, and is appropriately designed according to the situation depending on the electronic component to which the packaging material is applied.
[0346] When the electronic component packaging material of this embodiment is an extruded product, the overall thickness is preferably 50 μm to 4 mm, more preferably 0.1 mm to 2.0 mm, further preferably 0.1 mm to 1.5 mm, and still more preferably 0.2 mm to 1.2 mm. If the final use is a carrier tape, the wall tends to be thin, while if it is a transport pallet, the wall tends to be thick.
[0347] The thickness of the layer formed by the antistatic resin composition in contact with the electronic component product is preferably 5 μm to 1 mm, more preferably 10 μm to 0.1 mm, and further preferably 15 μm to 50 μm. When the raw material sheet is subjected to secondary processing such as vacuum forming or compression molding, there are also areas such as the embossed side that become thinner due to stretching, and it is preferred that the layer formed by the antistatic resin composition in the raw material sheet has a certain degree of thickness.
[0348] In the electronic component packaging material of the present embodiment, for the purpose of reuse in the process, the crushed material formed by crushing the scrap of the sheet can be blended in at least one layer of the intermediate layer and used. In this case, usually adopt the method that new material and reuse material are blended with arbitrary proportion, but reuse material can also be used separately. Reuse material is preferably a similar constituent produced by the same production line, but can also be blended in the scope of the effect of the present embodiment without hindering the different resin combinations produced by other series.
[0349] Furthermore, the electronic component packaging material of the present embodiment may be subjected to printing, discharge treatment such as corona discharge or glow discharge, or surface treatment such as acid treatment, on its surface within the scope of the present invention.
[0350] [Characteristics of electronic component packaging materials]
[0351] (Surface resistivity)
[0352] The surface resistivity of the antistatic resin composition and the electronic component packaging material obtained by molding the antistatic resin composition is 1×10 12 Ω / □ or less.
[0353] The surface resistivity of a resin composition or a molded article composed only of component (a) and component (b) without mixing the donor-acceptor system molecular compound (c) is generally 1×10 16 Ω / □ or more, it is an insulator. The effect of mixing the donor-acceptor system molecular compound (c) is to obtain 1×10 12 Surface resistivity below Ω / □.
[0354] However, when the vinyl aromatic hydrocarbon resin as component (a) is used alone, it is difficult to exert its performance even if the donor-acceptor molecular compound (c) is mixed, so the presence of the block copolymer as component (b) is indispensable.
[0355] The surface resistivity of the electronic component packaging material does not depend on the molding method or the shape of the product, but is determined only by the resin composition of the surface portion in contact with the electronic component.
[0356] Therefore, the surface resistivity of the electronic component packaging material and the surface resistivity of the antistatic resin composition in direct contact with the electronic component are the same value and have compatibility.
[0357] The surface resistivity can be measured by the method described in the examples, for example, using a simple surface resistivity meter "ST-3" manufactured by SIMCO Japan Co., Ltd. It is preferred to form the sample into a sheet and allow it to stand in a constant temperature room at 23°C and 50% humidity (for example, for 24 hours) before measuring. The surface resistivity of the extruded sheet sample can be the average value of the measured values of each surface and back side in the extrusion direction (MD) and the direction perpendicular to the extrusion (TD).
[0358] (Haze value)
[0359] The antistatic resin composition and electronic component packaging material of the present embodiment may preferably have visibility depending on the type of components to be packaged, and transparency can be used to expand the application. For example, in the use of transport pallets, visibility is often required, and in the use of carrier tapes, visibility is often required, and transparency is preferred.
[0360] The transparency shown in the examples is expressed as a haze value measured in accordance with ISO 14782 using a 1 mm thick flat plate produced by injection molding the antistatic resin composition.
[0361] The haze value area with visibility (the electronic components of the contents can be seen through the packaging material) is 20% or less, and the smaller the haze value is, the closer it is to zero, the better the visibility is. The haze value for clearly seeing the contents is 4.0% or less, and if the haze value is 2.0% or less, the outline of the contents is clearly visible.
[0362] In order to reduce the haze value of the antistatic resin composition of the present embodiment and improve the transparency, it is necessary to make each component monomer of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) have transparency, and the refractive index of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is similar. Specifically, when the difference in refractive index is below 0.004, the transparency is good and the haze value can be achieved below 4.0%.
[0363] As described above, the haze value of the antistatic resin composition of the present embodiment is a value measured using an injection molding flat plate, but actual electronic component packaging materials are often molded using extrusion molding, and the extrusion surface changes due to the dispersion form of the high-order structure of the resin composition, the roller temperature, the gap between the rollers, or the mirror finish of the roller surface, and the haze value also changes. In addition, in the case of a multilayer molded sheet formed of a surface layer and an intermediate layer, the transparency of the electronic component packaging material itself affects the transparency of each layer.
[0364] Example
[0365] The present embodiment is further described in detail with reference to specific examples and comparative examples below.
[0366] It should be noted that this embodiment is not limited by the following examples.
[0367] (Vinyl aromatic hydrocarbon resin (a) and donor-acceptor molecular compound (c) used in Examples and Comparative Examples)
[0368] As the vinyl aromatic hydrocarbon resins (a)-1 to 8 and the donor-acceptor molecular compound (c-1), commercially available products were used.
