Gas phase method for converting glycolaldehyde using aminating agents
By converting acetaldehyde and amination agent in the gas phase in the presence of hydrogen and catalyst, the problem of low liquid phase conversion in water is solved, and the efficient preparation of ethylene amines and ethanolamines is achieved, and the treatment of water is simplified. and recycling improves the economics and efficiency of the process.
Patent Information
- Application Number
- CN202080043292.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-11
- Filing Date
- 2020-06-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-06-02
AI Technical Summary
In aqueous solvents, especially in water, the liquid phase conversion of acetaldehyde and amination agent leads to low conversion and yields of ethylene amines and ethanolamines, and water is cheap and easy to obtain as a solvent but is processed and recycled There are challenges.
By converting acetaldehyde with an amination agent in the gas phase in the presence of hydrogen and catalyst, using preferred catalysts such as Raney cobalt catalysts, the catalyst precursors are prepared by impregnation or precipitation, and gas phase reactions are carried out at high temperatures and specific pressures. , improve conversion efficiency.
The preparation of ethylene amines and ethanolamines in a water environment is achieved with high yield and high conversion rates, simplifying the process of treating and recycling water, and improving the economic and efficiency of the process.
Smart Images

Figure BDA0003395890170000031 
Figure BDA0003395890170000151 
Figure BDA0003395890170000161
Abstract
Description
[0001] The present invention relates to a process for preparing ethyleneamines and ethanolamines by converting glycolaldehyde and an aminating agent in the gas phase.
[0002] Glycolaldehyde is a useful raw material for the preparation of ethyleneamines and ethanolamines.
[0003] US 6,534,441 describes a process for the reductive amination of lower aliphatic paraffin derivatives using a nickel / rhenium catalyst. A possible starting material mentioned in the specification is ethanolaldehyde.
[0004] German patent application DE-A1-400591 describes a process for preparing amino alcohols by reacting hydroxycarbonyl compounds with hydrogen and an aminating agent at temperatures of 0-300° C. and pressures of 1-400 bar over a catalyst comprising 50-100% by weight of ruthenium. Glycolaldehyde is disclosed as a suitable hydroxycarbonyl compound for use in the process.
[0005] US 6,147,261 discloses the conversion of hydroxyalkanals to diamines in the presence of ammonia and hydrogen in the presence of a catalyst comprising nickel or cobalt. US 6,147,261 teaches that hydroxyalkanals are very reactive and tend to oligomerize and polymerize.
[0006] Although US Pat. No. 6,147,261, DE-A1-4400591 and US Pat. No. 6,534,441 mention the use of glycolaldehyde as a starting material in the reaction with an aminating agent, the specific reaction illustrated in the examples is not described.
[0007] CN107011194 discloses a method for converting glycolaldehyde using a noble metal catalyst containing a rare earth metal in the presence of hydrogen with different aminating agents such as ammonia, methylamine, ethylamine and butylamine.
[0008] WO2011 / 082994 discloses the conversion of glycolaldehyde with an aminating agent such as ammonia in the presence of hydrogen. Since glycolaldehyde tends to form oligomers, such as dimer 2,5-dihydroxy-1,4-dioxane, the six-membered ring compound formed has high thermodynamic stability, the conversion requires preactivation of the non-precious metal amination catalyst to achieve high conversion.
[0009] The effect of catalyst preactivation was subsequently confirmed by Liang et al. (Angew. Chem. 2017, 129, 3096-3100), who studied the conversion of ethanolaldehyde with ammonia in the presence of hydrogen and Ru catalyst.
[0010] Pelckmans et al. (ACS Catal. 2018, 8, 4201-4212) studied the reductive amination of various sugars with dimethylamine in the presence of hydrogen and different metal catalysts. The formation of glycolaldehyde as an intermediate during the reductive aminolysis of sugars was proposed. Therefore, the authors studied the reaction behavior of pure glycolaldehyde with dimethylamine and hydrogen on a nickel catalyst as a model reaction. High TMEDA and DMEOA conversions were obtained in MeOH solution.
[0011] WO 2011 / 082967 discloses the amination of glycolaldehyde with aminating agents MEA and DEA in the presence of hydrogen and an amination catalyst to produce chain alcohol amines.
[0012] The above application discloses the liquid phase conversion of glycolaldehyde in the presence of a solvent.
[0013] In the framework of the present invention, it has been found that the liquid phase conversion of glycolaldehyde and aminating agent in a strong aqueous solvent, particularly water, results in a lower conversion rate and a lower yield of ethyleneamines and / or ethanolamines. However, from a processing point of view, the use of such solvents, particularly water, is highly desirable, since glycolaldehyde and aminating agents are often produced and prepared in the form of their aqueous solutions. In addition, water is an easily available and inexpensive solvent and has a high solubility for glycolaldehyde and aminating agents such as ammonia. In addition, the treatment and recycling of water is relatively problem-free and can be carried out in a wastewater treatment plant, thereby allowing the treated water to be discharged into the environment or used for other applications.
[0014] It was therefore an object of the present invention to provide a process for preparing ethyleneamines and ethanolamines in high yields and with high conversions which permits the workup of glycolaldehyde and the amination in aqueous solvents, in particular water.
[0015] The objects of the present invention are achieved by a process for preparing ethyleneamines and ethanolamines by converting glycolaldehyde with an aminating agent in the presence of hydrogen and a catalyst, wherein the conversion is carried out in the gas phase.
[0016] In the process of the present invention, glycolaldehyde is used.
