Cutting Tools
By forming a specific coating layer on the cutting tool, the tool's crack resistance, wear resistance and peel resistance of the alumina layer are improved, and the problem of shortening the tool life under high speed and high efficiency is solved, so as to achieve Longer service life.
Patent Information
- Application Number
- CN202080041426.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-04-10
AI Technical Summary
In the high-speed and high-efficiency cutting processing, the increase in load leads to a shorter life, making it difficult to meet the needs of improving crack resistance, wear resistance and peel resistance.
The coating layer consisting of a titanium carbonitride layer, an intermediate layer (composed of titanium, carbon, oxygen and nitrogen) and an alumina layer is formed by chemical vapor deposition method. The ratio of carbon atoms at the interface between the intermediate layer and the alumina layer is set. Set it as PC1/PC2≥1.03, the nitrogen atom ratio is set to PN1/PN2≥0.9, and the oxygen atom ratio PO1/PO2≥0.9 is optimized to improve tolerance.
The crack resistance, wear resistance and peel resistance of the cutting tool are significantly improved, and the service life of the tool is extended.
Smart Images

Figure CN113905842B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to cutting tools. Background Art
[0002] Cutting tools coated with a coating on a substrate have been used for a long time. For example, Japanese Patent Publication No. 09-174304 (Patent Document 1) discloses a cutting tool made of a surface-coated cemented carbide with excellent chipping resistance, wherein a hard coating layer is formed on the surface of a tungsten carbide-based cemented carbide substrate with an average layer thickness of 5 to 20 μm, and the hard coating layer is composed of an inner layer made of a single layer or a composite layer of two or more of a titanium carbide layer, a titanium nitride layer, and a titanium carbonitride layer, an intermediate layer made of a titanium oxycarbide layer and / or a titanium oxycarbonitride layer, and an outer layer made of an aluminum oxide layer, characterized in that the interface portion of the intermediate layer and the aluminum oxide layer as the outer layer is a sharp needle-shaped crystal structure.
[0003] In addition, Japanese Patent Gazette No. 2009-166216 (Patent Document 2) discloses a coated tool, wherein a single-layer film or a multilayer film of any one of carbides, nitrides, carbonitrides, oxides, carbon oxides, nitrogen oxides and carbonitride oxides of metal elements selected from Groups 4a, 5a, and 6a of the periodic table is formed on the surface of a substrate, and an α-type aluminum oxide film is formed on the upper layer of the film via a bonding film, characterized in that: the surface shape of the bonding film at the interface between the bonding film and the α-type aluminum oxide film has a tree branch shape composed of dendritic protrusions and branch-like protrusions connected thereto, and when the length (nm) of the dendritic protrusion is set to LB, 5≤LB≤200, and through observation under a transmission electron microscope, the interface between the dendritic protrusion and the α-type aluminum oxide film has a continuous lattice pattern.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 09-174304
[0007] Patent Document 2: Japanese Patent Application Publication No. 2009-166216 Summary of the invention
[0008] The cutting tool disclosed herein comprises a substrate and a coating layer disposed on the substrate, wherein:
[0009] The coating layer is composed of a titanium carbonitride layer provided on the substrate, an intermediate layer provided on the titanium carbonitride layer, and an aluminum oxide layer provided on the intermediate layer.
[0010] The intermediate layer is composed of a compound of titanium, carbon, oxygen and nitrogen.
[0011] The thickness of the intermediate layer exceeds 1 μm,
[0012] When the atomic ratio of carbon at the interface between the intermediate layer and the aluminum oxide layer is set to P C1 atomic %, and the atomic ratio of the carbon at a position A on the intermediate layer side 1 μm away from the interface is defined as P C2 At% P C1 Relative to P C2 The ratio of P C1 / P C2 It is above 1.03. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] [ Figure 1 ] Figure 1 A perspective view illustrating one embodiment of a base material of a cutting tool.
[0014] [ Figure 2 ] Figure 2 This is a schematic cross-sectional view of a cutting tool according to one form of the present embodiment.
[0015] [ Figure 3 ] Figure 3 This is a schematic cross-sectional view of another type of cutting tool according to the present embodiment.
[0016] [ Figure 4 ] Figure 4 This is a schematic cross-sectional view of a covering layer according to one form of the present embodiment.
[0017] [ Figure 5 ] Figure 5 This is a schematic cross-sectional view showing an example of a chemical vapor deposition apparatus used for manufacturing a coating film.
[0018] [ Figure 6 ] Figure 6 This is a photograph for explaining the line analysis method in a coating layer cross section.
[0019] [ Figure 7 ] Figure 7 To illustrate the use of AES Figure 6 A graph showing the results of line analysis of the coating layer cross section. DETAILED DESCRIPTION
[0020] [Problems to be Solved by the Present Disclosure]
[0021] In Patent Documents 1 and 2, by providing a coating having the above-described structure, adhesion between the aluminum oxide layer and other layers in contact with the aluminum oxide layer is improved, and thus it can be expected that the life of the cutting tool can be extended.
[0022] However, in recent years, with the development of high speed and high efficiency in cutting processing, the load imposed on the cutting tool has increased, and the life of the cutting tool tends to be shortened. Therefore, it is necessary to further improve the mechanical properties of the coating of the cutting tool (for example, peeling resistance, wear resistance, cracking resistance, etc.).
[0023] The present disclosure has been made in view of the above circumstances, and an object of the present invention is to provide a cutting tool having improved chipping resistance.
[0024] [Effects of the present disclosure]
[0025] According to the present disclosure, it is possible to provide a cutting tool having improved chipping resistance.
[0026] [Description of Embodiments of the Present Disclosure]
[0027] First, embodiments of the present disclosure are listed and described.
[0028] [1] The cutting tool disclosed herein comprises a substrate and a coating layer provided on the substrate, wherein:
[0029] The coating layer is composed of a titanium carbonitride layer provided on the substrate, an intermediate layer provided on the titanium carbonitride layer, and an aluminum oxide layer provided on the intermediate layer.
[0030] The intermediate layer is composed of a compound of titanium, carbon, oxygen and nitrogen.
[0031] The thickness of the intermediate layer exceeds 1 μm,
[0032] When the atomic ratio of carbon at the interface between the intermediate layer and the aluminum oxide layer is set to P C1 atomic %, and the atomic ratio of the carbon at a position A on the intermediate layer side 1 μm away from the interface is defined as P C2 At% P C1 Relative to P C2 The ratio of P C1 / P C2 It is above 1.03.
[0033] The above-mentioned cutting tool has the above-mentioned structure, so that the chipping resistance is improved. Here, "chipping resistance" refers to the resistance to the formation of micro-cracks in the coating film including the coating layer when used for cutting.
[0034] [2] The above P C1 It is preferably 25 atomic % or more and 65 atomic % or less. By setting it in this way, the chipping resistance can be further improved.
[0035] [3] When the atomic ratio of nitrogen at the interface is PN1 atomic %, and the atomic ratio of the nitrogen at the position A is P N2 At% P N1 Relative to P N2 The ratio of P N1 / P N2 It is preferably 0.9 or more and less than 1. By such a regulation, in addition to the chipping resistance, the peeling resistance of the aluminum oxide layer is also improved. Here, "peeling resistance of the aluminum oxide layer" refers to the resistance of the aluminum oxide layer to peeling from the intermediate layer of the cutting tool when used for cutting.
[0036] [4] When the atomic ratio of oxygen at the interface is P O1 atomic %, and the atomic ratio of the oxygen at the position A is P O2 At% P O1 Relative to P O2 The ratio of P O1 / P O2 It is preferably 0.9 or more and less than 1. By defining it in this way, in addition to chipping resistance, wear resistance is also improved. Here, "wear resistance" refers to the resistance to wear of the film including the coating layer when used for cutting.
