Catalyst for hydrogenation reaction and preparation method thereof

By supporting a nickel-based catalyst with copper and sulfur accelerator on the silica support, the problems of reduced activity of nickel-based catalysts and difficulty in selective hydrogenation are solved, and the effect of efficient preparation of water white resin is achieved.

CN114007742BActive Publication Date: 2024-11-01HANWHA SOLUTIONS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080041518.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2020-06-25
Publication Date
2024-11-01
Estimated Expiration
2040-06-25

AI Technical Summary

Technical Problem

In the hydrogenation reaction of petroleum resin, the existing nickel-based catalysts have the problem of increasing nickel crystal size and reducing activity, and it is difficult to achieve selective hydrogenation of aromatic and olefins, which affects the preparation of water white resin.

Method used

A nickel-based catalyst containing copper and sulfur as accelerator is used to support nickel on the silica support by deposition-precipitation method, which optimizes the particle size and dispersion of the catalyst, and improves the reduction degree and catalytic activity of nickel.

Benefits of technology

The control of nickel crystal size is achieved, the dispersion and activity of the catalyst is improved, the selective hydrogenation capacity of aromatics and olefins is enhanced, and the water white resin is easy to prepare.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114007742B_ABST
    Figure CN114007742B_ABST
Patent Text Reader

Abstract

The present invention uses copper and sulfur as promoters when preparing a hydrogenation catalyst containing nickel as an active substance, so that nickel can be easily reduced. In particular, a catalyst having a high nickel content and containing sulfur oxide and nickel oxide in a specific range can provide a catalyst having high catalyst activity and a higher degree of selective reduction of olefins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst for hydrogenation reaction and a preparation method thereof, and in particular to a nickel-based catalyst for hydrogenation reaction of petroleum resin, which contains nickel or nickel oxide as an active substance and contains copper and sulfur as promoters. Background Art

[0002] Lower olefins such as ethylene, propylene, butene and pentadiene and aromatic compounds are widely used as basic intermediates in petrochemical and chemical industries. Thermal cracking or steam pyrolysis is a typical process for forming these substances in the presence of steam and the absence of oxygen. The raw materials may include petroleum gases and distillates such as naphtha, kerosene and gas oil. At this time, naphtha etc. can be pyrolyzed to generate materials such as ethylene, propylene, C4 fractions including butane and butadiene, cracked gasoline (including benzene, toluene and xylene), cracked kerosene (C9 fractions), cracked heavy oil (ethylene residue (bottom oil)) and hydrogen, and the fractions can be polymerized to prepare petroleum resins.

[0003] However, some petroleum resins contain unsaturated bonds, so the quality is reduced. In this case, the unsaturated bonds can be removed through the hydrogenation process of hydrogenation, thereby improving the color and reducing the peculiar smell of petroleum resin. In addition, the petroleum resin after the unsaturated bonds are removed is colorless and transparent, so it is called water white resin and circulated as a high-grade resin with outstanding heat resistance and ultraviolet stability.

[0004] Petroleum resins copolymerized from C5 fractions, C9 fractions, and dicyclopentadiene (DCPD) have the characteristic of adjusting the compatibility with styrene-based polymers such as styrene-isoprene-styrene (SIS) and styrene-butadiene-styrene (SBS) according to the aromatic content. Therefore, when the petroleum resin is hydrogenated, in order to prepare a water-white resin while controlling the aromatic content, the olefin part of the resin needs to be selectively hydrogenated.

[0005] Therefore, in order to hydrogenate unsaturated petroleum resin raw materials, various catalysts have been studied, and in particular, in order to selectively hydrogenate olefins in aromatic unsaturated hydrocarbons, noble metal catalysts such as palladium (Pd) and platinum (Pt) are used, and because the activity and selectivity of palladium catalysts are more excellent compared with other metal catalysts, they are used as selective hydrogenation catalysts. However, when palladium catalysts are hydrogenated in liquid phase, there is a problem in that palladium loss occurs and a Pd complex is formed.

[0006] In addition, when using nickel (Ni) based catalyst, compared with the catalyst comprising other transition metals, there is the advantage of higher activity in hydrogenation. To this, in petroleum resin hydrogenation, preferably comprise at least 40 weight % nickel, to ensure the activity of catalyst. When nickel is loaded on carrier, the larger the nickel content, the smaller the dispersibility, thereby causing the size of nickel crystallization to increase, therefore, there is the problem of reduced activity of catalyst. When reducing nickel content in order to prevent this problem, although dispersibility can be improved relatively, there is the problem of reduced activity. Therefore, it is necessary to maintain the crystal size of nickel at a suitable level while carrying high-content nickel. In addition, olefin and aromatics can be hydrogenated together, therefore, it is difficult to be used for the selective hydrogenation of unsaturated hydrocarbons comprising aromatic groups.

