Negative photoresist composition, preparation method and method for forming photoresist pattern
By using a negative photoresist composition consisting of high-silica resin and photosensitive acid-generating agent, the problem of high dielectric constant was solved, and a photoresist pattern with low dielectric constant was achieved, which improved packaging efficiency and reduced costs.
Patent Information
- Application Number
- CN202111476489.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-06
AI Technical Summary
Existing photoresists have a high dielectric constant, which makes it difficult to meet the requirements for improved insulation performance in integrated circuit packaging processes, and the production cost is also high.
A negative photoresist composition consisting of high-silica resin and photosensitive acid-generating agent is used. By controlling the ratio and molecular weight of the resin and acid-generating agent and combining them with organic solvents, a photoresist pattern with a low dielectric constant is formed.
The dielectric constant of the photoresist was reduced to 2.8-3.2, which meets the insulation requirements of the packaging process, improves packaging efficiency, reduces production costs, and is suitable for mass production.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photoresists, and in particular to a negative photoresist composition, a preparation method and a method for forming a photoresist pattern. Background Art
[0002] Integrated circuit (IC) packaging is an essential link in the integrated circuit industry chain. Packaging refers to the process of processing tested wafers to obtain independent chips, which protects the circuit chips from the surrounding environment, protects the chips, enhances thermal conductivity, and communicates the internal and external circuits of the chips. Currently, the packaging and testing industry has become an important part of my country's integrated circuits.
[0003] A key photosensitive insulating material is needed in the packaging, and the dielectric constant of the material is required to be lower than 3.5. In the current process, polyimide photoresist is used to improve the insulation performance, and their dielectric constant can reach 3.3-3.6. There is no alternative product in China.
[0004] Existing photoresists cannot meet the increasingly higher insulation performance requirements for photoresists in packaging processes, and the dielectric constant is difficult to continue to decrease.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a negative photoresist composition, which solves the technical problem of high dielectric constant in the prior art.
[0007] The second object of the present invention is to provide a method for preparing a negative photoresist composition, which has simple procedures, large processing capacity, is suitable for mass production and has low cost.
[0008] The third object of the present invention is to provide an application of a negative photoresist composition in the manufacture of integrated circuits, which improves the production efficiency of integrated circuits and reduces production costs.
[0009] A fourth object of the present invention is to provide a method for forming a photoresist pattern, thereby ensuring that the formed pattern meets actual process requirements and achieving a better photoresist pattern.
[0010] In order to solve the above technical problems, the present invention particularly adopts the following technical solutions:
[0011] A first aspect of the present invention provides a negative photoresist composition comprising a high-silicon resin and a photosensitive acid generator.
[0012] Optionally, the mass ratio of the high silicone resin to the photosensitive acid generator is 10-70:0.5-10.
[0013] Optionally, the structural formula of the high silicone resin is:
[0014]
[0015] Here, n is an integer greater than 1.
[0016] Preferably, the molecular weight of the high silicone resin is 1000-10000.
[0017] Optionally, the photosensitive acid generator includes a non-ionic acid generator.
[0018] Preferably, the non-ionic acid generator includes triazine substances and / or sulfonic acid compounds.
[0019] Optionally, a solvent is also included.
[0020] Preferably, the solvent comprises an organic solvent.
[0021] Preferably, the organic solvent includes at least one of propylene glycol methyl ether, propylene glycol propyl ether, propylene glycol methyl ether acetate, ethyl acetate and ethyl lactate.
[0022] The second aspect of the present invention provides a method for preparing the above-mentioned negative photoresist composition, which is obtained by uniformly mixing the high-silicon resin, the photosensitive acid generator and optionally a solvent.
[0023] The third aspect of the present invention provides the use of the negative photoresist composition in manufacturing integrated circuits.