[0017] Glycolaldehyde is commercially available and can be prepared, for example, by oxidation of ethylene glycol (see, for example, JP 3246248 and JP 3279342).
[0018] Glycolaldehyde is preferably synthesized by reaction of formaldehyde with carbon monoxide and hydrogen, as described, for example, in US 2009012333, US2008081931, US2007249871, EP1697291, US4503260 and US4322568.
[0019] More preferably, glycolaldehyde can also be obtained by pyrolysis of organic raw materials such as aqueous solutions of sugars or wood at high temperatures.
[0020] In a more preferred embodiment, the glycolaldehyde solution is obtained by hydrothermal decomposition of sugars, such as the process disclosed in US 2004 / 0022912, which is incorporated herein by reference. Such processes preferably produce a stream of glycolaldehyde and water.
[0021] In another preferred embodiment, the glycolaldehyde solution is obtained by pyrolysis of wood, for example the method disclosed by D. Mohan et al. ("Pyrolysis of Wood / Biomass for Bio-Oil", Energy Fuels 2006, 20, 3, 848-889) or CRVitasari (Extraction of bio-based Glycolaldehyde from wood-derived pyrolysis oils Eindhoven: Technische Universiteit Eindhoven DOI: 10.6100 / IR738958).
[0022] Glycolaldehyde has a strong tendency to form oligomers in pure state or in solution. In particular, it forms the dimer 2,5-dihydroxy-1,4-dioxane, a six-membered ring compound with high thermodynamic stability.
[0023] Unless expressly stated otherwise, all indications of the weight and molar ratio of glycolaldehyde in this specification refer to monomeric glycolaldehyde, regardless of whether the glycolaldehyde used in the conversion is present in the form of monomer, dimer or oligomer.
[0024] Another starting material used in the process of the present invention is an aminating agent.
[0025] The aminating agent used in the hydrogenating amination of alcohols, aldehydes or ketones in the presence of hydrogen may be ammonia or a primary or secondary aliphatic or cycloaliphatic or aromatic amine.
[0026] The aminating agent is preferably a nitrogen compound of formula I:
[0027]
[0028] in:
[0029] R 1 , R 2 Each is hydrogen (H), alkyl such as C 1-20 Alkyl, cycloalkyl such as C 3-12 Cycloalkyl, alkoxyalkyl such as C 2-30 Alkoxyalkyl, dialkylaminoalkyl such as C 3-30 Dialkylaminoalkyl, aryl, aralkyl such as C 7-20 Arylalkyl, and alkylaryl such as C7-20 alkylaryl, or together with -(CH2) j -X-(CH2) k -,
[0030] X is CH2, CHR 3 , oxygen (O), sulfur (S) or NR 3 ,
[0031] R 3 is hydrogen (H), alkyl such as C 1-4 Alkyl, alkylphenyl such as C 7-40 The alkylphenyl group, j, and k are each an integer of 1-4.
[0032] Preferably, R 1 and R 2 Each of the same or different alkyl groups is, for example, C 1-20 Alkyl, preferably C 1-12 Alkyl, more preferably C 1-8 Alkyl, most preferably C 1-4 Alkyl aminating agent.
[0033] In a preferred embodiment, the following mono- and di-alkylamines are used as aminating agents: monomethylamine, dimethylamine, monoethylamine, diethylamine, n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, isopropylethylamine, n-butylamine, di-n-butylamine, sec-butylamine, di-sec-butylamine, isobutylamine, diisobutylamine, n-pentylamine, di-n-pentylamine, sec-pentylamine, di-sec-pentylamine, isopentylamine, diisopentylamine, n-hexylamine, di-n-hexylamine, sec-hexylamine, di-sec-hexylamine, isohexylamine and diisohexylamine.
[0034] Particularly preferred aminating agents are monomethylamine, monoethylamine, dimethylamine and diethylamine. Very particular preference is given to using dimethylamine and diethylamine as aminating agents.
[0035] The conversion of glycolaldehyde with the aminating agent is carried out in the presence of hydrogen.
[0036] Hydrogen is usually used in technical grade purity. Hydrogen can also be used in the form of a gas comprising hydrogen, i.e. a mixture with other inert gases such as nitrogen, helium, neon, argon or carbon dioxide. However, preference is given to using pure hydrogen or substantially pure hydrogen, for example hydrogen with a hydrogen content of more than 99% by weight, preferably more than 99.9% by weight of hydrogen, more preferably more than 99.99% by weight of hydrogen, in particular more than 99.999% by weight of hydrogen.
[0037] The conversion of glycolaldehyde with the aminating agent is carried out in the presence of a catalyst.
[0038] The catalyst may in principle comprise nickel, cobalt, iron, copper, chromium, manganese, copper, molybdenum, tungsten and / or other metals of Groups 8 and / or 9 and / or 10 and / or 11 of the Periodic Table of the Elements.
[0039] Preference is given to using a catalyst comprising at least one metal selected from the group consisting of Cu, Co, Ni, Pd, Pt, Ru, Rh, Ag, Au, Re and Ir.
[0040] More preferably, a catalyst comprising at least one metal selected from the group consisting of Cu, Co, Ni, Pd, Pt and Ru is used.
[0041] The abovementioned catalysts can be doped in a customary manner with promoters, for example with chromium, iron, cobalt, manganese, molybdenum, titanium, tin, metals of the alkali metal group, metals of the alkaline earth metal group and / or phosphorus.
[0042] The catalyst may be a supported or unsupported catalyst.