[0369] In the following [Table 1], in addition to the manufacturers, brand names, and categories thereof, the MFR values (described as MFRa in Table 1) of the component (a) are added and listed.
[0370]
[0371] (Melt Flow Rate (MFRa) of Vinyl Aromatic Hydrocarbon Resin (a))
[0372] The MFR of the component (a) is the value disclosed in the physical property table.
[0373] The measurement standard is based on ISO 1133 and is measured at a temperature of 200° C. and a load of 5 kgf. The same standard and conditions are used as for the MFRb of the block copolymer (b) described later.
[0374] (Block copolymer (b))
[0375] [Production Examples 1 to 8]
[0376] Regarding the block copolymer (b), each of block copolymers (b)-1 to 8 was produced according to the following production example.
[0377] [Production Example 1]
[0378] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium and 0.015 parts by mass of tetramethylmethylenediamine were added to a cyclohexane solution containing 20 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0379] Next, a cyclohexane solution containing 14 parts by mass of 1,3-butadiene and 10 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 30 minutes, and polymerization was performed at 80°C.
[0380] Next, a cyclohexane solution containing 16 parts by mass of 1,3-butadiene and 10 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 30 minutes, and polymerization was performed at 80°C.
[0381] Next, a cyclohexane solution containing 30 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization liquid, and polymerization was carried out at 80° C. for 30 minutes.
[0382] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.4 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate was added as a heat stabilizer relative to 100 parts by mass of the block copolymer, and then the solvent was removed to recover the block copolymer (b)-1.
[0383] [Production Example 2]
[0384] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium was added to a cyclohexane solution containing 31 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0385] Next, a cyclohexane solution containing 21 parts by mass of 1,3-butadiene and 20 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 30 minutes, and polymerization was performed at 80°C.
[0386] Next, a cyclohexane solution containing 2 parts by mass of 1,3-butadiene and 6 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization solution over 30 minutes, and polymerization was carried out at 80° C. Next, a cyclohexane solution containing 20 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization solution, and polymerization was carried out at 80° C. for 30 minutes.
[0387] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.3 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate was added as a heat stabilizer relative to 100 parts by mass of the block copolymer, and the solvent was then removed to recover the block copolymer (b)-2.
[0388] [Production Example 3]
[0389] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium was added to a cyclohexane solution containing 8 parts by mass of butadiene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0390] Next, a cyclohexane solution containing 14 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 15 minutes, and polymerization was performed at 80°C.
[0391] Next, a cyclohexane solution containing 22 parts by mass of 1,3-butadiene at a concentration of 25% by mass was continuously added to the polymerization liquid over 15 minutes, and polymerization was performed at 80°C.
[0392] Next, a cyclohexane solution containing 29 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization liquid, and polymerization was carried out at 80° C. for 30 minutes.
[0393] Thereafter, in order to stop a portion of the polymerization, ethanol in an amount of 0.5 times the mole of n-butyllithium was added to the reactor, and the polymerization solution was stirred for 10 minutes. A cyclohexane solution containing 27 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization solution, and polymerization was carried out at 80°C for 30 minutes.
[0394] Thereafter, in order to completely stop the polymerization, 0.5 times the molar amount of ethanol relative to n-butyl lithium was added to the reactor, and 0.4 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate as a heat stabilizer was added relative to 100 parts by mass of the block copolymer, and then the solvent was removed to recover the block copolymer (b)-3.
[0395] [Production Example 4]
[0396] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium and 0.015 parts by mass of tetramethylmethylenediamine were added to a cyclohexane solution containing 60 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0397] Next, a cyclohexane solution containing 30 parts by mass of 1,3-butadiene and 10 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 30 minutes, and polymerization was performed at 80°C.
[0398] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.3 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate as a heat stabilizer was added to 100 parts by mass of the block copolymer, and the solvent was then removed to recover the block copolymer (b)-4.
[0399] [Production Example 5]
[0400] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium and 0.015 parts by mass of tetramethylmethylenediamine were added to a cyclohexane solution containing 40 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0401] Next, a cyclohexane solution containing 15 parts by mass of 1,3-butadiene and 10 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 30 minutes, and polymerization was performed at 80°C.
[0402] Next, a cyclohexane solution containing 35 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization liquid, and polymerization was carried out at 80° C. for 30 minutes.
[0403] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.2 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate as a heat stabilizer was added to 100 parts by mass of the block copolymer, and the solvent was then removed to recover the block copolymer (b)-5.
[0404] [Production Example 6]
[0405] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium was added to a cyclohexane solution containing 42 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0406] Next, a cyclohexane solution containing 8 parts by mass of 1,3-butadiene at a concentration of 25% by mass was continuously added to the polymerization solution over 10 minutes, and polymerization was performed at 80° C. Next, a cyclohexane solution containing 50 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization solution, and polymerization was performed at 80° C. for 30 minutes.
[0407] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.2 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate as a heat stabilizer was added to 100 parts by mass of the block copolymer, and the solvent was then removed to recover the block copolymer (b)-6.
[0408] [Production Example 7]
[0409] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium was added to a cyclohexane solution containing 16 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 20 minutes.
