Chloroprene copolymer latex and method for producing the same, sulfide, and dip-molded article and method for producing the same

By adjusting the toluene insoluble content and the modulus of sulfide elongation in the chloroprene copolymer latex, and adopting a low-temperature and short-time vulcanization method, the problems of high vulcanization costs and allergic reactions in the existing technology are solved, and high mechanical properties are achieved. Characteristic chloroprene impregnated molded body.

CN113840850BActive Publication Date: 2024-10-25DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202080037029.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-05
Filing Date
2020-06-30
Publication Date
2024-10-25
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

In the existing technology, in order to improve the mechanical properties of chloroprene-impregnated molded bodies, high temperature or long-term vulcanization is required, but this will increase production costs and time, and the use of vulcanization accelerators may cause allergic reactions such as dermatitis, leading to Mechanical properties are reduced without the use of accelerators.

Method used

By adjusting the toluene insoluble content and the elongation modulus of the sulfide in the chloroprene copolymer latex, a low-temperature (100°C) short-time (30 minutes) vulcanization method can be used without using a vulcanization accelerator. Obtain excellent breaking strength and elongation at break.

Benefits of technology

It is realized that without the use of vulcanization accelerators, the chloroprene copolymer latex vulcanized at low temperature and for a short time can achieve the same or better mechanical properties as those using accelerators, reducing production costs and avoiding the risk of allergic reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003361637690000171
    Figure BDA0003361637690000171
  • Figure BDA0003361637690000172
    Figure BDA0003361637690000172
Patent Text Reader

Abstract

A chloroprene copolymer latex comprising a chloroprene copolymer having a structural unit derived from chloroprene and a structural unit derived from 2,3-dichloro-1,3-butadiene, wherein the toluene-insoluble matter content of the chloroprene copolymer is 50 to 95% by mass, and a film obtained by immersing a substrate in the chloroprene copolymer latex and vulcanizing it at 100° C. for 30 minutes on the substrate has a modulus of 4.0 MPa or less at 500% elongation in accordance with JIS K 6251.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a chloroprene copolymer latex and a method for producing the same, a sulfide, a dip-molded body and a method for producing the same, and the like. Background Art

[0002] Chloroprene polymers are known as materials for dip-molded articles such as medical surgical gloves, examination gloves, industrial gloves, balloons, catheters, and rubber boots.

[0003] Various techniques have been proposed relating to chloroprene polymers for impregnation of molded articles.

[0004] Patent Document 1 described below describes a latex composition comprising: a chloroprene polymer latex obtained by copolymerizing 2,3-dichloro-1,3-butadiene and sulfur at a specific ratio; a metal oxide; a vulcanization accelerator; and an antioxidant.

[0005] Patent Document 2 described below describes a rubber composition comprising a chloroprene polymer latex having a specific amount of tetrahydrofuran-insoluble matter, a metal oxide, an antioxidant, a surfactant, and a pH adjuster, and containing no vulcanization accelerator.

[0006] Patent Document 3 described below describes a polychloroprene latex containing a modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, water, an emulsifier, and potassium ions.

[0007] Patent Document 4 listed below describes a mercaptan-modified polychloroprene latex containing a copolymer of chloroprene and a specific copolymerization amount of 2,3-dichloro-1,3-butadiene.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2019-044116

[0011] Patent Document 2: International Publication No. 2016 / 166998

[0012] Patent Document 3: Japanese Patent Application Publication No. 2014-114342

[0013] Patent Document 4: International Publication No. 2019 / 009038 Summary of the invention

[0014] Problems to be solved by the invention

[0015] For the film of the impregnated molded body, it is required to improve the breaking strength and elongation at break as mechanical properties. In contrast, in the prior art, due to the insufficient adjustment of the polymer structure, it is necessary to improve the mechanical properties by performing high temperature or long-term vulcanization, but from the viewpoint of improving productivity and reducing costs, it is required to reduce the temperature and shorten the time of vulcanization. In this case, for example, in order to shorten the time of vulcanization, it is considered to use a vulcanization accelerator, but with respect to the vulcanization accelerator, there is a tendency to become an allergen (cause substance) of type IV allergy that causes skin diseases such as dermatitis, so it is required to reduce or not use the vulcanization accelerator. However, in the prior art, in order to make up for the reduction of mechanical properties caused by not using a vulcanization accelerator, a long-term vulcanization is required. In view of the above situation, it is necessary to obtain a sulfide with excellent breaking strength and elongation at break even when vulcanization is performed at low temperature and in a short time without using a vulcanization accelerator.

[0016] One aspect of the present invention aims to provide a chloroprene copolymer latex which can produce a vulcanizate having excellent breaking strength and breaking elongation even when vulcanization is performed at low temperature and in a short time (100° C., 30 minutes) without using a vulcanization accelerator. Another aspect of the present invention aims to provide a vulcanizate of the chloroprene copolymer latex, a dip-molded body of the chloroprene copolymer latex, and a method for producing the same. Another aspect of the present invention aims to provide a method for producing the chloroprene copolymer latex.

[0017] Means for solving problems

[0018] The inventors of the present application have found that the above-mentioned problems can be solved by adjusting the toluene-insoluble content in a chloroprene copolymer latex containing a chloroprene copolymer having a structural unit derived from chloroprene and a structural unit derived from 2,3-dichloro-1,3-butadiene, and by adjusting the modulus at 500% elongation of a predetermined vulcanized product provided by the chloroprene copolymer latex.