[0043] Suitable support materials are carbon compounds, for example graphite, carbon black and / or activated carbon, aluminum oxide (gamma, delta, theta, alpha, kappa, chi or mixtures thereof), silicon dioxide, zirconium dioxide, zeolites, aluminosilicates or mixtures thereof.
[0044] In a preferred embodiment of the present invention, Raney-type catalysts are used.
[0045] As the Raney catalyst, it is preferred to use a Raney cobalt catalyst, a Raney nickel catalyst and / or a Raney copper catalyst. A Raney cobalt catalyst is particularly preferred.
[0046] In another preferred embodiment of the present invention, the catalyst is prepared by reducing a catalyst precursor, wherein the above-mentioned metals are present in the form of oxygen-containing compounds, such as their oxides, carbonates or bicarbonates.
[0047] The catalyst precursor can be prepared by known methods, for example by precipitation, application by precipitation or impregnation.
[0048] In a preferred embodiment, catalyst precursors which have been prepared by impregnation of a support material are used in the process according to the invention (impregnated catalyst precursors).
[0049] The support material used in the impregnation can be used, for example, in the form of powders or shaped bodies, such as extrudates, tablets, spheres or rings. Support materials suitable for fluidized bed reactors are preferably obtained by spray drying.
[0050] Useful support materials include, for example, carbon such as graphite, carbon black and / or activated carbon, aluminum oxide (gamma, delta, theta, alpha, kappa, chi or mixtures thereof), silicon dioxide, zirconium dioxide, zeolites, aluminosilicates or mixtures thereof.
[0051] The above-mentioned support materials can be impregnated by conventional methods (ABStiles, Catalyst Manufacture-Laboratoryand Commercial Preparations, Marcel Dekker, New York, 1983), for example by applying a metal salt solution in one or more impregnation steps. Useful metal salts generally include water-soluble metal salts, such as nitrates, acetates or chlorides of the corresponding catalytically active components or doping elements, such as cobalt nitrate or cobalt chloride. Subsequently, the impregnated support material is usually dried and optionally calcined.
[0052] The impregnation can also be carried out by the so-called "incipient wetness method", in which the support material is wetted with the impregnation solution until maximum saturation, depending on the water absorption capacity of the support material. However, the impregnation can also be carried out in the supernatant.
[0053] In the case of a multi-step impregnation process, drying and, if appropriate, calcination between the individual impregnation steps is appropriate.Multi-step impregnation can be used advantageously when the support material is contacted with relatively large amounts of metal salt.
[0054] To apply a plurality of metal components to the support material, the impregnation can be carried out simultaneously with all metal salts or in any desired sequence of the individual metal salts.
[0055] In another preferred embodiment, the catalyst precursor is prepared by coprecipitation of all its components. To this end, usually, soluble compounds of the corresponding active components and doping elements and optionally soluble compounds of the support material are mixed with a precipitant in a liquid while heating and stirring until precipitation is complete.
[0056] The liquid used is usually water.
[0057] Useful soluble compounds of the active ingredients generally include the corresponding metal salts, for example nitrates, sulfates, acetates or chlorides of the abovementioned metals.
[0058] The soluble compounds of the support materials used are generally water-soluble compounds of Ti, Al, Zr, Si, etc., for example water-soluble nitrates, sulfates, acetates or chlorides of these elements.
[0059] The soluble compounds of the doping elements used are generally water-soluble compounds of the doping elements, for example water-soluble nitrates, sulfates, acetates or chlorides of these elements.
[0060] The catalyst precursor can also be prepared by precipitation application.
[0061] Application by precipitation is understood to mean a preparation process in which a sparingly soluble or insoluble support material is suspended in a liquid, to which a soluble compound of an appropriate metal oxide, for example a soluble metal salt, is then added and which is then precipitated onto the suspended support by adding a precipitant (described, for example, in EP-A2-1106600, page 4 and ABStiles, Catalyst Manufacture, Marcel Dekker, Inc., 1983, page 15).
[0062] Useful sparingly soluble or insoluble support materials include, for example, carbon compounds such as graphite, carbon black and / or activated carbon, aluminum oxide (gamma, delta, theta, alpha, kappa, chi or mixtures thereof), silicon dioxide, zirconium dioxide, zeolites, aluminosilicates or mixtures thereof.
[0063] The support material is usually in the form of a powder or chips.
[0064] The liquid used in which the carrier material is suspended is generally water.
[0065] Useful soluble compounds include soluble compounds of the above-mentioned active components or doping elements.
[0066] Typically, in a precipitation reaction, a soluble compound is precipitated as a sparingly soluble or insoluble basic salt by adding a precipitant.
[0067] The precipitating agent used is preferably a base, especially an inorganic base, such as an alkali metal base. Examples of precipitating agents are sodium carbonate, sodium hydroxide, potassium carbonate or potassium hydroxide.
[0068] The precipitants used may also be ammonium salts, for example ammonium halides, ammonium carbonate, ammonium hydroxide or ammonium carboxylates.
[0069] The precipitation reaction can be carried out, for example, at a temperature of 20-100°C, preferably 30-90°C, especially 50-70°C.
[0070] The precipitate formed in the precipitation reaction is generally chemically inhomogeneous and generally comprises a mixture of oxides, hydrated oxides, hydroxides, carbonates and / or bicarbonates of the metals used. It has been found that the filterability of the precipitate is favoured when the precipitate is aged, i.e. when, after precipitation, the precipitate is left alone for a certain period of time, if appropriate under hot conditions or with air passing through it.