[0410] Next, a cyclohexane solution containing 68 parts by mass of 1,3-butadiene at a concentration of 25% by mass was added to the polymerization liquid over 10 minutes, and polymerization was performed at 80°C.
[0411] Next, a cyclohexane solution containing 16 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization liquid, and polymerization was carried out at 80° C. for 30 minutes.
[0412] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.5 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate as a heat stabilizer was added to 100 parts by mass of the block copolymer, and the solvent was then removed to recover the block copolymer (b)-7.
[0413] [Production Example 8]
[0414] In a nitrogen atmosphere, 0.08 parts by mass of n-butyllithium was added to a cyclohexane solution containing 9 parts by mass of styrene at a concentration of 25% by mass, and polymerization was carried out at 80° C. for 15 minutes.
[0415] Next, a cyclohexane solution containing 75 parts by mass of 1,3-butadiene and 7 parts by mass of styrene at a concentration of 25% by mass was continuously added to the polymerization liquid over 30 minutes, and polymerization was performed at 80°C.
[0416] Next, a cyclohexane solution containing 9 parts by mass of styrene at a concentration of 25% by mass was added to the polymerization liquid, and polymerization was carried out at 80° C. for 30 minutes.
[0417] Thereafter, in order to completely stop the polymerization, ethanol in an amount equal to the molar amount of n-butyl lithium was added to the reactor, and 0.5 parts by mass of 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate as a heat stabilizer was added to 100 parts by mass of the block copolymer, and the solvent was then removed to recover the block copolymer (b)-8.
[0418] (Contents of Vinyl Aromatic Hydrocarbon Monomer Units (Styrene Units) and Conjugated Diene Monomer Units (Butadiene Units) in Each Block Copolymer (b)-1 to 8)
[0419] For each block copolymer obtained in the above-mentioned Production Examples 1 to 8, the copolymerization ratio of styrene and 1,3-butadiene as each monomer component was confirmed by the following analysis method whether it was different from the charging ratio during polymerization. As an analytical instrument, a UV-visible spectrophotometer manufactured by Shimadzu Corporation was used.
[0420] Specifically, about 30 mg (accurately weighed to 0.1 mg) of each block copolymer (b) 1 to 8 was dissolved in 100 mL of chloroform, and the polymer solution was filled into a quartz cell, placed in an ultraviolet visible spectrophotometer, and scanned using an ultraviolet wavelength of 260 to 290 nm. The aromatic ring of styrene exhibits light absorption in this wavelength region, and the absorption peak height value obtained by measurement is used. The calibration curve prepared from a known sample is used to determine the styrene composition ratio (mass %) contained in each block copolymer (b). The peak wavelength from styrene appears at 269.2 nm.
[0421] As a result, it was confirmed that there was no difference between the styrene charge ratio during polymerization and the styrene composition ratio in the block copolymer. On the other hand, the butadiene composition ratio (mass %) was determined by subtracting the styrene composition ratio (mass %) from 100.
[0422] (Weight average molecular weight Mw, number average molecular weight Mn, molecular weight distribution Mw / Mn, peak molecular weight and molecular weight peak number of each block copolymer (b)-1 to 8)
[0423] The weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn), peak molecular weight and molecular weight peak number of the block copolymers (b)-1 to 8 were measured by gel permeation chromatography (GPC) under the following measurement conditions.
[0424] (Measurement conditions)
[0425] GPC equipment: HLC-8220 manufactured by Tosoh Corporation
[0426] Column: SuperMultiporeHZ-M manufactured by Tosoh Corporation, 2 connected in series
[0427] Column temperature: 40°C
[0428] Liquid delivery volume: 0.2mL / min
[0429] Detector: Refractometer (RI)
[0430] In addition, tetrahydrofuran was used as a solvent, and about 10 mg of the polymer used for molecular weight measurement was dissolved in 20 mL of tetrahydrofuran, and the mixture was filtered to remove insoluble components to obtain a sample for GPC measurement.
[0431] The specific measurement method is as follows. First, a calibration curve is prepared using 9 standard polystyrene samples with different molecular weights and known molecular weights. The weight average molecular weight (Mw) of the standard polystyrene with the highest molecular weight is 1090000, and the weight average molecular weight (Mw) of the standard polystyrene with the lowest molecular weight is 1050. Next, using each block polymer for molecular weight measurement, a sample for measurement is prepared under the above-mentioned points.
[0432] After confirming that the temperature in the tank containing the column is constant, the solution sample is injected and the measurement is started. After the measurement is terminated, the obtained molecular weight distribution curve is statistically processed to calculate the weight average molecular weight (Mw) and the number average molecular weight (Mn). The molecular weight distribution (Mw / Mn) is the value obtained by dividing the obtained weight average molecular weight (Mw) by the number average molecular weight (Mn). In addition, the peak molecular weight and the number of molecular weight peaks are determined based on the above molecular weight distribution curve.
[0433] (Weight Average Molecular Weight (Mw), Number Average Molecular Weight (Mn) and Molecular Weight Distribution (Mw / Mn) of the Polymer Block S of Each Block Copolymer (b)-1 to 8)
[0434] Next, the molecular weight of the polymer block S composed only of the vinyl aromatic monomer unit constituting each of the block copolymers (b)-1 to 8 was measured.