[0024] A fourth aspect of the present invention provides a method for forming a photoresist pattern, the method comprising the following steps:
[0025] Step A: spin coating a negative photoresist composition on a substrate to form a photoresist layer;
[0026] Step B: performing i-line exposure on the photoresist layer after pre-baking to obtain an exposed photoresist layer;
[0027] Step C: baking the exposed photoresist layer and then developing it to obtain the photoresist pattern.
[0028] Optionally, the pre-baking temperature is 90-110°C.
[0029] Preferably, the pre-baking time is 30-90s.
[0030] Preferably, the temperature of the intermediate baking is 100-120°C.
[0031] Preferably, the intermediate baking time is 30-90s.
[0032] Optionally, in step B, the photoresist layer to be exposed is obtained by pre-baking before i-line exposure.
[0033] Preferably, the thickness of the photoresist layer to be exposed is 2-5 μm.
[0034] Preferably, in step C, a developer is added for development.
[0035] Preferably, the developer comprises a tetramethylammonium hydroxide solution.
[0036] Compared with the prior art, the present invention has at least the following beneficial effects:
[0037] The negative photoresist composition provided by the present invention has a unique chain structure of a high-silicon resin so that it has good chemical stability and insulation performance. At the same time, the silanol groups in the resin structure can react under acid catalysis to connect with each other to form a negative image, thereby reducing the dielectric constant of the negative photoresist composition. The dielectric constant is as low as 2.8-3.2, which can meet the insulation requirements of the packaging process, improve the packaging efficiency and effect, break the foreign monopoly, and reduce production costs.
[0038] The preparation method of the negative photoresist composition provided by the invention has simple procedures, large processing volume, is suitable for mass production and has low cost.
[0039] The negative photoresist composition provided by the present invention is used in manufacturing integrated circuits and can be applied to the packaging of 22nm key size chips, thereby improving the production efficiency of integrated circuits and reducing production costs.
[0040] The method for forming a photoresist pattern provided by the present invention ensures that the formed pattern meets actual process requirements and realizes a better photoresist pattern. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, but not all of the embodiments. The components of the embodiment of the present invention can be arranged and designed in various configurations.
[0042] According to a first aspect of the present invention, a negative photoresist composition is provided, comprising a high-silicon resin and a photosensitive acid generator.
[0043] The negative photoresist composition provided by the present invention uses a high-silicon resin with good chemical stability and insulation performance, which can reduce the dielectric constant of the negative photoresist composition to 2.8-3.2, which can meet the insulation requirements of the packaging process, improve the packaging efficiency and effect, break the foreign monopoly, and reduce production costs.
[0044] Optionally, the mass ratio of the high silicone resin to the photosensitive acid generator is 10-70:0.5-10.
[0045] When the mass ratio of high-silicone resin and photosensitive acid generator is higher than 70:0.5, the resin molecules cannot be well connected due to the low proportion of acid generator, and thus they are dissolved in the developer and cannot form a photolithography image; when the mass ratio of high-silicone resin and photosensitive acid generator is lower than 10:10, the proportion of high-silicone resin is too low to form a good photoresist film.
[0046] In some preferred embodiments of the present invention, the mass ratio of high silicone resin to photosensitive acid generator is typically but not limited to 10:0.5, 50:0.5, 70:0.5, 10:1, 50:1, 70:1, 10:5, 50:5, 70:5, 10:10, 50:10 or 70:10.
[0047] Optionally, the structural formula of the high silicone resin is:
[0048]
[0049] Here, n is an integer greater than 1.
[0050] Preferably, the molecular weight of the high silicone resin is 1000-10000.
[0051] When the molecular weight of the high silicone resin is less than 1000, the molecular weight is too low, resulting in insufficient connection efficiency, making it difficult to form large molecules insoluble in the developer, and thus unable to form a photolithography image; when the molecular weight of the high silicone resin is greater than 10000, the molecular weight is too high, resulting in the resin being difficult to dissolve in the developer without connection, thus unable to form a photolithography image.
[0052] In some embodiments of the present invention, the molecular weight of the high silicone resin is typically, but not limited to, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000 or 10000.