[0071] The precipitates obtained by these precipitation methods are usually processed by washing, drying, calcining and conditioning them.
[0072] After washing, the precipitate is generally dried at 80-200° C., preferably 100-150° C., and then calcined.
[0073] Calcination is usually carried out at a temperature of 300-800°C, preferably 350-600°C, especially 450-550°C.
[0074] After calcination, the pulverulent catalyst precursor obtained by precipitation reaction is generally conditioned.
[0075] Adjustment can be carried out, for example, by adjusting the precipitated catalyst to a specific particle size by grinding.
[0076] After grinding, the catalyst precursor obtained by precipitation reaction can be mixed with shaping aids such as graphite or stearic acid and processed further to give shaped bodies.
[0077] Commonly used shaping methods are described, for example, in Ullmann [Ullmann's Encyclopaedia Electronic Release 2000, chapter: "Catalysis and Catalysts", pages 28-32] and Ertl et al. [Ertl, Weitkamp, Handbook of Heterogeneous Catalysis, VCH Weinheim, 1997, pp. 98 ff.].
[0078] As described in the cited references, the shaping process can provide a shaped body of any three-dimensional shape, such as round, angular, elongated, etc., such as in the form of extrudates, tablets, granules, balls, cylinders or granules. Common shaping processes are, for example, extrusion, tableting, i.e. mechanical pressing, or granulation, i.e. compaction by circular and / or rotary motion.
[0079] After conditioning or shaping, a heat treatment is usually carried out. The temperature of the heat treatment usually corresponds to the calcination temperature.
[0080] The catalyst precursor obtained by the precipitation reaction comprises the catalytically active components in the form of a mixture of their oxygen compounds, ie in particular oxides, mixed oxides and / or hydroxides. The catalyst precursor prepared in this way can be stored as such.
[0081] The catalyst used in the process of the invention is obtained by reducing a catalyst precursor which has been prepared by impregnation or precipitation as described above after calcination or conditioning.
[0082] The reduction of the dry, usually pulverulent catalyst precursor can be carried out at elevated temperature in mobile or stationary reduction furnaces.
[0083] The reducing agent used is generally hydrogen or a gas containing hydrogen.
[0084] The hydrogen is usually used in technical purity. The hydrogen can also be used in the form of a hydrogen-containing gas, i.e. mixed with other inert gases such as nitrogen, helium, neon, argon or carbon dioxide. The hydrogen stream can also be circulated as cycle gas to the reduction reaction, optionally mixed with fresh hydrogen and optionally after removal of water by condensation.
[0085] The catalyst precursor is preferably reduced in a reactor in which the shaped catalyst bodies are arranged in the form of a fixed bed. The catalyst precursor is more preferably reduced in the same reactor in which the glycolaldehyde is converted with the aminating agent.
[0086] Alternatively, the catalyst precursor may be reduced in a fluidized bed in a separate fluidized bed reactor.
[0087] The catalyst precursor is generally reduced at a reduction temperature of 50-600°C, especially 100-500°C, more preferably 150-450°C.
[0088] The hydrogen partial pressure is generally in the range from 1 to 300 bar, in particular from 1 to 200 bar, more preferably from 1 to 100 bar, the pressure figures here and hereinafter being based on the absolute measured pressure.
[0089] The reduction time is preferably 1 to 20 hours, more preferably 5 to 15 hours.
[0090] During the reduction, a solvent may be provided to remove the reaction water formed and / or in order, for example, to be able to heat the reactor faster and / or to be able to remove heat better during the reduction. In this case, the solvent may also be provided in supercritical form.
[0091] Suitable solvents used may be the above-mentioned solvents. Preferred solvents are water; ethers, such as methyl tert-butyl ether, ethyl tert-butyl ether, dioxane or tetrahydrofuran. Particularly preferred are water or tetrahydrofuran. Suitable solvents also include suitable mixtures.
[0092] The catalyst precursor can also be reduced in suspension, for example in a stirred autoclave. The temperature is generally from 50 to 300°C, in particular from 100 to 250°C, more preferably from 120 to 200°C.
[0093] The suspension reduction is usually carried out at a hydrogen partial pressure of 1 to 300 bar, preferably 10 to 250 bar, more preferably 30 to 200 bar. Usable solvents include the above-mentioned solvents.
[0094] The suspension reduction time is preferably 5-20 hours, more preferably 8-15 hours.
[0095] After reduction, the catalyst can be handled under inert conditions. The catalyst can preferably be handled and stored under an inert gas such as nitrogen, or under an inert liquid such as an alcohol, water or the product of the specific reaction in which the catalyst is used. If appropriate, the inert liquid must be removed from the catalyst before the actual reaction begins.
[0096] Storage of the catalyst under inert substances makes handling and storage of the catalyst uncomplicated and safe.
[0097] After reduction, the catalyst can also be contacted with an oxygen-containing gas stream such as air or a mixture of air and nitrogen. This provides a passivated catalyst. The passivated catalyst generally has a protective oxide layer. The protective oxide layer simplifies the handling and storage of the catalyst, so that, for example, the installation of the passivated catalyst in the reactor is simplified.
[0098] After passivation, the catalyst is usually activated. The catalyst can be activated by reducing the passivated catalyst. The passivated catalyst can be reduced by treating the passivated catalyst with hydrogen or a gas containing hydrogen as described above. The reduction conditions usually correspond to the reduction conditions used in the reduction of the catalyst precursor. Activation usually eliminates the protective passivation layer.