[0019] One aspect of the present invention provides a chloroprene copolymer latex, comprising a chloroprene copolymer having a structural unit derived from chloroprene and a structural unit derived from 2,3-dichloro-1,3-butadiene, wherein the chloroprene copolymer has a toluene-insoluble matter content of 50 to 95% by mass, and a film obtained on a substrate by immersing the substrate in the chloroprene copolymer latex and then vulcanizing the film at 100° C. for 30 minutes has a modulus at 500% elongation in accordance with JIS K 6251 of 4.0 MPa or less.

[0020] By using such a chloroprene copolymer latex, even when vulcanization is performed at a low temperature and in a short time (100° C., 30 minutes) without using a vulcanization accelerator, a vulcanized product having excellent breaking strength and breaking elongation can be obtained.

[0021] Another aspect of the present invention provides a sulfide of the above-mentioned chloroprene copolymer latex. Another aspect of the present invention provides a dip-molded body of the above-mentioned chloroprene copolymer latex. Another aspect of the present invention provides a method for producing a dip-molded body comprising the step of dip-molding the above-mentioned chloroprene copolymer latex.

[0022] Another aspect of the present invention provides a method for obtaining the above-mentioned chloroprene copolymer latex, comprising a polymerization step of emulsion-polymerizing chloroprene and 2,3-dichloro-1,3-butadiene until the polymerization conversion rate reaches 60 to 95%, wherein in the above-mentioned polymerization step, the amount of 2,3-dichloro-1,3-butadiene is more than 0 part by mass and is 35 parts by mass or less based on 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene.

[0023] According to the method for producing a chloroprene copolymer latex, a chloroprene copolymer latex can be obtained which can produce a vulcanized product having excellent breaking strength and breaking elongation even when vulcanization is performed at a low temperature and for a short time (100° C., 30 minutes) without using a vulcanization accelerator.

[0024] Effects of the Invention

[0025] According to one aspect of the present invention, there is provided a chloroprene copolymer latex which can produce a vulcanizate having excellent breaking strength and breaking elongation even when vulcanization is performed at low temperature and in a short time (100° C., 30 minutes) without using a vulcanization accelerator. According to another aspect of the present invention, there is provided a vulcanizate of the chloroprene copolymer latex, a dip-molded body of the chloroprene copolymer latex, and a method for producing the same. According to another aspect of the present invention, there is provided a method for producing the chloroprene copolymer latex. DETAILED DESCRIPTION

[0026] Hereinafter, the mode for implementing the present invention will be described in detail. It should be noted that the present invention is not limited to the embodiment described below.

[0027] In this specification, the numerical range represented by "~" means a range including the numerical values ​​recorded before and after "~" as the minimum and maximum values, respectively. "Above A" in the numerical range refers to A, and a range exceeding A. "Below A" in the numerical range refers to A, and a range less than A. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of other stages. In the numerical ranges recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the values ​​shown in the embodiments. The so-called "A or B" includes either A and B, or both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. With respect to the content of each component in the composition, when there are multiple substances belonging to each component in the composition, unless otherwise specified, it refers to the total amount of the multiple substances present in the composition. The term "film" includes not only the structure of the shape formed on the entire surface when observed in the form of a top view, but also the structure of the shape formed on a part. The term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes as long as the desired effect of the process can be achieved. "(Meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. "JIS" refers to Japanese Industrial Standards.

[0028] <Chloroprene copolymer latex>

[0029] The chloroprene copolymer latex involved in the present embodiment contains the following chloroprene copolymer, and the chloroprene copolymer has a structural unit derived from chloroprene (2-chloro-1,3-butadiene) and a structural unit derived from 2,3-dichloro-1,3-butadiene. The chloroprene copolymer is a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene. The toluene insoluble content in the chloroprene copolymer is 50 to 95% by mass. The substrate is immersed in the chloroprene copolymer latex involved in the present embodiment and vulcanized at 100°C for 30 minutes to obtain a film on the substrate having a modulus of 4.0 MPa or less at 500% elongation in accordance with JIS K 6251.

[0030] According to the chloroprene copolymer latex involved in this embodiment, even when vulcanization is performed at low temperature and short time (100°C, 30 minutes) without using a vulcanization accelerator, a sulfide having excellent breaking strength and breaking elongation can be obtained, and such a sulfide can be obtained in the form of a dip molded film. According to the chloroprene copolymer latex involved in this embodiment, a breaking strength of 18 MPa or more (for example, 18 to 25 MPa) can be obtained, and an elongation at break of 1000% or more (for example, 1000 to 1500%) can be obtained. According to the chloroprene copolymer latex involved in this embodiment, when the chloroprene copolymer latex contains sulfur, zinc oxide, a butylation reaction product of p-cresol and dicyclopentadiene, and a sodium salt of β-naphthalenesulfonic acid formaldehyde condensate, even when vulcanization is performed at low temperature and short time (100°C, 30 minutes) without using a vulcanization accelerator, a sulfide having excellent breaking strength and breaking elongation can be obtained.

[0031] According to the chloroprene copolymer latex involved in the present embodiment, by vulcanization under milder conditions (100°C, 30 minutes) than before, it is possible to achieve increased productivity and reduced costs. By using the chloroprene copolymer latex involved in the present embodiment, it is possible to obtain a sulfide having excellent breaking strength and elongation at break while controlling the use of allergens of type IV allergies. By using the chloroprene copolymer latex involved in the present embodiment, it is possible to obtain mechanical properties equal to or better than those of sulfides obtained from conventional chloroprene copolymer latexes without using a vulcanization accelerator. By using the chloroprene copolymer latex involved in the present embodiment, it is possible to obtain a sulfide having excellent breaking strength and elongation at break even when a vulcanization accelerator is used.