[0435] Specifically, about 20 mg of the polymer was dissolved in about 10 mL of chloroform using an Erlenmeyer flask, 20 mL of an osmic acid solution was added, and the mixture was scalded with hot water at about 90° C. for 30 minutes to partially decompose the conjugated diene.
[0436] After scalding with hot water, the Erlenmeyer flask was cooled with running water, and about 200 mL of methanol was slowly poured into the decomposed polymer solution to precipitate the components insoluble in the solvent.
[0437] The precipitated solid component is a polymer block S formed only by vinyl aromatic monomer units, and the styrene monomer that does not form a block and the styrene with a low degree of polymerization are still dissolved in the methanol / tert-butyl alcohol / chloroform mixed solution. The precipitate is filtered using a glass filter, washed with pure methanol, and vacuum dried, thereby separating only the polymer block S from the block copolymer (b).
[0438] Here, the osmic acid solution is a solution prepared by dissolving and mixing 1 g of osmium (VIII) oxide and 2 kg of "Perbutyl H (chemical name: tert-butyl hydroperoxide, purity 69%)" available from NOF Corporation in 3 L of tert-butyl alcohol.
[0439] About 10 mg of the polymer block S thus obtained was dissolved again in 20 mL of tetrahydrofuran and measured using a GPC apparatus. The measurement conditions and method were the same as those for measuring the molecular weight of the block copolymer (b) described above.
[0440] (Melt Flow Rate (MFRb) of Block Copolymer (b))
[0441] The measurement was performed in accordance with ISO 1133 at a temperature of 200° C. and a load of 5 kgf.
[0442] The monomer charge composition and the ratio (mass %) of the vinyl aromatic monomer unit to the conjugated diene monomer unit of each block copolymer (b)-1 to 8 obtained in each Production Examples 1 to 8, molecular weight information based on GPC measurement results, and melt flow rate are shown in the following [Table 2].
[0443]
[0444] [Method for producing antistatic resin composition]
[0445] Using the vinyl aromatic hydrocarbon resins (a)-1 to 7 and the donor-acceptor molecular compound (c-1) shown in the above [Table 1] and the block copolymers (b)-1 to 8 shown in the above [Production Examples 1 to 8], an antistatic resin composition was produced by the following method.
[0446] First, components (a), (b) and (c) were dry-blended at a desired composition ratio at room temperature, and then fed into the feed hopper of a twin-screw extruder TEX30α (L / D=42) manufactured by The Japan Steel Works, Ltd., and melt-kneaded at a barrel temperature of 210°C.
[0447] It should be noted that the reaction was carried out at a cylinder temperature of 230° C. only when the compounding composition (a)-5 was used.
[0448] In order to fully exert the antistatic performance of the above-mentioned (c) component, it is necessary to make the above-mentioned (c) component highly finely dispersed in the above-mentioned (b) component. In any of the cases of manufacturing through high-concentration masterbatch (Examples 35 to 44) or directly manufacturing the antistatic resin composition without manufacturing through high-concentration masterbatch (Examples 1 to 34, Comparative Examples 1 to 24), a mixer with high mixing performance is used during the initial processing of each individual component, that is, in the melt-kneading step of the constituent components, specifically a twin-screw extruder.
[0449] On the other hand, in the case where an antistatic resin composition is manufactured based on a masterbatch containing a high concentration of component (c) by diluting the masterbatch using component (a) and / or component (b) (Examples 35 to 44), in the dilution process, the masterbatch is diluted using a single-screw extruder with slower mixing properties to manufacture an antistatic resin composition in the form of pellets.
[0450] Thereafter, a desired molded article is produced by injection molding, or a sheet-shaped antistatic resin composition having a desired thickness is produced by diluting the masterbatch using a single-screw extruder equipped with a T-die.
[0451] It has been confirmed that if a masterbatch in which component (c) is highly finely dispersed is prepared once, the antistatic performance can be fully exhibited even under slow kneading conditions in the subsequent dilution process.
[0452] In the case of dilution processing of high-concentration masterbatch (Examples 35 to 44), for the case of injection molding described later, a single screw extruder VS40-28V (L / D=28; with compression kneading zone) manufactured by Tanabe Plastic Machinery was used to manufacture the antistatic resin composition in the shape of pellets. In addition, for the case of extrusion sheet molding described later, a sheet extrusion molding machine described below was used to manufacture the antistatic resin composition in the form of a sheet having a desired thickness.
[0453] [Characteristics of antistatic resin composition]
[0454] (Extrusion molding and surface resistivity measurement of antistatic resin composition)
[0455] As described above, pellets formed by an antistatic resin composition in which a donor-acceptor system molecular compound as component (c) is highly finely dispersed (Examples 1 to 34, Comparative Examples 1 to 24), or a masterbatch containing component (c) at a high concentration is diluted with component (a) and / or component (b) (Examples 35 to 44), and extruded sheets are prepared using a single-screw T-die extruder.