[0099] The activated catalyst must be handled under inert conditions during and after its activation reduction.
[0100] The activated catalyst is preferably handled and stored under an inert gas such as nitrogen, or under an inert liquid such as an alcohol, water or the product of the specific reaction in which the catalyst is used. If appropriate, the activated catalyst must then be freed of the inert liquid before the actual reaction begins.
[0101] Activation of the catalyst can also be carried out in situ during the conversion step of converting glycolaldehyde with an aminating agent.
[0102] According to the invention, glycolaldehyde is converted with an aminating agent in the gas phase.
[0103] In the context of the present invention, "reacting or converting in the gas phase" means adjusting the reaction conditions such as pressure and temperature so that glycolaldehyde and the aminating agent are present in the gas phase and flow around the catalyst in gaseous form.
[0104] Suitable reactors for the gas phase conversion of glycolaldehyde with an aminating agent are generally tubular reactors and fluidized bed reactors.
[0105] The catalyst can be arranged in the tubular reactor as a moving bed or as a fixed bed.
[0106] Particular preference is given to converting glycolaldehyde with an aminating agent in a tubular reactor in which the catalyst is arranged in the form of a fixed bed.
[0107] In another particular embodiment, glycolaldehyde is converted with an aminating agent in a fluidized bed reactor.
[0108] Since the process according to the invention is carried out in the gas phase, glycolaldehyde is preferably provided to the process according to the invention in gaseous form.
[0109] In a preferred embodiment, the reactants are transferred to the gas phase by evaporating the reactants in pure form or by evaporating a mixture of the reactants and one or more solvents.
[0110] In a preferred embodiment, the glycolaldehyde is provided in gaseous form by evaporating pure glycolaldehyde and / or the aminating agent is provided in gaseous form by evaporating pure aminating agent.
[0111] In a more preferred embodiment, the reactants are transferred to the vapor phase by evaporating a mixture of the reactants in one or more solvents.
[0112] Preferably, the one or more solvents are selected from water, alcohols, acyclic or cyclic ethers, polyalkyl ethers and alkoxy polyalkyl ethers.
[0113] More preferably, the one or more solvents are selected from water, methanol, ethanol, methyl tert-butyl ether, ethyl tert-butyl ether, dioxane, tetrahydrofuran, tetraethylene glycol dimethyl ether (tetraglyme), dipropylene glycol dimethyl ether or bis(2-methoxyethyl) ether (diglyme).
[0114] It is generally preferred to transfer glycolaldehyde to the gas phase in the absence of an aminating agent, and vice versa. It has been found that glycolaldehyde and an aminating agent can form a higher boiling compound if they are present together in the liquid phase before evaporation.
[0115] Therefore, it is preferred that the content of aminating agent in the glycolaldehyde to be evaporated or its solvent mixture is less than 30% by weight, preferably less than 10% by weight, most preferably less than 1% by weight, based on the total weight of glycolaldehyde, one or more solvents and any aminating agent present in these mixtures. However, as mentioned above, it is preferred that the evaporation of glycolaldehyde is carried out in the absence of any aminating agent.
[0116] Thus, it is preferred that the glycolaldehyde content of the aminating agent or its solvent mixture to be evaporated is less than 30% by weight, preferably less than 10% by weight, most preferably less than 1% by weight, based on the total weight of the aminating agent, one or more solvents and any glycolaldehyde present in these mixtures. However, as previously mentioned, it is preferred that the evaporation of the aminating agent is carried out in the absence of any glycolaldehyde.
[0117] Most preferably, glycolaldehyde is transferred into the gas phase from a mixture wherein the fraction of water in the solvent or solvents in the mixture is 25-100 wt. %, preferably 50-100 wt. %, more preferably 75-100 wt. %.
[0118] Most preferably, the glycolaldehyde is transferred to the gas phase by evaporating a mixture of glycolaldehyde and a solvent, wherein water is the only solvent.
[0119] The weight content of glycolaldehyde in the mixture of one or more solvents is preferably from 1 to 90% by weight, based on the total weight of glycolaldehyde and the one or more solvents.
[0120] In a preferred embodiment, the weight content of glycolaldehyde in the mixture of one or more solvents is 2-50% by weight, more preferably 5-35% by weight, most preferably 5-20% by weight, based on the total weight of glycolaldehyde and the one or more solvents.
[0121] Most preferably, the aminating agent is transferred into the gas phase from a mixture wherein the fraction of water in the one or more solvents in the mixture is 50-100 wt. %, preferably 60-100 wt. %, more preferably 80-100 wt. %.
[0122] Most preferably, the aminating agent is transferred to the gas phase by evaporating a mixture of aminating agent and solvent, wherein water is the only solvent.
[0123] Most preferably, the aminating agent is transferred into the gas phase by evaporation of the pure compound.
[0124] The weight content of the aminating agent in the mixture of one or more solvents is preferably 1-90% by weight, more preferably 0-80% by weight, most preferably 25-75% by weight, based on the total weight of the aminating agent and the one or more solvents.
[0125] The evaporation of the reactants or their respective solvent mixtures can be carried out by operations well known in the art, such as by heating the liquid to a temperature above the boiling point of the reactants and / or by reducing the pressure and / or by passing a gas stream over the liquid reactants or solvent mixture.
[0126] Preferably, the reactants are transferred to the gas phase by heating the reactants or their solvent mixture in the gas stream to evaporate them.
[0127] The gas is preferably hydrogen or an inert gas, such as nitrogen or a rare gas, such as He, Ne, Ar, Kr or Xe. Preferably, the gas is hydrogen, nitrogen or a mixture thereof.