[0032] The content of the structural unit derived from chloroprene in the chloroprene copolymer contained in the chloroprene copolymer latex is more than 0% by mass and less than 100% by mass, preferably in the following range, based on the total amount of the structural unit derived from chloroprene and the structural unit derived from 2,3-dichloro-1,3-butadiene contained in the chloroprene copolymer or the total amount of the structural unit contained in the chloroprene copolymer. From the viewpoint that the sulfide is easy to obtain excellent breaking strength and elongation at break, the content of the structural unit derived from chloroprene is preferably 99% by mass or less, more preferably 97% by mass or less, and further preferably 96% by mass or less. From the viewpoint that the sulfide is easy to obtain excellent breaking strength and elongation at break, the content of the structural unit derived from chloroprene is preferably 65% ​​by mass or more, more preferably 68% by mass or more, and further preferably 70% by mass or more. From the above viewpoints, the content of the structural unit derived from chloroprene is preferably 65 to 99% by mass, more preferably 65 to 96% by mass. The content of the structural unit derived from chloroprene may be 95% by mass or less, 93% by mass or less, less than 93% by mass, 91% by mass or less, less than 91% by mass, 90% by mass or less, 88% by mass or less, 85% by mass or less, 82% by mass or less, 80% by mass or less, less than 80% by mass, 78% by mass or less, 76% by mass or less, less than 76% by mass, 75% by mass or less, 72% by mass or less, or 71% by mass or less. The content of the structural unit derived from chloroprene may be more than 70% by mass, 71% by mass or more, 72% by mass or more, 75% by mass or more, 76% by mass or more, more than 76% by mass, 78% by mass or more, 80% by mass or more, more than 80% by mass, 82% by mass or more, 85% by mass or more, 88% by mass or more, 90% by mass or more, 91% by mass or more, more than 91% by mass, 93% by mass or more, more than 93% by mass, or 95% by mass or more.

[0033] The content of the structural unit derived from 2,3-dichloro-1,3-butadiene in the chloroprene copolymer contained in the chloroprene copolymer latex (the copolymerization amount of 2,3-dichloro-1,3-butadiene) is more than 0% by mass and less than 100% by mass, preferably in the following range, based on the total amount of the structural unit derived from chloroprene and the structural unit derived from 2,3-dichloro-1,3-butadiene contained in the chloroprene copolymer or the total amount of the structural unit contained in the chloroprene copolymer. From the viewpoint that the sulfide is easy to obtain excellent breaking strength and elongation at break, the content of the structural unit derived from 2,3-dichloro-1,3-butadiene is preferably 1% by mass or more, more preferably 3% by mass or more, and further preferably 4% by mass or more. From the viewpoint that the sulfide is easy to obtain excellent breaking strength and elongation at break, the content of the structural unit derived from 2,3-dichloro-1,3-butadiene is preferably 35% by mass or less, more preferably 32% by mass or less, and further preferably 30% by mass or less. From the above viewpoints, the content of the structural unit derived from 2,3-dichloro-1,3-butadiene is preferably 1 to 35% by mass, and more preferably 4 to 35% by mass. The content of the structural unit derived from 2,3-dichloro-1,3-butadiene may be 5% by mass or more, 7% by mass or more, more than 7% by mass, 9% by mass or more, more than 9% by mass, 10% by mass or more, 12% by mass or more, 15% by mass or more, 18% by mass or more, 20% by mass or more, more than 20% by mass, 22% by mass or more, 24% by mass or more, more than 24% by mass, 25% by mass or more, 28% by mass or more, or 29% by mass or more. The content of structural units derived from 2,3-dichloro-1,3-butadiene may be less than 30% by mass, 29% by mass or less, 28% by mass or less, 25% by mass or less, 24% by mass or less, less than 24% by mass, 22% by mass or less, 20% by mass or less, less than 20% by mass, 18% by mass or less, 15% by mass or less, 12% by mass or less, 10% by mass or less, 9% by mass or less, less than 9% by mass, 7% by mass or less, less than 7% by mass, or 5% by mass or less.

[0034] The chloroprene copolymer may have a structural unit derived from a monomer other than chloroprene and 2,3-dichloro-1,3-butadiene, and may be a copolymer of three or more monomers including chloroprene and 2,3-dichloro-1,3-butadiene. Examples of such monomers include acrylic acid esters (methyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, etc.), methacrylic acid esters (methyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, etc.), (meth)acrylic acid hydroxy esters (2-hydroxyethyl (meth)acrylate, 2-hydroxymethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, etc. The chloroprene copolymer may have a structural unit derived from a carboxyl group-containing vinyl monomer (e.g., methacrylic acid), or may not have a structural unit derived from a carboxyl group-containing vinyl monomer (e.g., methacrylic acid). The content of the structural unit derived from the carboxyl group-containing vinyl monomer (eg, methacrylic acid) may be less than 0.5% by mass based on the total amount of the chloroprene copolymer.

[0035] The toluene insoluble content (content of components insoluble in toluene at 23° C.) in the chloroprene copolymer contained in the chloroprene copolymer latex according to the present embodiment is 50 to 95% by mass based on the total amount of the chloroprene copolymer. When the toluene insoluble content is less than 50% by mass or exceeds 95% by mass, the breaking strength of the sulfide is impaired.