[0037] [5] The thickness of the intermediate layer is preferably greater than 1 μm and less than 3 μm. By setting this specification, the chipping resistance is further improved.
[0038] [6] It is preferable to further provide a base layer between the substrate and the coating layer. By such a provision, in addition to chipping resistance, adhesion between the substrate and the coating layer is also improved.
[0039] [7] It is preferable to further provide a surface layer on the coating layer. By adopting such a provision, a cutting tool having excellent wear resistance in addition to chipping resistance can be provided.
[0040] [Details of the embodiments of the present disclosure]
[0041] Hereinafter, an embodiment of the present disclosure (hereinafter referred to as "this embodiment") is described. However, this embodiment is not limited thereto. In this specification, expressions in the form of "X to Z" refer to the upper and lower limits of a range (i.e., greater than X and less than Z). When no unit is recorded in X and only the unit is recorded in Z, the unit of X is the same as the unit of Z. In addition, in this specification, when a compound is represented by a chemical formula that does not limit the composition ratio of the constituent elements, such as "TiC", the chemical formula includes all the composition ratios (element ratios) known in the art. At this time, the above chemical formula includes not only the stoichiometric composition but also the non-stoichiometric composition. For example, in the chemical formula of "TiC", not only the stoichiometric composition "Ti1C1" is included, but also (for example) "Ti1C 0.8 " This is a non-stoichiometric composition. The same applies to the description of compounds other than "TiC".
[0042] Cutting Tools
[0043] The cutting tool disclosed herein comprises a substrate and a coating layer disposed on the substrate, wherein:
[0044] The coating layer is composed of a titanium carbonitride layer provided on the substrate, an intermediate layer provided on the titanium carbonitride layer, and an aluminum oxide layer provided on the intermediate layer.
[0045] The intermediate layer is composed of a compound of titanium, carbon, oxygen and nitrogen.
[0046] The thickness of the intermediate layer exceeds 1 μm,
[0047] When the atomic ratio of carbon at the interface between the intermediate layer and the aluminum oxide layer is set to P C1 atomic %, and the atomic ratio of the carbon at a position A on the intermediate layer side 1 μm away from the interface is defined as P C2 At% P C1 Relative to P C2 The ratio of P C1 / P C2 It is above 1.03.
[0048] The cutting tool 50 of the present embodiment includes a substrate 10 and a coating layer 40 (hereinafter sometimes simply referred to as a “cutting tool”) provided on the substrate 10. Figure 2 In addition to the coating layer 40, the cutting tool 50 may further include a base layer 23 ( Figure 3 The cutting tool 50 may further include a surface layer 24 ( Figure 3). Other layers such as the base layer 23 and the surface layer 24 will be described later.
[0049] It should be noted that the above-mentioned layers provided on the above-mentioned substrate 10 are sometimes collectively referred to as "coatings". That is, the above-mentioned cutting tool 50 has a coating 45 provided on the above-mentioned substrate 10, and the above-mentioned coating 45 includes the above-mentioned coating layer 40. In addition, the above-mentioned coating 45 may also include the above-mentioned base layer 23 or the above-mentioned surface layer 24.
[0050] The cutting tool (hereinafter sometimes simply referred to as “cutting tool”) 50 of the present embodiment includes a substrate 10 and a coating 45 (see Figure 2 , Figure 3 In one aspect of the present embodiment, the coating may cover the front cutting surface of the substrate, or may cover a portion other than the front cutting surface (e.g., the back cutting surface). The cutting tool may be, for example, a drill, an end mill, a replaceable cutting insert for a drill, a replaceable cutting insert for an end mill, a replaceable cutting insert for milling, a replaceable cutting insert for turning, a metal saw, a gear cutting tool, a reamer, a tap, etc.
[0051] <Base material>
[0052] The substrate of the present embodiment can use any substrate as long as it is a known material as such a substrate. For example, the substrate preferably includes at least one of the group consisting of cemented carbide (e.g., tungsten carbide (WC)-based cemented carbide, cemented carbide containing Co in addition to WC, cemented carbide with carbonitrides of Cr, Ti, Ta, Nb, etc. added in addition to WC, etc.), cermet (with TiC, TiN, TiCN, etc. as main components), high-speed steel, ceramic (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, etc.), cubic boron nitride sintered body (cBN sintered body) and diamond sintered body, and more preferably includes at least one of the group consisting of cemented carbide, cermet and cBN sintered body.
[0053] Among these various types of substrates, WC-based cemented carbide or cBN sintered body is particularly preferably selected because these substrates have a particularly excellent balance between hardness and strength at high temperatures and have excellent characteristics as substrates for cutting tools for the above-mentioned purposes.
[0054] When using cemented carbide as substrate, even if free carbon or an abnormal phase called η phase is included in the texture of such cemented carbide, the effect of the present embodiment can be shown. It should be noted that the surface of the substrate used in the present embodiment can be modified. For example, when it is cemented carbide, a de-β layer can be formed on its surface, or when it is a cBN sintered body, a surface hardening layer can be formed, and even if the surface is modified in this way, the effect of the present embodiment can be shown.
[0055] Figure 1 A perspective view showing one mode of a substrate for a cutting tool as an example. A substrate of this shape is used as a substrate for a replaceable cutting blade for (for example) turning. The substrate 10 has a front cutting face 1, a back cutting face 2, and a cutting edge ridge portion 3 at the intersection of the front cutting face 1 and the back cutting face 2. That is, the front cutting face 1 and the back cutting face 2 are surfaces connected by sandwiching the cutting edge ridge portion 3. The cutting edge ridge portion 3 constitutes the front end portion of the cutting edge of the substrate 10. The shape of this substrate 10 can also be understood as the shape of the above-mentioned cutting tool.
[0056] When the cutting tool is a cutting insert with replaceable cutting edges, the substrate 10 may include a shape with a chip breaker or a shape without a chip breaker. The shape of the cutting edge ridgeline portion 3 may include any of the following shapes: a sharp edge (a ridge formed by the intersection of the front cutting edge and the back cutting edge), a honed edge (a shape obtained by rounding a sharp edge), a negative land (a chamfered shape), or a shape obtained by combining a honed edge and a negative land.
[0057] Above, use Figure 1 The shape of the substrate 10 and the names of the various parts have been described, but in the cutting tool 50 involved in this embodiment, the same terms as above are used for the shapes and names of the various parts corresponding to the above substrate 10. That is, the above cutting tool has a rake face, a flank face, and a cutting edge ridge connecting the above rake face and the above flank face.
[0058] <Lamination>
[0059] The coating 45 according to the present embodiment includes a coating layer 40 (see Figure 2 ). The "film" has the function of improving the various properties of the cutting tool, such as chipping resistance, wear resistance, and peeling resistance, by covering at least a portion of the above-mentioned substrate (for example, the front cutting face that contacts the cut material during cutting). The above-mentioned film is not limited to covering a portion of the above-mentioned substrate, but preferably covers the entire surface of the above-mentioned substrate. However, even if a portion of the above-mentioned substrate is not covered by the above-mentioned film, or the composition of the film is partially different, this does not deviate from the scope of the present embodiment.