[0007] Therefore, in order to solve these problems, the development of catalysts for hydrogenation reactions is being actively carried out.

[0008] Korean Patent Publication No. 10-2015-0053772 discloses a self-supported mixed metal sulfide (MMS) catalyst for hydrotreating a hydrocarbon feedstock and a method for preparing the catalyst.

[0009] Korean Patent Publication No. 10-1122209 discloses an alumina carrier and a cobalt or nickel metal catalyst supported thereon.

[0010] However, the above patents do not propose a fundamental solution to the problem of selective hydrogenation of aromatics / olefins and simultaneously improve the dispersibility of high-content nickel catalysts, and therefore have limitations.

[0011] Therefore, the inventors of the present invention have developed a nickel-based catalyst containing copper and sulfur as promoters through research, thereby establishing a method for solving the problem of selective hydrogenation of aromatics / olefins and improving the dispersibility of high-content nickel catalysts.

[0012] Furthermore, the present invention has been completed in order to easily secure a water-white resin using the catalyst developed in this way.

[0013] Prior Art Literature

[0014] Patent Literature

[0015] (Patent Document 1) Korean Patent Publication No. 10-2015-0053772 (May 18, 2015)

[0016] (Patent Document 2) Korean Patent Publication No. 10-1122209 (February 23, 2012) Summary of the invention

[0017] Technical issues

[0018] The object of the present invention is to solve all the above problems.

[0019] An object of the present invention is to provide a hydrogenation reaction catalyst, which contains a high content of nickel and has a small nickel crystal size and improved dispersibility, thereby improving activity.

[0020] Another object of the present invention is to include sulfur as a promoter to significantly reduce the hydrogenation rate of aromatics compared to olefins during the hydrogenation reaction of unsaturated hydrocarbons containing aromatic groups, thereby causing olefins to react selectively.

[0021] Another object of the present invention is to control the aromatic content during hydrogenation of a petroleum resin, thereby easily producing a water-white resin.

[0022] Technical Solution

[0023] The characteristic configuration of the present invention for achieving the above-mentioned object of the present invention and realizing the characteristic effects of the present invention described below is as follows.

[0024] According to the present invention, a hydrogenation reaction catalyst is provided. The hydrogenation reaction catalyst comprises an active material, a promoter and a silica carrier.

[0025] According to the present invention, a catalyst for hydrogenation reaction is provided, which comprises 0.5 to 3 parts by weight of a first promoter selected from copper and copper oxide, 3 to 15 parts by weight of a second promoter selected from sulfur and sulfur oxide, and 10 to 40 parts by weight of a silica carrier, relative to 40 to 90 parts by weight of an active material selected from nickel and nickel oxide.

[0026] According to the present invention, the catalyst can be a hydrogenation catalyst in which a precursor forms a precipitate and is supported on a carrier, and can be preferably prepared by a deposition-precipitation (DP) method. The prepared catalyst can be used as a catalyst for hydrogenating petroleum resin by hydrogenation reaction.

[0027] According to another example of the present invention, a method for preparing a catalyst for a hydrogenation reaction is provided, which comprises the following steps: step (a), dissolving 0.01 to 5 parts by weight of one or more promoters selected from copper and copper oxide and 10 to 40 parts by weight of a silica carrier in a solvent relative to 40 to 90 parts by weight of one or more active materials selected from nickel and nickel oxide to prepare a first solution; step (b), adding the first solution to a precipitation container, stirring, and heating to 60 to 100° C.; step (c), after the heating, adding a pH adjuster and 3 to 15 parts by weight of one or more promoters selected from sulfur and sulfur oxide to the precipitation container to prepare a second solution, and dropwise adding the second solution to the first solution to prepare a precipitate; step (d), washing and filtering the precipitate, and then drying it to prepare a dried product; and step (e), reducing the dried product in a hydrogen atmosphere at a temperature of 200 to 500° C. to prepare a reduced product.

[0028] In addition, depending on the situation, the method may further include: after step (d), calcining the prepared dried product in an air atmosphere. The method may further include: after step (e), passivating the catalyst.

[0029] According to the present invention, there is provided a method for hydrogenating a petroleum resin, wherein the petroleum resin is contacted with hydrogen in the presence of a catalyst prepared by the preparation method.

[0030] Beneficial Effects

[0031] According to the present invention, there is provided a catalyst for hydrogenation reaction, which contains a high content of nickel and has a small nickel crystal size and improved dispersibility, thereby improving activity.