[0036] From the viewpoint that the sulfide is easy to obtain excellent breaking strength and elongation at break, the toluene insoluble content in the chloroprene copolymer is preferably 52% by mass or more, more preferably 55% by mass or more, and further preferably 57% by mass or more. The toluene insoluble content in the chloroprene copolymer can be 59% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, more than 70% by mass, 75% by mass or more, 80% by mass or more, 85% by mass or more, more than 85% by mass, 86% by mass or more, 88% by mass or more, 89% by mass or more, 90% by mass or more, 91% by mass or more, or 93% by mass or more. From the viewpoint that the sulfide (e.g., film-like sulfide) is easy to obtain excellent flexibility, the toluene insoluble content in the chloroprene copolymer is preferably less than 95% by mass, and more preferably 93% by mass or less. The toluene insoluble content in the chloroprene copolymer may be 91% by mass or less, 90% by mass or less, 89% by mass or less, 88% by mass or less, 86% by mass or less, 85% by mass or less, less than 85% by mass, 80% by mass or less, 75% by mass or less, 70% by mass or less, less than 70% by mass, 65% by mass or less, 60% by mass or less, 59% by mass or less, or 57% by mass or less. The toluene insoluble content in the chloroprene copolymer may be adjusted by the polymerization conversion during polymerization, the type and amount of the chain transfer agent, etc.

[0037] The "toluene insoluble content" can be measured by the following steps. First, a chloroprene copolymer obtained by freeze-drying a chloroprene copolymer latex is dissolved in toluene at 23°C to obtain a solution. The solution is centrifuged and then the gel component is separated using a 200-mesh metal mesh. The gel component is dried to obtain a dried product, and the mass of the dried product is measured to obtain the toluene insoluble content.

[0038] It is preferred that the chloroprene copolymer included in the chloroprene copolymer latex according to the present embodiment provides a peak derived from abietic acid in the gas chromatography of an extract (extract component) extracted from the chloroprene copolymer using an ethanol / toluene azeotropic mixture (ETA). In this case, a sulfide (e.g., a dip molded film) having better mechanical properties (e.g., breaking strength) can be obtained. As described later, whether the chloroprene copolymer has a peak derived from abietic acid depends on the type of rosin acids added as an emulsifier.

[0039] The peak derived from abietic acid can be measured by the following steps. First, a chloroprene copolymer obtained by freeze-drying a chloroprene copolymer latex is cut to obtain a test piece. The test piece is placed in an eggplant-shaped flask with a condenser, and an extract (rosin acids, etc.) is extracted using an ethanol / toluene azeotropic mixture (ETA) specified in JIS K 6229. The extract is measured by gas chromatography using a gas chromatograph, so that the peak derived from abietic acid can be confirmed.

[0040] The chloroprene copolymer latex according to the present embodiment may contain a vulcanizing agent. Examples of the vulcanizing agent include sulfur, zinc oxide, and magnesium oxide.

[0041] The chloroprene copolymer latex involved in this embodiment may contain a vulcanization accelerator or may not contain a vulcanization accelerator. Examples of the vulcanization accelerator include diethyl disulfide carbamate zinc, dibutyl disulfide carbamate zinc, dibutyl disulfide carbamate sodium disulfide carbamate and other disulfide carbamate salt-based vulcanization accelerators; ethylene thiourea, diethyl thiourea, trimethyl thiourea, triethyl thiourea, N,N'-diphenyl thiourea, N,N'-diethyl thiourea and other thiourea-based vulcanization accelerators; 1,3-diphenylguanidine and other guanidine-based vulcanization accelerators; tetramethylthiuram disulfide, tetraethylthiuram disulfide and other thiuram-based vulcanization accelerators; thiazole-based vulcanization accelerators; xanthogenic acid-based vulcanization accelerators, etc. The chloroprene copolymer latex according to the present embodiment may contain at least one selected from the group consisting of disulfide carbamate vulcanization accelerators, thiourea vulcanization accelerators, guanidine vulcanization accelerators, thiuram vulcanization accelerators, thiazole vulcanization accelerators, and xanthate vulcanization accelerators. Even if the chloroprene copolymer latex according to the present embodiment does not contain a vulcanization accelerator, a vulcanized product having excellent mechanical properties can be obtained.

[0042] The chloroprene copolymer latex according to the present embodiment may contain additives such as surfactants, freezing stabilizers, emulsion stabilizers, viscosity modifiers, antioxidants, preservatives, etc. The content of the surfactant may be less than 0.1 parts by mass relative to 100 parts by mass of the chloroprene copolymer.

[0043] In the chloroprene copolymer latex according to the present embodiment, from the viewpoint of obtaining excellent elongation at break of the sulfide, the modulus at 500% elongation in accordance with JIS K 6251 (modulus at 500% elongation measured in accordance with JIS K 6251) of the following film (sulfide) obtained on the substrate by immersing the substrate (for example, immersing for 10 seconds) in the chloroprene copolymer latex and vulcanizing at 100° C. for 30 minutes is 4.0 MPa or less. From the viewpoint of easily obtaining excellent elongation at break of the sulfide, the modulus at 500% elongation is preferably 3.5 MPa or less, more preferably 3.0 MPa or less, further preferably 2.5 MPa or less, particularly preferably 2.0 MPa or less, extremely preferably 1.8 MPa or less, and very preferably 1.5 MPa or less. The modulus at 500% elongation may be 1.4 MPa or less, 1.3 MPa or less, or 1.2 MPa or less. The modulus at 500% elongation can be 0.3 MPa or more, 0.5 MPa or more, 0.7 MPa or more, 0.8 MPa or more, 1.0 MPa or more, 1.2 MPa or more, 1.3 MPa or more, 1.4 MPa or more, or 1.5 MPa or more. From the above viewpoints, the modulus at 500% elongation can be 0.1-4.0 MPa, 0.1-2.0 MPa, or 0.7-1.2 MPa. The modulus at 500% elongation can be. The modulus at 500% elongation can be adjusted by the type and amount of monomers, the polymerization conversion rate during polymerization, the polymerization temperature, etc.