[0060] The thickness of the above-mentioned film is preferably 7 μm to 30 μm, more preferably 7 μm to 25 μm. Here, the thickness of the film refers to the sum of the thicknesses of the layers constituting the film. As "layers constituting the film", for example, there can be listed: the coating layer (titanium carbonitride layer, intermediate layer, aluminum oxide layer), base layer and surface layer described later. The thickness of the above-mentioned film (for example) can be obtained by measuring any 10 points in the cross-section sample in the normal direction parallel to the surface of the substrate using a scanning transmission electron microscope (STEM), and obtaining the average value of the thickness of the 10 measured points. The same is true when measuring the thickness of each of the coating layers (titanium carbonitride layer, intermediate layer, aluminum oxide layer), base layer and surface layer described later. As a scanning transmission electron microscope, for example, JEM-2100F (trade name) manufactured by JEOL Ltd. can be listed.
[0061] (Coating layer)
[0062] The coating layer in this embodiment is disposed on the above-mentioned substrate. Here, "disposed on the substrate" means: not limited to being disposed directly above the substrate (see Figure 2 ), and also includes a method of being provided on a substrate via other layers (refer to Figure 3 ). That is, as long as the effect of the present disclosure can be exerted, the coating layer can be arranged directly above the substrate, or can be arranged on the substrate via other layers such as the base layer described later. Other layers such as the surface layer can also be arranged on the coating layer. In addition, the coating layer can be the outermost surface of the coating.
[0063] The coating layer 40 is composed of a titanium carbonitride layer 20 provided on the substrate 10, an intermediate layer 21 provided on the titanium carbonitride layer 20, and an aluminum oxide layer 22 provided on the intermediate layer 21 (see Figure 2 ).
[0064] The thickness of the coating layer is preferably 7 μm to 30 μm, more preferably 7 μm to 25 μm. The thickness of the coating layer can be confirmed by observing the vertical cross-section of the substrate and the coating using STEM in the same manner as described above. The titanium carbonitride layer, the intermediate layer, and the aluminum oxide layer constituting the coating layer are described below.
[0065] (Titanium Carbonitride Layer)
[0066] The titanium carbonitride layer 20 involved in this embodiment is arranged on the above-mentioned substrate 10. The above-mentioned titanium carbonitride layer can be composed of titanium carbonitride (TiCN) alone, or it can be composed of titanium carbonitride and inevitable impurities. As the above-mentioned inevitable impurities, for example, oxygen, chlorine, etc. can be listed. The thickness of the titanium carbonitride layer is preferably 3 μm to 20 μm, and more preferably 3 μm to 15 μm. The thickness of the titanium carbonitride layer can be confirmed by observing the vertical section of the substrate and the coating using STEM in the same way as above.
[0067] (Middle layer)
[0068] The intermediate layer 21 involved in this embodiment is attached to the above-mentioned titanium carbonitride layer 20 and is provided. The above-mentioned intermediate layer is composed of a compound composed of titanium, carbon, oxygen and nitrogen. As the compound, for example, titanium carbonitride oxide (TiCNO) and the like can be listed. In one aspect of this embodiment, the intermediate layer is preferably composed of TiCNO. It should be noted that the above-mentioned intermediate layer can be composed only of a compound composed of titanium, carbon, oxygen and nitrogen, or it can be composed of the compound and inevitable impurities. As the above-mentioned inevitable impurities, for example, chlorine and the like can be listed.
[0069] The thickness of the intermediate layer exceeds 1 μm, preferably exceeds 1 μm and is 3 μm or less, and more preferably is 1.1 μm or more and 2 μm or less. The thickness of the intermediate layer can be confirmed by observing the vertical cross section of the substrate and the coating using STEM in the same manner as above.
[0070] (Aluminum oxide layer)
[0071] The aluminum oxide layer 22 in this embodiment is attached to the above-mentioned intermediate layer 21 and is provided. The above-mentioned aluminum oxide layer may be composed of aluminum oxide (Al2O3) alone, or may be composed of aluminum oxide and inevitable impurities. As the above-mentioned inevitable impurities, for example, chlorine, sulfur, etc. may be listed. The above-mentioned aluminum oxide is preferably α-type aluminum oxide (α-Al2O3). The thickness of the aluminum oxide layer is preferably 3 μm to 20 μm, and more preferably 3 μm to 15 μm. The thickness of the aluminum oxide layer can be confirmed by observing the vertical section of the substrate and the coating using STEM in the same way as above.
[0072] (Atomic Ratio of Carbon in the Vicinity of the Interface between the Intermediate Layer and the Aluminum Oxide Layer)
[0073] In this embodiment, when the atomic ratio of the carbon at the interface between the intermediate layer and the aluminum oxide layer is P C1 atomic %, and the atomic ratio of the carbon at a position A on the intermediate layer side 1 μm away from the interface is defined as P C2 At% P C1 Relative to PC2 The ratio of P C1 / P C2 is 1.03 or more, preferably 1.03 or more and 1.1 or less, more preferably 1.04 or more and 1.09 or less, and further preferably 1.05 or more and 1.08 or less. C1 and P C2 It is the atomic ratio based on the sum of titanium, carbon, oxygen and nitrogen.
[0074] In the intermediate layer having the above-mentioned structure, carbon atoms are unevenly present near the interface between the intermediate layer and the aluminum oxide layer. Therefore, the toughness of the intermediate layer near the interface between the intermediate layer and the aluminum oxide layer is improved. As a result, the inventors believe that the chipping resistance is improved.
[0075] The atomic ratio of carbon can be obtained by performing line analysis of the cross-section sample parallel to the normal direction of the substrate surface by Auger electron spectroscopy (AES method). Specifically, first, the cut surface of the cross-section sample is ground by cross-section polishing (CP processing) or the like. The ground cut surface is analyzed using a field emission scanning microscope (FE-SEM) to obtain Figure 6 The cross-sectional SEM image of the coating layer is shown in FIG. The measurement magnification at this time is 50,000 times. Figure 6 In the cross-sectional SEM image, the coated layer is placed horizontally, the intermediate layer is observed as a dark area, and the aluminum oxide layer is observed as a bright area. Next, in the field of view of the cross-sectional SEM image, from the titanium carbonitride layer side toward the aluminum oxide layer side in a direction parallel to the stacking direction of the intermediate layer ( Figure 6 The cut surface after the above grinding is analyzed by AES method in the direction of the white arrow in the figure and along the black line). The measurement spacing at this time is 0.016 μm. In addition, other measurement conditions of the AES method are as follows. As a measurement device of the AES method, for example, PHI700 (trade name) manufactured by Albuck Fischer Co., Ltd. can be cited.
[0076] (Measurement conditions of AES method)
[0077] Measurement acceleration voltage: 10kV
[0078] Measuring current: 10mA
[0079] Sample tilt angle: 30°
[0080] Sputtering voltage: 1kV
[0081] Figure 7 An example of a graph showing the results obtained by performing the above-mentioned line analysis is shown in FIG. Figure 7 In , the X-axis (horizontal axis) represents the distance from the measurement starting point. Figure 7In the graph, the Y axis (vertical axis) represents the atomic ratio (atomic %) of each element of the measurement object. It should be noted that there is oxygen ( Figure 7 O Ti ) and oxygen from the aluminum oxide layer ( Figure 7 O Al ), but by using a standard spectrum to perform waveform separation processing on the obtained measurement data, the two can be distinguished. Specifically, first, prepare an aluminum ingot with a purity of 99.99% (for example, manufactured by Nikora Corporation) as a standard sample of aluminum. Next, prepare a mixed powder of alumina powder with a purity of 99.99% (for example, manufactured by Ishizu Pharmaceutical Co., Ltd.) and high-purity carbon powder as a standard sample of alumina. At this time, the mixing ratio of the above-mentioned alumina powder and the above-mentioned high-purity carbon powder is set to 1:1 in terms of mass ratio. The two prepared standard samples are spectrally measured using the AES method to obtain their respective standard spectra. Then, using the two obtained standard spectra, waveform separation processing is performed on the measurement spectra at each measurement location represented by the horizontal axis of the above-mentioned measurement data, and the respective atomic ratios of oxygen derived from the intermediate layer and oxygen derived from the aluminum oxide layer are calculated. Next, based on the graph, the position where the atomic ratio of Al is 10 atomic % is set as the "interface between the intermediate layer and the aluminum oxide layer" (refer to Figure 4 , Figure 7 ). In addition, a position 1 μm away from the interface on the intermediate layer side is defined as “position A” (refer to Figure 4 , Figure 7 Then, based on the above graph, the atomic ratio of the carbon at the interface between the intermediate layer and the aluminum oxide layer (P C1 ), and the atomic ratio of the carbon at the position A (P C2 ).