[0128] Evaporators which can be used for evaporating glycolaldehyde and its respective solvent mixtures are natural or forced circulation evaporators, falling film evaporators, rising film (or long tube vertical) evaporators, rising and falling film plate evaporators, multiple effect evaporators and stirred thin film evaporators. The evaporation can also be carried out by flash evaporation.
[0129] In a more preferred embodiment, the gaseous reactants are provided to the process of the invention by feeding reactants obtained from a preparation process for providing the gaseous reactants.
[0130] Preferably, glycolaldehyde is provided in gaseous form by feeding in a gaseous effluent obtained from a process for the preparation of glycolaldehyde.
[0131] The gaseous glycolaldehyde is preferably obtained by cleaving an organic raw material, such as an aqueous sugar solution or wood, at high temperature.
[0132] More preferably, glycolaldehyde is in gaseous form, obtained by hydrothermal decomposition of sugars, for example as disclosed in US 2004 / 0022912 (which is incorporated herein by reference), or by pyrolysis of wood as described by D. Mohan et al. ("Pyrolysis of Wood / Biomass for Bio-Oil", Energy Fuels 2006, 20, 3, 848-889) or C.R. Vitasari (Extraction of bio-based Glycolaldehyde from wood-derived pyrolysis oils Eindhoven: Technische Universiteit Eindhoven DOI: 10.6100 / IR738958), which are also incorporated herein by reference.
[0133] Preferably, the glycolaldehyde concentration in the product stream of such processes is from 5 to 90% by weight, most preferably from 10 to 80% by weight, most preferably from 15 to 70% by weight.
[0134] The streams obtained by such processes may comprise other oxygenates, for example formaldehyde, hydroxyacetone (acetol), dihydroxyacetone, glyoxal, methylglyoxal (methylglyoxal), acetic acid, levulinic acid, propionic acid, acrylic acid, methanol, acetone and formic acid.
[0135] Preferably, the aminating agent is provided in gaseous form by feeding a gaseous effluent obtained from a process for the preparation of the aminating agent. This gaseous stream can be obtained during the refining of the aminating agent. For example, the preparation of ammonia or lower alkylamine provides ammonia or lower alkylamine in the gaseous phase when the aminating agent is separated from high-boiling components at the top of a distillation column. Instead of condensing the gaseous stream obtained at the top of a distillation column, the gaseous aminating agent can be directly provided to the process of the invention.
[0136] The glycolaldehyde provided in its gaseous form and the aminating agent provided in its gaseous form may be fed separately into the reactor, or they may be mixed to obtain a mixed feed stream.
[0137] The proportion of glycolaldehyde present in the process according to the invention is generally from 0.01 to 10% by volume, preferably from 0.1 to 8% by volume and even more preferably from 0.5 to 5% by volume.
[0138] The molar ratio of aminating agent to glycolaldehyde present in the process of the present invention is generally 1:1 to 100:1, preferably 5:1 to 75:1, more preferably 10:1 to 50:1, and particularly preferably 12.5:1 to 40:1.
[0139] The molar ratio of hydrogen to glycolaldehyde present in the process of the present invention is generally from 10:1 to 500:1, preferably from 20:1 to 400:1, more preferably from 50:1 to 250:1, even more preferably from 75:1 to 200:1.
[0140] The proportion of solvent in the gas stream present in the process of the invention is generally 0-20% by volume, preferably 0.1-15% by volume, even more preferably 0.5-10% by volume. The solvent present in the process is preferably (i) those solvents used to prepare the solution from which the reactant is evaporated, or (ii) those solvents together with the reactants from the gaseous effluent stream of its preparation process, for example, gaseous glycolaldehyde derived from the hydrothermal decomposition of sugars usually contains water. Most preferably, the water fraction in the one or more solvents present in the process is 50-100% by weight, preferably 60-100% by weight, more preferably 80-100% by weight.
[0141] Most preferably, water is the only solvent present in the process.
[0142] Optionally, the gas stream present in the process of the invention contains an inert gas. Preferred inert gases are rare gases, such as He, Ne, Ar, nitrogen and mixtures thereof. Very particularly preferred inert gases are Ar and nitrogen, or mixtures thereof. The proportion of inert gas in the gas stream contacted with the catalyst is generally 5-90% by volume, preferably 10-80% by volume, even more preferably 25-60% by volume, in particular 30-50% by volume.
[0143] The loading amount of the catalyst is preferably 0.01-2 kg / L / h, more preferably 0.025-1.5 kg / L / h, more preferably 0.05-1 kg / L / h.
[0144] Preferably, the reaction of glycolaldehyde with an aminating agent in the gas phase is carried out at a pressure of 0.1-200 bar (0.01-20 MPa), more preferably 0.5-100 bar (0.05-10 MPa), even more preferably 1-50 bar (0.1-5 MPa), particularly preferably 1-30 bar (0.1-3 MPa).
[0145] The temperature is preferably 120-600°C, more preferably 130-500°C, even more preferably 135-350°C, particularly preferably 140-270°C.
[0146] The product stream obtained by converting glycolaldehyde by amination in the process of the invention may comprise unreacted glycolaldehyde and unreacted aminating agent as well as hydrogen.
[0147] Furthermore, the product stream comprises substituted and unsubstituted ethyleneamines, ethanolamines and aminoethylamines.
[0148] If the aminating agent is ammonia, the product stream preferably comprises ethylenediamine, monoethanolamine, diethanolamine and triethanolamine.