[0456] T-die sheet molding uses Ikegai Co., Ltd.'s sheet extrusion molding machine FS40-36V+TS400 (single screw, with Durmacher mixing, screw diameter 40 mm, L / D=36, T-die width 400 mm, mirror roller). Under the conditions of barrel temperature 210°C and roller temperature 70°C, the screw speed and roller withdrawal speed are adjusted to produce single-layer sheets with a thickness of 0.20 mm.
[0457] It should be noted that the test was carried out under the conditions of a cylinder temperature of 230°C and a roll temperature of 80°C only when the compounding composition (a)-5 was used.
[0458] When evaluating the surface resistivity, the measurement was performed using a single-layer sheet, and the production of the measurement sheet was performed by single-layer extrusion.
[0459] The two ends of the extruded sheet were trimmed by about 30 mm to obtain a raw material sheet with a width of 220 mm.
[0460] The surface resistivity in Examples and Comparative Examples was measured using a simple surface resistivity meter "ST-3" manufactured by Simco Japan Co., Ltd. after the antistatic resin composition formed into a sheet was left to stand in a constant temperature room at 23°C and 50% humidity for 24 hours.
[0461] The surface resistivity of the extruded sheet sample is an average value of the values measured on each of the surface and the back surface in the extrusion direction (MD) and the direction perpendicular to the extrusion (TD).
[0462] (Injection molding and haze value of antistatic resin composition)
[0463] The haze value of the antistatic resin composition was evaluated using a flat plate by injection molding.
[0464] In the injection molding, a hybrid injection molding machine FNX110III-18A (mold clamping pressure of 110 tons) manufactured by Nissei Plastic Industry Co., Ltd. is used. The mold uses a mirror-finished flat mold with a thickness of 1 mm, a short side of 100 mm, a long side of 150 mm, and a film-shaped gate on the short side. Under the conditions of a barrel temperature of 210°C and a mold temperature of 50°C, an injection pressure of 5% is added at the short shot point to obtain a flat molded body with a thickness of 1 mm.
[0465] The molding cycle was 7 seconds for injection and 25 seconds for cooling.
[0466] It should be noted that only in the case of the compounding composition (a)-5, the process was carried out at a cylinder temperature of 230°C.
[0467] A test piece of an appropriate size was cut out from the molded product having a thickness of 1 mm obtained by the above injection molding to prepare a test piece for measurement, and the haze value was evaluated (unit: %) using a haze meter HZ-1 manufactured by SUGA TEST INSTRUMENTS.
[0468] In addition, when the haze value is larger than 40%, as clearly stated in ISO14782, it cannot be accurately measured, and therefore it is described as "larger than 40 (opaque)" in the results of Examples and Comparative Examples.
[0469] [Examples 1 to 34, Comparative Examples 1 to 24]
[0470] Using the vinyl aromatic hydrocarbon resins (a)-1 to 7 and donor-acceptor system molecular compounds (c)-1 shown in the above [Table 1] and the block copolymers (b)-1 to 8 of the above-mentioned manufacturing examples 1 to 8 shown in the above [Table 2], melt mixing is carried out using the above-mentioned twin-screw extruder, and each resin composition is obtained by one-stage processing. The surface resistivity of the sheet-like antistatic resin composition with a thickness of 0.25 mm obtained by the above-mentioned single-screw T-die extruder is measured, and the haze value is further measured using a 1 mm thick flat plate obtained by the above-mentioned injection molding machine.
[0471] The measurement results are shown in the following [Table 3] and [Table 4].
[0472] It should be noted that in the table, when the surface resistivity reaches 1×10 12 When the value is less than 1×10 12 When Ω / □ is less than or equal to □, it means that the surface resistivity is outside the range where antistatic performance can be exhibited, and is described as "Out".
[0473] [Table 3]
[0474]
[0475] [Table 4]
[0476]
[0477] [Production Examples 9 to 14]
[0478] A block copolymer (b), a donor-acceptor system molecular compound (c) and a vinyl aromatic hydrocarbon resin (a) are used, and melt-kneading is carried out using the above-mentioned twin-screw extruder in a mixing ratio shown in the following [Table 5] in such a way that the component (c) is 5 mass % or more and 20 mass % or less when the total amount of the masterbatch is 100 mass %, thereby manufacturing a masterbatch containing a high concentration of the component (c).
[0479] [Table 5]
[0480]
[0481] [Examples 35 to 44]
[0482] The masterbatch containing the high concentration of component (c) prepared in [Preparation Examples 9 to 14] was mixed with a vinyl aromatic hydrocarbon resin (a) and / or a block copolymer (b), and the masterbatch was diluted. A sheet-like resin composition having a thickness of 0.25 mm was obtained by the single-screw T-die extruder by the two-stage processing method, and its surface resistivity was measured. In addition, the haze value was measured using a 1 mm thick flat plate obtained by the injection molding machine.
[0483] The measurement results are shown in the following [Table 6] together with the production examples of the master batch used.
[0484] [Table 6]
[0485]
[0486] [Example 35] shown in [Table 6] above is an antistatic resin composition produced by two-stage processing of a masterbatch, but the final composition itself is the same as that of [Example 9] shown in [Table 3] above.