[0032] According to the present invention, sulfur is included as a promoter, and when an unsaturated hydrocarbon containing an aromatic group is hydrogenated, the aromatic hydrogenation rate is greatly reduced compared with that of olefins, thereby selectively hydrogenating olefins.

[0033] Therefore, the aromatic content of the unsaturated hydrocarbon containing an aromatic group can be adjusted.

[0034] In addition, the present invention can control the aromatic content when hydrogenating petroleum resin, thereby easily preparing water-white resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a graph showing the hydrogenation reaction results of Examples of the present invention and Comparative Examples. DETAILED DESCRIPTION

[0036] The detailed description of the present invention described below will refer to specific embodiments that can implement the present invention as examples. These embodiments are described in detail so that those skilled in the art can fully implement the present invention. The various embodiments of the present invention are different from each other, but they are not necessarily mutually exclusive. For example, the specific shapes, structures and characteristics recorded herein are associated with an embodiment, and can be implemented with other embodiments without departing from the spirit and scope of the present invention. In addition, the position or configuration of individual constituent elements in each disclosed embodiment can be changed without departing from the spirit and scope of the present invention. Therefore, the detailed description described below is not restrictive, and as long as it is properly described, the scope of the present invention is limited only by the attached claims and their equivalents.

[0037] Hereinafter, the present invention will be described in detail with reference to several preferred embodiments so that those skilled in the art can easily implement the present invention.

[0038] Generally, during the hydrogenation reaction, both olefins and aromatics contained in unsaturated hydrocarbons containing aromatic groups are hydrogenated by the catalyst reaction, so a catalyst capable of selectively hydrogenating olefins is required to adjust the aromatic content in the petroleum resin. When a nickel-based catalyst is used, its activity in the hydrogenation reaction is higher than that of other transition metals, but olefins and aromatics are hydrogenated together, so it is difficult to adjust the aromatic content in the petroleum resin.

[0039] However, the selective hydrogenation catalyst of one embodiment of the present invention uses sulfur as a promoter and supports it together with nickel, so that when unsaturated hydrocarbons containing aromatic groups are hydrogenated, the aromatic hydrogenation rate is greatly reduced compared with olefins, thereby selectively hydrogenating olefins.

[0040] The catalyst for hydrogenation reaction of the present invention comprises an active substance, a promoter and a silica carrier, comprising at least one selected from nickel and nickel oxide as the active substance, comprising at least one selected from copper, sulfur, copper oxide and sulfur oxide as the promoter, and using the silica carrier as a support.

[0041] Provided is a catalyst for hydrogenation reaction, comprising, relative to 40 to 90 parts by weight of one or more active materials selected from nickel and nickel oxide, 0.5 to 3 parts by weight of a first promoter selected from copper and copper oxide, 3 to 15 parts by weight of a second promoter selected from sulfur and sulfur oxide, and 10 to 40 parts by weight of a silica carrier.

[0042] According to the present invention, at this time, the nickel source (precursor) includes nickel and metal salts such as nitrates, acetates, sulfates, chlorides, etc., and the nickel sulfate precursor containing sulfate is most preferred.

[0043] In addition, the copper source (precursor) and the sulfur source (precursor) can be provided in a state of being bound to a metal salt such as nitrate, acetate, sulfate, chloride or a combination thereof, preferably sodium sulfide or copper sulfate. In addition, a precipitant such as sodium carbonate or sodium bicarbonate can be provided.

[0044] In addition, the nickel oxide may be preferably NiO, and the copper oxide may be CuO.

[0045] The catalyst for hydrogenation reaction of the present invention can be prepared by mixing nickel or nickel oxide compounds as active substances and promoters such as copper and copper oxide in a solvent, suspending a solid carrier therein, and allowing the nickel compound and the promoter to form a precipitate, thereby depositing on the silica carrier.

[0046] The nickel is deposited and precipitated (DP) in a manner of being supported on a silica carrier by forming a precipitate with the copper and a promoter such as sulfur.

[0047] The DP (Deposition-Precipitation) method allows a metal precursor salt solution to react with a pH regulator in a carrier dispersion to generate a precipitate, and these precipitates are adsorbed onto the carrier surface and solidified, which reflects the remarkable catalyst uniformity that cannot be matched by the existing metal catalysts prepared by co-precipitation and impregnation methods. Therefore, when preparing a catalyst by the DP method using silica with uniform particle size distribution as a carrier, a carrier with a particle size, size distribution, surface area, pore structure, etc. suitable for the reaction is selected, which has the advantage of being easy to optimize.