[0053] Optionally, the photosensitive acid generator includes a non-ionic acid generator.
[0054] Photoacid generators are light-sensitive compounds that decompose under light to produce acid (H + ). During the post-exposure baking (PEB) process, these acids act as catalysts to connect the silanol groups on the high-silicone resin to each other. After the molecular weight of the resin increases, it is no longer soluble in the developer. The unexposed part can continue to dissolve in the developer because there is no acid catalysis, so that the photoresist forms a negative image after development.
[0055] Preferably, the non-ionic acid generator includes triazine substances and / or sulfonic acid compounds. The compound molecules generated by the non-ionic acid generator after light irradiation can effectively catalyze the mutual connection of resin molecules.
[0056] Triazines include, but are not limited to, methylbischloromethyltriazine.
[0057] The sulfonic acid compounds include, but are not limited to, N-toluenesulfonyloxyphthalimide, naphthalimide trifluoromethanesulfonate, p-methoxyphenylacetonitrile p-toluenesulfonate, N-trifluoromethanesulfonyloxysuccinimide or N-trifluoromethanesulfonyloxynaphthalimide.
[0058] Optionally, a solvent is also included.
[0059] The solvent dissolves the high silicone resin therein to form a liquid substance, so that the formed negative photoresist composition has good fluidity and is convenient for covering the substrate.
[0060] Preferably, the solvent comprises an organic solvent.
[0061] Preferably, the organic solvent includes at least one of propylene glycol methyl ether, propylene glycol propyl ether, propylene glycol methyl ether acetate, ethyl acetate and ethyl lactate.
[0062] According to the second aspect of the present invention, the method for preparing the negative photoresist composition is prepared by uniformly mixing the high-silicon resin, the photosensitive acid generator and optionally a solvent.
[0063] The preparation method of the negative photoresist composition provided by the invention has simple procedures, large processing volume, is suitable for mass production and has low cost.
[0064] The third aspect of the present invention provides the use of the negative photoresist composition in manufacturing integrated circuits.
[0065] The negative photoresist composition provided by the present invention is used in manufacturing integrated circuits and can be applied to the packaging of 22nm key size chips, thereby improving the production efficiency of integrated circuits and reducing production costs.
[0066] A fourth aspect of the present invention provides a method for forming a photoresist pattern, the method comprising the following steps:
[0067] Step A: spin coating a negative photoresist composition on a substrate to form a photoresist layer;
[0068] Step B: performing i-line exposure on the photoresist layer after pre-baking to obtain an exposed photoresist layer;
[0069] Step C: baking the exposed photoresist layer and then developing it to obtain the photoresist pattern.
[0070] The method for forming a photoresist pattern provided by the present invention ensures that the formed pattern meets actual process requirements and realizes a better photoresist pattern.
[0071] Optionally, the pre-baking temperature is 90-110°C.
[0072] In some embodiments of the present invention, the pre-baking temperature is typically but not limited to 90°C, 95°C, 100°C, 105°C or 110°C.
[0073] Preferably, the pre-baking time is 30-90s.
[0074] In some embodiments of the present invention, the pre-baking time is 30 s, 40 s, 50 s, 60 s, 70 s, 80 s or 90 s.
[0075] Preferably, the temperature of the intermediate baking is 100-120°C.
[0076] In some embodiments of the present invention, the temperature of the intermediate baking is typically but not limited to 100°C, 105°C, 110°C, 115°C or 120°C.
[0077] Preferably, the intermediate baking time is 30-90s.
[0078] In some embodiments of the present invention, the intermediate baking time is 30 s, 40 s, 50 s, 60 s, 70 s, 80 s or 90 s.
[0079] Optionally, in step B, the photoresist layer to be exposed is obtained by pre-baking before i-line exposure.
[0080] Preferably, the thickness of the photoresist layer to be exposed is 2-5 μm.
[0081] In some embodiments of the present invention, the film thickness of the photoresist layer to be exposed is typically but not limited to 2 μm, 3 μm, 4 μm or 5 μm.