[0487] Similarly, [Example 36] and [Example 13], [Example 37] and [Example 15], [Example 38] and [Example 19], [Example 39] and [Example 44] and [Example 11], [Example 40] and [Example 14], [Example 41] and [Example 7], [Example 42] and [Example 10], [Example 43] and [Example 28] are antistatic resin compositions with the same final composition.
[0488] In the case of two-stage processing via a masterbatch, the haze value is improved by about 0.1 (%) or equivalent in terms of transparency.
[0489] In terms of surface resistivity, it can be seen that in any embodiment, the masterbatch exhibits a lower surface resistivity when subjected to two-stage processing.
[0490] When a two-step process is used in which a high-concentration masterbatch of the component (c) is prepared once and then diluted with the component (a) and / or the component (b), the surface resistivity is further reduced, resulting in the production of a more excellent antistatic resin composition.
[0491] In other words, it is found that the amount of component (c) required to express the same surface resistivity can be reduced, thereby achieving a balance between mechanical properties and economic efficiency.
[0492] In addition, from the comparison between Example 44 and Examples 35 to 43, it can be seen that when preparing the masterbatch, the block copolymer (b) and the donor-acceptor system molecular compound (c) are used as essential components, and the effect of reducing the surface resistivity is excellent.
[0493] Specifically, when a high-concentration masterbatch is produced using only a vinyl aromatic hydrocarbon resin (a) and a donor-acceptor molecular compound (c) without using a block copolymer (b), a comparison of [Example 11], [Example 39] and [Example 44] shows that the surface resistivity improvement effect based on the masterbatch method was not confirmed, and the result is no change compared to the one-stage mixing.
[0494] From the above results, it can be seen that the antistatic resin composition of the example exhibits a desired surface resistivity.
[0495] On the other hand, it is shown that in Comparative Examples 1 to 24, even if a large amount of the donor-acceptor system molecular compound (c) is mixed (which is mixed to express the original antistatic property), the surface resistivity does not reach 1×10 12 If the relative humidity is less than Ω / □, it is difficult to obtain the antistatic resin composition of the present invention.
[0496] In addition, in the comparison of the manufacturing method of obtaining an antistatic resin composition by one-stage processing and the manufacturing method of two-stage processing (manufacturing a high-concentration masterbatch with components (b) and components (c) as necessary components, and then diluting it as a basis using components (a) and / or components (b), thereby obtaining an antistatic resin composition), when comparing the above-mentioned embodiments with the same final composition, it can be seen that the surface resistivity of the antistatic resin composition obtained by two-stage processing of the manufacturing of the high-concentration masterbatch of the latter is further reduced and tends to be good. This is because the dispersion of the donor-acceptor system molecular compound as component (c) is further micro-dispersed, and the addition efficiency is improved.
[0497] [Example 45]
[0498] The antistatic resin composition obtained in the above-mentioned Example 40 is made into a surface layer / back layer with a thickness of 40 μm. In the core layer, a composition obtained by blending a block copolymer (b)-1 at a ratio of 10 mass% with 90 mass% of a vinyl aromatic hydrocarbon resin (a)-3 is used, and a multilayer extruded sheet with a thickness of 0.3 mm is molded using a multilayer sheet extruder equipped with a T die.
[0499] In the T-die multilayer sheet molding, a multilayer sheet extrusion molding machine GT-40-28-A+UT-25-28-H (single screw, with Maddock mixing, screw diameter 40mm (core layer) + 25mm (surface layer / back layer), L / D=28, T-die width 400mm, with embossed roller) manufactured by Plastics Engineering Research Institute Co., Ltd. was used. The screw speed and roller withdrawal speed were adjusted under the conditions of barrel temperature 210°C and roller temperature 70°C to produce the above-mentioned 0.3mm thick multilayer extruded sheet.
[0500] The formed sheet was heated at 110° C. and press-formed to obtain a transport tray capable of accommodating electronic components.
[0501] The obtained electronic component transport tray was confirmed to have a surface resistivity of 10 to the power of 10 and excellent antistatic properties, moderate rigidity and heat deformation resistance, good interlayer bonding strength between the surface layer / back layer and the core layer, and could be firmly bonded without peeling from the end surface. It had excellent strength that was not easily broken even if intentionally bent, and therefore could be suitably used in practical applications.
[0502] In this embodiment, the selectivity of the performance expression of the donor-acceptor system molecular compound with respect to the matrix resin composition and the resin composition spectrum that enables the antistatic performance to be expressed are clarified, especially for the styrene-based resin matrix.
[0503] Industrial Applicability
[0504] In the antistatic resin composition of the present invention, by showing 1×10 12 The surface resistivity is less than Ω / □, and good antistatic properties are exhibited. Furthermore, the donor-acceptor system molecular compound of the substance showing antistatic performance has minimal influence on the processability, mechanical properties, and optical properties of the resin composition. Therefore, when the resin composition itself has transparency, the antistatic resin composition also maintains transparency, and further, the mechanical properties such as folding strength are also excellent. The interlayer bonding strength when made into 2-layer, 3-layer, etc. extruded multilayer sheets is also excellent, and it has industrial practicality as a material for electronic component packaging molded products.
[0505] The antistatic resin composition of the present invention has industrial applicability as a material for packaging materials for electronic components such as carrier tapes, packaging tubes, and trays for transporting electronic components.