[0048] On the other hand, as described above, nickel catalysts have the characteristics of excellent catalytic activity in hydrogenation reactions, but in the DP method of deposition-precipitation in a manner of being supported on a silica support, when a high content of nickel is supported, the crystal size of nickel increases and the dispersibility decreases, so there is a problem of reduced activity. When the nickel content is reduced to prevent this problem, the dispersibility is relatively improved, but there is a problem of reduced catalyst activity, so it is difficult to achieve commercialization through the DP method. In addition, the existing DP method generally performs a reduction reaction at a high temperature of more than 450°C to provide catalyst activation.

[0049] According to the present invention, copper as a promoter is added to nickel and the catalyst composition is loaded on a carrier by a deposition-precipitation method, so that a high nickel reduction degree can be obtained at a lower reduction temperature compared with the existing known methods, and even if loaded by the DP method, the nickel content is high, the nickel crystal size is small, and the dispersion after reduction is high, so a catalyst with excellent activity in a hydrogenation reaction can be provided. That is, there is an effect of optimizing the process for preparing the catalyst, wherein the catalyst has physical properties such as particle size, size distribution, specific surface area, pore structure suitable for the reaction, and the reduction degree of nickel (Ni) metal is high.

[0050] According to the present invention, H2-TPR (Hydrogen-Temperature Program Reduction) can be used for measurement. H2-TPR is used to evaluate the reducing ability of catalyst particles. The reduction degree analysis method based on the analysis method is as follows.

[0051] [Reduction degree analysis method]

[0052]

[0053] ① The bottom area of ​​the TPR graph after hydrogenation

[0054] ②The bottom area of ​​the TPR pattern after firing

[0055] ①Analytical method

[0056] 1) Catalyst usage

[0057] -0.05g

[0058] 2) Catalyst pretreatment

[0059] -Introduce He and raise the temperature to 300℃

[0060] -Introduce H2 and maintain at 300°C for 45 minutes

[0061] -Introduce He and cool at 30℃ for analysis

[0062] 3) H2-TPR analysis

[0063] -Analysis gas: H2 / Ar mixed gas

[0064] - Temperature: from 30℃ to 810℃

[0065] ②Analysis method

[0066] 1) Catalyst usage

[0067] -0.05g

[0068] 2) Catalyst pretreatment

[0069] -Introduce He and raise the temperature to 300℃

[0070] -Introduce H2 and maintain at 300°C for 45 minutes

[0071] -Introduce He and raise the temperature to 400℃

[0072] -Introduce O2 and keep at 400℃ for 2 hours

[0073] - Cool down to 60℃

[0074] 3) H2-TPR analysis

[0075] -Analysis gas: H2 / Ar mixed gas

[0076] - Temperature: from 60℃ to 810℃

[0077] According to the present invention, the active material, the first promoter and the second promoter are included, and 3 to 15 parts by weight of the second promoter may be included relative to a total of 100 parts by weight of the active material, the first promoter and the second promoter. That is, the weight ratio of the second promoter / (active material+first promoter+second promoter) may be (3 to 15) / 100. Therefore, the promoter does not reduce the reduction degree of nickel as the active material, and can maximize the activity of the catalyst, and improve the selectivity for olefins compared to the selectivity for aromatics.

[0078] According to the present invention, the content of the active material may be 50 parts by weight or more, preferably 50 to 70 parts by weight, and includes a second promoter and an active material, and may include 5 to 20 parts by weight of the second promoter relative to 100 parts by weight of the active material. That is, the weight ratio of the second promoter / active material is (5 to 20) / 100. Therefore, the nickel content is high, and sulfur can be used to increase the dispersion, thereby further improving the selectivity for olefins compared to the selectivity for aromatics.

[0079] When the active material content is less than 50 parts by weight, there is a disadvantage that the hydrogenation performance of the catalyst per unit mass is reduced, thus resulting in economic losses due to the increase in the amount of catalyst used to meet productivity.

[0080] In addition, when the weight ratio of the second promoter / (active substance+first promoter+second promoter) is less than 3 / 100 and the weight ratio of the second promoter / active substance is less than 5 / 100, the hydrogenation selectivity for olefins is significantly reduced compared with the hydrogenation selectivity for aromatics. Therefore, there is a disadvantage that it is difficult to constantly control the aromatic content. When the weight ratio of the second promoter / (active substance+first promoter+second promoter) is greater than 15 / 100 and the weight ratio of the second promoter / active substance is greater than 20 / 100, the hydrogenation performance for olefins is sharply reduced, and there is a disadvantage of reduced productivity.