[0082] The above measurement is performed at least three times, and the average value of the atomic ratio of carbon obtained in each measurement is set as the atomic ratio of carbon in the coating layer (P C1 and P C2 The atomic ratio of nitrogen (P N1 and P N2 ), and the atomic ratio of oxygen (P O1 and P O2 ). Here, “the atomic ratio of oxygen” refers to the atomic ratio of oxygen derived from the intermediate layer.
[0083] The above P C1 It is preferably from 25 atomic % to 65 atomic %, more preferably from 35 atomic % to 60 atomic %, and even more preferably from 40 atomic % to 60 atomic %.
[0084] The above P C2It is preferably from 22 atomic % to 63 atomic %, and more preferably from 35 atomic % to 60 atomic %.
[0085] In this embodiment, the pair of B and the imaginary plane P containing the above position A A The atomic ratio of the carbon in the region between the two atoms is not particularly limited.
[0086] For example, when the atomic ratio of the carbon at a position M (not shown) on the intermediate layer side 0.5 μm away from the interface is defined as P C3 At% the above P C3 Can be P C1 Above, can also be P C2 The following can also be P C2 Above P C1 In one aspect of this embodiment, the above-mentioned P C3 Preferably P C2 Above and P C1 With P C2 In another aspect of this embodiment, the above P C3 It is preferably from 25 atomic % to 65 atomic %, more preferably from 35 atomic % to 60 atomic %, and even more preferably from 40 atomic % to 60 atomic %.
[0087] In addition, when the atomic ratio of the carbon at a position M (not shown) on the intermediate layer side 0.5 μm away from the interface is defined as P C3 At% P C3 Relative to P C2 The ratio of P C3 / P C2 It is preferably 0.9 to 1.1, and more preferably 0.95 to 1.05.
[0088] (Atomic Ratio of Nitrogen in the Vicinity of the Interface between the Intermediate Layer and the Aluminum Oxide Layer)
[0089] In this embodiment, when the atomic ratio of the nitrogen at the interface is P N1 atomic %, and the atomic ratio of the nitrogen at the position A is P N2 At% P N1 Relative to P N2 The ratio of P N1 / P N2 It is preferably 0.9 or more and less than 1, and more preferably 0.92 or more and 0.98 or less. N1 and P N2 It is the atomic ratio based on the sum of titanium, carbon, oxygen and nitrogen.
[0090] It is believed that in the intermediate layer having the above-mentioned structure, near the interface between the intermediate layer and the aluminum oxide layer, there is a tendency that the portion with more oxygen atoms and the portion with less oxygen atoms are uneven in the direction perpendicular to the thickness direction of the intermediate layer (in-plane direction). As a result, the inventors believe that in addition to the above-mentioned chipping resistance, the peeling resistance of the aluminum oxide layer is also improved.
[0091] The above P N1 It is preferably 5 atomic % to 35 atomic % and more preferably 10 atomic % to 30 atomic % both inclusive.
[0092] The above P N2 It is preferably 5 atomic % to 35 atomic % and more preferably 10 atomic % to 30 atomic % both inclusive.
[0093] (Atomic Ratio of Oxygen in the Vicinity of the Interface between the Intermediate Layer and the Aluminum Oxide Layer)
[0094] In this embodiment, when the atomic ratio of the oxygen at the interface is P O1 atomic %, and the atomic ratio of the oxygen at the position A is P O2 At% P O1 Relative to P O2 The ratio of P O1 / P O2 It is preferably 0.9 or more and less than 1, and more preferably 0.92 or more and 0.98 or less. O1 and P O2 The atomic ratio is based on the total of titanium, carbon, oxygen and nitrogen. In addition, the "atomic ratio of oxygen" refers to the atomic ratio of oxygen derived from the intermediate layer.
[0095] In the intermediate layer having the above-mentioned structure, near the interface between the intermediate layer and the aluminum oxide layer, there is a tendency that the nitrogen atom-rich portion and the nitrogen atom-poor portion are uneven in the direction perpendicular to the thickness direction of the intermediate layer (in-plane direction). As a result, the inventors believe that in addition to chipping resistance, wear resistance is also improved.
[0096] The above P O1 It is preferably 5 atomic % to 25 atomic % and more preferably 10 atomic % to 20 atomic % both inclusive.
[0097] The above P O2 It is preferably 5 atomic % to 25 atomic % and more preferably 10 atomic % to 20 atomic % both inclusive.
[0098] (basal layer)
[0099] The cutting tool preferably further includes a base layer (see Figure 3 ). The base layer 23 preferably includes TiN. The TiN is preferably a cubic crystal.
[0100] The thickness of the base layer is preferably 0.1 μm to 3 μm, more preferably 0.3 μm to 1 μm. As described above, such thickness can be confirmed by observing the vertical cross section of the substrate and the coating using a scanning transmission electron microscope (STEM) or the like.
[0101] (Surface layer)
[0102] The above-mentioned cutting tool is preferably provided with a surface layer further on the above-mentioned coating layer (see Figure 3 The surface layer 24 preferably includes a compound consisting of titanium and at least one element selected from the group consisting of C, N and B.
[0103] Examples of the compound contained in the surface include TiC, TiN, TiCN, and TiB 2 .
[0104] The thickness of the surface layer is preferably 0.1 μm to 3 μm, more preferably 0.3 μm to 1.5 μm. As described above, such thickness can be confirmed by observing the vertical cross section of the substrate and the coating using a scanning transmission electron microscope (STEM) or the like.
[0105] (Other layers)
[0106] The coating may further include other layers within the scope of not impairing the effect of the cutting tool involved in the present embodiment. The composition of the other layers may be different from or the same as that of the titanium carbonitride layer, the intermediate layer, the aluminum oxide layer, the base layer or the surface layer. Examples of compounds contained in the other layers include TiN, TiCN, TiBN and Al2O3. It should be noted that the stacking order of the other layers is not particularly limited. There is no particular limitation on the thickness of the other layers within the scope of not impairing the effect of the present embodiment, but for example, 0.1 μm to 20 μm may be included.
[0107] 《Manufacturing method of cutting tool》
[0108] The method for manufacturing a cutting tool according to the present embodiment includes:
[0109] a first step of preparing the substrate (hereinafter sometimes referred to as “first step”);
[0110] A second step of forming the titanium carbonitride layer on the substrate by chemical vapor deposition (hereinafter, sometimes referred to as “the second step”);
[0111] A third step (hereinafter sometimes referred to as “the third step”) of forming the intermediate layer just above the titanium carbonitride layer by chemical vapor deposition using a gas containing titanium as a constituent element, a gas containing nitrogen as a constituent element, and a raw material gas containing carbon monoxide gas and methane gas; and
[0112] a fourth step (hereinafter sometimes referred to as “the fourth step”) of forming the aluminum oxide layer just above the intermediate layer by chemical vapor deposition,
[0113] In the third step, the partial pressure ratio P of the methane gas to the gas containing nitrogen as a constituent element is set to CH4 / P N2g As the thickness increases, the above-mentioned intermediate layer is formed.