[0149] If the aminating agent is a primary alkylamine, the product stream preferably comprises N-alkylethanolamine, N-alkyldiethanolamine and dialkylethylenediamine. Thus, when methylamine (MA) is used as the aminating agent, the product stream comprises N-methylethanolamine, N-methyldiethanolamine and dimethyldiethylenediamine.
[0150] If the aminating agent is a secondary alkylamine, the product stream preferably comprises dialkylethanolamines and tetraalkylethylenediamines. Thus, when dimethylamine (DMA) is used as aminating agent, the product stream comprises dimethylethanolamine (DMEOA) and tetramethylethylenediamine (TMEDA).
[0151] Additionally, the product stream may contain one or more solvents.
[0152] Furthermore, the product stream may comprise other components which are fed into the GA reactor or which are formed as by-products during the conversion reaction, for example oxygenates such as formaldehyde, hydroxyacetone (acetol), dihydroxyacetone, glyoxal, methylglyoxal (methylglyoxal), methanol and acetone.
[0153] The output of the reactor, optionally comprising catalyst, is typically separated from the gaseous components by suitable means, such as by solids separation, typically configured as a centrifugal separator (or cyclone separator).
[0154] The gaseous output is usually worked up in such a way that the different components can be separated from one another.
[0155] For this purpose, the gaseous output is preferably partially condensed so that the hydrogen and any lower-boiling aminating agent remain in the gas phase and the other components present in the output are converted into the liquid phase. The gaseous components are usually separated from the liquid components in a gas / liquid separator. The gaseous components can be recycled to the amination reactor individually (after further work-up steps) or together.
[0156] After separation of hydrogen and any low-boiling aminating agent, the output of the amination reactor generally comprises aminating agent, unconverted glycolaldehyde, optionally solvent and amination product and other components, such as components introduced with the reactant stream or by-products formed during the conversion.
[0157] Preferably, the mixture is subjected to a multi-stage distillation, wherein the reaction product or a suitable fraction thereof can be obtained in purified form.
[0158] It has surprisingly been found that the conversion of glycolaldehyde with an aminating agent in the gas phase allows for the conversion of glycolaldehyde with an aminating agent in an aqueous environment.
[0159] Within the framework of the present invention, it was found that the conversion of glycolaldehyde and aminating agent in the liquid phase in water leads to lower conversions and lower yields of ethyleneamines and / or ethanolamines.
[0160] The process of the present invention allows the use of water which is highly desirable from a processing standpoint since glycolaldehyde and aminating agents are typically produced and prepared in the form of their aqueous solutions.
[0161] The conversion of glycolaldehyde in the presence of water has the additional advantage that water is a readily available and inexpensive solvent and has a high solubility for glycolaldehyde. In addition, the treatment and recycling of water is relatively unproblematic and can be carried out in waste treatment plants, allowing the treated water to be discharged into the environment or used for other applications. Example:
[0162] The present invention is illustrated by the following examples:
[0163] Example 1 (Comparative Example): Liquid Phase Conversion
[0164] Before introduction into the autoclave, the passivated catalysts A and B were activated as follows:
[0165] In run 1, catalyst A was reduced at 240°C and 1 bar hydrogen partial pressure for 8 hours. In run 2, catalyst B was reduced at 200°C and 1 bar hydrogen partial pressure for 8 hours.
[0166] Subsequently, an aqueous glycolaldehyde solution (7.5 wt % or 15 wt %) was added to an electrically heated 300 mL autoclave with a mechanical magnetic coupling stirrer under an inert atmosphere. Dimethylamine was metered in according to the molar ratios described in Table 1 and the mixture was heated to a reaction temperature of 160° C. After reaching this temperature, the reactor was pressurized to 100 bar by injecting hydrogen.
[0167] The product stream was analyzed by gas chromatography and is reported in Table 1:
[0168] Table 1:
[0169]
[0170] Example 2: Gas Phase Conversion
[0171] A 1000 mm long, 40 mm diameter double-walled glass reactor was installed vertically and the outlet (bottom) was connected to a collecting flask. The reactor had oil heating, a quartz glass frit at the bottom, a liquid and gas feed inlet connected to a pump at the top, and a gas feed (H2, optionally N2 and aminating agent) measured by a rotor flowmeter. It was equipped with a water cooler and an additional dry ice cooler. The exhaust gas was connected to a laboratory fume hood. In the center of the reactor, a glass tube was placed from top to bottom, and a flexible thermocouple was introduced into the tube. The reactor was filled with three layers. First, 400 mL of Raschig rings consisting of a steel mesh (5 mm in diameter) were loaded onto the quartz glass frit. Then, a catalyst (100 mL, see Table 2) was introduced. The height of the catalyst bed was about 80 mm. Above the catalyst bed, 450 mL of Raschig rings were loaded, which served as an evaporator and heating zone for liquid feed and gas feed. The feed port for the aminating agent was located at the center of about 10 cm above the catalyst bed through a steel capillary fixed on a thermocouple. The Raschig ring bed between the aminating agent feed inlet and the catalyst ensures thorough mixing of DMA and gaseous GA.
[0172] Prior to the experiments, the catalyst was activated at 240°C in a flow of hydrogen.
[0173] The tubular reactor was heated to the reaction temperature shown in Table 2.
[0174] Gaseous DMA was metered from a bottle and introduced into the reactor via a capillary. The amount of DMA in the gas stream corresponds to the amount stated in Table 2.