[0082] Preferably, in step C, a developer is added for development.
[0083] Preferably, the developer comprises a tetramethylammonium hydroxide solution.
[0084] In some embodiments of the present invention, the developer is typically, but not limited to, a tetramethylammonium hydroxide solution.
[0085] The concentration of the tetramethylammonium hydroxide solution is 2.38 wt %.
[0086] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0087] The specifications and types of raw materials used in the examples and comparative examples of the present invention are shown in Table 1 below. If no specific conditions are specified, conventional conditions or conditions recommended by the manufacturer shall be followed.
[0088] Table 1 Raw material specifications and models
[0089]
[0090]
[0091] Example 1
[0092] This embodiment provides a negative photoresist composition, which is prepared by uniformly mixing 50 g of a high-silicon resin with a molecular weight of 2000, 1 g of methylbischloromethyltriazine and 100 g of propylene glycol methyl ether acetate, and filtering the mixture with a filter membrane with a pore size of 0.2 μm to obtain the negative photoresist composition.
[0093] Example 2
[0094] This embodiment provides a negative photoresist composition, which is prepared by uniformly mixing 50 g of high-silicon resin with a molecular weight of 3000, 0.5 g of naphthalimide trifluoromethanesulfonate and 100 g of propylene glycol methyl ether acetate, and filtering the mixture with a filter membrane with a pore size of 0.2 μm to obtain the negative photoresist composition.
[0095] Example 3
[0096] This embodiment provides a negative photoresist composition, which is prepared by uniformly mixing 50 g of a high-silicon resin with a molecular weight of 4000, 1 g of p-methoxyphenylacetonitrile p-toluenesulfonate and 100 g of propylene glycol methyl ether acetate, and filtering the mixture with a filter membrane with a pore size of 0.2 μm to obtain the negative photoresist composition.
[0097] Example 4
[0098] This embodiment provides a negative photoresist composition, which is prepared by uniformly mixing 50 g of a high-silicon resin with a molecular weight of 8000, 1 g of methylbischloromethyltriazine and 100 g of propylene glycol methyl ether, and filtering the mixture with a filter membrane with a pore size of 0.2 μm to obtain the negative photoresist composition.
[0099] Example 5
[0100] This embodiment provides a negative photoresist composition. The difference from Embodiment 3 is that the mass of the high-silicon resin is 800 g, and the other raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0101] Example 6
[0102] This embodiment provides a negative photoresist composition. The difference from Embodiment 3 is that the mass of the high-silicon resin is 500 g, and the other raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0103] Example 7
[0104] This embodiment provides a negative photoresist composition. The difference from Embodiment 3 is that the mass of p-methoxyphenylacetonitrile p-toluenesulfonate is 10 g, and the other raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0105] Comparative Example 1
[0106] This comparative example provides a negative photoresist composition, which is prepared by uniformly mixing 50 g of comparative high silicone resin with a molecular weight of 3000, 1 g of methylbischloromethyltriazine and 100 g of propylene glycol methyl ether, and filtering with a filter membrane with a pore size of 0.2 μm to obtain the negative photoresist composition.
[0107] The structural formula of the comparative high silicone resin is shown below:
[0108]
[0109] Comparative Example 2
[0110] This comparative example provides a negative photoresist composition. The difference from Example 3 is that there is no high-silicon resin in the raw materials, and the resin used is polyimide resin SUN-PAA136. Other raw materials and preparation methods are the same as those in Example 3 and will not be repeated here.
[0111] Test Example 1
[0112] The negative photoresist compositions provided in Examples 1-7 and Comparative Examples 1-2 were respectively spin-coated on the treated silicon wafers, and pre-baked on a hot plate (PAB) at a temperature of 100°C for 60 seconds. The rotation speed was adjusted so that the film thickness after drying was 3 μm. After exposure through the mask and the i-line of the exposure machine, the exposure metering was 60 mJ / cm 2 , using hot plate baking (PEB), the baking temperature is 110℃, the baking time is 60s. Use 2.38wt% tetramethylammonium hydroxide solution (TMAH) for immersion development for 60s, use deionized water to wash, and then use 110℃ hot plate to harden the film for 60s, that is, the photolithography process is completed, and the dielectric constant of the film is recorded in Table 2.