[0044] In the chloroprene copolymer latex according to the present embodiment, the modulus at 100% elongation in accordance with JIS K6251 (modulus at 100% elongation measured in accordance with JIS K 6251) of the following film (sulfide) obtained on the substrate by immersing the substrate (for example, immersing for 10 seconds) in the chloroprene copolymer latex and vulcanizing at 100° C. for 30 minutes is preferably in the following range. From the viewpoint that the sulfide is easy to obtain excellent elongation at break, the modulus at 100% elongation is preferably 1.5 MPa or less, more preferably 1.2 MPa or less, further preferably 1.0 MPa or less, and particularly preferably 0.9 MPa or less. The modulus at 100% elongation may be 0.8 MPa or less, or 0.7 MPa or less. The modulus at 100% elongation can be 0.1 MPa or more, 0.3 MPa or more, 0.5 MPa or more, 0.7 MPa or more, 0.8 MPa or more, or 0.9 MPa or more. From the above viewpoints, the modulus at 100% elongation can be 0.1 to 1.5 MPa, 0.1 to 1.2 MPa, or 0.5 to 1.2 MPa. The modulus at 100% elongation can be adjusted by the type and amount of monomers, the polymerization conversion rate during polymerization, the polymerization temperature, etc.

[0045] The film providing the above-mentioned modulus during elongation can be obtained by the following method: after immersing the substrate in chloroprene copolymer latex, washing with running water at 45°C for 1 minute, and vulcanizing at 100°C for 30 minutes. The temperature of the chloroprene copolymer latex when the substrate is immersed can be 23°C. The film providing the above-mentioned modulus during elongation can be obtained by immersing the substrate in a coagulation liquid (e.g., 23°C) (e.g., immersing for 1 second) and then immersing the substrate in chloroprene copolymer latex. As the coagulation liquid, for example, a coagulation liquid obtained by mixing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate and 3 parts by mass of calcium carbonate can be used. The substrate can be, for example, a ceramic cylinder having an outer diameter of 50 mm.

[0046] <Method for producing chloroprene copolymer latex>

[0047] The method for producing a chloroprene copolymer latex according to the present embodiment is a method for producing a chloroprene copolymer latex according to the present embodiment. The method for producing a chloroprene copolymer latex according to the present embodiment includes a polymerization step of emulsion-polymerizing chloroprene and 2,3-dichloro-1,3-butadiene until the polymerization conversion rate reaches 60 to 95%, wherein in the polymerization step, the amount of 2,3-dichloro-1,3-butadiene exceeds 0 parts by mass and is 35 parts by mass or less relative to 100 parts by mass of the total amount of chloroprene and 2,3-dichloro-1,3-butadiene.

[0048] The amount of 2,3-dichloro-1,3-butadiene added before the start of emulsion polymerization in the polymerization step exceeds 0 parts by mass, preferably within the following range, based on 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene or the total amount of monomers used to obtain the chloroprene copolymer. From the viewpoint that the sulfide (e.g., film-like sulfide) easily obtains excellent flexibility, the amount of 2,3-dichloro-1,3-butadiene added is preferably 1 part by mass or more, more preferably 3 parts by mass or more, further preferably 4 parts by mass or more, and particularly preferably 5 parts by mass or more. From the viewpoint that the sulfide easily obtains excellent breaking strength and breaking elongation, the amount of 2,3-dichloro-1,3-butadiene added is preferably 32 parts by mass or less, more preferably 30 parts by mass or less. From the above viewpoints, the amount of 2,3-dichloro-1,3-butadiene added is preferably more than 0 parts by mass and 32 parts by mass or less, and more preferably 5 to 30 parts by mass. The amount of 2,3-dichloro-1,3-butadiene added may be 7 parts by mass or more, more than 7 parts by mass, 9 parts by mass or more, more than 9 parts by mass, 10 parts by mass or more, 12 parts by mass or more, 15 parts by mass or more, 18 parts by mass or more, 20 parts by mass or more, more than 20 parts by mass, 22 parts by mass or more, 24 parts by mass or more, more than 24 parts by mass, 25 parts by mass or more, 28 parts by mass or more, 29 parts by mass or more, or 30 parts by mass or more. The amount of 2,3-dichloro-1,3-butadiene added may be 29 parts by mass or less, 28 parts by mass or less, 25 parts by mass or less, 24 parts by mass or less, less than 24 parts by mass, 22 parts by mass or less, 20 parts by mass or less, less than 20 parts by mass, 18 parts by mass or less, 15 parts by mass or less, 12 parts by mass or less, 10 parts by mass or less, 9 parts by mass or less, less than 9 parts by mass, 7 parts by mass or less, less than 7 parts by mass, or 5 parts by mass or less.

[0049] The polymerization temperature in the polymerization step (polymerization temperature of emulsion polymerization) is preferably in the following range. From the viewpoint that the sulfide can easily obtain a suitable modulus during elongation, the polymerization temperature is preferably 10°C or more, more preferably 12°C or more, and further preferably 15°C or more. From the viewpoint that the sulfide can easily obtain excellent breaking strength, the polymerization temperature is preferably less than 30°C, more preferably 25°C or less, and further preferably 23°C or less. From the above viewpoints, the polymerization temperature is preferably 10°C or more and less than 30°C, and more preferably 10 to 25°C.