[0114] <Step 1: Step of preparing a base material>
[0115] In the first step, a substrate is prepared. For example, a cemented carbide substrate is prepared as a substrate. The cemented carbide substrate can be a commercial product or can be manufactured by a conventional powder metallurgy method. When manufactured by a conventional powder metallurgy method, (for example) a ball mill or the like is used to mix WC powder and Co powder to obtain a mixed powder. After drying the mixed powder, it is formed into a predetermined shape to obtain a formed body. Further, the formed body is sintered to obtain a WC-Co based cemented carbide (sintered body). Next, by performing predetermined cutting edge processing such as honing on the sintered body, a substrate made of WC-Co based cemented carbide can be manufactured. In the first step, any substrate other than the above can be prepared, as long as it is an existing known substrate of this type of substrate.
[0116] <Second step: step of forming a titanium carbonitride layer on a substrate>
[0117] In the second step, a titanium carbonitride layer is formed on the substrate by chemical vapor deposition (CVD).
[0118] Figure 5 1 is a schematic cross-sectional view showing an example of a chemical vapor deposition apparatus (CVD apparatus) used in the manufacture of a coating. Figure 5The second step will be described. The CVD device 30 includes: a plurality of substrate fixing jigs 31 for holding the substrate 10, and a reaction vessel 32 made of heat-resistant alloy steel and covering the substrate fixing jigs 31. In addition, a temperature control device 33 for controlling the temperature in the reaction vessel 32 is provided around the reaction vessel 32. The reaction vessel 32 is provided with a gas introduction pipe 35 having a gas introduction port 34. In the internal space of the reaction vessel 32 where the substrate fixing jig 31 is arranged, the gas introduction pipe 35 is arranged in a manner extending in the vertical direction and rotatable about the vertical direction as an axis. In addition, the gas introduction pipe 35 is provided with a plurality of ejection holes 36 for ejecting gas into the reaction vessel 32. Using this CVD device 30, the titanium carbonitride layer and the like constituting the above-mentioned coating layer can be formed as follows.
[0119] First, the substrate 10 is placed on the substrate fixing jig 31, and the temperature and pressure in the reaction container 32 are controlled within a predetermined range. At the same time, the raw material gas for the titanium carbonitride layer is introduced into the reaction container 32 from the gas introduction pipe 35. Thus, the titanium carbonitride layer 20 is formed on the substrate 10. Here, it is preferred that before forming the titanium carbonitride layer 20 (i.e., before the second step), the raw material gas for the base layer is introduced into the reaction container 32 from the gas introduction pipe 35, thereby forming a base layer (for example, a layer containing TiN) on the surface of the substrate 10. Hereinafter, a method of forming the titanium carbonitride layer 20 after forming the base layer on the surface of the substrate 10 will be described.
[0120] The raw material gas for the above-mentioned base layer is not particularly limited, and an example thereof is a mixed gas of TiCl 4 and N 2 .
[0121] The temperature in the reaction container 32 when forming the above-mentioned base layer is preferably controlled at 1000-1100° C. The pressure in the reaction container 32 when forming the above-mentioned base layer is preferably controlled at 0.1-1013 hPa. It should be noted that H2 is preferably used as a carrier gas. In addition, when introducing the gas, it is preferred to rotate the gas introduction pipe 35 by a driving unit not shown in the figure. In this way, each gas can be evenly dispersed in the reaction container 32.
[0122] In addition, the above-mentioned base layer can also be formed by MT (Medium Temperature)-CVD method. Unlike the CVD method (hereinafter also referred to as "HT-CVD method") performed at a temperature of 1000 to 1100°C, the MT-CVD method is a method of forming a layer by maintaining the temperature in the reaction container 32 at a relatively low temperature of 850 to 950°C. Compared with the HT-CVD method, the MT-CVD method is performed at a relatively low temperature, so the damage to the substrate 10 caused by heating can be reduced. In particular, when the above-mentioned base layer is a TiN layer, it is preferably formed by the MT-CVD method.
[0123] Next, the titanium carbonitride layer is formed on the base layer. As a raw material gas, for example, a mixed gas of TiCl4, CH3CN and N2 is used.
[0124] The content of TiCl4 in the raw material gas is preferably 0.8 to 3.0 volume %, more preferably 1.0 to 2.7 volume %, and even more preferably 1.5 to 2.5 volume %. The preferred flow rate of TiCl4 is 1.0 to 2.5 L / min.
[0125] The content of CH3CN in the raw material gas is preferably 0.2 to 1.5 volume %, more preferably 0.3 to 1.2 volume %, and even more preferably 0.5 to 1.0 volume %. The preferred flow rate of CH3CN is 0.5 to 2.0 L / min.
[0126] The content of N2 in the raw material gas is preferably 10 to 30% by volume, more preferably 15 to 28% by volume, and still more preferably 17 to 25% by volume. The preferred flow rate of N2 is 10 to 25 L / min.
[0127] The temperature in the reaction container 32 is preferably controlled at 950 to 1000° C. The pressure in the reaction container 32 is preferably controlled at 50 to 100 hPa. In addition, H 2 may be used as a carrier gas. It should be noted that, similarly to the above, the gas introduction pipe 35 is preferably rotated when introducing the gas.
[0128] In the above-mentioned manufacturing method, the morphology of each layer is changed by controlling various conditions of the CVD method. For example, the composition of each layer is determined by the composition of the raw material gas introduced into the reaction container 32. The thickness of each layer is controlled by the implementation time (film formation time).
[0129] <Third step: step of forming an intermediate layer directly on the titanium carbonitride layer>
[0130] In the third step, the intermediate layer is formed directly on the titanium carbonitride layer by chemical vapor deposition using a gas containing titanium as a constituent element, a gas containing nitrogen as a constituent element, and a raw material gas containing carbon monoxide gas and methane gas.
[0131] As the raw material gas, for example, a mixed gas of TiCl 4 (a gas containing titanium as a constituent element), CH 4 , CO, and N 2 (a gas containing nitrogen as a constituent element) is used.
[0132] The content of TiCl4 in the raw material gas is preferably 0.5 to 2.5 volume %, more preferably 0.7 to 2.0 volume %, and even more preferably 0.8 to 1.5 volume %. The preferred flow rate of TiCl4 is 0.5 to 1.0 L / min.
[0133] The content of CH 4 in the raw material gas is preferably 2.0 to 7.0 volume %, more preferably 2.0 to 6.0 volume %, and even more preferably 2.5 to 4.5 volume %. The preferred flow rate of CH 4 is 1.3 to 3.0 L / min.
[0134] The content of CO in the raw material gas is preferably 0.5 to 3.0% by volume, more preferably 0.7 to 2.5% by volume, and even more preferably 1.0 to 2.0% by volume. The preferred flow rate of CO is 0.6 to 1.5 L / min.
[0135] The content of N2 in the raw material gas is preferably 5 to 30% by volume, more preferably 7 to 25% by volume, and even more preferably 8 to 20% by volume. The preferred flow rate of N2 is 4 to 15 L / min.
[0136] Here, in the third step, it is preferable to set the partial pressure ratio P of the methane gas (CH4) to the gas containing nitrogen as a constituent element (for example, N2) to CH4 / P N2g The above-mentioned intermediate layer is formed while increasing.
[0137] Conventionally, there has been no idea to actively change the partial pressure of the raw material gas during film formation from the viewpoint of reducing production costs, etc. Furthermore, a film having a desired quality can be formed even without changing the partial pressure.