[0081] According to the present invention, the average crystal size of the active material is 1 to 10 nm, more preferably 3 to 7 nm. When the average crystal size of the nickel is out of the above range, the problem of reduced catalyst activity will occur.

[0082] According to the present invention, the specific surface area of ​​the silica carrier is 200 to 400 m 2 / g, and has a pore size of 10 to 30 nm. This can improve the activity and catalyst life, and can optimally improve the efficiency of the separation process of the product and the catalyst.

[0083] According to the present invention, a silica carrier having a particle size, size distribution, surface area, pore structure, etc. suitable for the reaction and a catalyst falling within the above optimal combination range are provided.

[0084] According to the present invention, in the hydrogenation reaction, the selectivity for olefins is higher than that for aromatics. After the hydrogenation reaction of unsaturated hydrocarbons of the olefinic type, petroleum resins containing a portion of aromatics are more compatible with base polymers such as styrene-isoprene-styrene (SIS), styrene-butadiene-styrene (SBS) and the like than petroleum resins that do not contain such aromatics.

[0085] According to the present invention, the reactant of the hydrogenation reaction may be a petroleum resin. In this case, the petroleum resin may contain dicyclopentadiene (DCPD).

[0086] In addition, in the hydrogenation reaction, the reactant may be a petroleum resin containing a C5 fraction or a petroleum resin containing a C9 fraction. In addition, it may be a petroleum resin composed of a DCPD fraction byproduct and a combination thereof, or may be composed of cyclodiene and benzene functional groups, but is not limited thereto.

[0087] Due to the unsaturated bonds (olefins, aromatic unsaturated bonds) remaining after polymerization, the dicyclopentadiene (DCPD) has characteristics such as yellowing, bad odor, and easy oxidation in the air. Therefore, when the nickel-based catalyst of the present invention is used to carry out hydrogenation reaction under high temperature and high pressure conditions in order to improve the quality of petroleum resin, a colorless and odorless transparent water-white petroleum resin with improved thermal stability can be provided with unsaturated bonds removed.

[0088] The catalyst of the present invention may be in the form of powder, particles or granules, preferably powder.

[0089] The catalyst for hydrogenation reaction of the present invention has the characteristic that the APHA value of the petroleum resin after the hydrogenation reaction is completed is less than 30. APHA color is called Hazen scale or Pt / Coscale. As a color standard analysis method (ASTM D1209) named by the American Public Health Association, the color of hydrogenated petroleum resin is analyzed by APHA value. When the color of the petroleum resin is less than 30, it will become a water-white resin in which the color and smell of the petroleum resin almost disappear, and the residual olefin content (NMR% area) is less than 0.1%. Therefore, when the catalyst for hydrogenation reaction of the present invention is used, it can help to improve the selectivity for olefins compared with the selectivity for aromatics.

[0090] On the other hand, according to another embodiment of the present invention, a method for preparing the above-mentioned catalyst for hydrogenation reaction is provided.

[0091] According to the present invention, a method for preparing a catalyst for a hydrogenation reaction is provided, which comprises the following steps: step (a), dissolving 0.01 to 5 parts by weight of one or more promoters selected from copper and copper oxide and 10 to 40 parts by weight of a silica carrier in a solvent relative to 40 to 90 parts by weight of one or more active materials selected from nickel and nickel oxide to prepare a first solution; step (b), adding the first solution into a precipitation container, stirring, and heating to 60 to 100° C.; step (c), after the heating, adding a pH adjuster and 3 to 15 parts by weight of one or more promoters selected from sulfur and sulfur oxide into the precipitation container to prepare a second solution, and dropwise adding the second solution into the first solution to prepare a precipitate; step (d), washing and filtering the precipitate, and then drying it to prepare a dried product; and step (e), reducing the dried product in a hydrogen atmosphere at a temperature of 200 to 500° C. to prepare a reduced product.

[0092] In addition, the method may further include: after step (e), a step of passivating the catalyst.

[0093] There are two methods for the passivation step: First, passivation is performed using an oxygen-nitrogen mixed gas containing 0.1% to 20% oxygen, or the passivation step is performed by depositing into a solution containing an organic solvent such as petroleum resin.

[0094] When the gas is used for passivation, the % in the 0.1% to 20% oxygen contained represents volume %. As the organic solvent, for example, D40 Exxsol can be used. Any organic solvent can be used as long as it can block air.

[0095] In addition, according to the present invention, the method may further include: after step (d) and before the reduction in step (e), the step of firing the prepared dried product in an air atmosphere. The step of firing in an air atmosphere is not necessarily implemented, and a person skilled in the art may appropriately select the step as needed. At this time, the temperature is 200 to 500°C.