[0050] During emulsion polymerization, a chain transfer agent may be used. The chain transfer agent is not particularly limited, and examples thereof include long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan; dialkyl xanthate disulfides such as diisopropyl xanthate and diethyl xanthate; and triiodomethane. As the chain transfer agent, a known chain transfer agent commonly used in emulsion polymerization of chloroprene may be used.

[0051] As for the amount of chain transfer agent added before the start of emulsion polymerization, the type and amount can be adjusted in such a way that the toluene insoluble content after the completion of polymerization becomes 50 to 95% by mass. In addition to the type and amount of the chain transfer agent, the toluene insoluble content is also affected by the polymerization conversion rate, so it is preferred to appropriately adjust the type and amount of the chain transfer agent, the polymerization conversion rate, etc. to adjust the toluene insoluble content. As an example, by adding 0.14 parts by mass of diisopropyl xanthate disulfide to 100 parts by mass of a total of chloroprene and 2,3-dichloro-1,3-butadiene, and polymerizing until the polymerization conversion rate is 60 to 95% (for example, about 90%), a chloroprene copolymer latex with a suitable toluene insoluble content can be obtained.

[0052] As the emulsifier used in the emulsion polymerization, rosin acids are suitable, and rosin acids that give a peak derived from abietic acid are preferred. Examples of rosin acids that give a peak derived from abietic acid include undisproportionated raw rosin acid and the like.

[0053] Other commonly used emulsifiers and / or fatty acids may also be used. Other emulsifiers include metal salts of aromatic sulfinic acid formaldehyde condensates (e.g., sodium salt of β-naphthalenesulfonic acid formaldehyde condensates), sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, sodium alkyl diphenyl ether sulfonate, potassium alkyl diphenyl ether sulfonate, sodium polyoxyethylene alkyl ether sulfonate, sodium polyoxypropylene alkyl ether sulfonate, potassium polyoxyethylene alkyl ether sulfonate, potassium polyoxypropylene alkyl ether sulfonate, and the like.

[0054] The pH of the aqueous emulsion at the start of emulsion polymerization is preferably 10.5 to 13.5. The so-called aqueous emulsion refers to a mixed solution containing a chain transfer agent, chloroprene, 2,3-dichloro-1,3-butadiene, etc. just before the start of emulsion polymerization, and also includes the following situation: the composition is changed by subsequent addition or batch addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or more, the polymerization reaction can be more stably controlled. When the pH is below 13.5, the excessive increase in viscosity during the polymerization process can be suppressed, thereby more stably controlling the polymerization reaction.

[0055] Examples of the polymerization initiator include potassium persulfate, benzoyl peroxide, ammonium persulfate, and hydrogen peroxide, which are generally used in radical polymerization.

[0056] The polymerization conversion rate in the polymerization process is 60 to 95%. The polymerization reaction can be stopped by adding a polymerization inhibitor. When the polymerization conversion rate is 60% or more, the reduction in the toluene insoluble content is suppressed, the fracture strength of the sulfide (such as an immersion molded film) is suppressed, and the cost increase can be avoided. From the viewpoint that the sulfide is easy to obtain excellent fracture strength, the polymerization conversion rate is preferably 63% or more, more preferably 65% ​​or more, and further preferably 67% or more. The polymerization conversion rate can be 70% or more, 75% or more, 80% or more, 85% or more, 86% or more, 88% or more, 89% or more, 90% or more, 92% or more, or 93% or more. When the polymerization conversion rate is 95% or less, the reduction in polymerization reactivity caused by the reduction of unreacted monomers can be suppressed, the reduction in productivity can be avoided, and the sulfide (such as an immersion molded film) can obtain excellent fracture strength. From the viewpoint that the sulfide is easy to obtain excellent fracture strength, the polymerization conversion rate is preferably 93% or less. The polymerization conversion rate may be 92% or less, 90% or less, 89% or less, 88% or less, 86% or less, 85% or less, 80% or less, 75% or less, 70% or less, 67% or less, or 65% or less.

[0057] Examples of the polymerization inhibitor include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, and a butylation product of p-cresol and dicyclopentadiene. Unreacted monomers after completion of the emulsion polymerization can be removed by a conventional method such as reduced pressure distillation.

[0058] In the method for producing the chloroprene copolymer latex according to the present embodiment, a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, and the like may be optionally added after the polymerization.

[0059] <Sulfide, impregnation molded body and their production methods>

[0060] The sulfide involved in the present embodiment is a sulfide of the chloroprene copolymer latex involved in the present embodiment, and is obtained by vulcanizing the chloroprene copolymer latex involved in the present embodiment. The method for manufacturing the sulfide involved in the present embodiment includes a step of vulcanizing the chloroprene copolymer latex involved in the present embodiment to obtain the sulfide. The sulfide involved in the present embodiment can be film-shaped. The thickness (e.g., minimum thickness) of the film-shaped sulfide can be 0.01 to 0.5 mm, 0.1 to 0.5 mm, 0.1 to 0.3 mm, or 0.1 to 0.2 mm.