Claims
1. An antistatic resin composition, comprising: block copolymer (b), and Donor-acceptor system molecular compound (c), in, The block copolymer (b) is a block copolymer comprising a vinyl aromatic hydrocarbon monomer unit and a conjugated diene monomer unit, and has a polymer block mainly composed of the vinyl aromatic hydrocarbon monomer unit, wherein the vinyl aromatic hydrocarbon monomer unit accounts for 30% to 90% by mass, and the conjugated diene monomer unit accounts for 70% to 10% by mass. When the total amount of the block copolymer (b) and the donor-acceptor system molecular compound (c) is 100 mass %, the content of the donor-acceptor system molecular compound (c) is 0.5 mass % or more and 5 mass % or less.
2. The antistatic resin composition according to claim 1, wherein The surface resistivity is 1×10 12 Ω / □ or less.
3. An antistatic resin composition, comprising: Vinyl aromatic hydrocarbon resin (a), block copolymer (b), and Donor-acceptor system molecular compound (c), in, The block copolymer (b) is a block copolymer comprising a vinyl aromatic hydrocarbon monomer unit and a conjugated diene monomer unit, and has a polymer block mainly composed of the vinyl aromatic hydrocarbon monomer unit, wherein the vinyl aromatic hydrocarbon monomer unit accounts for 30% to 90% by mass, and the conjugated diene monomer unit accounts for 70% to 10% by mass. When the total amount of the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b) is 100 mass %, the mass ratio of the vinyl aromatic hydrocarbon resin (a) is 81 mass % or less, and the mass ratio of the block copolymer (b) is 19 mass % or more and less than 100 mass %, When the total amount of the vinyl aromatic hydrocarbon resin (a), the block copolymer (b) and the donor-acceptor molecular compound (c) is 100 mass %, the content of the donor-acceptor molecular compound (c) is 0.5 mass % or more and 5 mass % or less, The surface resistivity is 1×10 12 Ω / □ or less.
4. The antistatic resin composition according to claim 3, wherein The vinyl aromatic hydrocarbon resin (a) is any one selected from the group consisting of a homopolymer (a1) of a vinyl aromatic hydrocarbon monomer, a graft copolymer (a2) of a vinyl aromatic hydrocarbon monomer, and a random copolymer (a3) of a vinyl aromatic hydrocarbon monomer unit and a (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer unit.
5. The antistatic resin composition according to claim 3, wherein In the melt flow rate MFR under 200°C and 5 kg load conditions specified in ISO 1133, the relationship between the MFR (MFRa) of the vinyl aromatic hydrocarbon resin (a) and the MFR (MFRb) of the block copolymer (b) satisfies any one of the following conditions (i) to (iv), <Condition (i)> When the total of the components (a) and (b) is 100% by mass, the component (a) is greater than 0% by mass and less than 30% by mass, and the component (b) is 70% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the components (a), (b) and (c) is 100% by mass, the component (c) is 0.5% by mass or more and less than 5% by mass; <Condition (ii)> When the total of the component (a) and the component (b) is 100% by mass, when the component (a) is more than 30% by mass and 50% by mass or less, and the component (b) is less than 70% by mass and 50% by mass or more, when satisfying the relationship of MFRa < MFRb (Formula 1), when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 0.5% by mass or more and 5% by mass or less. When satisfying the relationship of MFRa ≥ MFRb (Formula 2), when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 0.9% by mass or more and 5% by mass or less; <Condition (iii)> When the total of the component (a) and the component (b) is 100% by mass, when the component (a) is more than 50% by mass and 70% by mass or less, and the component (b) is less than 50% by mass and 30% by mass or more, satisfying the relationship of MFRa < MFRb (Formula 1), when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 0.9% by mass or more and 5% by mass or less; <Condition (iv)> When the total of the component (a) and the component (b) is 100% by mass, when the component (a) is more than 70% by mass and 81% by mass or less, and the component (b) is less than 30% by mass and 19% by mass or more, satisfying the relationship of MFRa < MFRb (Formula 1), when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 3% by mass or more and 5% by mass or less.
6. The antistatic resin composition according to claim 4, wherein In the melt flow rate MFR under the conditions of 200 °C and 5 kg load specified by ISO 1133, the relationship between MFRa, which is the MFR of the vinyl aromatic hydrocarbon resin (a), and MFRb, which is the MFR of the block copolymer (b), satisfies any one of the following (i) to (iv): <Condition (i)> When the total of the component (a) and the component (b) is 100% by mass, when the component (a) is more than 0% by mass and 30% by mass or less, and the component (b) is 70% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 0.5% by mass or more and 5% by mass or less; <Condition (ii)> When the total of the component (a) and the component (b) is 100% by mass, when the component (a) is more than 30% by mass and 50% by mass or less, and the component (b) is less than 70% by mass and 50% by mass or more, when satisfying When the relationship of MFRa < MFRb (Formula 1) is satisfied, when the total of the (a) component, the (b) component, and the (c) component is 100% by mass, the (c) component is 0.5% by mass or more and 5% by mass or less, and when satisfying When the relationship of MFRa ≥ MFRb (Formula 2) is satisfied, when the total of the (a) component, the (b) component, and the (c) component is 100% by mass, the (c) component is 0.9% by mass or more and 5% by mass or less; <Condition (iii)> When, when the total of the (a) component and the (b) component is 100% by mass, the (a) component is more than 50% by mass and 70% by mass or less, and the (b) component is less than 50% by mass and 30% by mass or more, the relationship of MFRa < MFRb (Formula 1) is satisfied, and when the total of the (a) component, the (b) component, and the (c) component is 100% by mass, the (c) component is 0.9% by mass or more and 5% by mass or less; <Condition (iv)> When, when the total of the (a) component and the (b) component is 100% by mass, the (a) component is more than 70% by mass and 81% by mass or less, and the (b) component is less than 30% by mass and 19% by mass or more, the relationship of MFRa < MFRb (Formula 1) is satisfied, and when the total of the (a) component, the (b) component, and the (c) component is 100% by mass, the (c) component is 3% by mass or more and 5% by mass or less.