[0175] The GA solution was fed directly to the top of the evaporator bed in the reactor. Hydrogen was added to the reactor from the top of the evaporator bed downward through the reactor at 1 bar. The GA solution was evaporated by a combination of heating and continuous entrainment of hydrogen, and the evaporator bed acted as a heater for the GA / hydrogen stream. The amount of GA in the gas stream corresponded to the amount described in Table 2. The concentration of the GA aqueous solution from which GA was evaporated is also given in Table 2.
[0176] The mixed gas stream of GA and water, hydrogen and aminated DMA passed through the catalyst bed and was partially condensed in the two coolers mentioned above. The condensed material was collected in a collection flask. Liquid samples were taken from the flask regularly.
[0177] The gas hourly space velocity (GHSV) is also given in Table 2.
[0178] The composition of the liquid sample was determined by gas chromatography to obtain the mass fraction of the main components. Taking into account the amount of the condensed product stream and the quality of the glycolaldehyde feed, the productive rates of the main valuable products ethylene glycol (MEG), dimethylethanolamine (DMEOA) and tetramethylethylenediamine (TMEDA) were calculated. The results are reported in Table 2.
[0179] Table 2:
[0180]
[0181] Catalyst A is a catalyst comprising 45% by weight of Cu and 10% by weight of Ni on an alumina support. The preparation of the catalyst was carried out according to the examples in EP-B1-2346602.
[0182] Catalyst B is a catalyst comprising 56% by weight of Cu on an alumina support, based on the total weight of the catalyst, as used in Example 1 of EP-A2-0514692.
[0183] Comparison of Example 1 with Example 2 shows that the liquid phase conversion of glycolaldehyde with an aminating agent in water produces only small amounts of the desired product. The gas phase conversion gives significantly higher yields.
Claims
1. A method for converting glycolaldehyde with an aminating agent in the presence of hydrogen and a catalyst, wherein the conversion is carried out in the gas phase in the presence of one or more solvents, wherein the weight fraction of water in the one or more solvents present in the method is 50-100 weight %, and wherein the aminating agent is a compound of formula (I): in: R 1 , R 2 For H, C 1-8 Alkyl, C 3-12 Cycloalkyl, C 2-30 Alkoxyalkyl, or together with -(CH 2 ) j -X-(CH 2 ) k -, X is CHR 3 , R 3 H or C 1-4 alkyl, j, k are integers of 1-4 respectively.
2. The process according to claim 1, wherein glycolaldehyde is supplied to the process in gaseous form and wherein the aminating agent is supplied to the process in gaseous form.
3. The process according to claim 2, wherein glycolaldehyde is provided to the process in gaseous form by evaporating glycolaldehyde from a mixture of glycolaldehyde and one or more solvents, wherein the content of glycolaldehyde is from 2 to 50% by weight, based on the total weight of glycolaldehyde and the one or more solvents.
4. The process according to claim 2, wherein the aminating agent is provided to the process in gaseous form by evaporating the aminating agent in pure form or by evaporating a mixture of the aminating agent in one or more solvents.
5. The process according to claim 3, wherein the aminating agent is provided to the process in gaseous form by evaporating the aminating agent in pure form or by evaporating a mixture of the aminating agent in one or more solvents.
6. The process according to claim 2, wherein glycolaldehyde is provided to the process in gaseous form by feeding a gaseous effluent obtained from the preparation of glycolaldehyde.
7. The method according to claim 6, wherein glycolaldehyde in gaseous form is obtained from the hydrothermal decomposition of sugars or the pyrolysis of wood.
8. The process according to any one of claims 2 to 7, wherein the aminating agent supplied to the process is converted into its gaseous form in the absence of glycolaldehyde, and the glycolaldehyde supplied to the process is converted into its gaseous form in the absence of the aminating agent.
9. The process according to any one of claims 2 to 7, wherein the gaseous aminating agent and the gaseous glycolaldehyde are supplied to the process separately, or wherein the gaseous aminating agent and the gaseous glycolaldehyde are mixed to obtain a mixed feed stream.
10. The process according to claim 8, wherein the gaseous aminating agent and the gaseous glycolaldehyde are supplied separately to the process, or wherein the gaseous aminating agent and the gaseous glycolaldehyde are mixed to obtain a mixed feed stream.
11. The process according to any one of claims 1 to 7, wherein glycolaldehyde is present in the process in a proportion of 1 to 50% by volume.
12. The process according to claim 10, wherein the glycolaldehyde is present in the process in a proportion of 1-50% by volume.
13. The process according to any one of claims 1 to 7, wherein the molar ratio of glycolaldehyde to aminating agent present in the process is from 1:1 to 100, and wherein the molar ratio of hydrogen to glycolaldehyde present in the process is from 10:1 to 500:
1.
14. The process of claim 12, wherein the molar ratio of glycolaldehyde to aminating agent present in the process is from 1:1 to 100, and wherein the molar ratio of hydrogen to glycolaldehyde present in the process is from 10:1 to 500:
1.
15. The process according to any one of claims 1 to 7, wherein the proportion of solvent present in the process is 1 to 50% by volume.
16. The process according to claim 14, wherein the solvent is present in the process in a proportion of 1-50% by volume.
17. The process according to any one of claims 1 to 7, wherein the conversion of glycolaldehyde is carried out at a pressure of 0.01 to 200 bar and a temperature of 120 to 600°C.
18. The process according to claim 16, wherein the conversion of glycolaldehyde is carried out at a pressure of 0.01-200 bar and a temperature of 120-600°C.