[0138] However, in recent years, with the development of high speed and high efficiency in cutting, the load on the cutting tool has increased, and the life of the cutting tool tends to be shortened. In view of this situation, the inventors have conducted in-depth research and found that when the above-mentioned partial pressure ratio P CH4 / P N2g The above-mentioned intermediate layer is formed while increasing, so that the above-mentioned ratio P C1 / P C2 Set within the predetermined range.
[0139] The partial pressure ratio P at the start of the third step CH4 / P N2g It is preferably 0.1 to 0.6, more preferably 0.2 to 0.5.
[0140] The partial pressure ratio P at the end of the third step CH4 / P N2g It is preferably 0.11 to 0.65, and more preferably 0.2 to 0.5. CH4 / P N2g Of course, it is greater than the partial pressure ratio P at the beginning CH4 / P N2g .
[0141] The temperature in the reaction container 32 is preferably controlled at 920 to 980° C. The pressure in the reaction container 32 is preferably controlled at 50 to 250 hPa. In addition, H 2 can be used as a carrier gas. It should be noted that, similarly to the above, the gas introduction pipe 35 is preferably rotated when introducing the gas.
[0142] <Step 4: Step of forming an aluminum oxide layer directly on the intermediate layer>
[0143] In the fourth step, an aluminum oxide layer is formed directly on the intermediate layer using chemical vapor deposition.
[0144] As the raw material gas, for example, a mixed gas of AlCl 3 , CO 2 , H 2 S and HCl is used.
[0145] The content of AlCl3 in the raw material gas is preferably 0.5 to 6.0 volume %, more preferably 1.0 to 5.0 volume %, and further preferably 2.0 to 4.0 volume %. The preferred flow rate of AlCl3 is 0.75 to 3.5 L / min.
[0146] The content of CO 2 in the raw material gas is preferably 0.3 to 3% by volume, more preferably 0.4 to 2.5% by volume, and still more preferably 0.5 to 2.0% by volume. The preferred flow rate of CO 2 is 0.25 to 2.0 L / min.
[0147] The content of H2S in the raw material gas is preferably 0.02 to 2.0 volume %, more preferably 0.04 to 1.8 volume %, and even more preferably 0.05 to 1.5 volume %. The preferred flow rate of H2S is 0.5 to 5.0 L / min.
[0148] The content of HCl in the raw material gas is preferably 0.5 to 6.0 volume %, more preferably 0.7 to 5.5 volume %, and even more preferably 1.0 to 5.0 volume %. The preferred flow rate of HCl is 0.5 to 5.0 L / min, and more preferably 1.0 to 5.0 L / min.
[0149] The temperature in the reaction container 32 is preferably controlled at 950 to 1000° C. The pressure in the reaction container 32 is preferably controlled at 50 to 200 hPa. In addition, H 2 is used as a carrier gas. It should be noted that, similarly to the above, the gas introduction pipe 35 is preferably rotated when introducing the gas.
[0150] <Other Process>
[0151] In the manufacturing method according to the present embodiment, in addition to the above-mentioned steps, additional steps may be appropriately performed within the scope of not impairing the effect of the present embodiment. As the above-mentioned additional steps, for example, there can be listed: a step of forming a surface layer on the above-mentioned aluminum oxide layer, and a step of sandblasting the coating. There is no particular limitation on the method of forming the surface layer, and for example, a method of forming by a CVD method or the like can be listed.
[0152] The above description includes the following additional features.
[0153] (Note 1)
[0154] A cutting tool comprises a substrate and a coating layer arranged on the substrate, wherein:
[0155] The coating layer is composed of a titanium carbonitride layer provided on the substrate, an intermediate layer provided on the titanium carbonitride layer, and an aluminum oxide layer provided on the intermediate layer.
[0156] The intermediate layer is composed of a compound composed of titanium, carbon, oxygen and nitrogen.
[0157] The thickness of the intermediate layer exceeds 1 μm,
[0158] When the atomic ratio of carbon at the interface between the intermediate layer and the aluminum oxide layer is set to P C1 atomic %, and the atomic ratio of the carbon at a position A on the intermediate layer side 1 μm away from the interface is defined as P C2 At% P C1 Relative to P C2 The ratio of P C1 / P C2 It is above 1.03.
[0159] (Note 2)
[0160] The cutting tool according to Supplementary Note 1, wherein when the atomic ratio of nitrogen at the interface is set to P N1 When the atomic percentage is P, the atomic ratio of nitrogen N1 It is not less than 5 atomic % and not more than 35 atomic %.
[0161] (Note 3)
[0162] The cutting tool according to Supplement 1 or 2, wherein when the atomic ratio of oxygen at the interface is set to P O1 When the atomic percentage of oxygen is O1 It is not less than 5 atomic % and not more than 25 atomic %.
[0163] (Note 4)
[0164] The cutting tool according to any one of Supplementary Notes 1 to 3, wherein the aluminum oxide layer has a thickness of 3 μm or more and 20 μm or less.
[0165] (Note 5)
[0166] The cutting tool according to any one of Supplementary Notes 1 to 4, wherein the titanium carbonitride layer has a thickness of 3 μm to 20 μm.
[0167] Example
[0168] Hereinafter, the present invention will be described in detail with reference to Examples, but the present invention is not limited thereto.
[0169] 《Manufacturing of cutting tools》
[0170] <Step 1: Step of preparing a base material>
[0171] As a substrate, a cemented carbide cutting insert (shape: CNMG120408N-UX, manufactured by Sumitomo Electric Hard Metal Co., Ltd., JIS B4120 (2013)) having a composition consisting of TaC (2.0 mass%), NbC (1.0 mass%), Co (10.0 mass%) and WC (balance) (however, including inevitable impurities) was prepared.
[0172] <Step of forming a base layer>
[0173] Before the second step described later, a base layer is formed on the prepared substrate using a CVD device. The formation conditions of the base layer are as follows. It should be noted that the values in parentheses after each gas composition represent the flow rate (L / min) of each gas. In addition, the thickness of the base layer and the composition of the base layer are shown in Table 1.
[0174] (Base layer: TiN)
[0175] Raw gas: TiCl4 (15L / min), N2 (20L / min), H2 (80L / min)
[0176] Pressure: 95hPa
[0177] Temperature: 860℃
[0178] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0179] <Second step: step of forming a titanium carbonitride layer on a substrate>
[0180] A titanium carbonitride layer was formed on the substrate with the base layer formed thereon using a CVD apparatus, and then the process proceeded to step 3, which was the subsequent process. The conditions for forming the titanium carbonitride layer were as follows. In addition, the thickness of the titanium carbonitride layer and the composition of the titanium carbonitride layer are shown in Table 1.
[0181] (Titanium carbonitride layer: TiCN)
[0182] Raw gas: TiCl4 (2.0L / min), CH3CN (0.8L / min), N2 (20L / min), H2 (65L / min)
[0183] Pressure: 75hPa
[0184] Temperature: 975℃
[0185] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0186] <Third step: step of forming an intermediate layer directly on the titanium carbonitride layer>
[0187] Next, an intermediate layer was formed on the substrate having the titanium carbonitride layer formed thereon using a CVD device. The conditions for forming the intermediate layer are as follows. In addition, the thickness of the intermediate layer and the composition of the intermediate layer are shown in Table 1. Here, the partial pressure ratio P of the methane gas to the nitrogen gas in the third step is CH4 / P N2g Shown in Table 2.