7. The antistatic resin composition according to claim 4, wherein In the melt flow rate MFR under the conditions of 200 °C · 5 kg load specified by ISO 1133, the relationship between the MFR of the random copolymer (a3) of the vinyl aromatic hydrocarbon monomer unit and the (meth)acrylic acid and / or (meth)acrylic acid alkyl ester monomer unit, that is, MFRa, and the MFR of the block copolymer (b), that is, MFRb, satisfies the following condition (v) or (vi), <Condition (v)> When, when the total of the (a3) component and the (b) component is 100% by mass, the (a3) component is more than 0% by mass and 20% by mass or less, and the (b) component is 80% by mass or more and less than 100% by mass, regardless of the values of MFRa and MFRb, when the total of the (a3) component, the (b) component, and the (c) component is 100% by mass, (c) is 0.5% by mass or more and 5% by mass or less; <Condition (vi)> When, when the total of the (a3) component and the (b) component is 100% by mass, the (a3) component is more than 20% by mass and 50% by mass or less, and the (b) component is less than 80% by mass and 50% by mass or more, satisfying The relationship of MFRa < MFRb (Formula 1), and when the total of the (a3) component, the (b) component, and the (c) component is 100% by mass, the (c) component is 3% by mass or more and 5% by mass or less.
8. The antistatic resin composition according to any one of claims 1 to 7, wherein The donor-acceptor system molecular compound (c) is represented by the following general formula (1), [Chemical formula 1] In formula (1), R1 and R2 are each independently CH3(CH2) n -CO-OCH2 or HOCH2, and at least one of them is CH3(CH2) n -CO-OCH3, wherein n is an integer from 12 to 22, R3 and R4 are each independently selected from the group consisting of CH3, C2H5, HOCH2, HOC2H4, and HOCH2CH(CH3), Here, "δ+" in the general formula (1) indicates the presence of polarity in the covalent bond within the molecule, (+) indicates that the oxygen atom has a strong electron-donating property, (-) indicates that the boron atom has a strong electron-withdrawing property, "→" indicates a path through which electrons are attracted, and "---" indicates a state in which the bonding force between atoms is weakened.
9. The antistatic resin composition according to any one of claims 1 to 7, wherein The surface resistivity is 5×10 11 Ω / □ or less.
10. The antistatic resin composition according to claim 5 or 6, wherein In the condition (iv), when the total of the component (a), the component (b), and the component (c) is 100% by mass, the component (c) is 3.5% by mass to 5% by mass.
11. The antistatic resin composition according to claim 7, wherein In the condition (v), when the total of the component (a3), the component (b) and the component (c) is 100% by mass, the component (c) is 1% by mass to 5% by mass; In the condition (vi), when the total of the component (a3), the component (b), and the component (c) is 100% by mass, the component (c) is 3.5% by mass to 5% by mass.
12. The antistatic resin composition according to any one of claims 1 to 7, wherein The haze value measured in accordance with ISO14782 using a 1 mm thick flat plate produced by injection molding the antistatic resin composition was 4.0% or less.
13. A method for producing an antistatic resin composition, which is the method for producing an antistatic resin composition according to claim 1 or 2, comprising the following steps: Step (I), using a block copolymer (b) and a donor-acceptor system molecular compound (c), when the total amount of the masterbatch is 100 mass%, melt-kneading with a composition ratio of the donor-acceptor system molecular compound (c) of 5 mass% to 20 mass%, thereby producing a masterbatch; and In step (II), the masterbatch is diluted by kneading the masterbatch with the block copolymer (b).
14. A method for producing an antistatic resin composition, which is the method for producing an antistatic resin composition according to any one of claims 3 to 12, comprising the following steps: Step (I), using a block copolymer (b) and a donor-acceptor system molecular compound (c), when the total amount of the masterbatch is 100 mass%, melt-kneading with a composition ratio of the donor-acceptor system molecular compound (c) of 5 mass% to 20 mass%, thereby producing a masterbatch; and In step (II), the masterbatch is diluted by kneading the masterbatch with the vinyl aromatic hydrocarbon resin (a) or by kneading the masterbatch with the vinyl aromatic hydrocarbon resin (a) and the block copolymer (b). 15 . An electronic component packaging material, which is a molded product of the antistatic resin composition according to claim 1 .