[0096] According to the present invention, the preparation of the precipitate in step (c) can be carried out by adding alkali or electrochemically in an environment with a pH value of 7 or above, and preferably the pH value is 7 to 9. At this time, in order to add alkali, an alkaline compound can be added, and the alkaline additive may include sodium carbonate, sodium hydroxide, sodium bicarbonate, ammonia or a hydrate thereof, but is not limited thereto, and preferably includes sodium carbonate or a hydrate thereof.

[0097] According to the present invention, there is provided a hydrogenation method, wherein a petroleum resin is contacted with hydrogen in the presence of a hydrogenation reaction catalyst prepared by the preparation method.

[0098] When hydrogenating petroleum resin, the temperature may be 100-400° C., preferably 200-300° C., and the pressure may be 1-200 bar, preferably 30-100 bar. The hydrogenation time mainly varies according to the temperature, the amount of catalyst and the degree of hydrogenation.

[0099] Furthermore, the hydrogenation reaction can be carried out in a variety of reactors, preferably in a continuous stirred reactor (CSTR) or a loop reactor. In addition, as mentioned above, the optimal activity can be exhibited when the reduction temperature is 200 to 500°C, preferably 350 to 450°C.

[0100] According to the present invention, in the hydrogenation reaction, the petroleum resin as a reactant contains dicyclopentadiene (DCPD). In addition, a petroleum resin containing a C5 fraction and a petroleum resin containing a C9 fraction can be provided.

[0101] In addition, after the petroleum resin is contacted with hydrogen and the hydrogenation reaction is completed, the APHA value is less than 30. In addition, in the hydrogenation reaction, the selectivity for olefins is higher than that for aromatics, and the aromatic / olefin hydrogenation ratio is 0.1 to 1.0.

[0102] Hereinafter, the constitution and function of the present invention will be described in more detail through the preferred embodiments of the present invention. This is only a preferred example of the present invention, and the present invention is not limited thereto regardless of any interpretation.

[0103] The contents not described here are parts that can be technically sufficiently inferred by a person skilled in the art, and thus the description thereof is omitted.

[0104] Example 1

[0105] The 40g has 310m 2 Porous silica powder with a surface area of ​​1.377 g and a pore size of 30 nm, 491 g of nickel sulfate, 6 g of copper sulfate and 2000 mL of distilled water were put into a precipitation container, stirred and heated to 80°C. After reaching 80°C, 1500 mL of a solution containing 262 g of sodium carbonate and 19.1 g of sodium sulfide was injected in 1 hour using a syringe pump. After precipitation, the pH value of the slurry was 7.6. After washing and filtering with about 30 L of distilled water, it was dried in a drying furnace at 100°C for more than 12 hours. After being divided into small portions, it was sintered at 400°C in an air atmosphere. After being divided into small portions again, it was reduced at 400°C in a hydrogen atmosphere. After reduction, the powder was passivated with an oxygen-nitrogen mixed gas containing 1% oxygen to prepare a hydrogenation catalyst.

[0106] It was measured that the active material content of the passivated catalyst was 74.6 parts by weight, the second promoter was 6.2 parts by weight, the first promoter was 0.95 parts by weight, and the average size of the nickel crystals was 4.4 nm based on the weight of the catalyst. 2 / g BET specific surface area, 0.32m 3 / g total pore volume, an average pore diameter of 5.2 nm, and a nickel (Ni) reduction degree analyzed by H2-TPR of 95%.

[0107] In the prepared catalyst, the weight ratio of the second promoter / (active substance+first promoter+second promoter) was 7.6 / 100, and the weight ratio of the second promoter / active substance was 8.3 / 100.

[0108] The hydrogenation reaction for testing the activity of the catalyst was carried out at a temperature of 230°C. The results are shown in Figure 1 middle.

[0109] Example 2

[0110] Using a syringe pump, 1500 mL of a solution containing 262 g of sodium carbonate as a precipitant and 22.5 g of sodium sulfide was injected in 1 hour to make the weight ratio of the second promoter / (active material+first promoter+second promoter) of the catalyst reach 9.2 / 100. After precipitation, the pH value of the slurry was 7.8.

[0111] The remaining steps including washing, filtering and drying were carried out in the same manner as in Example 1.

[0112] The active material content of the passivated catalyst was measured to be 74.0 parts by weight, the second promoter was 7.6 parts by weight, the first promoter was 0.97 parts by weight, and the average size of the nickel crystals was 4.5 nm, based on the weight of the catalyst. 2 / g BET specific surface area, 0.32m 3 / g total pore volume, an average pore diameter of 5.6nm. The nickel (Ni) reduction degree analyzed by H2-TPR was 97%. The weight ratio of the prepared second promoter / active material was 10.3 / 100.