[0113] Table 2 Dielectric constant data table
[0114] Dielectric constant Example 1 3.0 Example 2 2.9 Example 3 2.8 Example 4 3.0 Example 5 2.7 Example 6 2.7 Example 7 3.1 Comparative Example 1 3.3 Comparative Example 2 3.3
[0115] It can be seen from Table 2 that the dielectric constants of the negative photoresist compositions provided by Examples 1 to 7 are all lower than 3.2, which is better than the negative photoresist compositions provided by Comparative Examples 1 to 2. The comparative high silicone resin used in Comparative Example 1 has a spatial network structure, and the hydroxyl groups at both ends can undergo a dehydration condensation reaction under acid catalysis, but due to the low content of organic groups and the difference in arrangement, the dielectric constant k cannot be reduced to below 3.2.
[0116] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A negative photoresist composition, characterized in that It includes a high silicone resin and a photosensitive acid generator in a mass ratio of 10-70:0.5-10; The structural formula of the high silicone resin is: ; Wherein, n is an integer greater than 1; The molecular weight of the high silicone resin is 1000-10000.
2. The negative photoresist composition according to claim 1, characterized in that The photosensitive acid generator includes a non-ionic acid generator.
3. The negative photoresist composition according to claim 2, characterized in that: The non-ionic acid generator includes triazine substances and / or sulfonic acid compounds.
4. The negative photoresist composition according to claim 1, characterized in that Also included are solvents.
5. The negative photoresist composition according to claim 4, characterized in that: The solvent includes an organic solvent.
6. The negative photoresist composition according to claim 5, characterized in that The organic solvent includes at least one of propylene glycol methyl ether, propylene glycol propyl ether, propylene glycol methyl ether acetate, ethyl acetate and ethyl lactate.
7. The method for preparing a negative photoresist composition according to any one of claims 1 to 6, characterized in that: The high-silicon resin, the photosensitive acid generator and an optional solvent are uniformly mixed to obtain the above-mentioned product.
8. Use of the negative photoresist composition according to any one of claims 1 to 6 or the negative photoresist composition prepared by the preparation method according to claim 6 in manufacturing integrated circuits.
9. A method for forming a photoresist pattern, characterized in that: The method comprises the following steps: Step A: spin coating the negative photoresist composition according to any one of claims 1 to 6 or the negative photoresist composition prepared by the preparation method according to claim 7 on a substrate to form a photoresist layer; Step B: performing i-line exposure on the photoresist layer after pre-baking to obtain an exposed photoresist layer; Step C: baking the exposed photoresist layer and then developing it to obtain the photoresist pattern.
10. The method for forming a photoresist pattern according to claim 9, characterized in that: The pre-baking temperature is 90-110°C.
11. The method for forming a photoresist pattern according to claim 9, wherein: The pre-baking time is 30-90s.
12. The method for forming a photoresist pattern according to claim 9, characterized in that: The temperature of the intermediate baking is 100-120°C.
13. The method for forming a photoresist pattern according to claim 9, characterized in that: The intermediate baking time is 30-90s.
14. The method for forming a photoresist pattern according to claim 9, wherein: In step B, the photoresist layer to be exposed is obtained after pre-baking and before i-line exposure.
15. The method for forming a photoresist pattern according to claim 14, characterized in that: The thickness of the photoresist layer to be exposed is 2-5 μm.
16. The method for forming a photoresist pattern according to claim 9, wherein: Step C: Adding a developer to perform development.
17. The method for forming a photoresist pattern according to claim 16, wherein: The developer includes a tetramethylammonium hydroxide solution.