[0188] (Middle layer: TiCNO)
[0189] Raw gas: TiCl4 (0.8L / min), CH4 (1.3~3.0L / min), CO (1.0L / min), N2 (6~12L / min), H2 (35L / min)
[0190] Pressure: 175hPa
[0191] Temperature: 960℃
[0192] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0193] <Step 4: Step of forming an aluminum oxide layer directly on the intermediate layer>
[0194] Next, an aluminum oxide layer was formed on the substrate having the intermediate layer formed thereon using a CVD device. The conditions for forming the aluminum oxide layer are shown below. In addition, the thickness of the aluminum oxide layer and the composition of the aluminum oxide layer are shown in Table 1.
[0195] (Aluminum oxide layer: α-Al2O3)
[0196] Raw gas: AlCl3 (2.1L / min), CO2 (0.5L / min), H2S (0.5L / min), HCl (2.1L / min), H2 (50L / min)
[0197] Pressure: 150hPa
[0198] Temperature: 980℃
[0199] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0200] <Step of forming the surface layer>
[0201] Finally, a surface layer was formed on the substrate (except for samples 4, 12 and 103) on which the above-mentioned aluminum oxide layer was formed using a CVD device. The conditions for forming the surface layer are as follows. In addition, the thickness and composition of the surface layer are shown in Table 1. It should be noted that in Table 1, the place indicated by "-" indicates that the corresponding layer is not provided.
[0202] (Surface layer: TiN, TiC or TiCN)
[0203] (When it is TiN)
[0204] Raw gas: TiCl4 (4L / min), N2 (20L / min), H2 (70L / min)
[0205] Pressure: 140hPa
[0206] Temperature: 990℃
[0207] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0208] (When it is TiC)
[0209] Raw gas: TiCl4 (2L / min), CH4 (3L / min), H2 (75L / min)
[0210] Pressure: 300hPa
[0211] Temperature: 980℃
[0212] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0213] (When it is TiCN)
[0214] Raw gas: TiCl4 (4.5L / min), CH3CN (2.5L / min), N2 (35L / min), H2 (65L / min)
[0215] Pressure: 75hPa
[0216] Temperature: 975℃
[0217] Film forming time: appropriately adjusted to achieve the thickness shown in Table 1
[0218] [Table 1]
[0219]
[0220] [Table 2]
[0221]
[0222] Through the above steps, cutting tools of samples 1 to 15 and samples 101 to 104 were produced.
[0223] 《Evaluation of cutting tool characteristics》
[0224] Using the cutting tools of the samples prepared as described above, various characteristics of the cutting tools were evaluated as follows: Here, samples 1 to 15 correspond to Examples, and samples 101 to 104 correspond to Comparative Examples.
[0225] <Measurement of thickness of each layer constituting the coating>
[0226] The thickness of each layer constituting the coating was determined by measuring any 10 points in the cross-section sample parallel to the normal direction of the substrate surface using a scanning transmission electron microscope (STEM) (manufactured by JEOL Ltd., trade name: JEM-2100F), and taking the average value of the thickness of the 10 points measured. The results are shown in Table 1.
[0227] <Atomic Ratio of Each Element in the Vicinity of the Interface between the Intermediate Layer and the Aluminum Oxide Layer (AES Measurement)>
[0228] The atomic ratio of each element (oxygen, nitrogen, carbon, aluminum, etc.) near the interface between the intermediate layer and the aluminum oxide layer is obtained by line analysis of the cross-section sample parallel to the normal direction of the substrate surface by Auger electron spectroscopy (AES method). Specifically, first, the cut surface of the cross-section sample is ground by cross-section polishing. The cut surface after grinding is analyzed using a field emission scanning microscope (FE-SEM) to obtain a cross-sectional SEM image of the coating layer (for example, Figure 6 ). The measurement magnification at this time is 50000 times. Figure 6 Next, in the field of view of the cross-sectional SEM image, from the titanium carbonitride layer side toward the aluminum oxide layer side (for example, Figure 6 The cut surface after the grinding was analyzed by AES method in the direction of the white arrow in the figure and along the black line. The measurement interval at this time was 0.016 μm. Other measurement conditions of the AES method were as follows.
[0229] (Measurement conditions of AES method)
[0230] Measuring device: Made by アルバック・ファイ Co., Ltd., trade name: PHI700
[0231] Measurement acceleration voltage: 10kV
[0232] Measuring current: 10mA
[0233] Sample tilt angle: 30°
[0234] Sputtering voltage: 1kV
[0235] The data obtained by the above line analysis is plotted in a graph (e.g. Figure 7 In this graph, the X-axis (horizontal axis) represents the distance from the starting point of the measurement, and the Y-axis (vertical axis) represents the atomic ratio (atomic %) of each element of the measurement object. Here, in the above-mentioned cut surface after grinding, there is oxygen (O Ti ) and oxygen (O Al), but by using a standard spectrum to perform waveform separation processing on the obtained measurement data, the two can be distinguished. Specifically, first, an aluminum ingot with a purity of 99.99% (for example, manufactured by Nikora Corporation) is prepared as a standard sample of aluminum. Next, a mixed powder of alumina powder (manufactured by Ishizu Pharmaceutical Co., Ltd.) with a purity of 99.99% and high-purity carbon powder (manufactured by High Purity Chemical Research Institute) is prepared as a standard sample of aluminum oxide. At this time, the mixing ratio of the above-mentioned aluminum oxide powder and the above-mentioned high-purity carbon powder is set to 1:1 in terms of mass ratio. The two prepared standard samples are spectrally measured using the AES method to obtain their respective standard spectra. Then, using the two obtained standard spectra, the measured spectra at each measurement point represented by the horizontal axis of the above-mentioned measurement data are subjected to waveform separation processing, and the respective atomic ratios of oxygen derived from the intermediate layer and oxygen derived from the aluminum oxide layer are calculated. Next, based on the graph, the position where the atomic ratio of Al is 10 atomic % is set as the "interface between the intermediate layer and the aluminum oxide layer" (for example, refer to Figure 7 ). In addition, a position 1 μm away from the interface on the intermediate layer side is defined as “position A” (for example, refer to Figure 7 ). In addition, the position 0.5 μm away from the interface on the intermediate layer side is set as "position M" (not shown). Then, based on the above graph, the atomic ratios of oxygen, nitrogen and carbon at the interface between the intermediate layer and the aluminum oxide layer (P O1 , P N1 and P C1 ), the atomic ratios of oxygen, nitrogen and carbon at the position A (P O2 , P N2 and P C2 ), and the atomic ratio of the carbon at the position M (P C3 ). Such measurements were performed three times, and the average value of the atomic ratio of each element obtained by each measurement was set as the atomic ratio of the element in the coating layer. In addition, based on the above results, the ratio of each atomic ratio (P O1 / P O2 , P N1 / P N2 , P C1 / P C2 and P C3 / P C2 The results are shown in Table 3.
[0236] [Table 3]
[0237]
[0238] 《Cutting Test》
[0239] (Cutting evaluation (1): intermittent machining test, evaluation of chipping resistance)
[0240] Using the cutting tools of the samples prepared as above (samples 1 to 15 and samples 101 to 104), the number of contacts between the cutting tool and the cut material until chipping occurs at the cutting edge is measured according to the following cutting conditions. The results are shown in Table 4. The greater the number of contacts, the better the chipping resistance of the cutting tool can be evaluated. The number of contacts between the cutting tool and the cut material is measured by the following steps. Stop the cutting process every 30 seconds after the start of the cutting process, and observe the cutting edge ridge of the cutting tool using a stereoscopic microscope (magnification 100 times). Repeat the same operation until chipping of the cutting edge ridge is confirmed. The number of contacts with the discontinuous portion of the above-mentioned cut material is calculated from the cumulative time required for the cutting process until chipping occurs.