[0061] The dip molded body involved in the present embodiment is the dip molded body of the chloroprene copolymer latex involved in the present embodiment. The dip molded body involved in the present embodiment is the dip molded body obtained by using the chloroprene copolymer latex involved in the present embodiment, and is obtained by dip molding the chloroprene copolymer latex involved in the present embodiment. The manufacturing method of the dip molded body involved in the present embodiment includes the step of dip molding the chloroprene copolymer latex involved in the present embodiment. As a molding method when manufacturing the dip molded body involved in the present embodiment, for example, a coagulation liquid impregnation method can be cited, but it is not limited to this, and molding can be performed in a conventional manner. The dip molded body involved in the present embodiment can be a dip molded film formed on a substrate. The sulfide and the dip molded body involved in the present embodiment have excellent mechanical properties such as breaking strength and elongation at break. The dip molded body involved in the present embodiment can be a molded body of the sulfide involved in the present embodiment. The dip molded body involved in the present embodiment is preferably a glove, a balloon, a catheter or a boot.

[0062] The sulfide and the impregnation molded body involved in this embodiment may contain a vulcanizing agent and / or a vulcanization accelerator, or may not contain a vulcanizing agent and / or a vulcanization accelerator. Whether to mix a vulcanizing agent and / or a vulcanization accelerator can be determined according to the target sulfide and impregnation molded body. As the vulcanizing agent and the vulcanization accelerator, for example, the vulcanizing agent and the vulcanization accelerator exemplified above can be used.

[0063] Example

[0064] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0065] <Production of Chloroprene Polymer Latex>

[0066] (Example 1)

[0067] In a polymerization tank having an internal volume of 40 liters, 95 parts by mass of chloroprene monomer, 5 parts by mass of 2,3-dichloro-1,3-butadiene monomer, 0.14 parts by mass of diisopropyl xanthate disulfide, 100 parts by mass of pure water, 4.8 parts by mass of tallsen rosin (undisproportionated raw rosin acid, manufactured by HARIMA CHEMICALS, INC.), 1.50 parts by mass of potassium hydroxide, and 0.40 parts by mass of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (trade name "DEMOL N", manufactured by Kao Corporation) were added. The pH of the aqueous emulsion before the start of polymerization was 12.8. As a polymerization initiator, 0.1 parts by mass of potassium persulfate was added, and polymerization was carried out at a polymerization temperature of 15° C. under a nitrogen flow. At the time point when the polymerization conversion rate reached 89%, diethylhydroxylamine was added as a polymerization inhibitor to stop the polymerization, thereby obtaining a latex. The latex was distilled under reduced pressure to remove unreacted monomers, thereby obtaining a chloroprene polymer latex having a solid content concentration of 60% by mass.

[0068] (Examples 2 to 10 and Comparative Examples 1 to 6)

[0069] A chloroprene polymer latex was obtained in the same manner as in Example 1 except that the conditions (polymerization components, feed amounts, polymerization temperature, polymerization conversion, etc.) were changed to those shown in Tables 1 and 2 below. In Example 10, potassium disproportionate rosinate (trade name "RONDIS K-25", manufactured by Arakawa Chemical Industries, Ltd.) was used.

[0070] <Copolymerization Amount of 2,3-Dichloro-1,3-butadiene>

[0071] 3 g of the chloroprene polymer obtained by freeze-drying the chloroprene polymer latex was cut into 2 mm cubes to obtain test pieces. The copolymerization amount of 2,3-dichloro-1,3-butadiene in the test piece (base: the total amount of the structural unit derived from chloroprene and the structural unit derived from 2,3-dichloro-1,3-butadiene) was measured using a pyrolysis gas chromatograph (a device with a trade name "PY-3030D" manufactured by Frontier Laboratories Ltd. installed on a trade name "JMS-Q1050GC" manufactured by JEOL Ltd.). The results are shown in Tables 1 and 2.

[0072] <Measurement of abietic acid peak>

[0073] 3 g of the chloroprene polymer obtained by freeze-drying the above-mentioned chloroprene polymer latex was cut into 2 mm square cubes to obtain test pieces. The test piece was placed in an eggplant-shaped flask with a condenser, and an extract (rosin acids) was extracted using an ethanol / toluene azeotropic mixture (ETA) specified in JIS K6229. The extract was measured using a gas chromatograph (trade name "GC-2010 Plus", manufactured by Shimadzu Corporation) under the following measurement conditions. In the gas chromatograph, it was confirmed whether the chloroprene polymer had a peak (peak top) derived from abietic acid. The results are shown in Tables 1 and 2.

[0074] [Gas chromatography measurement conditions]

[0075] Column used: FFAP (Film thickness 0.3μm)

[0076] Column temperature: 200℃→250℃

[0077] Heating rate: 10℃ / min

[0078] Inlet temperature: 270℃

[0079] Detector temperature: 270℃

[0080] Injection volume: 2μL

[0081] <Determination of Toluene Insoluble Content>

[0082] 1 g of the chloroprene polymer obtained by freeze-drying the above-mentioned chloroprene polymer latex was cut into 2 mm square cubes to obtain test pieces. After the test piece was placed in a conical beaker, it was dissolved in toluene at 23°C for 16 hours to obtain a solution. After the solution was centrifuged (14000 rpm, 10 minutes), the gel component was separated using a 200-mesh metal mesh. The gel component was dried to obtain a dry product, and then the mass of the dry product was measured to obtain the toluene insoluble content. The results are shown in Tables 1 and 2.