[0113] The hydrogenation reaction for testing the activity of the catalyst was carried out at a temperature of 230°C. The results are shown in Figure 1 middle.

[0114] Example 3

[0115] Using a syringe pump, 1500 mL of a solution containing 262 g of sodium carbonate as a precipitant and 20.5 g of sodium sulfide was injected in 1 hour so that the weight ratio of the second promoter / (active substance+first promoter+second promoter) of the catalyst reached 6.5 / 100. After precipitation, the pH value of the slurry was 7.5. The remaining methods such as washing, filtering and drying were prepared in the same manner as in Example 1.

[0116] It was measured that the active material content of the passivated catalyst was 74.4 parts by weight, the weight of the second promoter was 5.3 parts by weight, the weight of the first promoter was 0.95 parts by weight, and the average size of the nickel crystals was 4.9 nm. 2 / g BET specific surface area, 0.34m 3 / g total pore volume, an average pore diameter of 5.7 nm, and a nickel (Ni) reduction degree analyzed by H2-TPR of 96%.

[0117] In the prepared catalyst, the weight ratio of the second promoter / (active substance+first promoter+second promoter) was 7.1 / 100.

[0118] The hydrogenation reaction for testing the activity of the catalyst was carried out at a temperature of 230°C. The results are shown in Figure 1 middle.

[0119] Comparative Example 1

[0120] A typical hydrogenation catalyst known to those skilled in the art for hydrogenation reactions was prepared in the same manner as in Example 1, but without the use of sodium sulfide.

[0121] It was measured that the active material content of the passivated catalyst was 78.6 parts by weight, the second promoter was 0.8 parts by weight, the first promoter was 1.02 parts by weight, and the average size of the nickel crystals was 3.8 nm based on the weight of the catalyst.

[0122] In the prepared catalyst, the weight ratio of the second promoter / (active substance+first promoter+second promoter) was 0.99 / 100, and the weight ratio of the second promoter / active substance was 1.02 / 100.

[0123] With 255m 2 / g BET specific surface area, 0.36m 3 / g total pore volume, an average pore diameter of 5.9 nm, and a nickel (Ni) reduction degree analyzed by H2-TPR of 85%.

[0124] The hydrogenation reaction for testing the activity of the catalyst was carried out at a temperature of 230°C. The results are shown in Figure 1 middle.

[0125] Table 1 below shows the constituent components of the catalyst compositions of Examples 1 to 3 and Comparative Example 1.

[0126]

Table 1

[0127]

[0128] Experimental Example 1 Catalyst Activity Test

[0129] A 300 mL autoclave was used, which included a hollow shaft stirrer and had a stirring speed of 1600 rpm. 30 wt% of non-hydrogenated petroleum resin was dissolved in Exxsol TM D40 to form a solution, at 230 ° C, 90 bar H2, to 75 g of the solution was added 1-2% (based on the mass of the petroleum resin) of catalyst (catalyst / DCPD resin), and hydrogenated for 1 hour. After hydrogenation, the color of the petroleum resin solution was measured according to ASTM D1209.

[0130] The color of the petroleum resin (APHA value, a standard for indicating the color of a solution), which is proportional to the olefin content in the petroleum resin, was 750 before hydrogenation, and the aromatic content (Aromaticity) was 18%.

[0131] Aromaticity was analyzed by 1H NMR.

[0132]

Table 2

[0133]

[0134]

[0135] Table 2 shows the results of the hydrogenation reaction carried out according to Experimental Example 1 under the conditions described in Table 2 above.

[0136] In the hydrogenation reaction result of Comparative Example 1, the aromatic / olefin hydrogenation ratio is high, so the olefin selectivity is low. It can be confirmed that when Examples 1 to 3 are used, although the APHA values ​​are similar, olefins are preferentially hydrogenated, so the aromatic content can be selectively adjusted. In addition, when the color of the petroleum resin is 30 or less, it will become a water-white resin. At this time, the residual olefin content (NMR% area) is less than 0.1%, which confirms that in the case of Examples 1 to 3, it can be used as an excellent catalyst that can provide a water-white petroleum resin through a hydrogenation reaction.

[0137] The present invention has been described above through specific matters such as specific constituent elements and limited embodiments, but this is only used to help a more comprehensive understanding of the present invention. The present invention is not limited to the above-mentioned multiple embodiments, and those skilled in the art can make various modifications and variations based on such descriptions.