[0241] Test conditions for intermittent machining
[0242] Cutting material: SCM415 intermittent material
[0243] Cutting speed: 220m / min
[0244] Feed speed: 0.3mm / rev
[0245] Cutting depth: 2mm
[0246] Cutting oil: Wet type
[0247] (Cutting evaluation (2): continuous machining test, evaluation of wear resistance)
[0248] The cutting tools of the samples (samples 1 to 15 and samples 101 to 104) prepared as described above were used to measure the average wear amount of the flank surface after 20 minutes of cutting under the following cutting conditions. The results are shown in Table 4. The smaller the average wear amount, the better the wear resistance of the cutting tool.
[0249] Test conditions for continuous processing
[0250] Cutting material: SCM435 round bar
[0251] Cutting speed: 240m / min
[0252] Feed speed: 0.2mm / rev
[0253] Cutting depth: 2mm
[0254] Cutting oil: Wet type
[0255] (Cutting evaluation (3): continuous processing test, evaluation of the peeling resistance of the aluminum oxide layer)
[0256] Using the cutting tools of the samples (Samples 1 to 15 and Samples 101 to 104) prepared as described above, the cutting time until the aluminum oxide layer in the front cutting surface peels off is measured according to the following cutting conditions. The results are shown in Table 4. The longer the above-mentioned cutting time is, the better the cutting tool can be evaluated as having the peeling resistance of the aluminum oxide layer. The cutting time until the aluminum oxide layer peels off is measured according to the following steps. After the start of the cutting process, the cutting process is stopped every 30 seconds, and the front cutting surface of the cutting tool near the cutting edge ridge is observed using a stereoscopic microscope (magnification of 100 times). The same operation is repeated until the aluminum oxide layer peels off, and the cumulative time required for the cutting process until the aluminum oxide layer peels off is set as the above-mentioned "cutting time until the aluminum oxide layer peels off".
[0257] Test conditions for continuous processing
[0258] Cutting material: S15C round bar
[0259] Cutting speed: 120m / min
[0260] Feed speed: 0.25mm / rev
[0261] Cutting depth: 2mm
[0262] Cutting oil: Wet type
[0263] [Table 4]
[0264]
[0265] “*” indicates the peeling resistance of the aluminum oxide layer.
[0266] From the results in Table 4, it can be seen that the cutting tools of samples 1 to 15 obtained a good result of more than 4800 contacts in the cutting evaluation (1). On the other hand, the cutting tools of samples 101 to 104 (cutting tools of comparative examples) obtained a good result of less than 1300 contacts in the cutting evaluation (1). As can be seen from the above results, the cutting tools of the embodiments (P C1 / P C2 The chipping resistance of cutting tools with a value of 1.03 or more is more excellent.
[0267] In addition, from the results in Table 4, it can be seen that the cutting tools of samples 1 to 5 and 9 to 13 achieved a good result of 0.2 mm or less in the wear amount of the flank face in the cutting evaluation (2). O1 / P O2 A cutting tool having a value of 0.9 or more and less than 1 is also excellent in wear resistance in addition to the above-mentioned chipping resistance.
[0268] In addition, from the results in Table 4, it can be seen that the cutting tools of samples 1 to 3, 6, 7, 9 to 12 and 14 obtained good results of cutting time of more than 6 minutes in the cutting evaluation (3). N1 / P N2 The cutting tool having a value of 0.9 or more and less than 1 is also excellent in the peeling resistance of the aluminum oxide layer in addition to the above-mentioned chipping resistance.
[0269] As mentioned above, although the embodiment and the example of the present invention have been described, it is initially intended that the configurations of the above-mentioned embodiments and the examples be appropriately combined.
[0270] The embodiments and examples disclosed this time should be considered to be illustrative and non-restrictive in all aspects. The scope of the present invention is indicated by the claims rather than the above embodiments and examples, and is intended to include all changes within the meaning and scope equivalent to the claims.
[0271] Explanation of symbols
[0272] 1 front cutting edge, 2 back cutting edge, 3 cutting edge ridge, 10 substrate, 20 titanium carbonitride layer, 21 intermediate layer, 22 aluminum oxide layer, 23 base layer, 24 surface layer, 30 CVD device, 31 substrate fixing jig, 32 reaction container, 33 temperature control device, 34 gas inlet, 35 gas inlet pipe, 36 ejection hole, 40 coating layer, 45 film, 50 cutting tool, A at a position 1 μm away from the interface between the intermediate layer and the aluminum oxide layer on the intermediate layer side, P A The imaginary plane containing position A, P B Interface between the intermediate layer and the aluminum oxide layer.
Claims
1. A cutting tool comprising a substrate and a coating layer provided on the substrate, in, The coating layer is composed of a titanium carbonitride layer provided on the substrate, an intermediate layer provided on the titanium carbonitride layer, and an aluminum oxide layer provided on the intermediate layer. The intermediate layer is composed of a compound composed of titanium, carbon, oxygen and nitrogen. The thickness of the intermediate layer is greater than 1 μm and less than 2 μm, When the atomic ratio of carbon at the interface between the intermediate layer and the aluminum oxide layer is set to P C1 atomic %, and the atomic ratio of the carbon at a position A on the intermediate layer side 1 μm away from the interface is defined as P C2 At% P C1 Relative to P C2 The ratio of P C1 / P C2 It is above 1.03 and below 1.
1.
2. The cutting tool according to claim 1, in, The P C2 It is not less than 22 atomic % and not more than 63 atomic %.
3. The cutting tool according to claim 1 or 2, in, The P C1 It is not less than 25 atomic % and not more than 65 atomic %.
4. The cutting tool according to claim 1 or 2, in, When the atomic ratio of the carbon at a position M on the intermediate layer side 0.5 μm away from the interface is defined as P C3 At% P C3 Relative to P C2 The ratio of P C3 / P C2 It is greater than 0.9 and less than 1.
1.
5. The cutting tool according to claim 1 or 2, in, When the atomic ratio of the carbon at a position M on the intermediate layer side 0.5 μm away from the interface is defined as P C3 At% when the P C3 P C2 Above and P C1 With P C2 below the average value.
6. The cutting tool according to claim 1 or 2, in, When the atomic ratio of nitrogen at the interface is set to P N1 atomic %, and the atomic ratio of nitrogen at the position A is set to P N2 At% P N1 Relative to P N2 The ratio of P N1 / P N2 It is greater than or equal to 0.9 and less than 1.
7. The cutting tool according to claim 1 or 2, in, When the atomic ratio of nitrogen at the interface is set to P N1 When the atomic percentage is P, the atomic ratio of nitrogen N1 It is not less than 5 atomic % and not more than 35 atomic %.
8. The cutting tool according to claim 1 or 2, in, When the atomic ratio of oxygen at the interface is set to P O1 atomic %, and the atomic ratio of oxygen at the position A is set to P O2 At% P O1 Relative to P O2 The ratio of P O1 / P O2 It is greater than or equal to 0.9 and less than 1.
9. The cutting tool according to claim 1 or 2, in, When the atomic ratio of oxygen at the interface is set to P O1 When the atomic percentage of oxygen is O1 It is not less than 5 atomic % and not more than 25 atomic %.
10. The cutting tool according to claim 1 or 2, in, The intermediate layer consists of titanium oxycarbonitride.
11. The cutting tool according to claim 1 or 2, in, A base layer is further provided between the substrate and the covering layer.
12. The cutting tool according to claim 1 or 2, in, A surface layer is also arranged on the coating layer.
Citation Information
Patent Citations
Surface coated cemented carbide-made cutting tool excellent in pitching resistance
JP1997174304A
Coated tool
JP2009166216A
Coated cutting tool
CN108453273A
Surface-coated cutting tool
CN1620349A
Multilayer coated cemented carbides
CN85104135A