[0083] <Preparation of Evaluation Samples>

[0084] (Preparation of Chloroprene Polymer Latex Composition)

[0085] 5.1 parts by mass of the aqueous dispersion described below were mixed with the above-mentioned chloroprene polymer latex (100 parts by mass as solid content. Hereinafter, "part by mass" means the amount relative to 100 parts by mass of the solid content of the chloroprene polymer latex), and then pure water was added to adjust the solid content concentration of the entire composition to 30% by mass, thereby preparing a chloroprene polymer latex composition. The aqueous dispersion was prepared by mixing 1 part by mass of sulfur, 2 types of zinc oxide (trade name "Zinc Oxide 2", manufactured by Sakai Chemical Industry Co., Ltd.), 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "NOCRACK PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formaldehyde condensate (trade name "DEMOL N", manufactured by Kao Corporation) and 13 parts by mass of pure water at 20° C. for 16 hours using a ceramic ball mill.

[0086] (Production of sulfur film)

[0087] A ceramic cylinder with an outer diameter of 50 mm was immersed in a coagulation solution (23° C.) obtained by mixing 62 parts by mass of pure water, 35 parts by mass of potassium nitrate tetrahydrate and 3 parts by mass of calcium carbonate for 1 second, and then taken out. After drying for 4 minutes, the above-mentioned cylinder was immersed in the above-mentioned chloroprene polymer latex composition at 23° C. for 10 seconds. Then, it was washed with running water at 45° C. for 1 minute, and then vulcanized at 100° C. for 30 minutes, thereby preparing a vulcanized film (evaluation sample) on the outer peripheral surface of the cylinder. The vulcanized film was peeled off from the outer peripheral surface of the cylinder, and the following evaluation was performed.

[0088] <Evaluation>

[0089] The thickness (film thickness) of the vulcanized film was measured at three locations in the center of the vulcanized film using a test piece thickness gauge (trade name "ASKER SDA-12", manufactured by Kobunsu Keiki Co., Ltd.), and the minimum thickness was determined as the thickness of the vulcanized film.

[0090] The vulcanized film was measured for modulus at 100% elongation, modulus at 500% elongation, breaking strength, and breaking elongation in accordance with JIS K 6251. The results are shown in Tables 1 and 2.

[0091] [Table 1]

[0092]

[0093] [Table 2]

[0094]

[0095] As can be seen from Tables 1 and 2, Examples 1 to 10 are excellent in mechanical properties such as breaking strength and breaking elongation. Comparison between Example 2 and Example 10 confirmed that the chloroprene copolymer provided a peak derived from abietic acid and that the use of undisproportionated raw rosin acid improved the breaking strength.

[0096] In Comparative Example 1, 2,3-dichloro-1,3-butadiene was not copolymerized, and the modulus at 500% elongation exceeded 4.0 MPa, so the elongation at break was poor. In Comparative Example 2, the modulus at 500% elongation exceeded 4.0 MPa, so the elongation at break was poor. In Comparative Examples 3 and 4, the toluene insoluble content in the chloroprene copolymer was less than 50% by mass, so the breaking strength was poor. In Comparative Examples 5 and 6, the toluene insoluble content in the chloroprene copolymer exceeded 95% by mass, so the breaking strength was poor.

Claims

1. A chloroprene copolymer latex comprising a chloroprene copolymer having a structural unit derived from chloroprene and a structural unit derived from 2,3-dichloro-1,3-butadiene, The toluene insoluble matter content of the chloroprene copolymer is 86 to 95% by mass. The modulus of a film obtained on the substrate by immersing the substrate in the chloroprene copolymer latex and then vulcanizing the film at 100° C. for 30 minutes is 3.5 MPa or less at 500% elongation in accordance with JIS K 6251.

2. The chloroprene copolymer latex according to claim 1, wherein The modulus of the film at 100% elongation in accordance with JIS K 6251 is 0.5 to 1.2 MPa.

3. The chloroprene copolymer latex according to claim 1 or 2, wherein In gas chromatography of an extract obtained by extraction from the chloroprene copolymer using an ethanol / toluene azeotropic mixture, the chloroprene copolymer provides a peak derived from abietic acid.

4. The chloroprene copolymer latex according to claim 1 or 2, wherein The content of the structural unit derived from 2,3-dichloro-1,3-butadiene is more than 0% by mass and not more than 35% by mass based on the total amount of the structural unit derived from chloroprene and the structural unit derived from 2,3-dichloro-1,3-butadiene.

5. The chloroprene copolymer latex according to claim 1 or 2, which does not contain a vulcanization accelerator. 6 . A sulfide of the chloroprene copolymer latex according to claim 1 .

7. A dip-molded article, which is a dip-molded article of the chloroprene copolymer latex according to any one of claims 1 to 5.

8. The dip-molded article according to claim 7, which is a glove, a balloon, a catheter or a boot.

9. A method for producing a dip-molded article, comprising the step of dip-molding the chloroprene copolymer latex according to any one of claims 1 to 5.

10. A method for producing the chloroprene copolymer latex according to any one of claims 1 to 5, The method comprises a polymerization step of emulsion-polymerizing chloroprene and 2,3-dichloro-1,3-butadiene until the polymerization conversion rate reaches 60 to 95%. In the polymerization step, the amount of 2,3-dichloro-1,3-butadiene is more than 0 parts by mass and not more than 35 parts by mass based on 100 parts by mass of the total of chloroprene and 2,3-dichloro-1,3-butadiene.

Citation Information

Patent Citations

  • Polychloroprene latex, polychloroprene latex composition, and dip molded product

    JP2014114342A

  • Chloroprene copolymer latex composition and its compact

    JP2019044116A

  • Composition for rubber and use thereof

    WO2016166998A1

  • Mercaptane-modified polychloroprene latex and production method therefor

    WO2019009038A1

  • Chloroprene polymer latex composition for manufacturing vulcanized rubber and manufacturing method of the same

    JP2009108195A