[0138] Therefore, the concept of the present invention is not limited to the embodiments described above, and the attached claims and all modifications that are equivalent or equivalent to the claims belong to the scope of the concept of the present invention.

Claims

1. A catalyst for hydrogenation reaction, characterized in that The invention relates to 50 to 90 parts by weight of one or more active materials selected from nickel and nickel oxide, 0.5 to 3 parts by weight of one or more first promoters selected from copper and copper oxide, 3 to 15 parts by weight of one or more second promoters selected from sulfur and sulfur oxide, and 10 to 40 parts by weight of a silica carrier. In the hydrogenation reaction, the selectivity for olefins is higher than that for aromatics. The content of the second accelerator is 3 to 15 parts by weight relative to 100 parts by weight of the total of the active material, the first accelerator and the second accelerator. The content of the second accelerator is 5 to 20 parts by weight relative to 100 parts by weight of the active material.

2. The catalyst for hydrogenation reaction according to claim 1, characterized in that The crystal size of the active material is 3 to 8 nm.

3. The catalyst for hydrogenation reaction according to claim 1, characterized in that The silica carrier has a specific surface area of ​​200 to 400 m 2 / g and a porous carrier with a pore size of 10 to 30 nm.

4. The catalyst for hydrogenation reaction according to claim 1, characterized in that In the hydrogenation reaction, the reactant is petroleum resin.

5. The catalyst for hydrogenation reaction according to claim 4, characterized in that The petroleum resin is at least one selected from dicyclopentadiene, a petroleum resin containing a C5 fraction, and a petroleum resin containing a C9 fraction.

6. The catalyst for hydrogenation reaction according to claim 1, characterized in that The catalyst has at least one shape selected from the group consisting of powder, particle, and granular.

7. A method for preparing a catalyst for hydrogenation reaction, characterized in that: The steps include: Step (a), dissolving 0.01 to 5 parts by weight of one or more promoters selected from copper and copper oxide and 10 to 40 parts by weight of a silica carrier in a solvent relative to 50 to 90 parts by weight of one or more active materials selected from nickel and nickel oxide to prepare a first solution; Step (b), adding the first solution into a precipitation container, stirring, and heating to 60-100° C.; Step (c), after the temperature is raised, adding a pH adjuster and 3 to 15 parts by weight of one or more promoters selected from sulfur and sulfur oxide into a precipitation container to prepare a second solution, and adding the second solution dropwise to the first solution to prepare a precipitate; Step (d), washing and filtering the precipitate, and then drying it to prepare a dried product; as well as Step (e), reducing the dried product under a hydrogen atmosphere at a temperature of 200 to 500° C. to prepare a reduced product, In the hydrogenation reaction, the selectivity for olefins is higher than that for aromatics. The content of the second accelerator is 3 to 15 parts by weight relative to 100 parts by weight of the total of the active material, the first accelerator and the second accelerator. The content of the second accelerator is 5 to 20 parts by weight relative to 100 parts by weight of the active material.

8. The method for preparing a catalyst for hydrogenation reaction according to claim 7, characterized in that: Further including: After the step (e), the catalyst is subjected to a passivation step.

9. The method for preparing a catalyst for hydrogenation reaction according to claim 8, characterized in that: The passivation is performed using an oxygen-nitrogen mixed gas containing 0.1% to 20% oxygen.

10. The method for preparing a catalyst for hydrogenation reaction according to claim 8, characterized in that: The passivation is carried out in the form of deposition into a solution containing an organic solvent.

11. The method for preparing a catalyst for hydrogenation reaction according to claim 7, characterized in that: Further including: After the step (d), the prepared dried product is fired at 200 to 500° C. in an air atmosphere.

12. The method for preparing a catalyst for hydrogenation reaction according to claim 7, characterized in that: The preparation of the precipitate in step (c) is carried out at a pH value of 7-9.

13. A method for hydrogenating a petroleum resin, characterized in that: The petroleum resin is contacted with hydrogen in the presence of the catalyst prepared by the preparation method according to any one of claims 7 to 12.

14. The method for hydrogenating a petroleum resin according to claim 13, characterized in that: The petroleum resin includes at least one selected from dicyclopentadiene, a petroleum resin containing a C5 fraction, and a petroleum resin containing a C9 fraction.

15. The method for hydrogenating a petroleum resin according to claim 13, characterized in that: The aromatic / olefin hydrogenation ratio of the petroleum resin after hydrogenation reaction is 0.1-1.

0.

16. The method for hydrogenating a petroleum resin according to claim 13, characterized in that: The APHA value of the petroleum resin after hydrogenation is less than 30.